Alkali-free glass

An alkali-free glass composition with specific oxide ratios and properties addresses TFT pattern misalignment by reducing thermal contraction and expansion, achieving high strain points without rare earth oxides, thereby enhancing display resolution and cost-effectiveness.

JP7583363B2Active Publication Date: 2024-11-14NIPPON ELECTRIC GLASS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020560043
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-13
Filing Date
2019-12-06
Publication Date
2024-11-14
Estimated Expiration
2039-12-06

AI Technical Summary

Technical Problem

Conventional alkali-free glass plates cause TFT pattern misalignment due to thermal contraction and temperature distribution during high-temperature processing, which is exacerbated by the use of rare and expensive rare earth oxides like Y2O3 and La2O3, increasing manufacturing costs and thermal expansion coefficients.

Method used

A glass composition comprising SiO2 60-90%, Al2O3 5-20%, B2O3 0-15%, P2O5 0.1-20%, Li2O+Na2O+K2O 0-0.5%, MgO 0-10%, CaO 0-5%, and SrO 0-1% is developed, with a strain point of 700°C or higher and a thermal expansion coefficient of 34.0×10-7/℃ or less, reducing thermal shrinkage and expansion without increasing costs.

Benefits of technology

The new glass composition effectively reduces TFT pattern deviation by minimizing thermal contraction and expansion, maintaining a high strain point while avoiding the use of expensive rare earth oxides, thus lowering manufacturing costs and improving display resolution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583363000001
    Figure 0007583363000001
  • Figure 0007583363000002
    Figure 0007583363000002
Patent Text Reader

Abstract

The alkali-free glass of the present invention has a glass composition containing, in mole percent, 60-90% SiO, 5-20% AlO, 0-15% BO, 0.1-20% PO, 0-0.5% LiO+NaO+KO, 0-10% MgO, 0.1-10% CaO, and 0-5% SrO, and has an average thermal expansion coefficient of 34.0 × 10 in a temperature range of 30 to 380°C. -7 / °C or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an alkali-free glass plate, and particularly to an alkali-free glass plate suitable as a substrate for forming a thin-film transistor (TFT) circuit or a substrate for supporting a resin substrate for forming a TFT circuit in a flat panel display such as a liquid crystal display or an organic EL display. [Background technology]

[0002] As is well known, liquid crystal panels and organic EL panels are equipped with TFTs for drive control.

[0003] Amorphous silicon, low-temperature polysilicon, high-temperature polysilicon, etc. are known materials for TFTs that drive displays. Recently, with the spread of large LCD displays, smartphones, tablet PCs, etc., there is a growing need for higher resolution displays. In VR devices, which have been attracting attention in recent years, there is also a growing need for even higher resolution.

[0004] Low-temperature polysilicon TFTs and high-temperature polysilicon TFTs can meet the above needs, but this technology requires high-temperature processes (such as film formation processes for TFT formation) at 500 to 600° C. However, conventional alkali-free glass sheets cause TFT pattern misalignment due to thermal shrinkage that occurs before and after the high-temperature process and temperature distribution during the heat treatment. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5769617 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0006] In order to reduce pattern misalignment in an alkali-free glass sheet, it is important to achieve both low thermal shrinkage and low thermal expansion at high levels.

[0007] There are mainly two methods for reducing the thermal shrinkage of alkali-free glass sheets. One is to hold the glass at a temperature close to the process temperature for a certain period of time and perform annealing. In this method, the glass relaxes and shrinks to a structure that is in equilibrium at the process temperature during annealing, thereby reducing the amount of thermal shrinkage of the glass in the subsequent film formation process. However, this method requires an annealing step, which lengthens the manufacturing time, thereby increasing the manufacturing cost of the alkali-free glass sheet.

[0008] The other method is to increase the strain point of the glass. In the overflow downdraw method, which is one of the methods for forming glass sheets, the glass sheet is generally cooled from the melting temperature to the forming temperature in a short time. This causes the fictive temperature of the glass sheet to increase, which increases the difference with the film-forming temperature and increases the amount of thermal contraction of the glass. Therefore, if the strain point of the glass is increased, the viscosity of the glass at the film-forming temperature increases and structural relaxation becomes less likely to proceed. As a result, the thermal contraction of the glass can be reduced.

[0009] Moreover, the higher the heat treatment temperature, the greater the contribution of a high strain point to reducing the amount of thermal shrinkage. Therefore, when assuming high-temperature polysilicon TFT, that is, when aiming at high-definition displays, an alkali-free glass plate with a high strain point is required. Patent Document 1 discloses high-strain-point glass containing Y2O3 and / or La2O3. However, since Y2O3 and La2O3 are rare earth oxides, they are scarce and the raw materials required for introduction are expensive. As a result, the manufacturing cost of the alkali-free glass plate rises. Furthermore, when Y2O3 and / or La2O3 are introduced into the glass composition, there is a risk that the thermal expansion coefficient becomes unduly high.

[0010] In addition, in the production of low-temperature polysilicon TFTs, the thermal expansion coefficient of alkali-free glass sheets has not been a major issue so far, because it can be corrected by adjusting the conditions of the film-forming equipment. However, in fields such as VR devices, pattern misalignment caused by temperature distribution in the film-forming equipment is also an issue, so when trying to produce panels with even higher resolution, alkali-free glass sheets with lower expansion than before are required.

[0011] The present invention has been made in view of the above circumstances, and its technical object is to create an alkali-free glass sheet having a high strain point and a low thermal expansion coefficient while preventing a sharp increase in production costs. [Means for solving the problem]

[0012] As a result of extensive investigations, the present inventors have found that the above technical problems can be solved by introducing P2O5 as an essential component and strictly controlling the contents of other components, and propose this as the present invention. That is, the alkali-free glass plate of the present invention contains, in mole percent, as a glass composition 60-90% SiO2, 5-20% Al2O3, 0-15% B2O3, 0.1-20% P2O5, 0-0.5% Li2O+Na2O+K2O, 0-10% MgO, 0.1-10% CaO, and 0-5% SrO, and has an average thermal expansion coefficient of 34.0×10 in a temperature range of 30 to 380° C. -7 / °C or less. In this way, it is possible to increase the strain point and decrease the thermal expansion coefficient without increasing the manufacturing cost. As a result, the amount of thermal contraction of the glass is small before and after the high-temperature process, and the influence of the temperature distribution in the film forming apparatus can be reduced, so that the pattern deviation of the TFT can be significantly reduced. Here, "Li2O+Na2O+K2O" refers to the total amount of Li2O, Na2O and K2O. "Average thermal expansion coefficient in the temperature range of 30 to 380°C" is a value measured by a dilatometer.

[0013] The alkali-free glass plate of the present invention preferably has an SrO content of 1 mol % or less.

[0014] In addition, the alkali-free glass plate of the present invention preferably contains B2O3 at 6 mol % or less.

[0015] The alkali-free glass plate of the present invention preferably has a strain point of at least 700° C. Here, the "strain point" refers to a value measured based on the method of ASTM C336.

[0016] In addition, the alkali-free glass plate of the present invention has a density of 2.50 g / cm 3 The average thermal expansion coefficient in the temperature range of 30 to 380°C is 34.0 x 10 -7 / °C or less, a strain point of 700°C or more, and a Young's modulus of 70 GPa or more. Here, the "density" can be measured by the well-known Archimedes method, and the "flexural resonance method" can be measured by the well-known flexural resonance method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] In the alkali-free glass plate of the present invention, the reasons for limiting the content of each component as described above are given below. In the explanation of the content of each component, % denotes mol %.

[0018] SiO2 is a component that forms a glass skeleton and increases the strain point. Furthermore, by increasing the amount of SiO2 (for example, 68% or more), the thermal expansion coefficient can be significantly reduced. Therefore, the content of SiO2 is preferably 60% or more, 63% or more, 65% or more, 67% or more, 68% or more, 69% or more, 70% or more, and particularly 71% or more. On the other hand, if the content of SiO2 is too high, the high-temperature viscosity increases and the melting property is easily reduced. And the increase in melting cost directly leads to an increase in production cost. Therefore, the content of SiO2 is preferably 90% or less, 85% or less, 80% or less, 77% or less, 76% or less, 75% or less, 74% or less, 73% or less, and particularly 72% or less.

[0019] Al2O3 is a component that forms the glass skeleton, increases the strain point, and suppresses phase separation. In particular, the present invention contains P2O5 as an essential component, and in this case, if the content of Al2O3 is too low, the glass is prone to phase separation. Therefore, the content of Al2O3 is preferably 5% or more, 8% or more, 9% or more, 10% or more, 11% or more, 12% or more, and particularly 12.5% ​​or more. On the other hand, if the content of Al2O3 is too high, the glass is prone to devitrification, and the manufacturing cost is likely to increase. Therefore, the content of Al2O3 is preferably 20% or less, 19% or less, 18% or less, 17% or less, 16% or less, 15% or less, and particularly 14% or less.

[0020] P2O5 is a component that significantly lowers the liquidus temperature of Al-based devitrified crystals while maintaining a high strain point. In conventional alkali-free glass, the liquidus temperature of Al-based devitrified crystals such as mullite was lowered by optimizing the content and ratio of alkaline earth metal oxides, but alkaline earth metal oxides have the effect of increasing the thermal expansion coefficient. On the other hand, P2O5 has the effect of lowering the liquidus temperature of Al-based devitrified crystals without increasing the thermal expansion coefficient. Therefore, the content of P2O5 is preferably 0.1% or more, 1% or more, 2% or more, 3% or more, 4% or more, and particularly 5% or more. However, if a large amount of P2O5 is contained, the Young's modulus will be too low or the glass will be prone to phase separation. In addition, there is a concern that P will diffuse from the glass and reduce the performance of the TFT. Therefore, the content of P2O5 is preferably 20% or less, 15% or less, 12% or less, 11% or less, 10% or less, 9% or less, 8% or less, 7% or less, particularly preferably 6% or less.

[0021] The content of Al2O3+P2O5 is preferably 14% or more, more than 15%, 17% or more, 18% or more, 19% or more, particularly 20 to 25%. If the content of Al2O3+P2O5 is too low, it is difficult to maintain a high strain point. Note that "Al2O3+P2O5" refers to the combined amount of Al2O3 and P2O5.

[0022] B2O3 is a component that increases the melting property and increases the liquidus temperature of Al-based devitrified crystals. It is also a component that decreases the thermal expansion coefficient. Therefore, the content of B2O3 is preferably 0% or more, 1% or more, 2% or more, 3% or more, 4% or more, and particularly 5% or more. On the other hand, if the content of B2O3 is too high, the strain point is significantly lowered and the water content in the glass is significantly increased. As a result, the thermal shrinkage of the glass increases. Therefore, the content of B2O3 is preferably 15% or less, 10% or less, 9% or less, 8% or less, 7% or less, and particularly 6% or less.

[0023] The content of P2O5-B2O3 is preferably -4% or more, -3% or more, -2% or more, -1% or more, more than 0%, 1% or more, 2% or more, 3% or more, particularly 4 to 10%. If the content of P2O5-B2O3 is too high, Al-based devitrified crystals are likely to precipitate during molding. Note that "P2O5-B2O3" is the content of P2O5 minus the content of B2O3.

[0024] The value of the mol% calculation formula 14.8×[Al2O3]-2.2×[B2O3]+[MgO]+6.5×([CaO]+[SrO]+[BaO])-11.1×[P2O5] is preferably 110% or more, 120% or more, 130% or more, 140% or more, 150% or more, 160% or more, 170% or more, 180% or more, and particularly 190% or more. If this value is too small, the glass is prone to phase separation. Note that [Al2O3] refers to the molar percentage content of Al2O3, [B2O3] refers to the molar percentage content of B2O3, [MgO] refers to the molar percentage content of MgO, [CaO] refers to the molar percentage content of CaO, [SrO] refers to the molar percentage content of SrO, [BaO] refers to the molar percentage content of BaO, and [P2O5] refers to the molar percentage content of P2O5.

[0025] MgO is a component that lowers high-temperature viscosity and increases melting property, and also increases devitrification resistance by balancing with other components. Furthermore, it is a component that significantly increases Young's modulus as a mechanical property. If Young's modulus is high, it is possible to enjoy the effect of reducing pattern shift in all TFT manufacturing processes. Furthermore, MgO has the smallest effect of increasing the thermal expansion coefficient among alkaline earth metal elements, so it is suitable for designing low-expansion glass. Therefore, the content of MgO is preferably 0% or more, 0.1% or more, 1% or more, 2% or more, 3% or more, and particularly 4% or more. On the other hand, if the content of MgO is too high, the strain point is likely to decrease, or the balance with other components is lost, and devitrification resistance is likely to decrease. Therefore, the content of MgO is preferably 10% or less, 9% or less, 8% or less, 7% or less, 6% or less, and particularly 5% or less.

[0026] Since the present invention contains P2O5 as an essential component and has a high ratio of glass-forming oxides, the introduction of CaO is essential from the viewpoint of optimizing devitrification resistance, melting property, and Young's modulus. Therefore, the CaO content is preferably 0.1% or more, 1% or more, 2% or more, 3% or more, and particularly 3.5% or more. On the other hand, if the CaO content is too high, the thermal expansion coefficient increases and the strain point tends to decrease. Therefore, the CaO content is preferably 10% or less, 9% or less, 8% or less, 7% or less, 6% or less, 5% or less, or 4% or less.

[0027] SrO is a component that lowers high-temperature viscosity and enhances melting property, and enhances devitrification resistance in balance with other components. Therefore, the content of SrO is preferably 0% or more, 0.1% or more, and particularly 0.5% or more. On the other hand, if the content of SrO is too high, the strain point is likely to decrease. Therefore, the content of SrO is preferably 5% or less, 4% or less, 3% or less, 2% or less, and particularly 1% or less.

[0028] BaO is a component that improves devitrification resistance in balance with other components. Therefore, the content of BaO is preferably 0% or more, 0.5% or more, and particularly 1% or more. On the other hand, if the content of BaO is too high, the thermal expansion coefficient becomes too high. In addition, the Young's modulus is easily reduced. Therefore, the content of BaO is preferably 10% or less, 5% or less, 4% or less, 3% or less, and particularly 2% or less.

[0029] If the combined amount of SrO and BaO is too small, the devitrification resistance is likely to decrease. Therefore, the combined amount of SrO and BaO is preferably 0% or more, 0.1% or more, and particularly 1% or more. On the other hand, if the combined amount of SrO and BaO is too large, the thermal expansion coefficient becomes high. Therefore, the combined amount of SrO and BaO is preferably 4% or less, 3% or less, 2% or less, and particularly 1% or less.

[0030] The total content of MgO, CaO, SrO and BaO is preferably 12% or less, 10% or less, 9% or less, 8% or less, 7% or less, 6% or less, particularly 5% or less, in order to reduce the thermal expansion coefficient. However, if the glass contains almost no alkaline earth metal oxides, the balance of the glass composition is lost, and the devitrification resistance is likely to decrease or the glass is likely to undergo phase separation. Therefore, the total content of MgO, CaO, SrO and BaO is preferably 0.1% or more, 1% or more, 2% or more, 3% or more, 4% or more, particularly 5% or more.

[0031] The molar ratio MgO / P2O5 is preferably 3 or less, 2 or less, 1.5 or less, 0.8 or less, 0.5 or less, or 0.3 or less, particularly 0.1 to 0.2. If the molar ratio MgO / P2O5 is too large, the thermal expansion coefficient becomes too high. Note that "MgO / P2O5" refers to the value obtained by dividing the content of MgO by the content of P2O5.

[0032] The molar ratio CaO / P2O5 is preferably 5 or less, 4 or less, 3 or less, 2 or less, 0.01 to 1, 0.1 to less than 1, particularly 0.3 to 0.7. If the molar ratio CaO / P2O5 is too large, the thermal expansion coefficient becomes too high. Note that "CaO / P2O5" refers to the value obtained by dividing the CaO content by the P2O5 content.

[0033] The molar ratio SrO / P2O5 is preferably 2 or less, 1 or less, 0.8 or less, 0.6 or less, 0.4 or less, 0.2 or less, 0.1 or less, and particularly less than 0.1. If the molar ratio SrO / P2O5 is too large, the thermal expansion coefficient becomes too high. Note that "SrO / P2O5" refers to the value obtained by dividing the SrO content by the P2O5 content.

[0034] The molar ratio BaO / P2O5 is preferably 2 or less, 1 or less, 0.8 or less, 0.6 or less, 0.4 or less, 0.2 or less, 0.1 or less, and particularly less than 0.1. If the molar ratio BaO / P2O5 is too large, the thermal expansion coefficient becomes too high. Note that "BaO / P2O5" refers to the value obtained by dividing the BaO content by the P2O5 content.

[0035] The molar ratio (MgO+CaO+SrO+BaO) / P2O5 is preferably 6 or less, 4 or less, 3 or less, 2 or less, 1.5 or less, 1 or less, less than 1, 0.9 or less, 0.8 or less, particularly 0.1 to 0.7. If the molar ratio (MgO+CaO+SrO+BaO) / P2O5 is too large, the thermal expansion coefficient becomes too high. Note that "(MgO+CaO+SrO+BaO) / P2O5" refers to the value obtained by dividing the total amount of MgO, CaO, SrO and BaO by the content of P2O5.

[0036] ZnO is a component that enhances meltability, but if a large amount of ZnO is contained, the glass becomes more susceptible to devitrification and the strain point becomes more likely to decrease. The ZnO content is preferably 0 to 5%, 0 to 3%, 0 to 0.5%, particularly preferably 0 to 0.2%.

[0037] TiO2 is a component that reduces high-temperature viscosity and enhances melting property, and also suppresses solarization. However, if TiO2 is contained in a large amount, the glass becomes colored and the transmittance is likely to decrease. Therefore, the content of TiO2 is preferably 0 to 3%, 0 to 1%, 0 to 0.1%, and particularly 0 to 0.02%.

[0038] The total amount of Li2O, Na2O and K2O is 0 to 0.5%, preferably 0 to 0.2%, and more preferably 0 to 0.15%. If the total amount of Li2O, Na2O and K2O is too high, there is a risk that alkali ions will diffuse into the semiconductor material formed in the heat treatment process.

[0039] SnO2 is a component that has a good clarifying effect in the high temperature range, and also increases the strain point and reduces the high temperature viscosity. The content of SnO2 is preferably 0 to 1%, 0.001 to 1%, 0.05 to 0.5%, and particularly 0.08 to 0.2%. If the content of SnO2 is too high, devitrified crystals of SnO2 are likely to precipitate. If the content of SnO2 is less than 0.001%, it is difficult to enjoy the above effects.

[0040] Although SnO2 is suitable as a fining agent, fining agents other than SnO2 may be used as long as they do not significantly impair the glass properties. Specifically, As2O3, Sb2O3, CeO2, F2, Cl2, SO3, and C may be added in a total amount of up to, for example, 1%, and metal powders such as Al and Si may be added in a total amount of up to, for example, 1%.

[0041] Although As2O3 and Sb2O3 have excellent clarity, it is preferable not to incorporate them as much as possible from an environmental viewpoint. Furthermore, since the inclusion of a large amount of As2O3 in glass tends to reduce solarization resistance, its content is preferably 0.5% or less, particularly 0.1% or less, and it is desirable to not include it substantially. Here, "substantially not including As2O3" refers to the case where the content of As2O3 in the glass composition is less than 0.05%. Moreover, the content of Sb2O3 is preferably 1% or less, particularly 0.5% or less, and it is desirable to not include it substantially. Here, "substantially not including Sb2O3" refers to the case where the content of Sb2O3 in the glass composition is less than 0.05%.

[0042] Cl has the effect of promoting the melting of alkali-free glass sheets, and adding Cl can lower the melting temperature and promote the action of the fining agent, which results in lowering the melting cost and extending the life of the glass manufacturing furnace. However, if the Cl content is too high, the strain point is likely to decrease. Therefore, the Cl content is preferably 0.5% or less, particularly 0.1% or less. In addition, chlorides of alkaline earth metal oxides such as strontium chloride, aluminum chloride, etc. can be used as Cl introduction raw materials.

[0043] In the alkali-free glass plate of the present invention, the contents of trace components are preferably as follows.

[0044] The content of Rh is preferably 0.1 to 3 ppm by mass, 0.2 to 2.5 ppm by mass, 0.3 to 2 ppm by mass, 0.4 to 1.5 ppm by mass, and particularly 0.5 to 1 ppm by mass. Rh is a component generally contained in melting equipment. When glass is melted at high temperature, Rh is easily dissolved into the glass base. However, when Rh and SnO2 coexist, the glass is easily colored. Therefore, it is desirable that the content of Rh is as small as possible. Although the alkali-free glass according to the present invention has a high strain point, the viscosity in the high temperature range is relatively low, so that it can be melted at a low temperature compared to alkali-free glass having a similar strain point. Therefore, the alkali-free glass according to the present invention can reduce the amount of Rh dissolved compared to alkali-free glass having a similar strain point. And, by reducing the content of Rh, it is possible to produce a high strain point glass at low cost without coloring.

[0045] The content of Ir is preferably 0.01 to 10 ppm by mass, 0.02 to 5 ppm by mass, 0.03 to 3 ppm by mass, 0.04 to 2 ppm by mass, particularly 0.05 to 1 ppm by mass. In the melting step of the alkali-free glass plate of the present invention, a melting equipment containing Ir is preferably used. Ir has higher heat resistance than Pt and Pt-Rh alloys, and can reduce foaming at the glass interface. However, when melting glass using a melting equipment containing Ir, elution of Ir is inevitable. If the amount of eluted Ir is too large, Ir crystal grains are likely to precipitate in the glass.

[0046] The content of MoO3 is preferably 3 to 50 ppm by mass, 4 to 40 ppm by mass, 5 to 30 ppm by mass, 5 to 25 ppm by mass, particularly preferably 5 to 20 ppm by mass. Mo is a component contained in the electrodes in the melting step. When glass is melted by electric melting and heating, the elution of MoO3 from the Mo electrode is inevitable. However, the alkali-free glass according to the present invention has a relatively low viscosity in the high temperature range despite its high strain point, and therefore the amount of MoO3 eluted during electric melting and heating can be reduced as much as possible.

[0047] The content of ZrO2 is preferably 500 to 2000 ppm by mass, 550 to 1500 ppm by mass, or 600 to 1200 ppm by mass. ZrO2 is generally a component contained in refractories in a melting process. When glass is melted at high temperature, ZrO2 is easily dissolved into the glass base. However, the alkali-free glass according to the present invention has a relatively low viscosity in a high temperature range despite its high strain point, so that the amount of ZrO2 dissolved can be reduced as much as possible. In addition, when the amount of ZrO2 dissolved is reduced by using another refractory, an expensive refractory is used, and the manufacturing cost increases. On the other hand, when a small amount of ZrO2 is introduced into the glass composition, the liquidus temperature is lowered and the weather resistance is improved.

[0048] The alkali-free glass plate of the present invention preferably has the following physical properties.

[0049] The density is preferably 2.50 g / cm 3Below, 2.45g / cm 3 Below 2.40g / cm 3 Below 2.35g / cm 3 Below 2.30g / cm 3 Below, especially 2.25g / cm 3 If the density is too high, the alkali-free glass sheet becomes prone to bending, and in addition, it becomes difficult to reduce the weight of the device.

[0050] The average thermal expansion coefficient in the temperature range of 30 to 380°C is 34.0×10 -7 / °C or less, preferably 32.0 × 10 -7 / ℃ or less, 30.0×10 -7 / ℃ or less, 27.0×10 -7 / ℃ or less, 25.0×10 -7 / ℃ or less, 22.0×10 -7 / ℃ or less, 20.0×10 -7 / ℃ or less, 19.0×10 -7 / ℃ or less, 18.0×10 -7 / ℃ or less, 17.0×10 -7 / ℃ or less, especially 10.0×10 -7 / ℃ or more and 16.0×10 -7 / ° C. or less. If the average thermal expansion coefficient in the temperature range of 30 to 380° C. is too high, the non-alkali glass sheet is prone to local dimensional changes due to temperature distribution in the film forming apparatus.

[0051] The strain point is preferably 700° C. or higher, 710° C. or higher, 720° C. or higher, 725° C. or higher, 730° C. or higher, 735° C. or higher, 740° C. or higher, 745° C. or higher, particularly 750 to 900° C. If the strain point is too low, the amount of thermal shrinkage of the glass is likely to increase in the manufacturing process of high-temperature polysilicon TFTs.

[0052] 10 2.5 The temperature in poise is preferably 1750° C. or less, 1720° C. or less, 1700° C. or less, 1690° C. or less, 1680° C. or less, and particularly 1670° C. or less. 2.5 If the temperature at poise is too high, the solubility and clarity will decrease, resulting in an increase in production costs.

[0053] The Young's modulus is preferably 70 GPa or more, 71 GPa or more, 72 GPa or more, 73 GPa or more, 74 GPa or more, 75 GPa or more, 76 GPa or more, 77 GPa or more, or 78 GPa or more, particularly 80 to 120 GPa. If the Young's modulus is too low, the alkali-free glass plate is easily bent, and stress-induced pattern displacement is likely to occur in the display manufacturing process, etc.

[0054] Specific Young's modulus is preferably 30 GPa / g cm -3 Above, 31GPa / g cm -3 Above, 32GPa / g cm -3 Above, especially 33 GPa / g cm -3 If the specific Young's modulus is too low, the alkali-free glass plate will be easily warped, and therefore, stress-induced pattern displacement will be easily caused during the display manufacturing process and the like.

[0055] In the alkali-free glass plate of the present invention, the strain point can be increased by decreasing the β-OH value. In addition, when the glass composition is the same, the smaller the β-OH value, the more the amount of thermal shrinkage (low-temperature thermal shrinkage) in the temperature range below the strain point can be reduced. The effect of reducing the amount of low-temperature thermal shrinkage is significantly greater than the effect of increasing the strain point due to the decrease in the β-OH value. The β-OH value is preferably 3.0 / mm or less, 2.5 / mm or less, 2.0 / mm or less, 1.5 / mm or less, 1.0 / mm or less, and particularly 0.9 / mm or less. If the β-OH value is too small, the melting property is likely to decrease. Therefore, the β-OH value is preferably 0.01 / mm or more, and particularly 0.03 / mm or more.

[0056] The following methods can be used to lower the β-OH value: (1) Select raw materials with low water content. (2) Add components (Cl, SO3, etc.) to the glass that lower the β-OH value. (3) Reduce the water content in the furnace atmosphere. (4) Bubble N2 in the molten glass. (5) Use a small melting furnace. (6) Increase the flow rate of the molten glass. (7) Use an electric melting method.

[0057] Here, the "β-OH value" refers to a value obtained by measuring the transmittance of glass using FT-IR and calculating using the following formula:

[0058] [Number 1] β-OH value = (1 / X) log(T1 / T2) X: Plate thickness (mm) T1: Reference wavelength 3846cm -1 Transmittance (%) T2: Hydroxyl group absorption wavelength 3600cm -1 Minimum transmittance (%) near

[0059] The alkali-free glass sheet of the present invention is preferably formed by the overflow down-draw method. The overflow down-draw method is a method in which molten glass is made to overflow from both sides of a heat-resistant trough-shaped structure, and the overflowed molten glass is drawn downward while joining at the lower end of the trough-shaped structure to form a glass sheet. In the overflow down-draw method, the surface to become the surface of the glass sheet does not contact the trough-shaped refractory and is formed in a free surface state. Therefore, an unpolished glass sheet with good surface quality can be produced at low cost.

[0060] In addition to the overflow downdraw method, it is also possible to form a glass sheet by, for example, a slot-down method, a float method, etc. In particular, when the liquidus viscosity is low and forming by the overflow downdraw method is not possible, forming by the slot-down or float method is preferable.

[0061] The alkali-free glass plate of the present invention preferably has a plate thickness of 0.7 mm or less, 0.5 mm or less, 0.4 mm or less, or 0.3 mm or less, particularly preferably 0.05 to 0.1 mm. The smaller the plate thickness, the easier it is to achieve a lighter, thinner, and more flexible display. EXAMPLES

[0062] The present invention will be described below based on examples. However, the following examples are merely illustrative and the present invention is not limited to the following examples.

[0063] Tables 1 and 2 show examples of the present invention (samples Nos. 1 to 20).

[0064] [Table 1]

[0065] [Table 2]

[0066] First, a glass batch prepared by mixing glass raw materials to obtain the glass composition shown in the table was placed in a platinum crucible and melted at 1600-1650°C for 24 hours. When melting the glass batch, a platinum stirrer was used to stir and homogenize the glass. Next, the molten glass was poured onto a carbon plate and formed into a plate shape, which was then slowly cooled for 30 minutes at a temperature near the annealing point. The density, average thermal expansion coefficient (αS) in the temperature range of 30-380°C, strain point (Ps), annealing point (Ta), softening point (Ts), high-temperature viscosity (10 4.5 Temperature in poise (10 4.5 dPa·s), high temperature viscosity 10 4.0 Temperature in poise (10 4.0 dPa·s), high temperature viscosity 10 3.0 Temperature in poise (10 3.0 dPa·s), high temperature viscosity 10 2.5 Temperature in poise (10 2.5 The physical properties of the material were evaluated as follows: elastic modulus (dPa s), Young's modulus (E), specific Young's modulus (E / ρ), liquidus temperature (TL), and liquidus viscosity (Log η at TL). Some of the physical properties in the table are predicted values ​​based on past measurements.

[0067] The density is a value measured by the well-known Archimedes method.

[0068] The average thermal expansion coefficient in the temperature range of 30 to 380° C. is a value measured with a dilatometer.

[0069] The strain point, annealing point and softening point are values ​​measured based on the method of ASTM C336.

[0070] High temperature viscosity 10 4.5 Temperature in poise, high temperature viscosity 10 4.0 Temperature in poise, high temperature viscosity 10 3.0 Temperature in poise, high temperature viscosity 10 2.5 The temperature in poise is a value measured by the platinum ball pull method.

[0071] The Young's modulus is a value measured by a bending resonance method.

[0072] Specific Young's modulus is the Young's modulus divided by the density.

[0073] The liquidus temperature is the temperature at which crystals (primary phase) precipitate when glass powder that passes through a standard sieve of 30 mesh (sieve opening 500 μm) and remains on a 50 mesh (sieve opening 300 μm) is placed in a platinum boat and held in a temperature gradient furnace for 24 hours. The liquidus viscosity is the viscosity of glass at the liquidus temperature TL, measured by the platinum ball pull-up method.

[0074] As is clear from Tables 1 and 2, samples No. 1 to 22 have a strain point of 713°C or higher and an average thermal expansion coefficient of 33.3 × 10 in the temperature range of 30 to 380°C. -7 / ° C. or less. Therefore, it is considered that Samples Nos. 1 to 22 can significantly reduce the pattern misalignment of TFTs in a high-temperature process at 500 to 600° C.

Claims

1. The glass composition is, in mol%, SiO 2 60-90%, Al 2 O 3 5-20%, B 2 O 3 1-6%, P 2 O 5 0.1 to 6%, Li 2 O+Na 2 O+K 2 The average thermal expansion coefficient in the temperature range of 30 to 380° C. is 34.0×10 -7 / °C or less and a density of 2.377 g / cm 3 or less.

2. 2. The alkali-free glass sheet according to claim 1, wherein the SrO content is 1 mol % or less.

3. 3. The alkali-free glass sheet according to claim 1, wherein the content of BaO is 0.5 mol % or more.

4. The alkali-free glass plate according to claim 1, wherein a molar ratio (MgO+CaO+SrO+BaO) / P 2 O 5 is 6 or less.

5. The alkali-free glass plate according to claim 1, wherein the content of Al 2 O 3 +P 2 O 5 is 14% or more.

6. The alkali-free glass plate according to claim 1, wherein the content of P 2 O 5 —B 2 O 3 is −4% or more.

7. The alkali-free glass plate according to any one of claims 1 to 6, characterized in that the value of the mole percentage calculation formula 14.8 x [Al 2 O 3 ] - 2.2 x [B 2 O 3 ] + [MgO] + 6.5 ([CaO] + [SrO] + [BaO]) - 11.1 x [P 2 O 5 ] is 110% or more.

8. The alkali-free glass sheet according to claim 1, which is substantially free of As 2 O 3 and Sb 2 O 3 .

9. The alkali-free glass sheet according to any one of claims 1 to 8, characterized in that it has a strain point of 700°C or higher.

10. An alkali-free glass plate according to claim 1, characterized in that the Young's modulus is 70 GPa or more.

Citation Information

Patent Citations

  • Method of producing compound superconductor

    JP1982069617A

  • Fire-resistant and heat-resistant glass

    JP1986261232A

  • Alkalifree glass, and glass substrate for display using the same

    JP2003335548A

  • Alkali-free glass

    JP2010215463A

  • Alkali-free phosphosilicate glass

    JP2016517841A