Semiconductor structure and method of manufacture thereof

The method of forming word lines in semiconductor structures through self-aligned deposition and etching processes addresses the challenges of precision and doping in GAA transistors, resulting in improved integration density and electrical performance.

JP7583164B2Active Publication Date: 2024-11-13CHANGXIN MEMORY TECH INC
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2023527715
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-01
Filing Date
2021-11-02
Publication Date
2024-11-13
Estimated Expiration
2041-11-02

AI Technical Summary

Technical Problem

The challenge in semiconductor manufacturing lies in forming small-sized word lines and semiconductor channels with high accuracy, particularly in GAA transistors, due to difficulties in etching precision and controlling doping concentrations, which affect the integration density and electrical performance of DRAMs.

Method used

A method is developed to form word lines without etching, by using self-aligned deposition and etching processes to create precise dimensions, ensuring high accuracy and simplifying the formation of word lines, while maintaining a junctionless transistor structure with uniform doping concentrations.

Benefits of technology

This approach allows for the formation of word lines with precise dimensions and improved integration density, reducing etching complexity and enhancing the electrical performance of semiconductor structures by avoiding etching-related inaccuracies and doping challenges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583164000001
    Figure 0007583164000001
  • Figure 0007583164000002
    Figure 0007583164000002
  • Figure 0007583164000003
    Figure 0007583164000003
Patent Text Reader

Abstract

The present disclosure discloses a semiconductor structure and a method for manufacturing the same, the method including the steps of: providing a base; forming a bit line on the base; and forming a semiconductor channel on a surface of the bit line away from the base, the semiconductor channel including a first doping region, a channel region, and a second doping region arranged in sequence; forming a first dielectric layer surrounding a sidewall of the semiconductor channel, wherein there is a first gap between the first dielectric layer located on the sidewall of adjacent semiconductor channels on the same bit line; forming a second dielectric layer filling the first gap with a material different from that of the first dielectric layer; removing a portion of the first dielectric layer until the sidewall of the channel region is exposed; forming an insulating layer covering at least the sidewall surface of the channel region, wherein there is a second gap between the insulating layer and the second dielectric layer; and forming a word line filling the second gap.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS-REFERENCE TO RELATED APPLICATIONS)

[0002] This application claims priority to a patent application filed with the China Patent Office on July 1, 2021, bearing application number 202110746053.8 and entitled "Semiconductor structure and manufacturing method thereof," the entire contents of which are incorporated herein by reference.

[0003] This disclosure relates to, but is not limited to, semiconductor structures and methods for their manufacture. [Background technology]

[0004] As semiconductor devices become increasingly more densely packed, researchers have begun to investigate ways to arrange transistors within the semiconductor structures and ways to reduce the size of individual functional devices within the semiconductor structures.

[0005] In the related art, the area occupied by a dynamic random access memory (DRAM) memory cell based on a saddle-type fin transistor is 6F2 (F is the minimum pattern size that can be obtained under a given process condition), and if the DRAM is scaled proportionally to further reduce the DRAM's area, problems such as the proximity gate effect will occur, which will adversely affect the electrical performance of the DRAM. If a vertical gate-all-around (GAA) transistor structure is used as an access transistor, the area occupied will be 4F2, which in principle can achieve higher density efficiency, but at some sizes, problems such as word line etching being difficult due to the constraints of the equipment and manufacturing process used in the manufacturing process exist. Summary of the Invention [Problem to be solved by the invention]

[0006] The following is a summary of the subject matter described in detail in this disclosure, which does not limit the scope of protection of the claims.

[0007] The embodiments of the present disclosure provide a semiconductor structure and a manufacturing method thereof that are advantageous for simplifying the word line formation process and for forming word lines and semiconductor channels with high size accuracy and small size. [Means for solving the problem]

[0008] In a first aspect of an embodiment of the present disclosure, a method for manufacturing a semiconductor structure is provided, the method including the steps of: providing a base; forming a bit line on the base; and forming a semiconductor channel on a surface of the bit line away from the base, the semiconductor channel including a first doping region, a channel region, and a second doping region arranged in sequence in a direction in which the base faces the bit line; forming a first dielectric layer surrounding a sidewall of the semiconductor channel, the first gap being between the first dielectric layer located on the sidewall of adjacent semiconductor channels on the same bit line; forming a second dielectric layer filling the first gap, the material of the second dielectric layer being different from the material of the first dielectric layer; removing a portion of the first dielectric layer until a sidewall of the channel region is exposed; forming an insulating layer covering at least a sidewall surface of the channel region, the second gap being between the insulating layer and the second dielectric layer; and forming a word line filling the second gap.

[0009] In a second aspect of the embodiment of the present disclosure, a semiconductor structure is provided, the semiconductor structure including a base, a bit line located on the base, a first doping region, a channel region, and a second doping region located on a surface of the bit line and arranged in order in a direction in which the base faces the bit line, the first doping region including a semiconductor channel in contact with the bit line, a first dielectric layer surrounding the first doping region, the first dielectric layer having a first gap between the first dielectric layer on sidewalls of adjacent first doping regions on the same bit line, an insulating layer covering at least a sidewall surface of the channel region, word lines surrounding the insulating layer located on the sidewalls of the channel region, the word lines having a second gap between adjacent word lines, and an isolation layer located at least in the first gap and the second gap, the upper surface of the isolation layer away from the base being base Away from Second doping region and an isolation layer not lower than the upper surface of the

[0010] Other aspects may be appreciated after reading and understanding the drawings and detailed description.

[0011] The drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the present disclosure and are used to interpret the principles of the embodiments of the present disclosure together with the description. In these drawings, similar reference numerals indicate similar components. The drawings in the following description are only some, but not all, embodiments of the present disclosure. Those skilled in the art can obtain other drawings based on these drawings without creative labor. [Brief description of the drawings]

[0012] [Figure 1] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Diagram 2] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Diagram 3]1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 4] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Diagram 5] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 6] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 7] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 8] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 9] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 10] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 11] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 12] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 13] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 14] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 15] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 16] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 17] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 18] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 19] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 20] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 21] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 22] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 23] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 24] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Diagram 25] 1A-1D are exemplary structural diagrams corresponding to steps in a method for manufacturing a semiconductor structure according to one embodiment of the present disclosure. [Figure 26] 5A-5C are exemplary structural diagrams corresponding to steps of a method for fabricating a semiconductor structure according to another embodiment of the present disclosure. [Figure 27] 5A-5C are exemplary structural diagrams corresponding to steps of a method for fabricating a semiconductor structure according to another embodiment of the present disclosure. [Figure 28] 5A-5C are exemplary structural diagrams corresponding to steps of a method for fabricating a semiconductor structure according to another embodiment of the present disclosure. [Figure 29] 5A-5C are exemplary structural diagrams corresponding to steps of a method for fabricating a semiconductor structure according to another embodiment of the present disclosure. [Diagram 30] 5A-5C are exemplary structural diagrams corresponding to steps of a method for fabricating a semiconductor structure according to another embodiment of the present disclosure. [Diagram 31] 5A-5C are exemplary structural diagrams corresponding to steps of a method for fabricating a semiconductor structure according to another embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the technical solutions of the embodiments of the present disclosure will be described clearly and completely in combination with the drawings of the embodiments of the present disclosure, but it is clear that the described embodiments are not all the embodiments of the present disclosure, but are only a part of the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by those skilled in the art without creative labor all belong to the scope of protection of the present disclosure. In addition, the embodiments and features of the embodiments of the present disclosure can be arbitrarily combined with each other without conflict.

[0014] The analysis revealed that when forming word lines surrounding the sidewalls of the channel region of the semiconductor channel in a GAA transistor, it is usually necessary to form multiple word lines separated from each other using two processes, deposition and etching. However, due to the high integration density and small spacing between adjacent semiconductor channels, it is difficult to control the etching accuracy in the process of forming word lines using an etching process, and therefore it is also difficult to control the size accuracy of the word lines. Furthermore, when the size of the GAA transistor is small, it is difficult to control the doping concentration in each region of the semiconductor channel when trying to form a vertical structure GAA junction transistor, which affects the yield of the PN junction that is finally formed.

[0015] The embodiment of the present disclosure provides a semiconductor structure and a method for manufacturing the same, in which a part of the first dielectric layer occupies the position of an insulating layer and a word line to be formed subsequently, and when the first dielectric layer located on the sidewall of the channel region is removed after the second dielectric layer is formed subsequently, the excess first dielectric layer is located on the sidewall of the first doped region, so that the excess first dielectric layer can protect the first doped region from being affected when the insulating layer is formed on the sidewall of the channel region, and when a second gap is formed between the insulating layer and the second dielectric layer, a word line having an accurate dimension can be formed in the second gap in a self-aligned manner, and a word line with high dimensional accuracy can be formed without an etching process, which is advantageous for simplifying the word line formation process, and a word line having a small size can be obtained by adjusting the size of the second gap. Furthermore, the doping concentrations of doping ions in the first doped region, the channel region, and the second doped region can be the same, so that the device formed by the semiconductor channel 105 is a junctionless transistor.

[0016] An embodiment of the present disclosure provides a method for manufacturing a semiconductor structure, and the method for manufacturing a semiconductor structure according to the embodiment of the present disclosure will be described in detail below in combination with the drawings. Figures 1 to 25 are exemplary structural diagrams corresponding to each step of the method for manufacturing a semiconductor structure according to the embodiment of the present disclosure. For convenience of explanation, in order to clearly show the steps of the method for manufacturing a semiconductor structure, all of Figures 1 to 25 in this embodiment are exemplary local structural diagrams of the semiconductor structure.

[0017] Referring to FIG. 1, a base 100 is provided, which in this embodiment includes a substrate 110, a buffer layer 120, and a protective layer 130 stacked on the substrate 110 in this order.

[0018] In this embodiment, providing the base 100 includes the following steps.

[0019] A substrate 110 is provided, and the material type of the substrate 110 can be an elemental semiconductor material or a crystalline inorganic compound semiconductor material. The elemental semiconductor material can be silicon or germanium, and the crystalline inorganic compound semiconductor material can be silicon carbide, silicon germanide, gallium arsenide, or indium gallium arsenide, etc.

[0020] The substrate 110 includes a semiconductor well layer 11 doped with a first type of ions and an initial semiconductor layer 10 disposed on the semiconductor well layer 11 .

[0021] The initial semiconductor layer 10 is subjected to a doping and annealing process to cause a second type of ion to be doped into the initial semiconductor layer 10, which is subsequently used to form bit lines and semiconductor channels beneath the initial semiconductor layer 10. The second type of ion is different from the first type of ion, and both the first type of ion and the second type of ion are either N-type ions or P-type ions. The N-type ions are at least one of arsenic ions, phosphorus ions, or antimony ions, and the P-type ions are at least one of boron ions, indium ions, or gallium ions.

[0022] The doping process can be performed by high-temperature diffusion or ion implantation. After the doping process is performed on the initial semiconductor layer 10 by ion implantation, the annealing temperature of the annealing process is 800°C to 1000°C.

[0023] In this embodiment, the second type ion doping concentration in the initial semiconductor layer 10 is 1×10 19 atom / cm 3 ~1×10 20 atom / cm 3and the doping depth of the second type ions in the initial semiconductor layer 10 is 150 nm to 250 nm in the direction in which the initial semiconductor layer 10 faces the semiconductor well layer 11. The first type ions are P-type ions and the second type ions are N-type ions. In other embodiments, the first type ions can be N-type ions and the second type ions can be P-type ions.

[0024] On one side of the initial semiconductor layer 10 away from the semiconductor well layer 11, a buffer layer 120 and a protective layer 130 are sequentially stacked to form the buffer layer 120 and the protective layer 130. In some examples, a deposition process may be used to form the buffer layer 120 and the protective layer 130, and the material of the buffer layer 120 is silicon oxide and the material of the protective layer 130 is silicon nitride.

[0025] Silicon nitride can be deposited using a chemical vapor deposition process to form the protective layer 130, which is advantageous in protecting the substrate 110 located below the silicon nitride film layer and preventing the substrate 110 from being oxidized because the oxidation rate of the silicon nitride film layer is very slow.

[0026] In some examples, the substrate 110 is a silicon substrate, and the mismatch between the lattice constant and thermal expansion coefficient of silicon nitride and the lattice constant and thermal expansion coefficient of silicon substrate is very large, so that when silicon nitride is directly formed on the silicon substrate, the defect density is large at the interface between silicon nitride and silicon, which is prone to carrier traps and complex centers, affecting the carrier mobility of silicon, and thus affecting the performance and operating life of the semiconductor structure. The stress of silicon nitride film is large, and it is prone to crack phenomenon when directly deposited on the silicon substrate. Before depositing silicon nitride on the silicon substrate, silicon oxide is first deposited as a buffer layer 120, which is advantageous to improve the performance and operating life of the conductor structure.

[0027] 1 to 4, a bit line 104 is formed on a base 100, and a semiconductor channel 105 is formed on a surface of the bit line 104 away from the base 100, and in a direction Z in which the base 100 faces the bit line 104, the semiconductor channel 105 includes a first doping region I, a channel region II, and a second doping region III arranged in sequence.

[0028] In this embodiment, the steps of forming the bit line 104 and the semiconductor channel 105 include the following steps.

[0029] Referring to FIG. 1, a first mask layer 102 having a plurality of first openings b separated from each other is formed on a base 100, and the length of the first openings b along an extension direction X of the first openings b corresponds to the length of a bit line to be subsequently formed.

[0030] 2, the base 100 is etched using the first mask layer 102 as a mask to form a plurality of first trenches a, and the first mask layer 102 is then removed.

[0031] In this embodiment, the depth of the first trench a is 250 nm to 300 nm in the direction Z perpendicular to the surface of the base 100. Since the depth of the first trench a is greater than the doping depth of the second type ions in the initial semiconductor layer 10, it is advantageous to ensure complete etching of the initial semiconductor layer 10 doped with the second type ions, and it is easy to subsequently form a semiconductor channel and a bit line with a high doping concentration of the second type ions.

[0032] Referring to FIG. 3, a fifth dielectric layer 153 is formed in the first trench a.

[0033] In this embodiment, the following process can be adopted to form the fifth dielectric layer 153. A deposition process is performed to form a fifth dielectric film covering and filling the upper surface of the protective layer 130, and a chemical mechanical planarization process is performed on the fifth dielectric film until the upper surface of the protective layer 130 is exposed, and the excess fifth dielectric film is used as the fifth dielectric layer 153. The material of the fifth dielectric film includes silicon oxide.

[0034] A second mask layer 112 having a plurality of second openings c separated from each other is formed on an upper surface commonly formed by the fifth dielectric layer 153 and the excess base 100, and the length of the second openings c along the extension direction Y of the second openings c coincides with the length of the word lines to be formed subsequently.

[0035] 1 and 3 in combination, in this embodiment, the extension direction X of the first opening b is perpendicular to the extension direction Y of the second opening c, so that the subsequently formed semiconductor channel has a 4F2 configuration, which is favorable for further improving the integration density of the semiconductor structure. In another embodiment, the extension direction of the first opening intersects with the extension direction of the second opening, and the included angle between them may be 90°.

[0036] The ratio of the opening width of the first opening b in the direction Y to the opening width of the second opening c in the direction X is 2 to 1, so as to ensure that a through hole exposing the first dielectric layer surrounding the sidewall of the channel region II can be subsequently formed, which is advantageous for forming a second gap for manufacturing a word line. In some examples, the opening width of the first opening b in the direction Y is equal to the opening width of the second opening c in the direction X, and the spacing between adjacent first openings b is equal to the spacing between adjacent second openings c, which is advantageous for, on the one hand, aligning a plurality of semiconductor channels to be subsequently formed to further improve the integration density of the semiconductor structure, and, on the other hand, reducing the manufacturing cost of the semiconductor structure, since the first mask layer 102 and the second mask layer 112 can be formed by the same mask plate.

[0037] In this embodiment, the methods of forming the first mask layer 102 and the second mask layer 112 both include Self-Aligned Quadruple Patterning (SAQP) or Self-Aligned Double Patterning (SADP).

[0038] Referring to FIG. 4, the base 100 (see FIG. 1) and the fifth dielectric layer 153 are etched using the second mask layer 112 as a mask to form a plurality of second trenches d, bit lines 104 and semiconductor channels 105. In the direction Z perpendicular to the surface of the base 100, the depth of the second trenches d is smaller than the depth of the first trenches a, which is advantageous for forming the bit lines 104 and forming a plurality of semiconductor channels 105 separated from each other on one side of the bit lines 104 away from the semiconductor well layer 11, and the bit lines 104 contact the first doping regions I of the semiconductor channels 105, and the second mask layer 112 is removed.

[0039] In some examples, the depth of the second trench d is between 100 nm and 150 nm, and the doping depth of the second type of ions in the initial semiconductor layer 10 (see FIG. 1 ) is between 150 nm and 250 nm, which is advantageous for converting most or all of the initial semiconductor layer 10 doped with the second type of ions into the semiconductor channel 105 by two etchings.

[0040] The material of the substrate 110 is silicon, and the material of the fifth dielectric layer 153 is silicon oxide. In the process of etching the base 100 and the fifth dielectric layer 153 using the second mask layer 112 as a mask, the etching rate of silicon oxide is higher than the etching rate of silicon in the etching process, so that a portion of the sidewall of the bit line 104 may be exposed.

[0041] In this embodiment, a plurality of bit lines 104 arranged at intervals may be formed on the semiconductor well layer 11, and each bit line 104 may contact at least one first doping region I. In FIG. 4, four bit lines 104 are arranged at intervals from each other, and each bit line 104 contacts four first doping regions I. The number of bit lines 104 and the number of first doping regions I contacting each bit line 104 may be reasonably set according to actual electrical requirements.

[0042] In order to achieve electrical isolation between adjacent bit lines 104 and adjacent semiconductor channels 105, after etching the base 100 and the fifth dielectric layer 153 using the second mask layer 112 as a mask, an excess of the fifth dielectric layer 153 is further disposed in the spaces between adjacent bit lines 104 and in the spaces between adjacent semiconductor channels 105.

[0043] In this embodiment, since the initial semiconductor layer 10 (see FIG. 1) is doped with N-type ions, the bit line 104 and the semiconductor channel 105 formed in this step can be doped with N-type ions.

[0044] The bit line 104 is doped with N-type ions and the semiconductor well layer 11 is doped with P-type ions, so that the bit line 104 and the semiconductor well layer 11 form a PN junction, which is beneficial to prevent leakage of the bit line 104 and further improve the electrical performance of the semiconductor structure. In other embodiments, the base does not include a semiconductor well layer, i.e., the base is the initial semiconductor layer and the bit line is located at the surface of the initial semiconductor layer.

[0045] The device formed by the semiconductor channel 105 is a junctionless transistor, i.e. the type of doping ions in the first doping region I, the channel region II and the second doping region III are the same. For example, the doping ions may all be N-type ions, and further the doping ions in the first doping region I, the channel region II and the second doping region III may be similar. "Junctionless" here means that there is no PN junction, i.e. the transistor formed by the semiconductor channel 105 has no PN junction, i.e. the doping concentration of the doping ions in the first doping region I, the channel region II and the second doping region III are the same. This has the following advantages: On the one hand, there is no need to perform additional doping on the first doping region I and the second doping region III, thereby avoiding the problem of the difficulty of controlling the doping process on the first doping region I and the second doping region III, especially as the transistor size is further reduced, if additional doping is performed on the first doping region I and the second doping region III, it becomes even more difficult to control the doping concentration; on the other hand, since the device is a junctionless transistor, it is advantageous to adopt an ultra-steep source-drain concentration gradient doping process to avoid the phenomenon of manufacturing an ultra-steep PN junction in the nanoscale range, which can avoid problems such as threshold voltage drift and increased leakage current caused by doping abrupt change, and is also advantageous to suppress the short channel effect, and can still operate within a few nanoscale range, thereby contributing to further improving the integration density and electrical performance of the semiconductor structure. The additional doping here refers to doping performed to make the doping ion type of the first doping region I and the second doping region III different from the doping ion type of the channel region II.

[0046] A GAA transistor that forms a semiconductor channel 105 vertically on the top surface of the bit line 104 away from the semiconductor well layer 11 can form a 3D stacked semiconductor structure, which is advantageous for establishing a GAA transistor with smaller size features to improve the integration density of the semiconductor structure without adversely affecting the electrical performance of the GAA transistor.

[0047] In this embodiment, the first mask layer 102 and the second mask layer 112 are used to simultaneously form the bit line 104 and the semiconductor channel 105 through two etching processes, which, on the one hand, adjusts the size of the semiconductor channel 105 by adjusting the size of the first opening b and the second opening c to form the semiconductor channel 105 with high dimensional accuracy; on the other hand, the bit line 104 and the semiconductor channel 105 are both formed by etching the substrate 110, that is, the bit line 104 and the semiconductor channel 105 are formed with the same film layer structure, so that the bit line 104 and the semiconductor channel 105 are integrated into one structure, thereby improving the interface state defects between the bit line 104 and the semiconductor channel 105 and improving the performance of the semiconductor structure. After etching the base 100 using the first mask layer 102 as a mask, a fifth dielectric layer 153 is further formed in the first trench a to prepare for the subsequent formation of a gap between the sidewall of the channel region II and the second dielectric layer, which is advantageous for forming a second gap for the subsequent fabrication of the word line.

[0048] 5 to 8, a first dielectric layer 113 is formed surrounding the sidewalls of the semiconductor channel 105, and a first gap e is formed between the first dielectric layers 113 located on the sidewalls of adjacent semiconductor channels 105 on the same bit line 104.

[0049] Fig. 7 is an exemplary cross-sectional view along the first cross-sectional direction AA1 of the structure shown in Fig. 6, and Fig. 8 is an exemplary cross-sectional view along the second cross-sectional direction BB1 of the structure shown in Fig. 6. Note that, as necessary for the following description, one or both of the exemplary cross-sectional view along the first cross-sectional direction AA1 and the exemplary cross-sectional view along the second cross-sectional direction BB1 are set, and when only one drawing is referred to, the drawing is an exemplary cross-sectional view along the first cross-sectional direction AA1, and when two drawings are referred to simultaneously, the drawing is first an exemplary cross-sectional view along the first cross-sectional direction AA1, and then an exemplary cross-sectional view along the second cross-sectional direction BB1.

[0050] In this embodiment, the step of forming the first dielectric layer includes the following steps.

[0051] Referring to FIG. 5, a sixth dielectric film 103 is formed conformally covering the sidewalls and bottom of the second trench d, and is further disposed on the top surfaces of a protective layer 130 and a fifth dielectric layer 153 .

[0052] Referring to Figures 5 and 6 in combination, a maskless dry etching process is performed on the sixth dielectric film 103 until the protective layer 130 is exposed, and a sixth dielectric layer 163 is formed by utilizing the fact that the thicknesses etched in different areas of the sixth dielectric film 103 by the etching process are the same within the same etching time.

[0053] 6 to 8 in combination, the sixth dielectric layer 163 is located on the sidewall of the second trench d, the fifth dielectric layer 153 is located in the space between adjacent semiconductor channels 105, the fifth dielectric layer 153 and the sixth dielectric layer 163 together constitute the first dielectric layer 113, and there is a first gap e between the sixth dielectric layers 163 located on the sidewall of the second trench d.

[0054] The material of the sixth dielectric layer 163 is the same as that of the fifth dielectric layer 153, and the sixth dielectric layer 163 and the fifth dielectric layer 153 corresponding to the sidewall of the channel region II can be easily removed together by a subsequent etching process, thereby forming a gap between the sidewall of the channel region II and the second dielectric layer to be formed subsequently, which is advantageous for forming a second gap for manufacturing the subsequent word line. The material of the sixth dielectric layer 163 and the material of the fifth dielectric layer 153 are all silicon oxide.

[0055] In another embodiment, the material of the sixth dielectric layer may be different from that of the fifth dielectric layer, as long as the material of the sixth dielectric layer and the material of the fifth dielectric layer are materials with good insulating effect. Then, the sixth dielectric layer and the fifth dielectric layer corresponding to the sidewall of the channel region can be removed step by step.

[0056] 7 and 9 in combination, a second dielectric layer 123 is formed to fill the first gap e, and the material of the second dielectric layer 123 is different from the material of the first dielectric layer 113.

[0057] In some examples, the following steps can be adopted to form the second dielectric layer 123. A deposition step is performed to form a second dielectric film covering the upper surface of the protective layer 130 and filling the first gap e, and a chemical mechanical planarization process is performed on the second dielectric film, the protective layer 130, the buffer layer 120 and the first dielectric layer 113 (see FIG. 6) until the upper surface of the second doping region III is exposed, and the excess of the second dielectric film is used as the second dielectric layer 123. The material of the second dielectric film includes silicon nitride.

[0058] 10 to 17, a portion of the first dielectric layer 113 is removed until the sidewall of the channel region II is exposed.

[0059] In some examples, removing portions of the first dielectric layer 113 until the sidewalls of the channel region II are exposed includes the following steps.

[0060] 9 and 10 in combination, a portion of the first dielectric layer 113 is etched using the semiconductor channel 105 and the second dielectric layer 123 as a mask until a sidewall of the second doping region III is exposed. In some examples, the height of the second doping region III is 30 nm to 50 nm in a direction Z perpendicular to the bit line 104 and oriented toward the semiconductor channel 105.

[0061] 11 to 14, FIG. 12 is an exemplary plan view of FIG. 11, FIG. 13 is an exemplary cross-sectional view along the third cross-sectional direction CC1, and FIG. 14 is an exemplary cross-sectional view along the second cross-sectional direction BB1.

[0062] A third dielectric layer 133 is formed to surround the sidewall of the second doping region III and to be located on the sidewall of the second dielectric layer 123, and the third dielectric layer 133 located on the sidewall of the second doping region III and the third dielectric layer 133 located on the sidewall of the second dielectric layer 123 commonly surround each other to form a through hole f whose bottom exposes the first dielectric layer 113, and the material of the third dielectric layer 133 is different from the material of the first dielectric layer 113.

[0063] 13 and 14, the third dielectric layer 133 surrounds the sidewall of the second doping region III and covers the upper surface of the sixth dielectric layer 163 and part of the upper surface of the fifth dielectric layer 153, and the through hole f is exposed from part of the upper surface of the fifth dielectric layer 153.

[0064] In this embodiment, the following steps can be adopted to form the third dielectric layer 133. A deposition step is performed to form a third dielectric film conformally covering the surface commonly composed of the semiconductor channel 105, the first dielectric layer 113 and the second dielectric layer 123, a maskless dry etching step is performed on the third dielectric film until the top surface of the second doping region III is exposed, and the third dielectric layer 133 exposing the first dielectric layer 113 is formed by utilizing the fact that the thicknesses etched by the etching step in different regions of the third dielectric film are the same within the same etching time. The material of the third dielectric layer 133 includes silicon nitride.

[0065] In the above-mentioned first mask layer 102 and second mask layer 112, the ratio of the opening width of the first opening b in the direction Y to the opening width of the second opening c in the direction X is 2 to 1, which is advantageous to ensure that, when forming the third dielectric layer 133, the third dielectric layer 133 fills the gap between adjacent semiconductor channels 105 on the same bit line 104 but does not fill the gap between adjacent semiconductor channels 105 on adjacent bit lines 104, thereby ensuring the formation of a through hole f exposing a part of the upper surface of the fifth dielectric layer 153, and making it easy to subsequently remove a part of the first dielectric layer 113 using the through hole f.

[0066] 15 to 17, the first dielectric layer 113 located on the sidewall of the channel region II where the through hole f is exposed is removed, and the excess first dielectric layer 113 surrounds the sidewall of the first doping region I.

[0067] Since the through hole f exposes a portion of the upper surface of the first dielectric layer 113, when the material of the first dielectric layer 113 is different from the materials of the second dielectric layer 123 and the third dielectric layer 133, an etching solution can be injected into the through hole f to perform a wet etching process to remove the first dielectric layer 113 located on the sidewall of the channel region II and leave the first dielectric layer 113 located on the sidewall of the first doping region I.

[0068] The second dielectric layer 123 and the third dielectric layer 133 together constitute a supporting skeleton, which is in contact with and connected to the second doping region III, and a part of the supporting skeleton is embedded in the first dielectric layer 113. In the step of performing the wet etching process, on the one hand, the supporting skeleton plays a role in supporting and fixing the semiconductor channel 105, and generates a pressing force against the semiconductor channel 105 when the etching solution flows, which is advantageous to avoid the inclination or deviation of the semiconductor channel 105 due to the pressing force so as to improve the stability of the semiconductor structure, and on the other hand, the supporting skeleton wraps around the sidewall of the second doping region III, which is advantageous to avoid the damage of the second doping region III caused by the etching solution.

[0069] After removing the first dielectric layer 113 located on the sidewall of the channel region II, a third gap g is formed between the channel region II and the second dielectric layer 123, and the through hole f and the third gap g together form a cave structure h.

[0070] 18 and 19, an insulating layer 106 is formed to cover at least the sidewall surface of the channel region II, and a second gap i is formed between the insulating layer 106 and the second dielectric layer 123. Referring to FIG. 19, the second gap i is also located between the insulating layers 106 on the sidewalls of the semiconductor channels 105 of adjacent bit lines 104.

[0071] In this embodiment, since the material of the semiconductor channel 105 is silicon, the step of forming the insulating layer 106 includes the step of performing a thermal oxidation process on the sidewall of the exposed channel region II to form the insulating layer 106, which covers the sidewall surface of the excess channel region II. The material of the insulating layer 106 is silicon oxide. In another embodiment, the insulating layer covering the sidewall surface of the channel region can also be formed by a deposition process.

[0072] By performing a thermal oxidation process on the exposed sidewall of the channel region II, a part of the area of ​​the channel region II is converted into an insulating layer 106, so that the orthogonal projection of the channel region II on the bit line 104 is smaller than the orthogonal projection of the second doping region III on the bit line 104 and is smaller than the orthogonal projection of the first doping region I on the bit line 104, which is advantageous for forming a channel region II with a smaller cross-sectional area in a cross section perpendicular to the direction Z in which the bit line 104 faces the semiconductor channel 105 without adopting an etching process, and is advantageous for improving the control ability of the subsequently formed word line to the channel region II, thereby making it easier to control the on / off of the GAA transistor.

[0073] In some examples, in a cross section perpendicular to the direction Z, the width W and the length L of the channel region II are 10 nm or less, which is advantageous for ensuring good controllability of the subsequently formed word lines to the channel region II. In the direction Z, the height of the channel region II is 30 nm to 50 nm.

[0074] Since the top surface of the second doping region III is exposed, a part of the region adjacent to the top surface of the second doping region II is also converted into the insulating layer 106 during the thermal oxidation process. In this embodiment, the insulating layer 106 located on the top surface of the excess second doping region III is removed in a subsequent process. In another embodiment, after the thermal oxidation process, the insulating layer located on the top surface of the excess second doping region may be removed, leaving only the insulating layer covering the sidewall surface of the excess channel region.

[0075] 18 and 19, the orthogonal projection of the outer periphery of the insulating layer 106 on the bit line 104 is smaller than the orthogonal projection of the outer periphery of the third dielectric layer 133 on the bit line 104, i.e., the outer wall of the insulating layer 106 away from the semiconductor channel 105 is closer to the semiconductor channel 105 than the outer wall of the third dielectric layer 133 away from the semiconductor channel 105, thereby ensuring a second gap i between the insulating layer 106 and the second dielectric layer 123 so that the subsequent word line can surround the insulating layer 106 located on the sidewall of the channel region II. The outer wall of the insulating layer 106 away from the semiconductor channel 105 may be closer to the semiconductor channel 105 than the outer wall of the first dielectric layer 113 (see FIG. 15) away from the semiconductor channel 105.

[0076] 20 and 22, FIG. 22 is a partial cross-sectional view of one word line 107 of FIG. 21 surrounding four semiconductor channels 105.

[0077] A word line 107 is formed filling the second gap i.

[0078] In this embodiment, the step of forming the word line 107 includes a step of forming an initial word line filling the second gap i and the through hole f. The initial word line is located between the insulating layer 106 and the second dielectric layer 123, and is located between the insulating layer 106 on the sidewall of the adjacent channel region II on the adjacent bit line 104, the initial word line located in the through hole f is removed, and the excess initial word line is used as the word line 107. The initial word line can be formed by a deposition process, and the material of the initial word line includes at least one of polysilicon, titanium nitride, tantalum nitride, copper, or tungsten.

[0079] The initial word line fills the cave structure h (see FIG. 15) in a self-aligned manner, and after removing the initial word line located in the through hole f, it is advantageous to form the word line 107 of accurate dimensions in a self-aligned manner without the need to design the dimensions of the word line 107 through an etching process, which is advantageous to simplify the formation process of the word line 107, and by adjusting the size of the second gap i, a small-sized word line 107 can be obtained.

[0080] Referring to FIG. 23, after the word lines 107 are formed, a fourth dielectric layer 143 is further formed to fill the through holes f (see FIG. 21).

[0081] In this embodiment, the following process can be adopted to form the fourth dielectric layer 143. A deposition process is performed to form a fourth dielectric film covering the upper surface of the insulating layer 106 located on the upper surface of the second doping region III and filling the through hole f, and the fourth dielectric film is chemically mechanically planarized until the upper surface of the insulating layer 106 is exposed, and the excess fourth dielectric film is used as the fourth dielectric layer 143. The fourth dielectric film is similar to the material of the second dielectric layer and the third dielectric layer, both of which include silicon nitride. In another embodiment, the fourth dielectric film can be chemically mechanically planarized until the upper surface of the second doping region is exposed, i.e., the insulating layer located on the upper surface of the second doping region is synchronously removed, and the excess fourth dielectric film can be used as the fourth dielectric layer.

[0082] 23 to 25, the insulating layer 106 located on the upper surface of the second doping region III is removed, and an epitaxial growth process is adopted to form a capacitor contact layer 108 on the upper surface of the second doping region III, such that the orthogonal projection of the capacitor contact layer 108 on the bit line 104 covers the orthogonal projection of the second doping region III on the bit line 104.

[0083] On the one hand, the epitaxial growth process is advantageous for improving the continuity between the second doping region III and the capacitor contact layer 108, reducing contact defects caused by differences in lattice properties and lattice misalignment, reducing the contact resistance caused by contact defects, improving the carrier transmission ability and movement speed, and further improving the conductivity between the second doping region III and the capacitor contact layer 108, thereby reducing the heat generation during the operation of the semiconductor structure; on the other hand, the epitaxial growth process is advantageous for increasing the orthogonal projection of the capacitor contact layer 108 on the bit line 104, so that when the lower electrode of the capacitive structure is subsequently formed on the capacitor contact layer 108, the contact area between the capacitor contact layer 108 and the lower electrode is increased, thereby reducing the contact resistance between the capacitor contact layer 108 and the lower electrode.

[0084] In the step of the epitaxial growth process, the capacitor contact layer 108 is doped with the same type of doping ions as the second doping region III, and the doping concentration of the doping ions in the capacitor contact layer 108 is greater than the doping concentration of the doping ions in the second doping region III, so that the resistance of the capacitor contact layer 108 is smaller than the resistance of the second doping region III, which is favorable for further reducing the transmission resistance between the second doping region III and the lower electrode.

[0085] A capacitive structure (not shown) is formed on the surface shared by the capacitor contact layer 108 and the fourth dielectric layer 143 .

[0086] In another embodiment, after forming the word lines, a wet etching process is adopted to remove the second dielectric layer and the third dielectric layer to form a fourth gap exposing the entire surface of the word lines and the first dielectric layer, and a deposition process is adopted to form a seventh dielectric layer filling the fourth gap, and since the seventh dielectric layer is an integral structure, the seventh dielectric layer has high density and few internal defects, which is favorable for enhancing the isolation effect of the seventh dielectric layer between adjacent semiconductor channels and adjacent bit lines. The material of the seventh dielectric layer may be the same as the material of the second dielectric layer, and in some examples, the material of the seventh dielectric layer and the material of the second dielectric layer are both silicon nitride.

[0087] In another embodiment, the capacitor contact layer may not be formed, and the capacitive structure may be formed directly on the top surface of the second doped region after removing the insulating layer located on the top surface of the second doped region.

[0088] In summary, by forming the first dielectric layer 113 and the second dielectric layer 123, the second dielectric layer 123 is used as a mask to etch the first dielectric layer 113 to form a cave structure h, and a deposition process is adopted to form the word line 107 with an accurate dimension in a self-aligned manner to the cave structure h without the need to design the dimension of the word line 107 through an etching process, which is advantageous to simplify the formation process of the word line 107, and a small size of the word line 107 can be obtained by adjusting the size of the second gap i.

[0089] The present disclosure further provides a method for manufacturing a semiconductor structure, which is substantially the same as the above-mentioned embodiment, except that the step of removing a portion of the first dielectric layer until the sidewall of the channel region is exposed is different. Hereinafter, a method for manufacturing a semiconductor structure according to another embodiment of the present disclosure will be described in detail in combination with the drawings, and the same or corresponding parts as the above-mentioned embodiment may refer to the detailed description of the above-mentioned embodiment.

[0090] 26 to 31 are exemplary structural diagrams corresponding to each step of the manufacturing method of the semiconductor structure according to another embodiment of the present disclosure. For convenience of explanation, in order to clearly show the steps of the manufacturing method of the semiconductor structure, all of FIGS. 26 to 31 in this embodiment are exemplary local structural diagrams of the semiconductor structure, and one or both of an exemplary cross-sectional view along the first cross-sectional direction AA1 and an exemplary cross-sectional view along the second cross-sectional direction BB1 in the structure are set as necessary for subsequent explanation. When only one drawing is referred to, the drawing is an exemplary cross-sectional view along the second cross-sectional direction BB1, and when two drawings are referred to simultaneously, the drawing is first an exemplary cross-sectional view along the first cross-sectional direction AA1, and then an exemplary cross-sectional view along the second cross-sectional direction BB1.

[0091] 26 and 27, in this embodiment, a bit line 204 and a semiconductor channel 205 are formed on a base, a first dielectric layer 213 and a second dielectric layer 223 are formed, the base has a semiconductor well layer 21, and the first dielectric layer 213 includes a fifth dielectric layer 253 and a sixth dielectric layer 263. The steps of forming the bit line 204, the semiconductor channel 205, the first dielectric layer 213 and the second dielectric layer 223 are similar to those of the above-mentioned embodiment, and therefore will not be repeated here.

[0092] Referring to FIG. 27, the process of removing a portion of the first dielectric layer 213 until the sidewall of the channel region II is exposed includes a process of removing the first dielectric layer 213 located on the sidewall of the second doping region III, i.e., the excess first dielectric layer 213 is located only on the sidewall surface of the first doping region I.

[0093] 28 and 29, an insulating layer 206 is formed, which not only covers the sidewall surface of the channel region II, but also is located on the sidewall surface and upper surface of the second doping region III, and has a second gap i between the insulating layer 206 and the second dielectric layer 223.

[0094] In this embodiment, since the material of the semiconductor channel 205 is silicon, the step of forming the insulating layer 206 includes thermally oxidizing the exposed sidewalls of the channel region II and the sidewalls and top surface of the second doping region III to form the insulating layer 206, which covers the sidewall surfaces of the excess channel region II and the excess second doping region III. In another embodiment, the insulating layer covering the sidewalls of the channel region and the sidewalls and top surface of the second doping region can also be formed by a deposition process.

[0095] By subjecting the exposed sidewalls of the channel region II and the second doping region III to thermal oxidation treatment, a part of the area of ​​the channel region II and the second doping region III is converted into an insulating layer 206, so that the orthogonal projections of the channel region II and the second doping region III on the bit line 204 are all smaller than the orthogonal projections of the first doping region I on the bit line 204, which forms the channel region II and the second doping region III with smaller cross-sectional areas in a cross section perpendicular to the direction Z in which the bit line 204 faces the semiconductor channel 205 without adopting an etching process, which is advantageous for lowering the threshold voltage of the transistor formed by the semiconductor channel 205, and realizing the transistor to be turned on / off at a low threshold voltage.

[0096] In some examples, in a cross section perpendicular to the direction Z, the width W of the channel region II and the length of the channel region II are 10 nm or less, which is advantageous for ensuring a small threshold voltage of the transistor. In the direction Z, the height of the channel region II is 30 nm to 50 nm.

[0097] In this embodiment, the insulating layer 206 located on the upper surface of the excess second doping region III is removed in a subsequent process. In another embodiment, after the thermal oxidation process, the insulating layer located on the upper surface of the excess second doping region may be removed, and only the insulating layer covering the excess channel region and the sidewall surface of the excess second doping region may be left.

[0098] 30 and 31, the word line 207 is formed. The process of forming the word line 207 includes the following steps.

[0099] An initial word line is formed filling the second gap i (see FIG. 29), i.e., the initial word line is located between the insulating layer 206 on the sidewall of the channel region II and the second doping region III on the adjacent bit line 204. The initial word line can be formed by a deposition process.

[0100] A part of the initial word line is removed, and the remaining initial word line is used as the word line 207, which surrounds the insulating layer 206 located on the sidewall of the channel region II.

[0101] Since the initial word lines fill the second gaps i in a self-aligned manner, it is advantageous to subsequently form word lines 207 of accurate dimensions in a self-aligned manner without the need to design the dimensions of the word lines 207 through an etching process, which is advantageous in simplifying the process of forming the word lines 207, and by adjusting the size of the second gaps i, it is possible to obtain word lines 207 of a small size.

[0102] A fourth dielectric layer is formed to fill the gap between the insulating layers 206 located on the sidewalls of the second doping regions III, and then the insulating layer 206 located on the top surface of the second doping regions III is removed. The process of forming the fourth dielectric layer and removing a part of the insulating layer 206 is similar to the process of the above-mentioned embodiment. In another embodiment, before forming the fourth dielectric layer, the insulating layer located on the sidewalls and top surface of the second doping regions may be removed, and then the fourth dielectric layer exposing the top surface of the first doping region may be formed.

[0103] In this embodiment, a capacitor contact layer and a capacitance structure may be formed on the top surface of the second doping region III, and the process of forming the capacitor contact layer and the capacitance structure is similar to the process of the above-mentioned embodiment.

[0104] In summary, by forming the first dielectric layer 213 and the second dielectric layer 223, the second dielectric layer 223 is used as a mask to etch the first dielectric layer 213 to form the second gap i, and a deposition process is adopted to form the word line 207 with an accurate dimension in the second gap i in a self-aligned manner without the need to design the dimension of the word line 207 through an etching process, which is advantageous to simplify the formation process of the word line 207, and a small size of the word line 207 can be obtained by adjusting the size of the second gap i.

[0105] The present disclosure further provides a semiconductor structure, manufactured by a method for manufacturing a semiconductor structure according to any of the embodiments described above.

[0106] 24 and 25, the semiconductor structure includes a base including a semiconductor well layer 11, a bit line 104 located on the semiconductor well layer 11, and a first doping region I, a channel region II and a second doping region III located on the surface of the bit line 104 and arranged in order in a direction Z in which the base faces the bit line 104, and the first doping region I includes a semiconductor channel 105 in contact with the bit line 104.

[0107] In this embodiment, the base, bit line 104 and semiconductor channel 105 are made of the same semiconductor element In the case where the semiconductor channel 105 and the bit line 104 have a element Since the semiconductor channel 105 and the bit line 104 are formed of the same film layer structure, the semiconductor channel 105 and the bit line 104 are an integral structure, which improves interface state defects between the semiconductor channel 105 and the bit line 104 and enhances the performance of the semiconductor structure.

[0108] semiconductor element may include at least one of silicon, carbon, germanium, arsenic, gallium, indium. The material type of the base, the bit line 104 and the semiconductor channel 105 may be an elemental semiconductor material or a crystalline inorganic compound semiconductor material. The elemental semiconductor material may be silicon or germanium, and the crystalline inorganic compound semiconductor material may be silicon carbide, silicon germanide, gallium arsenide, or indium gallium arsenide, etc.

[0109] The first doping region I, the channel region II and the second doping region III are doped with the same type of doping ions, and when the doping concentration of the doping ions in the first doping region I is consistent with the doping concentration of the doping ions in the channel region II and the doping concentration of the doping ions in the second doping region III, the device formed by the semiconductor channel 105 is a junctionless transistor, which is advantageous in adopting the ultra-steep source-drain concentration gradient doping process to avoid the phenomenon of manufacturing ultra-steep PN junctions in the nanoscale range, so that problems such as threshold voltage drift and increased leakage current caused by doping abrupt change can be avoided, and it is also advantageous in suppressing the short channel effect, and it can still operate within a few nanoscale range, which contributes to further improving the integration density and electrical performance of the semiconductor structure. The doping ions are one of N-type ions or P-type ions.

[0110] The orthogonal projection of the channel region II on the bit line 104 is smaller than the orthogonal projection of the second doping region III on the bit line 104, and is also smaller than the orthogonal projection of the first doping region I on the bit line 104. Without adopting an etching process, it is advantageous to form a channel region II with a smaller cross-sectional area in a cross section perpendicular to the direction Z in which the bit line 104 faces the semiconductor channel 105, and is advantageous to improve the controllability of the word line 107 to the channel region II, thereby making it easier to control the on / off of the GAA transistor.

[0111] In some examples, in a cross section perpendicular to the direction Z, the width W and the length L of the channel region II are 10 nm or less, which is advantageous for ensuring a small threshold voltage of the transistor. In the direction Z, the height of the channel region II is 30 nm to 50 nm.

[0112] Referring to Figures 6 and 24 to 25 in combination, the semiconductor structure further includes a first dielectric layer 113 surrounding the first doping region I, and has a first gap between the first dielectric layers 113 on the sidewalls of adjacent first doping regions I on the same bit line 104.

[0113] The first dielectric layer 113 may include a fifth dielectric layer 153 and a sixth dielectric layer 163, where the fifth dielectric layer 153 is located in the space between adjacent bit lines 104 and in the space between adjacent first doping regions I on the adjacent bit lines 104, and the sixth dielectric layer 163 is located on the sidewalls of adjacent first doping regions I on the same bit line 104 and on the sidewalls of the fifth dielectric layer 153. The first dielectric layer 113 is used to achieve electrical isolation between adjacent semiconductor channels 105 and adjacent bit lines 104.

[0114] The semiconductor structure further includes an insulating layer 106 covering at least the sidewall surface of the channel region II. In this embodiment, the insulating layer 106 covers only the sidewall surface of the channel region II. In other embodiments, the insulating layer can cover the sidewall surfaces of both the channel region and the second doping region.

[0115] The semiconductor structure further includes word lines 107 and an isolation layer 109, the word lines 107 surrounding the insulating layer 106 located on the sidewalls of the channel region II and having a second gap between adjacent word lines 107, the isolation layer 109 located at least in the first gap and the second gap, and an upper surface of the isolation layer 109 away from the base is not lower than an upper surface of the second doping region III away from the base.

[0116] The isolation layer 109 may include a second dielectric layer 123 and a third dielectric layer 133, where the second dielectric layer 123 is located in the first gap and the second gap, the top surface of the second dielectric layer 123 away from the base is not lower than the top surface of the second doping region III away from the base, and the third dielectric layer 133 covers the sidewalls of the second doping region III.

[0117] In some examples, the top surface of the second dielectric layer 123 is flush with the top surface of the second doping region III, and the isolation layer 109 further includes a fourth dielectric layer 143. Referring to FIG. 25, the fourth dielectric layer 143 is located on the top surface of the second dielectric layer 123 and the third dielectric layer 133, and is located at the interval of the adjacent third dielectric layer 133. The second dielectric layer 123, the third dielectric layer 133, and the fourth dielectric layer 143 are made of the same material, and the isolation layer 109 is commonly formed to realize electrical insulation between the adjacent semiconductor channels 105 and the adjacent bit lines 104. In other examples, the second dielectric layer, the third dielectric layer, and the fourth dielectric layer may be an integrally molded structure, in which case the isolation layer has high density and few internal defects, which is advantageous for enhancing the isolation effect of the isolation layer between the adjacent semiconductor channels and the adjacent bit lines.

[0118] In another embodiment, when the insulating layer covers the sidewall surfaces of both the channel region and the second doping region, the isolation layer includes a second dielectric layer and a fourth dielectric layer, in which the second dielectric layer is located in the first gap and the second gap, and an upper surface of the second dielectric layer away from the base is not lower than an upper surface of the second doping region away from the base, and the fourth dielectric layer is located in a space defined by the second dielectric layer and the insulating layer and a space defined by an adjacent insulating layer, and the fourth dielectric layer covers an upper surface of the second dielectric layer.

[0119] The orthogonal projection of the periphery of the insulating layer 106 on the bit line 104 is smaller than the orthogonal projection of the periphery of the third dielectric layer 133 on the bit line 104 .

[0120] The semiconductor structure may further include a capacitor contact layer 108 located on an upper surface of the second doping region III, where the orthogonal projection of the capacitor contact layer 108 on the bit line 104 covers the orthogonal projection of the second doping region III on the bit line 104, the capacitor contact layer 108 having doping ions, and a doping concentration of the doping ions in the capacitor contact layer 108 greater than a doping concentration of the doping ions in the second doping region II.

[0121] The capacitor contact layer 108 and the second doping region III are doped with the same type of doping ions, and the doping concentration of the doping ions in the capacitor contact layer 108 is greater than that of the doping ions in the second doping region III, which is advantageous to further improve the conductive performance of the capacitor contact layer 108. Since the orthogonal projection of the capacitor contact layer 108 on the bit line 104 covers the orthogonal projection of the second doping region III on the bit line 104, it is advantageous to increase the contact area between the capacitor contact layer 108 and other subsequent conductive structures, thereby reducing the contact resistance between the capacitor contact layer 108 and other subsequent conductive structures.

[0122] The semiconductor structure may further include a capacitive structure (not shown) located on a common surface of the capacitor contact layer 108 and the fourth dielectric layer 143 .

[0123] In summary, in a cross section perpendicular to the direction Z in which the bit line 104 points to the semiconductor channel 105, the cross-sectional area of ​​the channel region II is smaller than the cross-sectional areas of the first doping region I and the second doping region II, which is advantageous for lowering the threshold voltage of the transistor formed by the semiconductor channel 105, and the transistor can be turned on / off at a low threshold voltage. The device formed by the semiconductor channel 105 is a junctionless transistor, which employs an ultra-steep source-drain concentration gradient doping process to avoid problems such as threshold voltage drift and increased leakage current caused by a sudden change in doping, and is also advantageous for suppressing the short channel effect, thereby contributing to further improving the integration density and electrical performance of the semiconductor structure.

[0124] It should be understood that the present disclosure is not limited to the detailed construction and arrangement of the components described herein. The present disclosure may have other embodiments and may be realized and carried out in various forms. The above variations and modifications are within the scope of the present disclosure. It should be understood that the present disclosure as disclosed and limited herein extends to all alternative combinations of two or more individual features described or illustrated in the present specification and / or drawings. All these different combinations constitute multiple alternative aspects of the present disclosure. The embodiments described herein show the best known ways to realize the present disclosure and allow those skilled in the art to utilize the present disclosure. [Industrial Applicability]

[0125] SUMMARY OF THE DISCLOSURE The embodiments of the present disclosure provide a semiconductor structure and a method for manufacturing the same that are advantageous in simplifying the process of forming word lines and in forming word lines that are small in size and highly accurate.

Claims

1. 1. A method for manufacturing a semiconductor structure, comprising the steps of: Providing a base; forming a bit line on the base and a semiconductor channel on a surface of the bit line away from the base, in a direction in which the base points towards the bit line, the semiconductor channel comprises a first doping region, a channel region and a second doping region arranged in sequence, the first doping region, the channel region and the second doping region being doped with the same type of doping ions, and a doping concentration of the doping ions in the first doping region being equal to a doping concentration of the doping ions in the channel region and a doping concentration of the doping ions in the second doping region; forming a first dielectric layer surrounding sidewalls of the semiconductor channel, the first dielectric layer having a first gap between adjacent sidewalls of the semiconductor channel on the same bit line; forming a second dielectric layer filling the first gap, the second dielectric layer being made of a different material than the first dielectric layer; removing a portion of the first dielectric layer until a sidewall of the channel region is exposed; forming an insulating layer covering at least a sidewall surface of the channel region, the insulating layer having a second gap between the insulating layer and the second dielectric layer; forming a word line filling the second gap; The step of forming the word line includes: forming an initial word line filling the second gap, the initial word line further located between the insulating layer on a portion of a sidewall of the semiconductor channel on an adjacent bit line; and removing a portion of the initial word line, the excess initial word line being used as the word line surrounding only the insulating layer located on a sidewall of the channel region.

2. removing a portion of the first dielectric layer until a sidewall of the channel region is exposed; etching a portion of the first dielectric layer until a sidewall of the second doped region is exposed; a step of forming a third dielectric layer, the third dielectric layer surrounding a sidewall of the second doped region and being located on a sidewall of the second dielectric layer, the third dielectric layer located on the sidewall of the second doped region and the third dielectric layer located on the sidewall of the second dielectric layer commonly surrounding each other to form a through hole whose bottom exposes the first dielectric layer, and the material of the third dielectric layer is different from that of the first dielectric layer; removing the first dielectric layer located on a sidewall of the channel region where the through hole is exposed, the excess first dielectric layer surrounding the sidewall of the first doped region; A method for manufacturing a semiconductor structure according to claim 1.

3. The step of forming the insulating layer includes: a step of thermally oxidizing the exposed sidewall of the channel region to form the insulating layer, the insulating layer covering an excess sidewall surface of the channel region; A method for manufacturing a semiconductor structure according to claim 2.

4. After forming the word lines, the method for manufacturing the semiconductor structure further includes forming a fourth dielectric layer filling the through holes. A method for manufacturing a semiconductor structure according to claim 2.

5. The step of removing a portion of the first dielectric layer until the sidewall of the channel region is exposed further includes removing the first dielectric layer located on the sidewall of the second doped region, and in the step of forming the insulating layer, the insulating layer further covers the sidewall of the second doped region. A method for manufacturing a semiconductor structure according to claim 1.

6. The step of forming the bit line and the semiconductor channel includes: forming a first mask layer over the base; etching the base using the first mask layer as a mask to form a plurality of first trenches; removing the first mask layer and forming a fifth dielectric layer in the first trench; forming a second mask layer on a common upper surface of the fifth dielectric layer and the excess base; etching the base and the fifth dielectric layer using the second mask layer as a mask to form a plurality of second trenches, the bit lines, and the semiconductor channel, wherein a depth of the second trenches is less than a depth of the first trenches in a direction perpendicular to a surface of the base; removing the second mask layer. A method for manufacturing a semiconductor structure according to claim 1.

7. the first mask layer has a plurality of first openings separated from one another, the second mask layer has a plurality of second openings separated from one another, and an extension direction of the first openings is perpendicular to an extension direction of the second openings; A method for manufacturing a semiconductor structure according to claim 6.

8. a ratio of an opening width of the first opening to an opening width of the second opening in a direction perpendicular to a sidewall of the semiconductor channel is 2 to 1, and a distance between adjacent first openings is equal to a distance between adjacent second openings; A method for manufacturing a semiconductor structure according to claim 7.

9. The step of forming the first dielectric layer includes: forming a sixth dielectric layer located on a sidewall of the second trench, wherein an excess of the fifth dielectric layer and the sixth dielectric layer commonly form the first dielectric layer, and the sixth dielectric layer located on the sidewall of the second trench has the first gap therebetween; A method for manufacturing a semiconductor structure according to claim 6.

10. The method for manufacturing the semiconductor structure includes: forming a capacitor contact layer on a top surface of the second doped region using an epitaxial growth process, the orthogonal projection of the capacitor contact layer on the bit line covering the orthogonal projection of the second doped region on the bit line; A method for manufacturing a semiconductor structure according to claim 1.

11. 1. A semiconductor structure comprising: With the base, a bit line located on the base; a semiconductor channel located on a surface of the bit line, the semiconductor channel including a first doping region, a channel region, and a second doping region arranged in sequence in a direction in which the base faces the bit line, the first doping region contacting the bit line, the first doping region, the channel region, and the second doping region being doped with the same type of doping ions, and a doping concentration of the doping ions in the first doping region being equal to a doping concentration of the doping ions in the channel region and a doping concentration of the doping ions in the second doping region; a first dielectric layer surrounding the first doped region, the first dielectric layer having a first gap between the first dielectric layer on sidewalls of adjacent first doped regions on the same bit line; an insulating layer covering at least a sidewall surface of the channel region, the insulating layer having a second gap between the insulating layer and a second dielectric layer formed in the first gap, and the insulating layer further having the second gap between the insulating layer on the sidewalls of adjacent semiconductor channels of adjacent bit lines; a word line surrounding the insulating layer located on a sidewall of the channel region, the word line being formed in the second gap; an isolation layer located at least in the first gap and the second gap, the isolation layer including the second dielectric layer, and a top surface of the second dielectric layer away from the base is not lower than a top surface of the second doped region away from the base.

12. the base, the bit line and the semiconductor channel are composed of the same semiconductor element; 12. The semiconductor structure of claim 11.

13. The doping ions are either N-type ions or P-type ions.

12. The semiconductor structure of claim 11.

14. The semiconductor structure further includes a capacitor contact layer located on an upper surface of the second doped region, an orthogonal projection of the capacitor contact layer on the bit line overlies an orthogonal projection of the second doped region on the bit line, the capacitor contact layer having the doping ions, and a doping concentration of the doping ions in the capacitor contact layer that is greater than a doping concentration of the doping ions in the second doped region.

14. The semiconductor structure of claim 13.

15. an orthogonal projection of the channel region on the bit line is smaller than an orthogonal projection of the second doped region on the bit line and smaller than an orthogonal projection of the first doped region on the bit line; 12. The semiconductor structure of claim 11.

16. The isolation layer comprises: a third dielectric layer covering a sidewall of the second doped region; 12. The semiconductor structure of claim 11.

17. an orthogonal projection of an outer periphery of the insulating layer on the bit line is smaller than an orthogonal projection of an outer periphery of the third dielectric layer on the bit line; 20. The semiconductor structure of claim 16.

18. The first dielectric layer is a fifth dielectric layer located between adjacent bit lines and between adjacent first doped regions on adjacent bit lines; a sixth dielectric layer located on a sidewall of the first doped region adjacent to the same bit line and located on a sidewall of the fifth dielectric layer; 12. The semiconductor structure of claim 11.

Citation Information

Patent Citations

  • Semiconductor storage device, manufacturing method thereof and electronic equipment including storage device

    CN109285836A

  • Memory cell

    JP1998229175A

  • Storage

    JP2018163907A

  • Semiconductor device and method for forming the same

    KR1020070047572A

  • Semiconductor device having 4f2 transistor and the method for manufacturing the same

    KR1020090132298A