Modified Polytetrafluoroethylene

The modified PTFE formulation with TFE and CTFE units addresses the challenge of high breaking strength and low extrusion pressure, ensuring uniform processing and improved moldability.

JP7583316B2Active Publication Date: 2024-11-14DAIKIN INDUSTRIES LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023131061
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-08-10
Filing Date
2023-08-10
Publication Date
2024-11-14
Estimated Expiration
2043-08-10

AI Technical Summary

Technical Problem

Existing polytetrafluoroethylene (PTFE) formulations face challenges in achieving high breaking strength while maintaining low extrusion pressure, leading to issues with moldability and processing difficulties.

Method used

A modified PTFE composition containing tetrafluoroethylene (TFE) and chlorotrifluoroethylene (CTFE) units, with CTFE units limited to 1.0% by mass, enhances breaking strength and reduces extrusion pressure, resulting in improved moldability and stretchability.

Benefits of technology

The modified PTFE achieves high breaking strength with low extrusion pressure, ensuring uniform processing and preventing breakage during stretching, while maintaining excellent moldability and stretchability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583316000001
    Figure 0007583316000001
Patent Text Reader

Abstract

To provide modified polytetrafluoroethylene which has a low extrusion pressure in spite of high break strength.SOLUTION: Modified polytetrafluoroethylene is drawable and contains a tetrafluoroethylene unit and a chlorotrifluoroethylene unit. An amount of the chlorotrifluoroethylene unit is 1.0 mass% or less relative to all polymer units.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to modified polytetrafluoroethylene. [Background technology]

[0002] When polytetrafluoroethylene is molded and highly stretched in an unsintered state, a porous polytetrafluoroethylene film is obtained. This porous film allows gases such as water vapor to pass through, but does not allow water droplets to pass through due to the strong water repellency of polytetrafluoroethylene. Taking advantage of this unique property, it is used in clothing, separation membranes, etc.

[0003] Patent Document 1 describes a modified tetrafluoroethylene polymer obtained by a specific production method using chlorotrifluoroethylene as a modifier for the purpose of improving paste extrudability.

[0004] Patent Documents 2 to 4 describe tetrafluoroethylene homopolymers and modified polytetrafluoroethylenes having units based on perfluoro(propyl vinyl ether) or hexafluoropropylene, which are used for stretching. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 51-36291 [Patent Document 2] JP 2000-143707 A [Patent Document 3] International Publication No. 2007 / 046345 [Patent Document 4] International Publication No. 2010 / 113950 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present disclosure is to provide a modified polytetrafluoroethylene that has high breaking strength yet requires low extrusion pressure. [Means for solving the problem]

[0007] The present disclosure (1) is directed to a stretchable modified polytetrafluoroethylene which contains tetrafluoroethylene units and chlorotrifluoroethylene units, in which the amount of the chlorotrifluoroethylene units is 1.0 mass % or less based on all polymerized units.

[0008] The present disclosure (2) is the modified polytetrafluoroethylene according to the present disclosure (1), which has a breaking strength of 20.0 N or more.

[0009] The present disclosure (3) is the modified polytetrafluoroethylene according to the present disclosure (1) or (2), which has an extrusion pressure of 5 MPa or more.

[0010] The present disclosure (4) is a modified polytetrafluoroethylene in any combination with any of the present disclosures (1) to (3) having an extrusion pressure of 50 MPa or less.

[0011] The present disclosure (5) is a modified polytetrafluoroethylene in any combination with any of the present disclosures (1) to (4), having a strength ratio expressed by breaking strength / extrusion pressure of more than 1.90 N / MPa.

[0012] The present disclosure (6) is a modified polytetrafluoroethylene in any combination with any of the present disclosures (1) to (5) in powder form.

[0013] The present disclosure (7) is a modified polytetrafluoroethylene in any combination with any of the present disclosures (1) to (6) which are fine powders. Effect of the Invention

[0014] According to the present disclosure, it is possible to provide a modified polytetrafluoroethylene that has high breaking strength but low extrusion pressure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] When polytetrafluoroethylene (PTFE) is modified into PTFE, the primary particle size becomes smaller, and the extrusion pressure tends to increase accordingly. In general, the breaking strength can be increased by increasing the extrusion pressure, but the paste extrudate tends to become hard and the moldability of the extrudate tends to deteriorate. In addition, if the paste extrudate is hard, it may become non-uniform in post-processing and may break during processing, such as during stretching, so a low extrusion pressure is preferable. However, after extensive research, it was discovered that by using chlorotrifluoroethylene as a modified monomer and controlling the polymerization conditions to produce a high molecular weight polymer that can be stretched, it is possible to obtain PTFE that has high breaking strength but low extrusion pressure, contrary to common technical knowledge.

[0016] The present disclosure will now be described in detail.

[0017] The present disclosure provides a stretchable modified PTFE which contains tetrafluoroethylene (TFE) units and chlorotrifluoroethylene (CTFE) units, in which the amount of the CTFE units is 1.0 mass % or less based on all polymerized units. The modified PTFE of the present disclosure has the above-mentioned configuration, and therefore has high breaking strength, low extrusion pressure, and excellent moldability. CTFE has a structure similar to TFE, and it is presumed that the increase in extrusion pressure is suppressed because the PTFE crystal structure is less likely to collapse.

[0018] The modified PTFE of the present disclosure contains TFE units (polymerized units based on TFE) and CTFE units (polymerized units based on CTFE), and the amount of CTFE units is 1.0 mass % or less based on the total polymerized units. The content of TFE units in the modified PTFE may be 99.0% by mass or more.

[0019] The modified PTFE may further contain polymerization units (other modified monomer units) based on modified monomers other than TFE and CTFE, or may consist only of TFE units and CTFE units, but is preferably composed only of TFE units and CTFE units.

[0020] Examples of the other modifying monomers include fluorine-containing olefins such as hexafluoropropylene; fluoro(alkyl vinyl ethers) having an alkyl group having 1 to 5 carbon atoms, particularly 1 to 3 carbon atoms; cyclic fluorinated monomers such as fluorodioxole; perfluoroalkylethylene; and ω-hydroperfluoroolefins.

[0021] The content of the other modified monomer units is preferably less than 1.0% by mass, and more preferably 0.1% by mass or less, based on the total polymerized units. The total amount of the CTFE units and the other modified monomer units is preferably 1.0% by mass or less based on the total polymerized units.

[0022] The content of the CTFE units is 1.0% by mass or less based on the total polymerization units, but in terms of lowering the extrusion pressure and increasing the breaking strength, it is preferably 0.50% by mass or less based on the total polymerization units, more preferably 0.30% by mass or less, even more preferably 0.20% by mass or less, even more preferably 0.10% by mass or less, and even more preferably 0.08% by mass or less. The content of the CTFE units may be 0.0001% by mass or more, or may be 0.001% by mass or more, based on the total polymerized units. In this specification, the CTFE unit means a portion of the molecular structure of the modified PTFE that is derived from CTFE.

[0023] The content of each of the above-mentioned polymer units can be calculated by appropriately combining NMR, FT-IR, elemental analysis, and X-ray fluorescence analysis depending on the type of monomer.

[0024] The modified PTFE of the present disclosure is stretchable. The conventional CTFE-modified PTFE described in Patent Document 1, which is intended to improve paste extrudability, is not sufficiently high-molecular-weight and cannot be stretched. In this specification, "stretchable" is determined according to the following criteria. The bead obtained by paste extrusion, as described below, is heated at 230°C for 30 minutes to remove the lubricant from the bead. The bead (extrudate) is then cut to the appropriate length, clamped at each end with a clamp distance of 2.0 inches (51 mm) between the clamps, and heated to 300°C in an air circulating oven. The clamps are then moved apart at a desired speed (stretch rate) until a separation distance corresponding to the desired stretch (total stretch) is achieved, and a stretch test is performed. This stretching method essentially follows that disclosed in U.S. Pat. No. 4,576,869, except for the extrusion speed (51 cm / min instead of 84 cm / min). "Stretch" is the increase in length due to stretching, and is usually expressed in relation to the original length. In the above preparation method, the stretch rate is 1000% / sec and the total stretch is 2400%. A stretchable material is considered to be stretchable if it does not break before the stretch is completed.

[0025] In the above-mentioned production method, the modified PTFE of the present disclosure is preferably subjected to a stretch test under conditions of a stretch rate of 100% / sec and a total stretch of 2400%, and does not break before the above-mentioned stretching is completed.

[0026] The modified PTFE of the present disclosure preferably has a breaking strength of 20.0 N or more, more preferably 25.0 N or more, even more preferably 30.0 N or more, even more preferably 32.0 N or more, and even more preferably 35.0 N or more. The higher the breaking strength, the better, but it may be 100.0 N or less, 80.0 N or less, or 50.0 N or less. The breaking strength is a value determined by the following method. The stretched bead (produced by stretching the bead) obtained in the stretching test carried out at the above stretch speed of 100% / sec is clamped and fixed in a movable jaw having a gauge length of 5.0 cm, and a tensile test is carried out at 25°C and a speed of 300 mm / min, and the strength at the time of break is measured as the breaking strength.

[0027] The modified PTFE of the present disclosure has an extrusion pressure of preferably 50.0 MPa or less, more preferably 40.0 MPa or less, even more preferably 30.0 MPa or less, even more preferably 25.0 MPa or less, even more preferably 23.0 MPa or less, even more preferably 21.0 MPa or less, and particularly preferably 20.0 MPa or less. The extrusion pressure may be 5.0 MPa or more, 10.0 MPa or more, 12.0 MPa or more, 15.0 MPa or more, or 17.0 MPa or more. The above extrusion pressure is a value determined by the following method. 21.7 g of lubricant (trade name: Isopar H (registered trademark), manufactured by Exxon Corp.) is added to 100 g of modified PTFE powder, and mixed at room temperature for 3 minutes to obtain a PTFE fine powder mixture. The obtained PTFE fine powder mixture is then left at room temperature (25°C) for at least 1 hour before extrusion, and then paste extruded at room temperature through an orifice (diameter 2.5 mm, land length 11 mm, introduction angle 30°) at a reduction ratio of 100:1 (ratio of cross-sectional area of ​​the inlet and outlet of the die) to obtain a uniform bead (beading; extrusion molded body). The extrusion speed, i.e., the ram speed, is 20 inches / min (51 cm / min). The extrusion pressure is the value obtained by measuring the load when the extrusion load reaches equilibrium in the paste extrusion and dividing it by the cross-sectional area of ​​the cylinder used for the paste extrusion.

[0028] The modified PTFE of the present disclosure has a strength ratio expressed by breaking strength (N) / extrusion pressure (MPa) of preferably more than 1.90 N / MPa, more preferably 1.95 N / MPa or more, even more preferably 2.00 N / MPa or more, even more preferably 2.05 N / MPa or more, and particularly preferably 2.10 N / MPa or more. The higher the strength ratio, the better, but it may be 5.00 N / MPa or less, or may be 4.00 N / MPa or less. A higher strength ratio means a higher breaking strength and a lower extrusion pressure. The breaking strength and extrusion pressure are values ​​determined by the above-mentioned method.

[0029] In view of excellent extensibility, the modified PTFE of the present disclosure more preferably has a standard specific gravity (SSG) of 2.180 or less, even more preferably 2.170 or less, and particularly preferably 2.160 or less. The standard specific gravity is also preferably 2.130 or more. The standard specific gravity is measured by a water displacement method according to ASTM D 792 using a sample molded according to ASTM D 4895.

[0030] The modified PTFE of the present disclosure generally has non-melt secondary processability. The non-melt secondary processability means that the melt flow rate cannot be measured at a temperature higher than the melting point in accordance with ASTM D-1238 and D-2116, in other words, that the PTFE does not flow easily even in the melting temperature range.

[0031] In the modified PTFE of the present disclosure, in the absence of a history of heating to a temperature of 300°C or higher, it is preferable that in a heat of fusion curve obtained by heating at a rate of 10°C / min using a differential scanning calorimeter [DSC], one or more endothermic peaks appear in the range of 333 to 347°C, and the heat of fusion at 290 to 350°C calculated from the heat of fusion curve is 62 mJ / mg or more.

[0032] The modified PTFE of the present disclosure can be produced, for example, by a production method including a step of emulsion polymerization of TFE and CTFE (and other modifying monomers as necessary).

[0033] The above emulsion polymerization can be carried out, for example, in an aqueous medium in the presence of an anionic fluorine-containing surfactant and a polymerization initiator. The emulsion polymerization can be carried out by charging an aqueous medium, the anionic fluorine-containing surfactant, monomers and, if necessary, other additives into a polymerization reactor, stirring the contents of the reactor, maintaining the reactor at a predetermined polymerization temperature, and then adding a predetermined amount of polymerization initiator to initiate the polymerization reaction. After the start of the polymerization reaction, monomers, polymerization initiators, chain transfer agents, the surfactants and the like may be additionally added depending on the purpose.

[0034] In terms of easily obtaining the above-mentioned properties, the CTFE concentration in the gas in the reactor at the start of polymerization (when the initiator is added) is preferably 0.001 mol% or more, more preferably 0.01 mol% or more. The above concentration is also preferably 3.0 mol% or less, more preferably 1.0 mol% or less. The modified monomer concentration may be maintained until the end of the polymerization reaction, or pressure may be released during the reaction. In terms of obtaining excellent stretching properties, it is preferable to charge CTFE all at once before the start of polymerization, but a portion of it may be added continuously or intermittently after the start of polymerization.

[0035] The polymerization initiator is not particularly limited as long as it can generate radicals within the polymerization temperature range, and known oil-soluble and / or water-soluble polymerization initiators can be used. Furthermore, it can also be combined with a reducing agent or the like to initiate polymerization as a redox. The concentration of the polymerization initiator is appropriately determined depending on the type of monomer, the molecular weight of the desired modified PTFE, and the reaction rate.

[0036] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical polymerization initiator can be used.

[0037] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, for example, dialkyl peroxycarbonates such as diisopropyl peroxydicarbonate and disec-butyl peroxydicarbonate, peroxyesters such as t-butyl peroxyisobutyrate and t-butyl peroxypivalate, dialkyl peroxides such as di-t-butyl peroxide, and the like. In addition, di(ω-hydro-dodecafluoroheptanoyl) peroxide, di(ω-hydro-tetradecafluoroheptanoyl) peroxide, di(ω-hydro-hexadecafluorononanoyl) peroxide, di(perfluorobutyryl) peroxide, di(perfluorovaleryl) peroxide, di(perfluorohexanoyl) peroxide, di(perfluoroheptanoyl) peroxide, di(perfluorooctanoyl) peroxide, di(perfluorononanoyl) peroxide, di(ω-chloro Representative examples include di[perfluoro(or fluorochloro)acyl]peroxides such as di(ω-hexafluorobutyryl) peroxide, di(ω-chloro-decafluorohexanoyl) peroxide, di(ω-chloro-tetradecafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexadecafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydrododecafluoroheptanoyl-perfluorobutyryl-peroxide, di(dichloropentafluorobutanoyl) peroxide, di(trichlorooctafluorohexanoyl) peroxide, di(tetrachloroundecafluorooctanoyl) peroxide, di(pentachlorotetradecafluorodecanoyl) peroxide, and di(undecachlorodotriacontafluorodocosanoyl) peroxide.

[0038] The water-soluble radical polymerization initiator may be a known water-soluble peroxide, such as ammonium salts, potassium salts, or sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, or percarbonic acid, t-butyl permaleate, or t-butyl hydroperoxide, etc. A reducing agent such as sulfites or sulfites may also be contained, and the amount used may be 0.1 to 20 times that of the peroxide.

[0039] The amount of the water-soluble radical polymerization initiator to be added is not particularly limited, but may be added all at once, stepwise, or continuously at the beginning of polymerization in an amount (for example, several ppm to water concentration) that does not significantly reduce the polymerization rate. The upper limit is a range in which the reaction temperature may be increased while removing heat from the equipment side by the polymerization reaction heat, and a more preferred upper limit is a range in which the polymerization reaction heat can be removed from the equipment side. More specifically, for example, the amount is preferably 1 ppm or more, more preferably 10 ppm or more, and even more preferably 50 ppm or more, relative to the aqueous medium. Also, the amount is preferably 100,000 ppm or less, more preferably 10,000 ppm or less, and even more preferably 5,000 ppm or less. In terms of easily obtaining the above-mentioned physical properties, the amount of the polymerization initiator added is preferably an amount equivalent to 0.1 ppm or more, more preferably an amount equivalent to 1.0 ppm or more, and is preferably an amount equivalent to 100 ppm or less, more preferably an amount equivalent to 10 ppm or less, relative to the aqueous medium.

[0040] For example, when polymerization is carried out at a low temperature of 30° C. or less, it is preferable to use a redox initiator that combines an oxidizing agent and a reducing agent as the polymerization initiator. Examples of the oxidizing agent include persulfates, organic peroxides, potassium permanganate, manganese triacetate, cerium ammonium nitrate, and bromates. Examples of the reducing agent include sulfites, bisulfites, bromates, diimines, and oxalic acid. Examples of the persulfates include ammonium persulfate and potassium persulfate. Examples of the sulfites include sodium sulfite and ammonium sulfite. In order to increase the decomposition rate of the initiator, it is also preferable to add a copper salt or an iron salt to the combination of the redox initiator. Examples of the copper salt include copper(II) sulfate, and examples of the iron salt include iron(II) sulfate.

[0041] As the redox initiator, it is preferred that the oxidizing agent is permanganic acid or a salt thereof, a persulfate, manganese triacetate, a cerium (IV) salt, or bromic acid or a salt thereof, and the reducing agent is a dicarboxylic acid or a salt thereof, or a diimine. More preferably, the oxidizing agent is permanganic acid or a salt thereof, a persulfate, or bromic acid or a salt thereof, and the reducing agent is a dicarboxylic acid or a salt thereof.

[0042] Examples of the redox initiator include combinations of potassium permanganate / oxalic acid, potassium permanganate / ammonium oxalate, manganese triacetate / oxalic acid, manganese triacetate / ammonium oxalate, cerium ammonium nitrate / oxalic acid, and cerium ammonium nitrate / ammonium oxalate. When a redox initiator is used, either the oxidizing agent or the reducing agent may be charged in advance in a polymerization tank, and then the other may be added continuously or intermittently to initiate polymerization. For example, when potassium permanganate / ammonium oxalate is used, it is preferable to charge ammonium oxalate in a polymerization tank and continuously add potassium permanganate thereto. In this specification, when the redox initiator is described as "potassium permanganate / ammonium oxalate," it means a combination of potassium permanganate and ammonium oxalate. The same applies to other compounds.

[0043] The redox initiator is particularly preferably a combination of an oxidizing agent that is a salt and a reducing agent that is a salt. For example, the oxidizing agent which is the salt is more preferably at least one selected from the group consisting of persulfates, permanganates, cerium (IV) salts, and bromates, further preferably permanganates, and particularly preferably potassium permanganate. The reducing agent which is the salt is more preferably at least one selected from the group consisting of oxalates, malonates, succinates, glutarates and bromates, further preferably oxalates, and particularly preferably ammonium oxalate.

[0044] Specifically, the redox initiator is preferably at least one selected from the group consisting of potassium permanganate / oxalic acid, potassium permanganate / ammonium oxalate, potassium bromate / ammonium sulfite, manganese triacetate / ammonium oxalate, and cerium ammonium nitrate / ammonium oxalate, more preferably at least one selected from the group consisting of potassium permanganate / oxalic acid, potassium permanganate / ammonium oxalate, potassium bromate / ammonium sulfite, and cerium ammonium nitrate / ammonium oxalate, and even more preferably potassium permanganate / oxalic acid.

[0045] When a redox initiator is used, the oxidizing agent and the reducing agent may be added all at once at the beginning of the polymerization, the reducing agent may be added all at once at the beginning of the polymerization and the oxidizing agent may be added continuously, the oxidizing agent may be added all at once at the beginning of the polymerization and the reducing agent may be added continuously, or both the oxidizing agent and the reducing agent may be added continuously. When a redox initiator is used as a polymerization initiator, the amount of the oxidizing agent added is preferably 5 ppm or more, more preferably 10 ppm or more, and preferably 10000 ppm or less, more preferably 1000 ppm or less, relative to the aqueous medium. The amount of the reducing agent added is preferably 5 ppm or more, more preferably 10 ppm or more, and preferably 10000 ppm or less, more preferably 1000 ppm or less. In order to easily obtain a modified PTFE suitable for stretching applications, the amount of the oxidizing agent added to the aqueous medium is preferably 0.1 ppm or more, more preferably 1.0 ppm or more, and preferably 100 ppm or less, more preferably 10 ppm or less. The amount of the reducing agent added is preferably 0.1 ppm or more, more preferably 1.0 ppm or more, and preferably 100 ppm or less, more preferably 10 ppm or less. When a redox initiator is used in the emulsion polymerization, the polymerization temperature is preferably 100° C. or lower, more preferably 95° C. or lower, and even more preferably 90° C. or lower. The polymerization temperature is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher.

[0046] As the polymerization initiator, a water-soluble radical polymerization initiator and a redox initiator are preferred, since the above-mentioned properties can be easily obtained.

[0047] The aqueous medium is a reaction medium for polymerization, and refers to a liquid containing water. The aqueous medium is not particularly limited as long as it contains water, and may contain water and, for example, a fluorine-free organic solvent such as an alcohol, ether, or ketone, and / or a fluorine-containing organic solvent having a boiling point of 40° C. or less.

[0048] In the above emulsion polymerization, a nucleating agent, a chain transfer agent, a buffering agent, a pH adjusting agent, a stabilizing aid, a dispersion stabilizer, a radical scavenger, a decomposing agent for the polymerization initiator, and the like may be used, if necessary.

[0049] The emulsion polymerization is preferably carried out with the addition of a nucleating agent for the purpose of adjusting the particle size. The nucleating agent is preferably added before the start of the polymerization reaction. As the nucleating agent, a known agent can be used. For example, it is preferable that the nucleating agent is at least one selected from the group consisting of fluoropolyethers, nonionic surfactants, and chain transfer agents, and it is more preferable that the nucleating agent is a nonionic surfactant.

[0050] The fluoropolyether may, for example, be a perfluoropolyether (PFPE) acid or a salt thereof. The perfluoropolyether (PFPE) acid or salt thereof may have any chain structure in which oxygen atoms in the backbone of the molecule are separated by saturated fluorocarbon groups having 1 to 3 carbon atoms. Also, two or more types of fluorocarbon groups may be present in the molecule. A representative structure has a repeating unit represented by the following formula: (-CFCF3-CF2-O-) n (-CF2-CF2-CF2-O-) n (-CF2-CF2-O-) n -(-CF2-O-) m (-CF2-CFCF3-O-) n -(-CF2-O-) m

[0051] These structures are described by Kasai in J. Appl. Polymer Sci. 57, 797 (1995). As disclosed therein, the PFPE acid or its salt may have a carboxylic acid group or its salt at one or both ends. The PFPE acid or its salt may also have a sulfonic acid, phosphonic acid group or their salt at one or both ends. The PFPE acid or its salt may also have a different group at each end. For monofunctional PFPEs, the other end of the molecule is usually perfluorinated, but may contain hydrogen or chlorine atoms. The PFPE acid or its salt has at least two ether oxygens, preferably at least four ether oxygens, and even more preferably at least six ether oxygens. Preferably, at least one of the fluorocarbon groups separating the ether oxygens, more preferably at least two of such fluorocarbon groups, has two or three carbon atoms. Even more preferably, at least 50% of the fluorocarbon groups separating the ether oxygens have 2 or 3 carbon atoms. Also preferably, the PFPE acid or salt thereof has a total of at least 15 carbon atoms, for example, the preferred minimum value of n or n+m in the repeating unit structure above is at least 5. Two or more of the PFPE acids or salts thereof having an acid group at one or both termini may be used in the manufacturing method of the present disclosure. The PFPE acid or salt thereof preferably has a number average molecular weight of less than 6000 g / mol.

[0052] The emulsion polymerization is preferably carried out by adding a radical scavenger or a decomposer of the polymerization initiator, since it is possible to further increase the molecular weight of the modified PTFE and improve the stretchability. The radical scavenger or the decomposer of the polymerization initiator is preferably added after the start of the polymerization reaction, preferably before 10% by mass or more, preferably 20% by mass or more of the total TFE consumed in the polymerization reaction is polymerized, and preferably before 50% by mass or less, preferably 40% by mass or less is polymerized. When depressurization and repressurization are performed as described below, it is preferable to add it after that.

[0053] The radical scavenger is a compound that does not have the ability to restart after addition or chain transfer to the free radical in the polymerization system. Specifically, a compound that easily undergoes a chain transfer reaction with a primary radical or a growing radical, and then generates a stable radical that does not react with a monomer, or a compound that easily undergoes an addition reaction with a primary radical or a growing radical, and generates a stable radical, is used. Generally, the activity of what is called a chain transfer agent is characterized by the chain transfer constant and the reinitiation efficiency, but among chain transfer agents, those with a reinitiation efficiency of almost 0% are called radical scavengers. The radical scavenger can be, for example, a compound whose chain transfer constant with TFE at the polymerization temperature is greater than the polymerization rate constant and whose reinitiation efficiency is substantially zero percent. "Reinitiation efficiency is substantially zero percent" means that the generated radicals turn the radical scavenger into stable radicals. Preferably, the compound has a chain transfer constant (Cs) with TFE at the polymerization temperature (=chain transfer rate constant (kc) / polymerization rate constant (kp)) of more than 0.1. The above compound has a chain transfer constant (Cs) of more preferably 0.5 or more, even more preferably 1.0 or more, even more preferably 5.0 or more, and particularly preferably 10 or more.

[0054] The radical scavenger is preferably at least one selected from the group consisting of, for example, aromatic hydroxy compounds, aromatic amines, N,N-diethylhydroxylamine, quinone compounds, terpenes, thiocyanates, and cupric chloride (CuCl2). Examples of the aromatic hydroxy compound include unsubstituted phenol, polyhydric phenol, salicylic acid, m- or p-salicylic acid, gallic acid, and naphthol. The unsubstituted phenols include o-, m-, or p-nitrophenol, o-, m-, or p-aminophenol, p-nitrosophenol, etc. The polyhydric phenols include catechol, resorcinol, hydroquinone, pyrogallol, phloroglucinol, naphthresorcinol, etc. Examples of aromatic amines include o-, m- or p-phenylenediamine, benzidine, and the like. Examples of the quinone compound include o-, m- or p-benzoquinone, 1,4-naphthoquinone, alizarin, and the like. Examples of thiocyanates include ammonium thiocyanate (NH4SCN), potassium thiocyanate (KSCN), and sodium thiocyanate (NaSCN). Of the above radical scavengers, aromatic hydroxy compounds are preferred, unsubstituted phenols or polyhydric phenols are more preferred, and hydroquinone is even more preferred.

[0055] The amount of the radical scavenger added is preferably an amount equivalent to 3 to 500% (molar basis) of the polymerization initiator concentration from the viewpoint of appropriately reducing the standard specific gravity. A more preferred lower limit is 10% (molar basis), and even more preferred is 15% (molar basis). A more preferred upper limit is 400% (molar basis), and even more preferred is 300% (molar basis).

[0056] The decomposer for the polymerization initiator may be any compound capable of decomposing the polymerization initiator used, and is preferably at least one selected from the group consisting of sulfites, bisulfites, bromates, diimines, diimine salts, oxalic acid, oxalates, copper salts, and iron salts. Examples of sulfites include sodium sulfite and ammonium sulfite. Examples of copper salts include copper(II) sulfate, and examples of iron salts include iron(II) sulfate. The amount of the decomposition agent added is preferably an amount equivalent to 3 to 500% (molar basis) of the initiator concentration from the viewpoint of appropriately reducing the standard specific gravity. A more preferred lower limit is 10% (molar basis), and even more preferred is 15% (molar basis). A more preferred upper limit is 400% (molar basis), and even more preferred is 300% (molar basis).

[0057] In the above emulsion polymerization, the polymerization temperature and polymerization pressure are appropriately determined depending on the type of monomer used, the molecular weight of the desired modified PTFE, and the reaction rate. Usually, the polymerization temperature is 5 to 150°C, preferably 10°C or higher, more preferably 30°C or higher, and even more preferably 50°C or higher. Also, it is more preferably 120°C or lower, and even more preferably 100°C or lower. The polymerization pressure is 0.05 to 10 MPaG. The polymerization pressure is more preferably 0.3 MPaG or more, and even more preferably 0.5 MPaG or more. Also, the polymerization pressure is more preferably 5.0 MPaG or less, and even more preferably 3.0 MPaG or less.

[0058] In the emulsion polymerization, it is preferable not to release the pressure after the modified monomer is charged into the polymerization vessel until the polymerization is completed, so that the modified monomer can be left in the system until the end of the polymerization, and the breaking strength of the resulting modified PTFE can be further increased.

[0059] The above-mentioned production method may include a step of coagulating the above-mentioned aqueous dispersion to obtain a wet powder of the above-mentioned modified PTFE. The above-mentioned coagulation can be carried out by a known method.

[0060] The manufacturing method may include a step of drying the wet powder. The drying is usually performed by using a means such as vacuum, high frequency, or hot air while keeping the wet powder in a state where it is not very fluid, preferably in a state where it is left stationary. Friction between powders, especially at high temperatures, generally has an undesirable effect on fine powder-type PTFE. This is because particles made of this type of PTFE have the property of easily fibrillating even with a small shear force and losing the original stable particle structure state. From the viewpoint of further increasing the breaking strength, the drying may be performed at a temperature of 10°C or higher, preferably 100°C or higher, more preferably 150°C or higher, even more preferably 170°C or higher, even more preferably 190°C or higher, even more preferably 210°C or higher, even more preferably 230°C or higher, and particularly preferably 250°C or higher. From the viewpoint of further reducing the extrusion pressure, the temperature may be 300° C. or less, preferably 250° C. or less, more preferably 230° C. or less, even more preferably 210° C. or less, even more preferably 190° C. or less, and particularly preferably 170° C. or less. In order to further increase the strength ratio, it is preferable to appropriately adjust the temperature within this range.

[0061] The modified PTFE of the present disclosure is preferably in the form of a powder, and more preferably in the form of a fine powder.

[0062] The modified PTFE of the present disclosure may also be provided in the form of an aqueous dispersion. Aqueous dispersions containing particles of the modified PTFE of the present disclosure are also preferred embodiments of the present disclosure.

[0063] The average primary particle size of the modified PTFE of the present disclosure is preferably 500 nm or less, more preferably 350 nm or less, even more preferably 300 nm or less, and particularly preferably 280 nm or less, and is preferably 100 nm or more, more preferably 150 nm or more, even more preferably 170 nm or more, and particularly preferably 200 nm or more. The average primary particle size is measured by the following method. The modified PTFE aqueous dispersion is diluted with water until the solid content is 0.15% by mass, and the transmittance of the 550 nm projected light per unit length of the diluted latex obtained and the number-based length average particle diameter determined by measuring a specific direction using a transmission electron microscope photograph are measured to create a calibration curve. Using this calibration curve, the number-average particle diameter is determined from the measured transmittance of the 550 nm projected light of each sample, and is taken as the average primary particle diameter.

[0064] The modified PTFE of the present disclosure may have an average aspect ratio of primary particles of 2.0 or less, preferably 1.8 or less, more preferably 1.7 or less, even more preferably 1.6 or less, even more preferably 1.5 or less, even more preferably 1.4 or less, especially preferably 1.3 or less, particularly preferably 1.2 or less, and most preferably 1.1 or less. The average aspect ratio may also be 1.0 or more. The above average aspect ratio is determined by observing the fluororesin powder or an aqueous fluororesin dispersion diluted to a solid content of approximately 1% by mass with a scanning electron microscope (SEM), processing the images of 200 or more particles randomly selected, and averaging the ratio of the long axis to the short axis.

[0065] The modified PTFE of the present disclosure has an average secondary particle size of preferably 100 μm or more, more preferably 200 μm or more, and even more preferably 300 μm or more, and preferably 2000 μm or less, more preferably 1000 μm or less, even more preferably 800 μm or less, and particularly preferably 700 μm or less. The average secondary particle size is measured in accordance with JIS K 6891.

[0066] The modified PTFE of the present disclosure is particularly useful as a raw material for an expanded body. The expanded body formed from the modified PTFE of the present disclosure is also a preferred embodiment of the present disclosure.

[0067] The above-mentioned expanded body can be obtained by expanding the modified PTFE of the present disclosure.

[0068] The above-mentioned stretched body is also preferably in the form of a film, a tube, a fiber, or a rod.

[0069] When the stretched body is a membrane (stretched membrane or porous membrane), it can be stretched by a known PTFE stretching method. Preferably, a sheet-like or rod-like paste extrudate is roll-stretched in the extrusion direction to obtain a uniaxially stretched film. Furthermore, a biaxially stretched film can also be obtained by stretching the film in the width direction using a tenter or the like. It is also preferable to carry out a semi-baking treatment before stretching.

[0070] The stretched body can be made into a porous body having a high porosity, and can be suitably used as a filter medium for various precision filters such as air filters and chemical filters, a support material for polymer electrolyte membranes, and the like. They are also useful as materials for products used in the fields of textiles, medicine, electrochemicals, sealing materials, air filtration, ventilation / internal pressure regulation, liquid filtration, and general consumer goods. Specific applications are given below as examples.

[0071] Electrochemical Field Dielectric material prepreg, EMI shielding material, heat transfer material, etc. More specifically, printed wiring board, electromagnetic shielding material, insulating heat transfer material, insulating material, etc. Sealing materials field Gaskets, packing, pump diaphragms, pump tubes, aircraft sealing materials, etc.

[0072] Air Filtration Field ULPA filters (for semiconductor manufacturing), HEPA filters (for hospitals and semiconductor manufacturing), cylindrical cartridge filters (for industrial use), bag filters (for industrial use), heat-resistant bag filters (for exhaust gas treatment), heat-resistant pleated filters (for exhaust gas treatment), SINBRAN filters (for industrial use), catalyst filters (for exhaust gas treatment), adsorbent filters (for HDD installation), adsorbent vent filters (for HDD installation), vent filters (for HDD installation and others), vacuum cleaner filters (for vacuum cleaners), general-purpose multi-layer felt material, GT cartridge filters (for GT compatible products), cooling filters (for electronic device housings), etc.

[0073] Ventilation / internal pressure regulation field Freeze-drying materials such as freeze-drying containers, automotive ventilation materials for electronic circuits and lamps, container applications such as container caps, protective ventilation applications for electronic devices including small terminals such as tablet terminals and mobile phones, medical ventilation applications, etc.

[0074] Liquid Filtration Semiconductor liquid filtration filters (for semiconductor manufacturing), hydrophilic PTFE filters (for semiconductor manufacturing), chemical filters (for chemical liquid treatment), pure water production line filters (for pure water production), backwash type liquid filtration filters (for industrial wastewater treatment), etc.

[0075] General consumer goods field Clothing, cable guides (movable wires for motorcycles), motorcycle clothing, cast liners (medical supporters), vacuum cleaner filters, bagpipes (musical instruments), cables (signal cables for guitars, etc.), strings (for stringed instruments), etc.

[0076] Textiles PTFE fiber (textile material), sewing thread (textile), weaving thread (textile), rope, etc.

[0077] Medical field Internal implants (extended products), artificial blood vessels, catheters, general surgery (tissue reinforcement materials), head and neck products (dura substitutes), oral health (tissue regenerative medicine), orthopedics (bandages), etc.

[0078] The modified PTFE of the present disclosure can also be suitably used as a dustproof additive, an anti-drip agent, a binder for batteries, or other various additives, in coating applications, and in glass cloth impregnation processing applications. Furthermore, the aqueous dispersion containing the modified PTFE particles of the present disclosure can be used in a variety of applications, for example, as a surface coating agent for cooking utensils, or for impregnating glass fiber, carbon fiber, Kevlar (registered trademark) fiber, etc., to produce impregnated bodies such as roofing materials, and can also be used to form films by applying the dispersion to an object to be coated and baking it in applications such as high-frequency printed circuit boards, conveyor belts, and packing.

[0079] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES

[0080] The present disclosure will now be described in more detail with reference to examples, but the present disclosure is not limited to these examples.

[0081] Various physical properties were measured by the following methods.

[0082] Average primary particle size The modified PTFE aqueous dispersion was diluted with water to a solid content concentration of 0.15% by mass, and the transmittance of the 550 nm projected light relative to the unit length of the obtained diluted latex and the number-based length average particle diameter determined by measuring a specific direction using a transmission electron microscope photograph were measured to create a calibration curve. Using this calibration curve, the number-average particle diameter was determined from the measured transmittance of the 550 nm projected light of each sample, and was taken as the average primary particle diameter.

[0083] Polymer Solids Content 1 g of the modified PTFE aqueous dispersion was dried in a blower dryer at 150° C. for 60 minutes, and the ratio of the mass of the heating residue to the mass (1 g) of the aqueous dispersion was expressed as a percentage and used.

[0084] Modified Monomer Content The CTFE content was determined by press-molding PTFE powder to create a thin film disk, measuring the infrared absorbance of the thin film disk by FT-IR, and determining the CTFE content at 957 cm -1 Absorbance / 2360cm -1 The absorbance ratio was multiplied by 0.58.

[0085] Standard specific gravity (SSG) The measurements were made using samples formed in accordance with ASTM D 4895 and by the water displacement method in accordance with ASTM D 792.

[0086] Endothermic peak temperature The endothermic peak temperature was determined as the temperature corresponding to the minimum point on the heat of fusion curve when PTFE that had not been heated to a temperature of 300°C or higher was heated at a rate of 10°C / min using a differential scanning calorimeter (DSC).

[0087] Extrusion Pressure 21.7 g of lubricant (trade name: Isopar H (registered trademark), manufactured by Exxon Corp.) was added to 100 g of modified PTFE powder, and mixed at room temperature for 3 minutes to obtain a PTFE fine powder mixture. The obtained PTFE fine powder mixture was then left at room temperature (25°C) for at least 1 hour before extrusion, and then paste extruded at room temperature through an orifice (diameter 2.5 mm, land length 11 mm, introduction angle 30°) at a reduction ratio of 100:1 (ratio of cross-sectional area of ​​the inlet and outlet of the die) to obtain a uniform bead (beading; extrusion molded body). The extrusion speed, i.e., the ram speed, was 20 inches / min (51 cm / min). The extrusion pressure was determined by measuring the load when the extrusion load reached equilibrium in the paste extrusion and dividing it by the cross-sectional area of ​​the cylinder used for paste extrusion.

[0088] Extension test The bead obtained by the above paste extrusion was heated at 230°C for 30 minutes to remove the lubricant from the bead. The bead (extrudate) was then cut to the appropriate length, clamped at each end with a clamp distance of 2.0 inches (51 mm) between the clamps, and heated to 300°C in an air circulating oven. The clamps were then moved apart at a desired speed (stretch rate) until a separation distance corresponding to the desired stretch (total stretch) was achieved, and stretch testing was performed. The stretching method essentially follows that disclosed in U.S. Pat. No. 4,576,869, except for the extrusion speed (51 cm / min instead of 84 cm / min). "Stretch" is the increase in length due to drawing, and is usually expressed in relation to the original length. In the above preparation method, the stretch rate is 100% / sec and the total stretch is 2400%.

[0089] Breaking Strength The stretched bead (produced by stretching the bead) obtained in the above stretching test was clamped and fixed in a movable jaw having a gauge length of 5.0 cm, and a tensile test was performed at 25°C and a speed of 300 mm / min, and the strength at the time of break was measured as the breaking strength.

[0090] strength ratio It was calculated by breaking strength (N) / extrusion pressure (MPa).

[0091] Synthesis Example 1 A white solid A was obtained by the method described in Synthesis Example 1 of WO 2021 / 045228.

[0092] Example 1 In a 6L stainless steel reactor equipped with a stirrer, 3600g of deionized water, 180g of paraffin wax, 5.4g of white solid A, and 26.5mg of oxalic acid were placed. The contents of the reactor were then heated to 70°C while being aspirated, and purged with tetrafluoroethylene (TFE) to remove oxygen from the reactor, and the contents were stirred. 2.60g of chlorotrifluoroethylene (CTFE) was pressed into the reactor with TFE, and TFE was then added to make the pressure 2.70MPaG. An aqueous solution of potassium permanganate, in which 3.4mg of potassium permanganate was dissolved in deionized water, was continuously added to the reactor as an initiator. After the injection of the initiator, a drop in pressure occurred and the start of polymerization was observed. TFE was added to the reactor to keep the pressure constant at 2.70MPaG. When the amount of TFE charged reached 430g, the charging of the aqueous potassium permanganate solution was stopped. When the amount of TFE charged reached 1660 g, the supply of TFE was stopped, stirring was stopped, and the reaction was terminated. After that, the pressure in the reactor was evacuated until it reached normal pressure, and nitrogen replacement was performed, and the contents were removed from the reactor and cooled. The paraffin wax was removed to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 31.4 mass%, and the average primary particle size was 248 nm. The obtained PTFE aqueous dispersion was diluted to a solid content concentration of 13% by mass and coagulated by vigorously stirring in a container equipped with a stirrer. The coagulated wet powder was taken out and dried at 210°C for 18 hours to obtain a PTFE powder. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.

[0093] Example 2 Polymerization was carried out under the same conditions as in Example 1, except that the amount of CTFE charged was changed to 1.28 g, the amount of potassium permanganate charged was changed to 3.87 mg, and the final amount of TFE was changed to 1790 g, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 33.0 mass%, and the average primary particle size was 263 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.

[0094] Comparative Example 1 Polymerization was carried out under the same conditions as in Example 1, except that CTFE was not charged, the amount of succinic acid charged was changed to 0.108 g, the amount of potassium permanganate charged was changed to 3.5 mg, and the final amount of TFE charged was changed to 1500 g, to obtain a PTFE aqueous dispersion. The solid content concentration of the obtained PTFE aqueous dispersion was 29.5 mass%, and the average primary particle size was 380 nm. The resulting PTFE aqueous dispersion was used to obtain a PTFE powder in the same manner as in Example 1. Various physical properties of the resulting PTFE powder were measured. The results are shown in Table 1.

[0095] [Table 1]

Claims

1. A modified polytetrafluoroethylene which contains tetrafluoroethylene units and chlorotrifluoroethylene units, the amount of said chlorotrifluoroethylene units being 1.0 mass% or less based on all polymerized units, and which is stretchable in the following stretching test. (Extension test) 21.7 g of lubricant (trade name: Isopar H (registered trademark), manufactured by Exxon Corp.) is added to 100 g of modified polytetrafluoroethylene powder, and mixed at room temperature for 3 minutes to obtain a polytetrafluoroethylene fine powder mixture. The resulting polytetrafluoroethylene fine powder mixture is then left at room temperature (25°C) for at least 1 hour before extrusion, and then paste-extruded through an orifice (diameter 2.5 mm, land length 11 mm, introduction angle 30°) at room temperature with a reduction ratio of 100:1 (ratio of cross-sectional area of ​​the die inlet to the cross-sectional area of ​​the die outlet) to obtain a uniform bead (beading; extrusion molded product). The extrusion speed, i.e., the ram speed, is 20 inches / min (51 cm / min). The bead obtained by paste extrusion is heated at 230°C for 30 minutes to remove the lubricant from the bead. The bead (extrudate) is then cut to the appropriate length, clamped at each end with a clamp distance of 2.0 inches (51 mm) between the clamps, and heated to 300°C in an air circulating oven. The clamps are then moved apart at the desired speed (stretch rate) until a separation distance corresponding to the desired stretch (total stretch) is reached, and the stretch test is performed. The stretching method essentially follows that disclosed in U.S. Pat. No. 4,576,869, except for the extrusion speed (51 cm / min instead of 84 cm / min). "Stretch" is the increase in length due to stretching, and is usually expressed in relation to the original length. In the method, the stretch rate is 1000% / sec and the total stretch is 2400%. A specimen is considered stretchable if it does not break before the stretch is completed.

2. The modified polytetrafluoroethylene according to claim 1, having a breaking strength of 20.0 N or more.

3. 3. The modified polytetrafluoroethylene according to claim 1, wherein the extrusion pressure is 5 MPa or more.

4. 3. The modified polytetrafluoroethylene according to claim 1, wherein the extrusion pressure is 50 MPa or less.

5. The modified polytetrafluoroethylene according to claim 1 or 2, having a strength ratio expressed as breaking strength / extrusion pressure of more than 1.90 N / MPa.

6. The modified polytetrafluoroethylene according to claim 1 or 2, in the form of a powder.

7. The modified polytetrafluoroethylene according to claim 1 or 2, which is in the form of a fine powder.

Citation Information

Patent Citations

  • Henseitetorafuruoroechirenjugotai no seizohoho

    JP1976036291A

  • Porous hollow fiber of polytetrafluoroethylene and production thereof

    JP1990006832A

  • Polymerization of tetrafluoroethylene

    JP2000143707A

  • Method for manufacturing fluorine-containing polymer latex