Method for estimating solidified shell thickness and method for continuous casting of molten metal

By correlating local heat flux with shell thickness, the method accurately predicts breakouts, facilitating preventive measures to ensure continuous casting operations.

JP7583267B2Active Publication Date: 2024-11-14NIPPON STEEL CORPORATION
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2021021617
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-15
Publication Date
2024-11-14
Estimated Expiration
2041-02-15

AI Technical Summary

Technical Problem

Existing methods fail to accurately predict breakouts during continuous casting of molten metal, leading to interruptions and equipment damage.

Method used

A method to estimate the thickness of the solidified shell by correlating local heat flux measured by a temperature sensor with the shell thickness, allowing for accurate prediction and prevention of breakouts by controlling casting parameters.

Benefits of technology

Accurately predicts breakouts, enabling proactive measures to prevent equipment damage and maintain continuous casting operations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583267000006
    Figure 0007583267000006
  • Figure 0007583267000007
    Figure 0007583267000007
  • Figure 0007583267000008
    Figure 0007583267000008
Patent Text Reader

Abstract

To accurately predict breakout with redissolvability, during continuous casting of molten metal.SOLUTION: A method for estimating a thickness of a solidification shell is a method for estimating a thickness T of a portion P with which discharge flow from a submerged nozzle, of portions of a solidification shell generated in a casting mold during continuous casting of molten metal, collides, and includes: confirming a relation between a local heat flux Q in the portion P and the thickness T of the solidification shell in the portion P before the continuous casting; determining the local heat flux Q in the portion P by a temperature sensor installed in the casting mold during the continuous casting; and estimating the thickness T of the solidification shell in the portion P, on the basis of the local heat flux Q determined by the temperature sensor and the relation, during the continuous casting. A method for continuous casting of molten metal determines the possibility of breakout with redissolvability, utilizing the estimation method.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a method for estimating solidified shell thickness and a method for continuous casting of molten metal. [Background technology]

[0002] Breakout (BO) is an operational problem that occurs during continuous casting of molten metal. If a BO occurs during continuous casting, operations must be stopped to remove the solidified metal and repair the equipment. Therefore, technology is needed to accurately predict the occurrence of BO.

[0003] One type of BO is remelt breakout, which occurs when the solidified shell remelts and the thickness of the solidified shell becomes partially thin, leading to BO. In order to accurately predict the occurrence of remelt breakout, for example, it is considered effective to accurately estimate the thickness of the solidified shell in the mold.

[0004] Patent Documents 1 to 5 disclose techniques for predicting BO and estimating solidified shell thickness by focusing on heat flux measured by a temperature sensor installed in the mold. Patent Documents 6 and 7 disclose techniques for detecting drift in the mold by focusing on heat flux measured by a temperature sensor installed in the mold. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 58-148061 [Patent Document 2] International Publication No. 2009 / 107865 [Patent Document 3] JP 2010-105040 A [Patent Document 4] JP 2011-079023 A [Patent Document 5] JP 2019-072749 A [Patent Document 6] Japanese Patent Application Publication No. 1-262050 [Patent Document 7] Japanese Patent Application Publication No. 3-032457 Summary of the Invention [Problem to be solved by the invention]

[0006] A new technique is needed to accurately predict breakout during continuous casting of molten metal. [Means for solving the problem]

[0007] As one of the means for solving the above problems, the present application provides: A method for estimating a thickness T of a portion P of a solidified shell formed in a mold during continuous casting of molten metal, the portion P being struck by a discharge flow from a submerged entry nozzle, comprising the steps of: Before continuous casting, a relationship between a local heat flux Q in the portion P and a thickness T of the solidified shell in the portion P is confirmed; During continuous casting, a local heat flux Q in the portion P is measured by a temperature sensor installed in the mold; And, During continuous casting, estimating a thickness T of the solidified shell at the portion P based on the relationship and the local heat flux Q obtained by the temperature sensor; A method for estimating the solidified shell thickness, including Disclose.

[0008] As one of the means for solving the above problems, the present application provides: A method for continuously casting molten metal by discharging the molten metal from a submerged nozzle into a mold and forming a solidified shell in the mold, comprising the steps of: Before continuous casting, a relationship between a local heat flux Q at a portion P of the solidified shell generated in the mold where the discharge flow from the submerged nozzle collides and a thickness T of the solidified shell at the portion P is confirmed; During continuous casting, a local heat flux Q in the portion P is measured by a temperature sensor installed in the mold; determining an estimated value of a thickness T of the solidified shell at the portion P based on the relationship and the local heat flux Q determined by the temperature sensor during continuous casting; And, During continuous casting, determining the possibility of a breakout occurring based on the estimated value of the thickness T; A method for continuous casting of molten metal, comprising: Disclose.

[0009] The continuous casting method of the present disclosure includes: When the estimated value of the thickness T becomes 0 during continuous casting, it is determined that there is a possibility of a breakout occurring. may also include

[0010] As one of the means for solving the above problems, the present application provides: A method for continuously casting molten metal by discharging the molten metal from a submerged nozzle into a mold and forming a solidified shell in the mold, comprising the steps of: Before continuous casting, a relationship between a local heat flux Q at a portion P of the solidified shell generated in the mold where the discharge flow from the submerged nozzle collides and a thickness T of the solidified shell at the portion P is confirmed; Before or during continuous casting, the local heat flow is determined so that the thickness T falls within a predetermined range based on the relationship. bundle Upper limit of Q limit Identifying During continuous casting, a local heat flux Q in the portion P is measured by a temperature sensor installed in the mold; And, During continuous casting, the upper limit Q limit and comparing the local heat flux Q determined by the temperature sensor to determine the possibility of a breakout. A method for continuous casting of molten metal, comprising: Disclose.

[0011] The continuous casting method of the present disclosure includes: Casting speed during continuous casting Vc Considering the upper limit Q limit Identifying may also include

[0012] The continuous casting method of the present disclosure includes: Before or during continuous casting, the upper limit Q is set so that the thickness T becomes 0 based on the relationship. limit Identifying may also include

[0013] The continuous casting method of the present disclosure includes: When the molten metal is a high carbon steel containing 1.0 mass% or more of C, the upper limit Q limit is determined based on the following formula (1); may also include Q limit =1.28×V c +1.49 ··· (1) Here, Q limit is the local heat flux (MW / m 2 ) and V c is the casting speed (m / min). Effect of the Invention

[0014] According to the method for estimating the solidified shell thickness of the present disclosure, it is possible to accurately estimate the thickness T of a portion P of the solidified shell in a mold where the discharge flow from the submerged entry nozzle collides with the solidified shell during continuous casting of molten metal. Furthermore, according to the method for continuous casting of molten metal of the present disclosure, it is possible to accurately predict breakout. [Brief description of the drawings]

[0015] [Figure 1] FIG. 11 is a diagram for explaining an example of a flow of a method for estimating a solidified shell thickness. [Diagram 2] FIG. 2 is a diagram for explaining an example of a flow of a method for continuously casting molten metal. [Diagram 3] FIG. 4 is a diagram for explaining another example of the flow of a method for continuously casting molten metal. [Figure 4]FIG. 1 is a diagram showing a cross-sectional shape of a solidified shell obtained from a mold after breakout (solidified shell after BO). [Diagram 5] FIG. 1 is a graph showing the relationship between the theoretical thickness of the solidified shell after BO (when there is no discharge flow) and the actually measured thickness. [Figure 6] FIG. 1 shows local heat flux profiles every 5 seconds. [Figure 7] FIG. 13 is a graph showing the change over time in local heat flux at a point about 300 mm from the meniscus. [Figure 8] FIG. 6 is a diagram showing the difference between the theoretical value and the actually measured value of the solidified shell thickness shown in FIG. 5. [Figure 9] FIG. 13 is a graph showing the change in solidified shell thickness at point A over time and the change in local heat flux at point A over time. [Figure 10] FIG. 1 shows the relationship between the solidified shell thickness and the local heat flux at point A. [Figure 11] FIG. 1 is a diagram showing the relationship between casting speed and local heat flux. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] 1. Method for estimating solidified shell thickness The method for estimating a solidified shell thickness disclosed herein is a method for estimating a thickness T of a portion P of a solidified shell generated in a mold during continuous casting of molten metal, the portion P being struck by a discharge flow from a submerged entry nozzle. As shown in Fig. 1, the method for estimating a solidified shell thickness disclosed herein includes confirming a relationship between a local heat flux Q at the portion P and a thickness T of the solidified shell at the portion P before continuous casting (S1), determining the local heat flux Q at the portion P during continuous casting by a temperature sensor installed in the mold (S2), and estimating the thickness T of the solidified shell at the portion P based on the relationship and the local heat flux Q determined by the temperature sensor during continuous casting (S3).

[0017] 1.1 S1 In S1, before continuous casting, the relationship between the local heat flux Q in the portion P and the thickness T of the solidified shell in the portion P is confirmed.

[0018] The present inventor had an opportunity to obtain the solidified shell (solidified shell after BO) remaining in the mold of the continuous casting machine after breakout. When the properties of the solidified shell after BO were observed and analyzed, it was found that the thickness of the solidified shell was thinner in the part P where the discharge flow from the submerged nozzle collided with the part P compared with other parts. In addition, when the actual value (history) of the local heat flux Q obtained by the temperature sensor installed in the mold during the continuous casting was compared with the properties of the solidified shell after BO, it was found that the local heat flux Q was higher in the part P where the discharge flow from the submerged nozzle collided with the part P and the thickness of the solidified shell was thinner than in other parts. Furthermore, it was found that there is a clear correlation between the local heat flux Q and the thickness T of the solidified shell in the part P. That is, it was found that the relationship between the local heat flux Q obtained by the temperature sensor installed in the mold and the thickness T of the solidified shell in the part P can be expressed by a mathematical formula (relational formula). In the method of the present disclosure, for example, the relationship between the local heat flux Q in the part P and the thickness T of the solidified shell in the part P may be expressed by a linear equation (Q=aT+b, where the constants a and b are each determined according to the operating conditions of continuous casting).

[0019] The method of confirming the relationship between the local heat flux Q at the portion P and the thickness T of the solidified shell at the portion P before continuous casting is not limited to the above-mentioned method of observing and analyzing the solidified shell after BO. In the method disclosed herein, it is not necessary to perform continuous casting with an actual machine just to confirm the relationship between the local heat flux Q at the portion P and the thickness T of the solidified shell at the portion P in advance. The position of the portion P may be confirmed before continuous casting, for example, by a simulation experiment using a water model or an analysis using a simulation. The solidified shell thickness may be estimated, for example, by adding FeS or the like during casting. However, it is considered that the relationship can be obtained more accurately when the relationship is confirmed based on the result of continuous casting with an actual machine (for example, the above-mentioned solidified shell after BO). In this regard, in the method disclosed herein, the relationship between the local heat flux Q at the portion P and the thickness T of the solidified shell at the portion P may be confirmed based on the actual value of the local heat flux Q obtained by a temperature sensor installed in the mold during continuous casting and the properties of the solidified shell after BO obtained after breakout during the continuous casting.

[0020] The present inventors also found that, from the actual values ​​of the local heat flux obtained by a temperature sensor installed in the mold during continuous casting and from the observation and analysis of the solidified shell after BO, the local heat flux Q changes over time at the portion P where the discharge flow from the submerged nozzle collides, and the solidified shell becomes thinner or thicker. In this regard, by monitoring the change over time of the local heat flux Q at the portion P during continuous casting, it is also possible to monitor the change in the flow rate of the discharge flow from the submerged nozzle. In addition, when the flow rate of the discharge flow from the submerged nozzle changes and the thickness T of the solidified shell at the portion P becomes thinner, breakout (e.g., remelting breakout) is likely to occur. According to the method disclosed herein, the thickness T of the solidified shell at the portion P can be accurately estimated, making it easier to prevent such breakout.

[0021] The "portion P of the solidified shell with which the discharge flow from the submerged entry nozzle collides" may be specified by taking into consideration the direction and shape of the discharge port of the submerged entry nozzle, the shape of the mold, the flow rate of the discharge flow, etc. In the method of the present disclosure, the portion P with which the discharge flow from the submerged entry nozzle collides may be specified as a point or as a range. In the method of the present disclosure, the thickness of the entire portion with which the discharge flow from the submerged entry nozzle collides may be estimated, or the thickness of a portion of the portion with which the discharge flow from the submerged entry nozzle collides may be estimated.

[0022] 1.2 S2 In S2, during continuous casting, the local heat flux Q in the part P is obtained by a temperature sensor installed in the mold.

[0023] The method disclosed herein accurately estimates the thickness T of the solidified shell at a portion P where the discharge flow from the submerged entry nozzle collides with the solidified shell during continuous casting, and provides the desired effect regardless of the type of continuous casting machine, the operating conditions of continuous casting, etc. In the method disclosed herein, any of general continuous casting machines and general operating conditions can be adopted.

[0024] The type of temperature sensor installed in the mold is not particularly limited, and for example, a known thermocouple or FBG sensor may be used. In the method of the present disclosure, at least one temperature sensor may be installed in at least a portion of the mold corresponding to the portion P where the discharge flow from the submerged nozzle collides with the solidified shell (for example, a portion facing the portion P). The temperature sensor may be embedded in the wall of the mold. The temperature sensor may be embedded in a plurality of locations on the long and short sides of the mold. The method of determining the local heat flux Q in the portion P based on the measurement results by the temperature sensor embedded in the mold is also not particularly limited, and a known method may be used. The local heat flux Q may be determined, for example, by dividing the difference in temperature measured by two temperature sensors at different distances from the molten metal by the distance between the sensors and multiplying the result by the thermal conductivity of the mold wall (copper plate).

[0025] 1.3 S3 In S3, during continuous casting, the thickness T of the solidified shell at the portion P is estimated based on the relationship confirmed in S1 and the local heat flux Q obtained by the temperature sensor in S2.

[0026] For example, in S1, a relational equation between the local heat flux Q at part P and the thickness T of the solidified shell at part P is specified, and then in S2, the local heat flux Q at part P is obtained by a temperature sensor installed at a part corresponding to part P where the discharge flow from the submerged entry nozzle collides with the solidified shell, and the thickness T of the solidified shell can be estimated by substituting the local heat flux Q obtained by the temperature sensor into the relational equation.

[0027] As described above, by going through S1 to S3, it is possible to accurately estimate the thickness T of the portion P of the solidified shell in the mold where the discharge flow from the submerged entry nozzle collides with the solidified shell during continuous casting of molten metal. The thickness T of the solidified shell in the portion P is likely to vary due to changes in the flow rate of the discharge flow, etc., and is considered to be a portion that is likely to cause a breakout. In this regard, by accurately estimating the thickness T of the solidified shell in the portion P using the method disclosed herein, it becomes easier to prevent a breakout.

[0028] 2. Continuous casting method of molten metal As described above, in the portion P where the discharge flow from the submerged nozzle collides, the thickness T of the solidified shell becomes thinner than in other portions, and the local heat flux Q increases compared to other portions. In addition, the discharge flow from the submerged nozzle does not always maintain a constant flow rate, and the thickness T of the solidified shell in the portion P also changes over time, and the local heat flux Q also changes over time. If the thickness T of the solidified shell in the portion P becomes too thin, it is likely to cause a breakout, so it is necessary to accurately estimate the thickness T of the solidified shell in the portion P and control the thickness T so that it does not become too thin. Here, as described above, the present inventor has found that there is a clear correlation between the local heat flux Q and the thickness T of the solidified shell in the portion P. By utilizing this relationship, it becomes easier to prevent a breakout by monitoring the local heat flux Q and the solidified shell thickness T in the portion P.

[0029] 2.1 First form FIG. 2 shows an example of the flow of a method for continuous casting of molten metal. The continuous casting method of the present disclosure is a method for continuously casting the molten metal while discharging the molten metal from a submerged nozzle into a mold and forming a solidified shell in the mold. As shown in FIG. 2, the continuous casting method according to the first embodiment includes confirming, before continuous casting, a relationship between a local heat flux Q at a portion P of the solidified shell formed in the mold where the discharge flow from the submerged nozzle collides and a thickness T of the solidified shell at the portion P (S11), determining the local heat flux Q at the portion P during continuous casting by a temperature sensor installed in the mold (S12), determining an estimated value of the thickness T of the solidified shell at the portion P based on the relationship and the local heat flux Q determined by the temperature sensor during continuous casting (S13), and determining the possibility of breakout based on the estimated value of the thickness T during continuous casting (S14).

[0030] 2.1.1 S11 to S13 S11 to S13 may be the same as S1 to S3 above.

[0031] 2.1.2 S14 In S14, during continuous casting, a determination is made as to the possibility of a breakout occurring based on the estimated value of thickness T obtained in S13.

[0032] As described above, if the thickness T of the portion P becomes too thin, the possibility of breakout increases. In this regard, in the method disclosed herein, for example, when the estimated value of the thickness T of the portion P is small outside a predetermined range, it may be determined that the thickness T of the portion P is too thin, and that there is a possibility of breakout. In this case, a threshold value may be set for the estimated value of the thickness T, and when the estimated value of the thickness T becomes small based on the threshold value (when the estimated value of the thickness T falls below the threshold value or becomes equal to or less than the threshold value), it may be determined that the solidified shell in the portion P is excessively remelted, and that there is a possibility of remelting breakout. The threshold value may be appropriately determined according to the operating conditions of continuous casting, etc. Also, the threshold value may be changed according to the casting speed of continuous casting.

[0033] In S14, when the estimated value of the thickness T obtained in S13 during continuous casting becomes 0, it may be determined that there is a possibility of a breakout. This is because when the estimated value of the thickness T is 0, there is a high possibility that the solidified shell is interrupted and broken (or is about to break) at the portion P, which is considered to further increase the possibility of a breakout.

[0034] 2.1.3 Other processes In the continuous casting method of the present disclosure, when it is determined in S14 that there is a possibility of breakout, the occurrence of breakout can be prevented by promoting the growth of the solidified shell by slowing down the casting speed, increasing the amount of cooling (amount of heat removal) of the mold, etc. In other words, the method of the present disclosure may include controlling the casting speed based on the above-mentioned determination of breakout, or may include controlling the amount of cooling of the mold based on the above-mentioned determination of breakout.

[0035] 2.2 Second form In the first embodiment, a form in which a breakout is predicted based on an estimated value of the thickness T of the solidified shell at a portion P has been described, but the continuous casting method of the present disclosure is not limited to this form. FIG. 3 shows another example of the flow of a continuous casting method for molten metal. The continuous casting method of the present disclosure is a method in which molten metal is discharged from an immersion nozzle into a mold, and the molten metal is continuously cast while a solidified shell is formed in the mold. As shown in FIG. 3, the continuous casting method of the second embodiment includes the steps of: confirming, before continuous casting, the relationship between a local heat flux Q at a portion P of the solidified shell formed in the mold with which the discharge flow from the immersion nozzle collides, and a thickness T of the solidified shell at the portion P (S21); and calculating, based on the relationship, the local heat flux Q at which the thickness T falls within a predetermined range before or during continuous casting. bundle Upper limit of Q limit (S22), determining a local heat flux Q in the portion P during continuous casting by a temperature sensor installed in the mold (S23), and determining the upper limit value Q during continuous casting. limit and comparing the local heat flux Q determined by the temperature sensor with the measured local heat flux Q to determine the possibility of a breakout (S24).

[0036] 2.2.1 S21 S21 may be the same as S1 above.

[0037] 2.2.2 S22 In step S22, a local heat flow rate that causes the thickness T of the solidified shell to fall within a predetermined range is determined based on the relationship confirmed in step S21 before or during continuous casting. bundle Upper limit of Q limit Identify.

[0038] As described above, if the thickness T of the solidified shell in the portion P is too thin, the possibility of a breakout increases. In this regard, in the continuous casting method of the present disclosure, a threshold value (upper limit value) is set for the local heat flux Q so that the thickness T does not become too thin. For example, as described above, there is a clear correlation between the thickness T in the portion P and the local heat flux Q in the portion P, and as the thickness T becomes thinner, the local heat flux Q increases. Therefore, it is necessary to set the thickness T to the minimum necessary thickness (lower limit value T limit ) The upper limit of the local heat flux Q when limit When the above relationship is expressed by a formula, the lower limit T of the thickness T is specified in the formula. limit By substituting, the upper limit Q of the local heat flux Q limit can be identified.

[0039] Upper limit of local heat flux Q limit The upper limit Q of the local heat flux Q may be appropriately determined depending on the operating conditions during continuous casting. limit , the casting speed during continuous casting V c That is, in the continuous casting method of the present disclosure, the casting speed V c Considering the upper limit Q limit For example, V c and Q limit Based on the formula, any V c Q in limit It is possible to identify V c and Q limit The relationship may be expressed by a linear equation.

[0040] In S22, the upper limit Q such that the thickness T becomes 0 is determined based on the relationship confirmed in S21 before or during continuous casting. limit This is because, when the thickness T is 0, it is highly likely that the solidified shell is interrupted and broken (or is about to break) at the portion P, which is considered to further increase the possibility of breakout.

[0041] In S22, the casting speed V cIn addition, depending on the type of molten metal, limit For example, when the molten metal is a high carbon steel containing 1.0 mass % or more of C, the upper limit value Q limit may be determined based on the following formula (1): Q limit =1.28×V c +1.49 ··· (1) Here, Q limit is the local heat flux (MW / m 2 ) and V c is the casting speed (m / min).

[0042] As described above, the timing of performing S22 may be before continuous casting, during continuous casting, or both before and during continuous casting. In S22, the casting speed V c During continuous casting, Q limit may be varied.

[0043] 2.2.3 S23 S23 may be the same as S2 above.

[0044] 2.2.4 S24 In S24, during continuous casting, the upper limit value Q limit This is compared with the local heat flux Q obtained by the temperature sensor in S23 to determine the possibility of a breakout.

[0045] As described above, if the thickness T in the portion P becomes too thin, the possibility of breakout increases. Here, there is a clear correlation between the thickness T and the local heat flux Q, and the greater the local heat flux Q, the thinner the thickness T becomes. In this regard, in the method of the present disclosure, the upper limit value Q specified in S22 is limit If the local heat flux Q is too large (for example, the local heat flux Q is greater than the upper limit Q limit If it exceeds the upper limit Q limitor more), it may be determined that the thickness T at the portion P is too thin, and that there is a possibility of a breakout occurring.

[0046] 2.2.5 Other processes In the continuous casting method according to the second embodiment, similarly to the continuous casting method according to the first embodiment, when it is determined in S24 that there is a possibility of breakout, the occurrence of breakout can be prevented by promoting the growth of the solidified shell by slowing down the casting speed, increasing the amount of cooling (amount of heat removal) of the mold, etc. In other words, the method disclosed herein may include controlling the casting speed based on the above-mentioned determination of breakout, or may include controlling the amount of cooling of the mold based on the above-mentioned determination of breakout.

[0047] As described above, in either of the continuous casting methods of the first and second embodiments, it is possible to predict the breakout with high accuracy.

[0048] 3. Supplementary Information In the technology of the present disclosure, there is no particular limitation on the type of molten metal to be continuously cast. The molten metal may be molten steel or a molten metal other than molten steel.

[0049] In the technology of the present disclosure, the thickness of the solidified shell generated in the mold other than the portion P where the discharge flow from the submerged entry nozzle collides may or may not be estimated. When the thickness of the solidified shell is estimated, the thickness may be estimated in the same manner as the method of the present disclosure. EXAMPLES

[0050] The effects of the technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples. In the following examples, a continuous casting method for high carbon steel containing 1.0 mass % or more of C is illustrated, but the type of molten metal to be continuously cast in the technology of the present disclosure is not particularly limited. In addition, other continuous casting conditions are not limited to the following conditions.

[0051] 1. Continuous casting test conditions Continuous casting tests were carried out under the following conditions. The material to be cast was molten steel (railway steel) with the composition shown in Table 1 below. In each test, the casting speed was 1 m / min, the size of the mold was 600 mm wide x 100 mm thick, the position of the submerged entry nozzle was the center of the mold width and thickness directions, and the outlet angle of the submerged entry nozzle was 10° upward. In addition, a temperature sensor (FBG (Fiber Bragg Grating) sensor: a temperature sensor using optical fiber) installed in the center of the short side made it possible to measure the temperature of the copper plate of the mold at 47 mm intervals in the casting direction.

[0052] [Table 1]

[0053] In the above continuous casting test, the solidified shell was restrained at one short side of the mold, causing a breakout. At this time, a sound solidified shell could be obtained from the other short side of the mold. Figure 4 shows a cut surface at the center of the thickness of the obtained solidified shell. The thickness distribution of this solidified shell was compared with the heat flux at the short side of the mold.

[0054] 2.Analysis It is assumed that the strong discharge flow impinges on the short side of the mold, increasing the heat transfer coefficient from the molten steel and causing the heat flux at that location to be higher than the surrounding area, and so the local heat flux was organized according to the distance from the meniscus. Hereafter, the distance from the meniscus on the horizontal axis and local heat flux on the vertical axis are referred to as the local heat flux profile. The local heat flux was calculated by dividing the difference in temperature measured by two FEB sensors at different distances from the molten steel by the distance between the sensors, and multiplying this by the thermal conductivity of the copper plate (Equation I below). The manufacturer's published value of 352 MW / m K was used for the copper plate heat transfer coefficient.

[0055]

number

[0056] To verify whether instantaneous drift in the flow could be detected, the local heat flux profile and solidified shell thickness at a specified time were compared. The obtained distribution of solidified shell thickness is shown in Figure 5. As shown in Figure 5, the actual measured value of the solidified shell thickness is thinner than the theoretical value from approximately 200 mm to approximately 600 mm from the meniscus, and it is believed that re-melting is occurring due to the discharge flow.

[0057] The local heat flux profile when the solidified shell was generated is shown in Figure 6. The local heat flux shown in Figure 6 is a time average every 5 seconds, and is for the 25 seconds just before the breakout. Looking at Figure 6, an increase in the local heat flux can be confirmed at a position about 300 mm from the meniscus between 152 seconds and 162 seconds. Figure 7 shows the time change in the local heat flux at a position about 300 mm from the meniscus. The local heat flux increases for 14 seconds just before the breakout, and the length cast during this 14 seconds is about 250 mm. The part of the solidified shell that seems to have remelted is 400 mm from 200 to 600 mm, and this result is not contradictory if we consider that the solidified shell above and below the collision position of the strong discharge flow was also affected by the strong discharge flow.

[0058] From the above results, it was found that the effect of the discharge flow can be captured by calculating the local heat flux at the position where the discharge flow collides with the solidified shell at regular intervals and monitoring its changes.

[0059] Here, the values ​​of the solidified shell thickness and the local heat flux are organized in order to calculate the critical heat flux leading to breakout. To organize, the solidified shell thickness at a point 286 mm from the molten metal surface (hereinafter referred to as "point A") was calculated by the following method. Figure 8 shows the difference between the theoretical value and the actual value of the solidified shell thickness. The difference between the theoretical value and the actual value corresponds to the change over time in the influence of the discharge flow. Below, assuming that remelting occurs at point A by this difference, the relationship between the solidified shell thickness and the local heat flux at point A is organized in Figures 9 and 10. As shown in Figure 9, at point A, the actual measured value of the local heat flux fluctuates, and the solidified shell thickness also fluctuates accordingly. Looking at the relationship between the solidified shell thickness and the local heat flux as in Figure 10, it is possible to organize it by a linear equation such as the following equation (II).

[0060]

number

[0061] From the above formula (II), for example, the solidified shell thickness becomes 0 mm when the local heat flux is about 2.8 MW / m 2 That is, under the continuous casting conditions in this embodiment, when the casting speed is 1.0 m / min, the local heat flux is about 2.8 MW / m 2 When the price exceeds this threshold, it may be determined that a breakout is likely.

[0062] It is considered that the local heat flux increases as the casting speed increases. In other words, the critical local heat flux Q limit When considering the effect of the casting speed, it is preferable to consider the influence of the casting speed. Therefore, the casting speed and the local heat flux at point A were arranged based on other tests (Fig. 11). As a result, the average value of the local heat flux Q, Q ave and casting speed V cIt was found that this can be expressed by the following formula (III):

[0063]

number

[0064] Critical local heat flux Q leading to breakout limit Assuming that the slope is the same even in limit is determined by the following formula (IV): Formula (IV) is considered to be applicable to the continuous casting of high carbon steel containing 1.0 mass % or more of C.

[0065]

number

[0066] 3. Summary As described above, a casting test was performed using a mold with a built-in temperature sensor (FBG sensor), and the local heat flux profile of the mold short side was calculated from the temperature measurement data obtained during the casting test. It was found that the heat flux at the discharge flow impingement position increased at the time when remelting of the solidified shell was observed. There is a clear correlation between the local heat flux Q at the discharge flow impingement position and the solidified shell thickness T, and it can be said that the solidified shell thickness at the discharge flow impingement position can be accurately estimated from this correlation. The relationship between the local heat flux Q and the solidified shell thickness T can be arranged, for example, by a linear equation. In addition, it can be said that the occurrence of a breakout can be accurately predicted by determining that there is a possibility of a breakout occurring when the estimated value of the solidified shell thickness T falls outside a predetermined range and becomes thin. Alternatively, it can be said that the occurrence of a breakout can be accurately predicted by determining that there is a possibility of a breakout occurring when the estimated value of the solidified shell thickness T falls outside a predetermined range. limit Calculate the actual value Q of the local heat flux and the upper limit Q limit For example, the actual measured value Q is compared with the upper limit value Q limit If the casting speed V exceeds the casting speed V, it is judged that there is a possibility of a breakout.c The upper limit of the local heat flux Q is Q limit Since the casting speed V can change, for example, c and upper limit Q limit After sorting out the relationship with V c Depending on Q limit It is preferable to specify c and Q limit The relationship between these two can be expressed, for example, by a linear equation.

Claims

1. A method for estimating a thickness T of a portion P of a solidified shell formed in a mold during continuous casting of molten metal, the portion P being struck by a discharge flow from an immersion nozzle, the method comprising: Before continuous casting, a relationship between a local heat flux Q in the portion P and a thickness T of the solidified shell in the portion P is confirmed; During continuous casting, a change in local heat flux Q over time in the portion P is determined by a temperature sensor installed in the mold; and, estimating a change in thickness T of the solidified shell over time at the portion P based on the relationship and the change in thickness T of the local heat flux Q determined by the temperature sensor during continuous casting; A method for estimating solidified shell thickness, including:

2. A method for continuously casting molten metal by discharging the molten metal from an immersion nozzle into a mold and forming a solidified shell in the mold, comprising: Before continuous casting, a relationship between a local heat flux Q at a portion P of the solidified shell generated in the mold with which the discharge flow from the submerged entry nozzle collides and a thickness T of the solidified shell at the portion P is confirmed. During continuous casting, a change in local heat flux Q over time in the portion P is determined by a temperature sensor installed in the mold; determining, during continuous casting, a change over time in an estimated value of a thickness T of the solidified shell at the portion P based on the relationship and the change over time in the local heat flux Q determined by the temperature sensor; and, During continuous casting, determining the possibility of breakout based on a change over time in the estimated value of the thickness T; A method for continuous casting of molten metal, comprising:

3. When the estimated value of the thickness T becomes 0 during continuous casting, it is determined that there is a possibility of breakout.

3. The method for continuous casting of molten metal according to claim 2, comprising:

4. A method for continuously casting molten metal by discharging the molten metal from an immersion nozzle into a mold and forming a solidified shell in the mold, comprising: Before continuous casting, a relationship between a local heat flux Q at a portion P of the solidified shell generated in the mold with which the discharge flow from the submerged entry nozzle collides and a thickness T of the solidified shell at the portion P is confirmed. Before or during continuous casting, based on the relationship, an upper limit value Q of the local heat flux Q that makes the thickness T fall within a predetermined range is determined. limit Identifying the During continuous casting, a change in local heat flux Q over time in the portion P is determined by a temperature sensor installed in the mold; and, During continuous casting, the upper limit Q limit and comparing the change over time in the local heat flux Q obtained by the temperature sensor to determine whether or not a breakout is likely to occur. A method for continuous casting of molten metal, comprising:

5. Casting speed during continuous casting V c Considering the upper limit Q limit Identifying the The continuous casting method according to claim 4, comprising:

6. Before or during continuous casting, the upper limit Q is set based on the relationship so that the thickness T becomes 0. limit Identifying the The continuous casting method according to claim 4 or 5, comprising:

7. When the molten metal is a high carbon steel containing 1.0 mass % or more of C, the upper limit Q limit is determined based on the following formula (1): The continuous casting method according to any one of claims 4 to 6, comprising: Q limit =1.28×V c +1.49 ・・・ (1) Here, Q limit is the local heat flux (MW / m 2 ) and V c is the casting speed (m / min).

Citation Information

Patent Citations

  • Method for predicting breakout in continuous casting

    JP1983148061A

  • Detection of leaning flow of molten steel in mold at continuous casting of steel and method for continuous casting steel

    JP1989262050A

  • Preventing method for drifting break-out

    JP1990052158A

  • Method for detecting channeling flow of molten steel in continuous casting mold

    JP1991032457A

  • Method for measuring thickness of solidified shell in continuous casing and instrument therefor

    JP1998277716A