Sinter manufacturing method
By incorporating high-flammability carbon materials and low oxidation degree iron-based raw materials in the granulation process, the method enhances sintered ore production yield and productivity through multi-stage combustion optimization.
Patent Information
- Application Number
- JP2020137572
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-17
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-08-17
AI Technical Summary
Existing methods for producing sintered ore for blast furnaces primarily use low-flammability carbon materials like coke and anthracite, which do not effectively utilize high-flammability carbon materials in the granulation process, limiting the improvement of coalescence and productivity.
A method involving the use of both low and high-flammability carbonaceous materials as coagulants, with a preferred blending ratio of 25% to 75% by mass, added in the latter half of the granulation process, along with low oxidation degree iron-based raw materials, to enhance coalescence and yield.
This approach improves the sintering yield by creating a multi-stage combustion zone, extending high-temperature retention time, and optimizing the combustion characteristics of different carbon materials, resulting in enhanced productivity.
Smart Images

Figure 0007583245000008 
Figure 0007583245000009 
Figure 0007583245000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing sintered ore for use as a blast furnace raw material, and more particularly to a method for producing sintered ore using a highly combustible carbonaceous material having a lower combustion start temperature than coke and anthracite as a coagulant (carbonaceous material). [Background technology]
[0002] Currently, the main raw material for blast furnace pig iron production is sintered ore. Sintered ore is usually produced as follows. First, as raw materials for sintered ore production (sintering raw materials), iron raw materials such as iron ore (powder), iron-containing miscellaneous raw materials such as scale and iron-making dust, MgO-containing auxiliary raw materials such as olivine, CaO-containing auxiliary raw materials such as limestone, return ore, and carbonaceous material (agglomeration material) that serves as fuel for sintering (agglomerating) sintered ore by combustion heat are mixed in a specified ratio. The mixed raw materials are granulated to form a granulated raw material mixture. Next, the granulated raw material mixture is loaded from a hopper onto a pallet (sintering pallet) of a downward suction type Dwight Lloyd (DL) sintering machine to form a raw material packed bed (sintering packed bed). The carbonaceous material in the raw material packed bed is ignited from the top (surface) of the formed raw material packed bed by an ignition furnace (igniter). Then, air is sucked from below the pallet while the pallet is continuously moved. Oxygen is supplied into the raw material packed bed by suction, and the combustion of the carbonaceous material in the raw material packed bed proceeds from the top to the bottom, and the raw material packed bed is successively sintered by the combustion heat of the carbonaceous material. The sintered part (sintered cake) obtained by sintering is crushed to a specified grain size, sized by sieving, etc., and becomes sintered ore, which is the raw material for blast furnaces.
[0003] Coke and anthracite are mainly used as carbonaceous materials (aggregating agents) for sintering. Coke for sintering is made by crushing coke of a grain size unsuitable for use in blast furnaces (usually 40mm or less) to 3mm or less, which is suitable for sintering, during the process of producing coke for blast furnaces. Sintered coke is also called breeze coke, as opposed to lump coke for blast furnaces. Anthracite is one of the classifications given to coal (lignite, bituminous coal, anthracite), and is the most carbonized coal. Coal with a fuel ratio (fixed carbon / volatile matter (mass ratio)) of 4 or more, or simply coal with a carbon content of 90% or more by mass, is classified as anthracite.
[0004] In order to produce sintered ore suitable as a raw material for blast furnaces, various methods for producing sintered ore have been proposed. For example, Patent Document 1 discloses a method for producing sintered ore using a solid fuel containing 10 mass% or more of a low-temperature combustion solid fuel (subbituminous coal, lignite, or char obtained by carbonizing a mixed coal of subbituminous coal and lignite at a relatively low temperature of about 800°C) whose combustion reaction initiation temperature is less than 450°C. By using the low-temperature combustion solid fuel as a solid fuel together with coke powder, anthracite, or carbon-containing dust, the combustibility of the solid fuel is essentially improved, and productivity is improved.
[0005] Patent Document 2 and Patent Document 3 disclose a technique for post-adding a carbonaceous material (agglomeration material) (carbonaceous material post-addition sintering method). The carbonaceous material post-addition sintering method is a technique for producing sintered raw material granules by adding a carbonaceous material to granulated sintered raw materials other than the carbonaceous material during or after granulation of the sintered raw materials other than the carbonaceous material.
[0006] Patent Document 2 discloses a carbonaceous material post-addition sintering method that uses a carbonaceous material with a volatile content of 10 mass% or less as the carbonaceous material, and describes that even when coal char obtained by pyrolysis of lignite or the like is used, a sintering raw material can be obtained that can increase the particle size of the granulated particles and improve the combustibility of the carbonaceous material, and that by producing sintered ore using the obtained sintering raw material, the combustion yield and productivity of the sintered ore can be increased.
[0007] Patent Document 3 discloses a carbonaceous material post-addition sintering method that uses coal with a Roga index of 10 or less as a raw material for sintering carbonaceous material, and describes that this method can reduce NOx emissions generated when producing sintered ore, and that it is possible to select the raw material for sintering carbonaceous material simply by calculating the Roga index of coal without producing carbonaceous material for sintering from coal. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. WO2010-106756 [Patent Document 2] JP 2018-3081 A [Patent Document 3] JP 2020-56086 A Summary of the Invention [Problem to be solved by the invention]
[0009] As described above, Patent Document 1 discloses a technique of using a low-temperature combustion solid fuel together with coke or anthracite as a solid fuel. Patent Documents 2 and 3 disclose a carbonaceous material post-addition sintering method. However, up until now, there has been no consideration of a method for producing sintered ore in which coke and / or anthracite (coke and anthracite are classified as low combustible carbonaceous materials, which will be described later) and a highly combustible carbonaceous material having a lower combustion start temperature than the low combustible carbonaceous material are used together as agglomerating materials, and the agglomerating material (part or all) is added later in the granulation process of the sintering raw material.
[0010] The present invention aims to present a preferred mixing ratio of highly combustible carbonaceous material to all coagulants (preferable mixing ratio of low combustible carbonaceous material to highly combustible carbonaceous material) that enables improvement of the sintering yield in a sinter ore manufacturing method in which low combustible carbonaceous material and highly combustible carbonaceous material are used in combination as coagulants and the coagulant is added later in the granulation process of the sintering raw material. [Means for solving the problem]
[0011] (1) As a coagulant for the sintering raw material, a low combustibility carbonaceous material consisting of at least one of coke powder and anthracite, and a high combustibility carbonaceous material having a lower combustion start temperature than the low combustibility carbonaceous material are used, The carbon content of the highly combustible carbonaceous material is 25% by mass to 75% by mass relative to the carbon content of the agglomerate, The method for producing sintered ore, wherein at least one of the low combustibility carbonaceous material and the high combustibility carbonaceous material is added in a latter half of a granulation process of the sintering raw material. (2) A method for producing sintered ore according to (1), in which, as the sintering raw material, a low-oxidized iron-based raw material that is an iron-based raw material containing metallic iron or divalent iron ions is blended in an amount of 2 mass% or more based on the total new raw materials. Effect of the Invention
[0012] According to the present invention, when low combustible carbonaceous material and high combustible carbonaceous material are used in combination as agglomeration materials, the carbon content of the high combustible carbonaceous material is set to a mass ratio of 25 mass% to 75 mass% relative to the carbon content of the agglomeration material, and at least one of the low combustible carbonaceous material and the high combustible carbonaceous material is added in the latter half of the granulation process of the sintering raw material, thereby improving the sintering yield. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram illustrating the firing state in a sintered packed bed. [Diagram 2] FIG. 1 is a diagram showing the relationship between the blending ratio of lignite char and coke powder and the sintering heat pattern. [Diagram 3] FIG. 1 shows the experimental results of Test 1. [Figure 4] FIG. 13 is a diagram showing the experimental results of Test 2. [Diagram 5] FIG. 13 is a diagram showing the experimental results of Test 3. [Figure 6] FIG. 13 is a diagram showing the experimental results of Test 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] First, the low combustibility carbonaceous material and the high combustibility carbonaceous material, and the low oxidation degree iron-based raw material used as raw materials (sintering raw materials) for producing sintered ore will be described in order, and then an embodiment of the present invention will be described.
[0015] (Low combustibility carbonaceous materials and high combustibility carbonaceous materials) Carbonaceous materials (aggregating materials) used as raw materials for sintering are classified into low combustibility carbonaceous materials and high combustibility carbonaceous materials. Low combustibility carbonaceous materials are coke and anthracite, while high combustibility carbonaceous materials are those with higher combustibility than low combustibility carbonaceous materials. Specifically, low combustibility carbonaceous materials and high combustibility carbonaceous materials are classified based on the combustion start temperature obtained by differential thermobalance, with low combustibility carbonaceous materials being carbonaceous materials with a temperature above 550°C and high combustibility carbonaceous materials being carbonaceous materials with a temperature below 550°C.
[0016] Highly combustible carbonaceous materials include, for example, coal char and biomass char (oil kernel shell charcoal and charcoal char produced by carbonization of wood). The ignition temperature of coke is about 670°C and that of anthracite is about 690°C, whereas the ignition temperature of coal char (semi-coke, lignite char, and subbituminous coal char) is about 430°C to 550°C, and the ignition temperature of biomass charcoal (oil kernel shell charcoal) is low at about 470°C. Coal char and biomass charcoal (oil kernel shell charcoal) have roughly the same ignition temperature, and therefore have similar combustibility.
[0017] Here, coal char refers to a carbonaceous material (char) produced by carbonizing low-caking bituminous coal, lignite, and subbituminous coal at 700 to 900°C. Carbonaceous materials produced by carbonizing low-caking bituminous coal, lignite, and subbituminous coal are called semi-coke, lignite char, and subbituminous char, respectively. These carbonaceous materials are produced by carbonizing raw coal (including mixed coal) in a pyrolysis furnace (e.g., a rotary kiln). Biomass charcoal is a carbonaceous material produced by heat-treating biological resources (biomass) such as oil palm kernels and wood. Oil palm kernel shell charcoal (PKS charcoal) is a solid charcoal produced by heat-treating (carbonizing) oil palm kernel shells. The method for producing PKS charcoal is described in JP 2014-218713 (Hara et al.) and other publications, so details will be omitted here.
[0018] (Low oxidation degree iron-based raw material) Low-oxidized iron-based raw materials contain at least one of metallic iron or divalent iron ions and have oxidative exothermic properties. In the mineral phase, they contain at least one of metallic iron (Fe), wustite (FeO), and magnetite (Fe3O4). Examples of low-oxidized iron-based raw materials include scale (mill scale and scarfing scale generated in steelworks) and converter dust. In the sintering process at high temperatures, metallic iron (Fe), wustite (FeO), and magnetite (Fe3O4) are oxidized, for example, metallic iron (Fe) and wustite (FeO) change to magnetite (Fe3O4) and hematite (Fe2O3), and magnetite (Fe3O4) changes to hematite (Fe2O3). These oxidation reactions are exothermic, so low-oxidized iron-based raw materials can also be used as heat sources.
[0019] In the sintered ore manufacturing method of the present invention, a low combustible carbonaceous material and a high combustible carbonaceous material are used together as a coagulant for the sintering raw material, the carbon content contained in the high combustible carbonaceous material is 25% by mass to 75% by mass relative to the carbon content contained in the total coagulant, and at least one of the low combustible carbonaceous material and the high combustible carbonaceous material is added in the latter half of the granulation process of the sintering raw material. By using such a blending ratio and post-addition, the product yield of the sintering is improved. The basis for this is based on the examples described later. Here, the low combustible carbonaceous material used as the coagulant is at least one of coke powder and anthracite. The high combustible carbonaceous material used as the coagulant may be made of one type of raw material or a mixture of multiple types of raw materials (for example, a mixture of multiple types of coal char, a mixture of coal char and biomass coal, coal char produced from a mixed raw material coal in which multiple raw material coals are mixed, etc.).
[0020] In the present invention, as the agglomerating material, a highly combustible carbonaceous material, which has a lower combustion start temperature than the low combustible carbonaceous material, is used together with a conventional low combustible carbonaceous material (coke powder, anthracite). Since the low combustible carbonaceous material and the highly combustible carbonaceous material have different combustion start temperatures, the combustion positions (combustion zones) of the two materials differ during the sintering process in which sintering progresses due to downward suction. When the blending ratio of the low combustible carbonaceous material and the highly combustible carbonaceous material is within an appropriate range, multiple carbonaceous materials with different combustion characteristics are combusted during the sintering process, thereby making it possible to expand the width of the combustion zone in the bed height direction of the sintered packed bed and to extend the high temperature retention time of the combustion zone.
[0021] In the present invention, at least one of low combustibility carbonaceous material and high combustibility carbonaceous material is added later in the granulation process (at least one of low combustibility carbonaceous material and high combustibility carbonaceous material added later is hereinafter also referred to as later-added carbonaceous material). That is, in the granulation process in which sintering raw material granules (granules of sintering raw material) are produced from sintering raw material using a granulator, the sintering raw material except for the later-added carbonaceous material is first charged into the granulator, mixed, and granulation is started after humidity adjustment. Then, the later-added carbonaceous material is charged later (in the middle of the granulation process) into the granulator to produce sintering raw material granules. By adding the later-added carbonaceous material later at an appropriate timing, the later-added carbonaceous material is sheathed in the sintering raw material granules, that is, it is not included in the granules, and exists as independent particles attached or not attached to the surface layer of the granules. By using the sintering raw material granules (mixed raw material granules) sheathed in the later-added carbonaceous material, it is possible to adjust the timing of the start of combustion of the later-added carbonaceous material in the sintering process. The post-added carbonaceous material may be either a low combustibility carbonaceous material or a high combustibility carbonaceous material.
[0022] The post-addition in the granulation process is carried out, for example, as follows. For granulation, a piston-flow type cylindrical granulator with a central axis inclined downward toward the downstream side is used, and a small transport conveyor is inserted from the downstream outlet to a predetermined position inside the granulator. When the sintering raw materials excluding the post-added carbonaceous material (hereinafter also referred to as the post-added pre-sintering raw materials) are charged from the upstream inlet, the charged sintering raw materials move downstream while being mixed and granulated. The post-added carbonaceous material is carried on the transport conveyor and transported from the downstream outlet of the granulator to the internal upstream side. The post-added carbonaceous material is added at a predetermined position to the granulated material of the post-added pre-sintering raw materials that have been granulated and moved from the upstream side inside the granulator, and all the sintering raw materials are further granulated and discharged from the downstream outlet as sintering raw material granules (mixed raw material granules).
[0023] In addition, it is preferable that the granulation time of the pre-added sintering raw material before adding the post-added carbonaceous material is 80% to 96% of the total granulation time of the sintering raw material, that is, the timing of the post-addition is within the range of 80% to 96% of the total granulation time of the sintering raw material in the granulation process. If the post-addition is earlier than 80% of the total granulation time, it is not possible to sufficiently prevent the post-added carbonaceous material from being included in the granulated material. Also, if the post-addition is later than 96% of the total granulation time, the granulation process of the post-added carbonaceous material becomes insufficient. Here, the total granulation time in the granulation process does not include the time (mixing time) during which the sintering raw material is simply mixed from when it is put into the granulator until water is added. In sintering, a drum mixer is mainly used, which is a piston flow type with a constant speed. Therefore, the post-addition position can be handled by the distance in the machine length direction of the drum mixer.
[0024] In addition, under the above-mentioned conditions of the blending ratio and timing of post-addition, an iron-based raw material containing metallic iron and / or divalent iron ions (low-oxidized iron-based raw material) may be blended as the sintering raw material in an amount of 2 mass% or more relative to the total new raw materials. In the sintering process, the metallic iron and divalent iron ions in the low-oxidized iron-based raw material are oxidized, and the heat of oxidation further improves the yield.
[0025] The progress of the combustion reaction in the sintered packed bed will now be described with reference to the drawings. FIG. 1 is an explanatory diagram for explaining the firing state in the sintering packed bed when a highly combustible carbonaceous material (such as brown coal char) and a low-oxidized iron source (such as mill scale) are used as sintering raw materials together with a conventional low-combustible carbonaceous material (such as coke powder). FIG. 1(A) is a schematic diagram showing the state in the sintering packed bed at time t1, and FIG. 1(B) is a schematic diagram showing the state in the sintering packed bed at time t2, where time t2 is a time after a predetermined time has elapsed from time t1. FIG. 1(C) is a diagram showing the temperature and oxygen concentration distribution in the bed height direction in the sintering packed bed at time t2, corresponding to the position in the bed height direction in the sintering packed bed in FIG. 1(B). Note that the graphs showing the temperature and oxygen concentration in FIG. 1(C) show that the temperature and oxygen concentration increase from left to right.
[0026] In the sintering process, combustion progresses downward from the surface of the ignited sintered packed bed. As shown in Figure 1 (A), the sintered packed bed during sintering is divided into three regions in the top and bottom of the bed height direction depending on the progress of sintering. Specifically, the upper layer contains sintered cake that has been sintered, the lower layer contains the sintered raw materials before sintering, and in the middle part between them is the oxidation (combustion) zone where the combustion reaction of the coagulation material and the oxidation reaction of the low-oxidized iron source are occurring. As shown in Figures 1 (A) and 1 (B), sintering progresses over time (from time t1 to time t2), and the oxidation (combustion) zone descends.
[0027] As shown in Figure 1(B), the oxidation (combustion) zone is further divided into three regions A, B, and C from bottom to top in the bed height direction depending on the progress of the combustion and oxidation reactions. In region A, the combustion reaction of highly combustible carbonaceous materials mainly occurs, in region B, the combustion reaction of low combustible carbonaceous materials mainly occurs, and in region C, the oxidation reaction of low-oxidized iron sources mainly occurs. Below, the progress of the combustion and oxidation reactions in the oxidation (combustion) zone will be explained using Figures 1(B) and 1(C).
[0028] When the oxidation (combustion) zone descends to the layer of unsintered sintered raw materials below, the highly combustible carbonaceous material with the lowest combustion start temperature among the aggregates starts to burn first and then disappears. In other words, the very bottom of the oxidation (combustion) zone is the combustion start position of the highly combustible carbonaceous material, and the combustion range of the highly combustible carbonaceous material is the lower part (area A) of the oxidation (combustion) zone. When the temperature in the sintered layer rises due to the combustion of the highly combustible carbonaceous material, as shown in Figure 1 (C), the low combustible carbonaceous material with the highest combustion start temperature starts to burn and then disappears. Since the low combustible carbonaceous material starts to burn later than the high combustible carbonaceous material, its combustion range is the middle part (area B) of the oxidation (combustion) zone, which is above area A. Here, as shown in Figure 1 (C), in area B, the combustion of the low combustible carbonaceous material creates a high-temperature environment, but the combustion of the low combustible carbonaceous material consumes oxygen, CO is generated, and a reducing atmosphere is created, so the oxidation of the low-oxidized iron source is suppressed. In the upper part of the oxidation (combustion) zone (area C), which is above area B, the low-combustibility carbonaceous material is burned and disappeared, reducing the consumption of atmospheric oxygen supplied from above and the amount of CO generated. This promotes the oxidation of the low-oxidization iron source, and oxidation heat is generated by this oxidation reaction.
[0029] In this way, by blending multiple raw materials with different oxidation (combustion) conditions (two types of agglomerates, low combustibility carbonaceous material and high combustibility carbonaceous material, and low oxidation iron-based raw materials) into the sintering raw materials, multi-stage combustion can be realized as shown in regions A to C in Figure 1 (B), and the combustion and oxidation region (oxidation (combustion) zone) in the bed height direction expands as sintering progresses. As a result, the high temperature holding time at any position in the bed height direction is extended, and product yield is expected to improve. In the above explanation, the case where low oxidation iron-based raw materials are blended into the sintering raw materials has been described, but even if low oxidation iron-based raw materials are not blended, multi-stage combustion can be realized in regions A and B in Figure 1 (B) by using two types of agglomerates, low combustibility carbonaceous material and high combustibility carbonaceous material. Since the oxidation (combustion) region in the bed height direction expands compared to when only low combustion carbonaceous material is used, product yield is expected to improve.
[0030] However, in order to realize the multi-stage combustion in which the combustion of the high combustibility carbonaceous material and the combustion of the low combustibility carbonaceous material are successively performed as described above, it is necessary to make the blending ratio of the low combustibility carbonaceous material and the high combustibility carbonaceous material appropriate. Therefore, before carrying out the examples described later that serve as the basis for the above-mentioned blending ratio and the timing of post-addition, the inventors conducted a batch experiment to investigate the effect of the blending ratio (blending ratio) of the low combustibility carbonaceous material and the high combustibility carbonaceous material on the change over time of the sintered layer temperature (hereinafter referred to as the heat pattern). The batch experiment will be described below. In the batch experiment, coke powder was used as the low combustibility carbonaceous material, and lignite char was used as the high combustibility carbonaceous material.
[0031] In the batch experiment, a cylindrical pot with a diameter of 100 mm and a height of 160 mm was used. Five samples (mixed raw materials) were prepared, in which the mixing ratio of fine coke and lignite char was changed (mixing ratio based on the carbon content mass ratio described later) and the agglomerates were mixed, and each was sintered and the temperature inside the sintered layer was measured. The temperature was measured at a depth of 140 mm from the top surface in the layer height direction and at the center of the pot in the horizontal direction, and the heat pattern at this position inside the sintered layer was investigated.
[0032] FIG. 2 shows the heat patterns of each sample measured in the batch experiment. As shown in Figure 2, the cases where the lignite char blending ratio was 0% and 100% had a lower maximum temperature and a shorter high-temperature retention time than the cases where the lignite char blending ratio was 25% to 75%. As shown in the examples described later, when the lignite char blending ratio is less than 25%, the effect of improving the combustion front descent velocity, which is the effect of blending highly combustible carbonaceous materials, cannot be obtained, and when the lignite char blending ratio exceeds 75%, the product yield decreases due to the high-speed combustion specific to highly combustible carbonaceous materials.
[0033] Furthermore, an important feature of the present invention is that the agglomeration agent is added at the final stage of the granulation process. If the agglomeration agent is granulated together with other sintering raw materials, it will be included in the attached powder layer of the granulated material. If it is included, the start of combustion of the agglomeration agent will be controlled by the heat transfer time of the attached powder layer, and the difference in the combustion characteristics of the agglomeration agents will not be apparent. As a result of various studies, the inventors of the present invention have found that it is necessary to add at least one of two types of agglomeration agents (low combustibility carbonaceous material and high combustibility carbonaceous material) at the granulation process. In addition, in the above-mentioned batch experiment, it has been found that the product yield is improved when the sintering raw material granulated material granulated with one or more types of agglomeration agents (low combustibility carbonaceous material and / or high combustibility carbonaceous material) is sintered. EXAMPLES
[0034] An example showing the basis for determining the carbonaceous material composition ratio of the present invention will be described. Among the test cases performed in Tests 1 to 4 described later, the examples show the cases in which the yield was 74.5% or more. The present invention is not limited to the following examples. For example, the same effect can be obtained even when anthracite is used as the low combustibility carbonaceous material.
[0035] In the embodiment, verification was performed using a method commonly known as the sintering pot test. The sintering pot test is a test in which sintering raw materials (mixed raw materials) containing carbonaceous material as fuel are charged into a container of a specified size, ignited from the top, and sucked downward to proceed with sintering. The sintering pot test device does not move the raw material packed bed using a pallet like the Dwight Lloyd (DL) type sintering machine, but it is a test device that can simulate sintering using a DL type sintering machine. Four tests, Tests 1 to 4, which will be described later, were performed. First, the raw materials used in the tests and the test method will be described, and then each test will be described in order. The sintering raw materials in a state in which the raw materials are mixed in a specified ratio are called mixed raw materials.
[0036] (raw materials) Table 1 shows the results of proximate and elemental analysis of the low and high combustibility carbonaceous materials used in the test. As shown in Table 1, coke breeze was prepared as the low combustibility carbonaceous material, and lignite char, subbituminous coal char, and semi-coke were prepared as the high combustibility carbonaceous materials.
[0037] [Table 1]
[0038] The low-oxidation iron-based raw material was scale derived from downstream processes in a steelworks. The scale contained 74% total iron by mass, 66% divalent iron by mass (as FeO), and 4% metallic iron by mass.
[0039] (Raw material blend) Table 2 shows the blending ratio of each raw material in the raw material blend used as the standard in this test (hereinafter referred to as the standard raw material blend). As shown in Table 2, the standard raw material blend does not contain high combustibility carbonaceous material and scale, and only low combustibility carbonaceous material (coke fines) shown in Table 1 is used as the carbonaceous material. In addition, iron ores A to E are iron ores from different origins, and the blending ratios of coke fines and return ore were 4.5% by mass and 15.0% by mass, respectively, with the new raw materials (iron ore, olivine, quicklime, and limestone) being 100% by mass.
[0040] [Table 2]
[0041] Details will be described later, but in tests 1 to 4, the experiments were conducted by appropriately blending the above-mentioned highly combustible carbonaceous material (see Table 1) and / or a blended raw material containing a predetermined amount of the above-mentioned scale (hereinafter referred to as the comparative blended raw material) based on the standard blended raw material in Table 2.
[0042] When highly combustible carbonaceous materials were blended with the standard blended raw materials, the blending ratio was adjusted by replacing the low combustible carbonaceous materials in the standard blended raw materials with highly combustible carbonaceous materials so that the industrial analysis carbon content of all carbonaceous materials (low combustible carbonaceous materials and highly combustible carbonaceous materials) contained in each blended raw material (standard blended raw materials and comparative blended raw materials) was the same. In addition, when scale was added to the standard raw material blend, iron ore D was replaced with scale so that the masses were the same, and the blending ratio was adjusted to reduce the blending amount of low-combustible carbonaceous material (coke breeze) so that the total estimated heat value in both raw material blends was the same (so that the amount of heat generated by oxidation when FeO and metallic iron in the blended scale are oxidized to Fe2O3 is equivalent to the amount of heat generated by oxidation when the replaced low-combustible carbonaceous material is completely burned). Specific values were 394 kJ / mol, 135 kJ / mol, and 412 kJ / mol per mole of carbon, FeO, and metallic iron, respectively, for the heat values generated by combustion and oxidation to CO and Fe2O3. Furthermore, when blending both highly combustible carbonaceous material and scale, the blending ratio of the highly combustible carbonaceous material described above was first adjusted, and then the blending ratio of the scale described above was adjusted to determine the blending ratio of each raw material.
[0043] The details of the blending ratio of the raw materials used in each test will be described later. First, the test methods and the results evaluation methods in Tests 1 to 3 will be described below.
[0044] (Granulation method) A cylindrical batch drum mixer with a diameter of 600 mm and a length of 800 mm was used as the granulator. The raw materials were fed from the upstream side of the granulator and mixed for 4 minutes, after which water was added (humidity control) and mixed for another 4 minutes to granulate. The amount of water added depends on the type of carbonaceous material to be mixed. This is because the amount of water absorption differs depending on the carbonaceous material. Specifically, the value was determined by the blending ratio of coke fines and highly combustible carbonaceous material, with 7.0% by mass for coke fines and 7.6% for highly combustible carbonaceous material, as the outside number for each raw material blend. In addition, in the case where carbonaceous material (low combustible carbonaceous material or / and highly combustible carbonaceous material) was added later instead of lump granulation, a part of the raw materials except for the carbonaceous material to be added later was fed and humidified, mixed for 3 minutes and 50 seconds, and then the carbonaceous material to be added later was added and mixed for another 10 seconds to granulate. After the series of mixing processes was completed, the raw material moisture was measured to confirm the moisture content. In this case, the granulation time was 4 minutes after humidity control.
[0045] (Charging / ignition method) The pot test equipment used was a cylindrical pot with a diameter of 300 mm and a height of 500 mm. The granulated raw materials were charged vertically without segregation to a bed height of 500 mm, and the surface of the raw material bed was ignited for 1 minute (heat amount 25 MJ / t of raw material) to sinter. The valve opening on the suction side of the blower was adjusted so that the negative suction pressure during sintering was constant at 1300 mmAq (12.7 kPa) measured below the pot from the start of ignition.
[0046] (sintering time) The sintering time was measured as follows. A thermocouple was inserted under the pot to measure the temperature of the exhaust gas. In the sintering process, when the combustion zone reaches the bottom of the sintering layer, the temperature of the exhaust gas under the pot starts to rise, eventually peaks, and then drops as the combustion of the carbonaceous material is completed. Three minutes after the exhaust gas temperature reaches its peak, the suction of the blower is stopped and sintering is completed. The sintering time was defined as the time required from the start of ignition until the exhaust gas temperature reaches its peak.
[0047] (Yield) The yield was measured as follows. After firing, the sintered cake was dropped four times from a height of 2 m, and the mass of the sintered product was calculated from the particle size + 5 mm (5 mm or more) excluding the bedding ore. The ratio (mass%) of the sintered product to the mass of the sinter cake excluding the bedding ore was defined as the product yield (+ 5 mm%).
[0048] (burn front descent speed) The combustion front descending velocity (mm / min) was calculated by dividing the bed height of the raw material packed bed (500 mm) by the above-mentioned sintering time.
[0049] (Production rate) The productivity was calculated based on the above-mentioned sintering time by the following formula (1). Production rate (t / d / m 2 )=Product quantity (t) / pan bottom area (m 2 ) / sintering time (days) ···(1)
[0050] Test 1 In Test 1, an experiment was conducted to verify the optimum blend ratio of low combustibility carbonaceous material and high combustibility carbonaceous material and the effect of post-addition. Table 3 shows the blending conditions used in Test 1. As shown in Table 3, five types of blended raw materials (R0, R1, R2, R3) with different blending ratios of low combustibility carbonaceous material and high combustibility carbonaceous material were used. 25 ,R 50 ,R 75 ,R 100 ) was prepared. 25 ,R 50 ,R 75 ,R 100 In the comparative examples, the lignite char shown in Table 1 was used as the highly combustible carbon material, and the coke powder was replaced with lignite char so that the carbon content of the industrial analysis was the same as that of the standard blended raw material R0 in Table 2. Specifically, the carbon content of the lignite char relative to the total carbon material was 0 mass% for R0 (Comparative Example 1 and Comparative Example 6), 0 mass% for R1 (Comparative Example 2 and Comparative Example 3), 0 mass% for R2 (Comparative Example 3 and Comparative Example 4), 0 mass% for R3 (Comparative Example 4 and Comparative Example 5), 0 mass% for R4 (Comparative Example 5 and Comparative Example 6), 0 mass% for R5 (Comparative Example 6 and Comparative Example 7), 0 mass% for R6 (Comparative Example 7 and Comparative Example 8), 0 mass% for R7 (Comparative Example 8 and Comparative Example 9), 0 mass% for R8 (Comparative Example 9 and Comparative Example 10), 0 mass% for R9 (Comparative Example 10 and Comparative Example 11), 0 mass% for R10 (Comparative Example 11 and Comparative Example 12), 0 mass% for R11 (Comparative Example 12 and Comparative Example 13), 0 mass% for R12 (Comparative Example 13 and Comparative Example 14), 0 mass% for R13 (Comparative Example 14 and Comparative Example 15), 0 mass% for R14 (Comparative Example 15 and Comparative Example 16), 0 mass% for R15 (Comparative Example 16 and Comparative Example 17), 0 mass% for R16 (Comparative Example 17 and Comparative Example 18), 0 mass% for R17 (Comparative Example 18 and Comparative Example 19), 0 mass% for R18 (Comparative Example 19 and Comparative Example 20), 0 mass% for R21 (Comparative Example 25 is 25% by mass (Comparative Example 2 and Example 1), R 50 is 50 mass% (Comparative Example 3 and Example 2), R 75 is 75% by mass (Comparative Example 4 and Example 3), R 100The amount of the low-combustibility carbonaceous material (coke powder) was 100% by mass (Comparative Example 5). 25 ,R 50 ,R 75 Specifically, in regard to the above, there were two cases: one in which all the raw materials were granulated at once (Comparative Examples 1 to 4), and the other in which only fine coke was added to all the raw materials and granulated later (Comparative Example 6 and Examples 1 to 3). A total of nine types of sinter raw material granules were produced, and experiments were performed using the above-mentioned pot test using each sinter raw material granule.
[0051] [Table 3]
[0052] (Test 1 results) Figure 3 shows the results of Test 1. In Figure 3, the cases where all the raw materials were granulated at once are shown by white circles, and the cases where coke fines were added later are shown by black circles. As shown in Figure 3, when the lignite char blending ratio was 0 mass%, the product yield decreased in the case where coke fines were added later compared to the case where all raw materials were granulated at once, but the FFS increased, resulting in an increase in productivity. Also, when the lignite char blending ratio was 25, 50, or 75 mass%, i.e., when both lignite char and coke fines were blended, both the product yield and the FFS increased, resulting in a significant increase in productivity.
[0053] Test 2 In test 2, an experiment was conducted to verify the difference in effect depending on the type of carbonaceous material added later. Table 4 shows the sintering raw material granulated material used in Test 2. Comparative Example 3 and Example 2 in Table 3 are relisted from Table 3. As shown in Table 4, Experiments 4 and 5 were carried out in which the carbon mass ratio was fixed at 50% and different types of carbonaceous material were added later. Specifically, in Comparative Example 3 of Test 1, all the raw materials were granulated at once, in Example 2, only coke fines was added later, in Example 3, only lignite char was added later, and in Example 4, both coke fines and lignite char were added later.
[0054] [Table 4]
[0055] (Test 2 results) FIG. 4 shows the results of test 2. As shown in Fig. 4, when lignite char and / or coke fines were added later, the product yield, FFS and productivity were improved compared to when all sinter raw materials were granulated at once (no post-addition).
[0056] Test 3 In Test 3, an experiment was conducted to verify the effect of different amounts of scale when scale was mixed as a raw material. Table 5 shows the sintered raw material granulated material used in Test 3. Example 5 in Table 5 is a reprint of Table 4. As shown in Table 5, the carbon mass ratio of the lignite char was fixed at 50% (however, the reduction in the coke fines due to the scale blending was not considered), and the scale blending amount was changed to 0, 1, 2, and 5 mass% under the condition that both the coke fines and the lignite char were added later. The scale was blended by replacing it with iron ore D in Table 2, and the scale blending amount is the blending ratio (internal number) when the new raw material is 100 mass%. As described in the column of the low combustible carbonaceous material in the blending raw material type and blending ratio of Examples 6 to 8, the coke fines blending ratio (blended amount) was adjusted to reduce the blended amount of scale by the amount of heat equivalent to the blended amount of scale, taking into account the oxidation heat of scale. Specifically, the coke powder blending ratio (blending amount) was 50% (carbon mass ratio) in Example 5, whereas in Examples 6, 7, and 8, it was 49.94%, 49.89%, and 49.72%, respectively. The blending amount of high combustible carbonaceous material was the same in Examples 5 to 8. The values shown in Table 6 are values calculated for the blending ratios of low combustible carbonaceous material and high combustible carbonaceous material in Examples 5 to 8 shown in Table 5, with the total carbon mass of low combustible carbonaceous material and high combustible carbonaceous material (total carbon mass of aggregate material) being 100% by mass.
[0057] [Table 5]
[0058] [Table 6]
[0059] (Test 3 results) FIG. 5 shows the results of test 3. As shown in Fig. 5, the yield improved with an increase in the amount of scale blended. However, the improvement effect became moderate when the amount of scale blended was 2% or more. On the other hand, the combustion front descent velocity slightly decreased with an increase in the amount of scale blended, but the productivity was slightly higher when the amount of scale blended was 2% or more.
[0060] Test 4 In Test 4, an experiment was conducted to comparatively verify high combustibility carbon materials. Table 7 shows the sintering raw material granulated material used in Test 4. Example 2 in Table 7 is a reprint of Tables 3 and 4. As shown in Table 7, in addition to an experiment (Example 2) in which the highly combustible carbonaceous material was lignite char under conditions in which the carbon mass ratio of the highly combustible carbonaceous material was 50% and coke powder was added later, an experiment was also conducted in Example 9 in which the highly combustible carbonaceous material was subbituminous char and an experiment in Example 10 in which the highly combustible carbonaceous material was semi-coke.
[0061] [Table 7]
[0062] (Test 4 results) FIG. 6 shows the results of test 4. As shown in Fig. 6, when subbituminous coal char or semi-coke was used as the highly combustible coal material, the yield was higher than when lignite char was used. The productivity was higher when subbituminous coal char was used than when lignite char was used, but it decreased with the flame front descent velocity when semi-coke was used.
Claims
[Claim 1] A low combustibility carbonaceous material consisting of at least one of coke powder and anthracite, and a high combustibility carbonaceous material having a lower combustion start temperature than the low combustibility carbonaceous material are used as a coagulant for the sintering raw material, The carbon content of the highly combustible carbonaceous material is 25% by mass to 75% by mass relative to the carbon content of the agglomerate, As the sintering raw material, a low-oxidized iron-based raw material that is an iron-based raw material containing metallic iron or divalent iron ions is blended in an amount of 2 mass% or more based on the total new raw materials, The low combustible carbonaceous material and the high combustible carbonaceous material are added in the latter half of the granulation process of the sintering raw material, A method for producing sintered ore, in which the granulation time of the sintering raw material until the addition of the low combustible carbonaceous material and the highly combustible carbonaceous material is 80% or more and 96% or less of the total granulation time of the sintering raw material.
Citation Information
Patent Citations
Multistage ignition-type sintering method
JP1987060828A
Production of sintered ore
JP1994158185A
Method for producing sintered ore
JP2011127184A
Method for producing sintered ore
JP2014133937A
Method of producing sintered ore
JP2014218713A