Glass for covering semiconductor elements and semiconductor covering material using the same
A glass composition with specific ratios of SiO2, ZnO, B2O3, Al2O3, and MgO+CaO addresses environmental concerns and durability issues, enabling efficient and environmentally friendly coating of semiconductor elements with reduced firing temperatures.
Patent Information
- Application Number
- JP2021548788
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-24
- Filing Date
- 2020-09-10
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-09-10
AI Technical Summary
Existing glasses for covering semiconductor elements, such as ZnO-B and lead-based glasses, pose environmental hazards due to lead content and have issues with chemical durability and high firing temperatures, which can deteriorate semiconductor characteristics.
A glass composition comprising SiO2 20-36%, ZnO 8-40%, B2O3 10-24%, Al2O3 10-20%, MgO+CaO 8-22%, with a molar ratio of SiO2/ZnO between 0.6 and 3.3, and minimal lead content, ensuring low environmental impact, improved acid resistance, and reduced firing temperatures.
The proposed glass composition provides a low environmental footprint, excellent acid resistance, and lower firing temperatures, facilitating stable coating processes for semiconductor elements.
Smart Images

Figure 0007583374000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass for covering semiconductor elements and a semiconductor covering material using the same. [Background technology]
[0002] In general, the surfaces of semiconductor elements such as silicon diodes and transistors, including the PN junctions, are covered with glass, which stabilizes the surface of the semiconductor elements and prevents deterioration of their characteristics over time.
[0003] The properties required for glass for covering semiconductor elements include: (1) a thermal expansion coefficient that matches that of the semiconductor element to prevent cracks due to differences in the thermal expansion coefficient between the semiconductor element and the glass; (2) the glass must be capable of covering the semiconductor element at low temperatures (e.g., 860°C or lower) to prevent deterioration of the characteristics of the semiconductor element; and (3) the glass must be free of impurities such as alkaline components that have adverse effects on the surface of the semiconductor element.
[0004] Conventionally, zinc-based glasses such as ZnO-B2O3-SiO2-based glasses and lead-based glasses such as PbO-SiO2-Al2O3-based glasses and PbO-SiO2-B2O3-Al2O3-based glasses have been known as glasses for covering semiconductor elements. However, from the viewpoint of workability, lead-based glasses such as PbO-SiO2-Al2O3-based glasses and PbO-SiO2-B2O3-Al2O3-based glasses are currently mainstream (see, for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 48-43275 [Patent Document 2] Japanese Patent Publication No. 50-129181 [Patent Document 3] Japan Special Publication No. 1-49653 [Patent Document 4] Japanese Patent Application Publication No. 2008-162881 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the lead component of lead-based glass is a component that is harmful to the environment, and the above zinc-based glass contains small amounts of lead and bismuth components, so it cannot be said that it is completely harmless to the environment.
[0007] In addition, zinc-based glass has a problem that it is inferior in chemical durability to lead-based glass and is easily corroded in the acid treatment step after the formation of the coating layer, so that it is necessary to further form a protective film on the surface of the coating layer before the acid treatment.
[0008] On the other hand, increasing the SiO2 content in the glass composition improves the acid resistance and the reverse voltage of the semiconductor element. However, the firing temperature of the glass increases, which may degrade the characteristics of the semiconductor element during the coating process.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a glass for covering semiconductor elements which has a small environmental impact, is excellent in acid resistance, and can be fired at a low temperature. [Means for solving the problem]
[0010] The present inventors have found that the above technical problems can be solved by regulating the ratio of SiO2 to ZnO in a SiO2-B2O3-Al2O3-ZnO-based glass having a specific glass composition and introducing a predetermined amount of MgO and / or CaO, and propose this invention. That is, the glass for covering semiconductor elements of the present invention contains, in mole percent, 20-36% SiO2, 8-40% ZnO, 10-24% B2O3, 10-20% Al2O3, and 8-22% MgO+CaO as a glass composition, and is characterized in that the molar ratio of SiO2 / ZnO is 0.6 or more and less than 3.3, and is substantially free of lead components. Here, "MgO+CaO" means the total content of MgO and CaO, and "SiO2 / ZnO" means the value obtained by dividing the content of SiO2 by the content of ZnO. Moreover, "substantially free of" means that the component is not intentionally added as a glass component, and does not mean that impurities that are inevitably mixed in are completely excluded. Specifically, it means that the content of the component, including impurities, is less than 0.1 mass%.
[0011] As described above, the glass for covering semiconductor elements of the present invention has the content range of each component regulated, which reduces the environmental load, improves acid resistance, and makes it easier to lower the firing temperature.
[0012] The glass for covering a semiconductor element of the present invention preferably contains, in mol %, 8 to 22% CaO.
[0013] The material for covering a semiconductor element of the present invention preferably contains 75 to 100 mass % of glass powder made of the above-mentioned glass for covering a semiconductor element, and 0 to 25 mass % of ceramic powder.
[0014] The semiconductor element coating material of the present invention has a thermal expansion coefficient of 20×10 -7 / ℃~55×10 -7 / ° C. Here, the "coefficient of thermal expansion in the temperature range of 30 to 300° C." refers to a value measured using a push rod type thermal expansion coefficient measuring device. Effect of the Invention
[0015] According to the present invention, it is possible to provide a glass for covering semiconductor elements which has a small environmental impact, is excellent in acid resistance, and can be fired at a low temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] In this specification, a numerical range indicated using "to" means a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively.
[0017] The glass for covering semiconductor elements of the present invention is characterized in that it contains, in mole percent, SiO2 20-36%, ZnO 8-40%, B2O3 10-24%, Al2O3 10-20%, and MgO+CaO 8-22% as a glass composition, and has a molar ratio of SiO2 / ZnO of 0.6 or more and less than 3.3, and is substantially free of lead components. The reasons for limiting the content of each component as described above are explained below. In the following explanation of the content of each component, % means mol % unless otherwise specified.
[0018] SiO2 is a component that forms the glass network and enhances acid resistance. The SiO2 content is 20 to 36%, preferably 21 to 33%, and particularly preferably 22 to 30%. If the SiO2 content is too low, the acid resistance is likely to decrease and vitrification is difficult. On the other hand, if the SiO2 content is too high, the firing temperature of the glass becomes high, which is likely to deteriorate the characteristics of the semiconductor element in the coating process.
[0019] ZnO is a component that stabilizes glass. The ZnO content is 8 to 40%, preferably 12 to 38%, and particularly preferably 14 to 32%. If the ZnO content is too low, the glass becomes more prone to devitrification during melting, making it difficult to obtain a homogeneous glass. On the other hand, if the ZnO content is too high, the acid resistance is easily reduced.
[0020] SiO2 / ZnO is 0.6 or more and less than 3.3, preferably 0.8 to 2.4, and particularly preferably 1 to 1.8. If SiO2 / ZnO is too small, the glass is likely to undergo phase separation and the acid resistance is likely to decrease. On the other hand, if SiO2 / ZnO is too large, the firing temperature of the glass becomes high, which is likely to deteriorate the characteristics of the semiconductor element in the coating process.
[0021] B2O3 is a component that forms a glass network and enhances softening and fluidity. The content of B2O3 is 10 to 24%, preferably 11 to 22%, and particularly preferably 12 to 20%. If the content of B2O3 is too low, the crystallinity becomes strong, which impairs the softening and fluidity during coating, making it difficult to uniformly coat the surface of the semiconductor element. On the other hand, if the content of B2O3 is too high, the acid resistance tends to decrease.
[0022] Al2O3 is a component that stabilizes glass. The content of Al2O3 is 10 to 20%, preferably 11 to 19%, and particularly preferably 12 to 18%. If the content of Al2O3 is too low, vitrification becomes difficult. On the other hand, if the content of Al2O3 is too high, the firing temperature of the glass becomes high, which tends to deteriorate the characteristics of the semiconductor element in the coating process.
[0023] MgO and CaO are components that reduce the viscosity of glass. By including a predetermined amount of MgO and / or CaO, low-temperature firing is possible even when a large amount of SiO2 is included. MgO+CaO is 8-22%, preferably 9-21%, and particularly preferably 10-20%. If the amount of MgO+CaO is too small, the softening temperature of the glass tends to increase. On the other hand, if the amount of MgO+CaO is too large, the thermal expansion coefficient tends to become too high and the insulating properties tend to decrease.
[0024] The preferred ranges of the MgO and CaO contents are as follows:
[0025] The MgO content is preferably 0 to 22%, 4 to 22%, 8 to 22%, or 9 to 21%, and particularly preferably 10 to 20%.
[0026] The CaO content is preferably 0 to 22%, 4 to 22%, 8 to 22%, or 9 to 21%, and particularly preferably 10 to 20%.
[0027] In addition to the above components, other components (for example, SrO, BaO, MnO2, Bi2O3, Ta2O5, Nb2O5, CeO2, Sb2O3, etc.) may be contained up to 7% (preferably up to 3%).
[0028] From an environmental standpoint, it is preferable that the material contains substantially no lead components (e.g., PbO, etc.) and substantially no F or Cl. It is also preferable that the material contains substantially no alkali metal components (e.g., Li2O, Na2O, and K2O) that adversely affect the surface of semiconductor elements.
[0029] The glass for covering a semiconductor element of the present invention is preferably in a powder form, that is, in the form of glass powder. If it is processed into glass powder, it can be easily used to cover the surface of a semiconductor element by, for example, a paste method or an electrophoretic coating method.
[0030] Average particle size of glass powder D 50 The average particle diameter D of the glass powder is preferably 25 μm or less, and more preferably 15 μm or less. 50 If the average particle diameter D of the glass powder is too large, it becomes difficult to form a paste. Also, it becomes difficult to apply the paste by electrophoresis. 50 The lower limit of the average particle diameter D is not particularly limited, but in reality, it is preferably 0.1 μm or more. 50 " is a value measured on a volume basis and refers to a value measured by a laser diffraction method.
[0031] The glass for covering semiconductor elements of the present invention can be obtained, for example, by blending raw material powders of each oxide component into a batch, melting the batch at about 1500°C for about 1 hour to vitrify the batch, and then molding the batch (and then crushing and classifying the batch, if necessary).
[0032] The material for covering a semiconductor element of the present invention contains a glass powder made of the glass for covering a semiconductor element, and may be mixed with a ceramic powder (e.g., cordierite powder) to form a composite powder, if necessary. The addition of the ceramic powder makes it easier to adjust the thermal expansion coefficient.
[0033] The material for covering a semiconductor element of the present invention preferably contains 75 to 100 mass % of a glass powder made of the glass for covering a semiconductor element, and 0 to 25 mass % of a ceramic powder.
[0034] The amount of the ceramic powder is preferably less than 25 parts by mass, particularly less than 20 parts by mass, per 100 parts by mass of the glass powder. If the content of the ceramic powder is too high, the softening and flowability of the glass is impaired, making it difficult to coat the surface of the semiconductor element.
[0035] Average particle size of ceramic powder D 50 The average particle diameter D of the ceramic powder is preferably 30 μm or less, and more preferably 20 μm or less. 50 If the average particle diameter D of the ceramic powder is too large, the surface smoothness of the coating layer is likely to decrease. 50 The lower limit is not particularly limited, but is practically 0.1 μm or more.
[0036] In the semiconductor element coating material of the present invention, the thermal expansion coefficient in the temperature range of 30 to 300°C is 20 × 10 -7 / ℃~55×10 -7 / ℃, especially 30×10 -7 / ℃~50×10 -7 / ° C. If the thermal expansion coefficient is outside the above range, cracks, warping, etc. are likely to occur due to the difference in thermal expansion coefficient with the semiconductor element.
[0037] In the semiconductor element covering material of the present invention, the firing temperature when forming the covering layer is preferably 900° C. or less, particularly 880° C. or less. If the firing temperature is too high, the semiconductor element is likely to deteriorate. EXAMPLES
[0038] The present invention will be described in detail below based on examples. Note that the following examples are merely illustrative and the present invention is not limited to the following examples in any way.
[0039] Table 1 shows examples of the present invention (samples Nos. 1 to 4) and comparative examples (samples Nos. 5 to 8).
[0040] [Table 1]
[0041] Each sample was prepared as follows. First, raw material powders were mixed to obtain the glass composition shown in Table 1 to prepare a batch, which was then melted at 1500°C for 1 hour to form a glass. The molten glass was then formed into a film, pulverized in a ball mill, and classified using a 350 mesh sieve to obtain the average particle diameter D 50 In sample No. 1, the amount of cordierite powder (average particle diameter D 50 : 12 μm) was added to form a composite powder.
[0042] The thermal expansion coefficient, softening point, and acid resistance of each sample were evaluated, and the results are shown in Table 1.
[0043] The thermal expansion coefficient is a value measured in a temperature range of 30 to 300°C using a push rod type thermal expansion coefficient measuring device.
[0044] The softening point was measured using a macro-type differential thermal analyzer. Specifically, the value of the fourth inflection point in the chart obtained by measuring each glass powder sample using the macro-type differential thermal analyzer was taken as the softening point.
[0045] Acid resistance was evaluated as follows. Each sample was press molded into a size of about 20 mm in diameter and 4 mm in thickness, and then fired at the firing temperature in Table 1 to prepare a pellet-shaped sample. This sample was immersed in 30% nitric acid at 25°C for 1 minute, and the mass change per unit area was calculated from the mass loss, which was used as an index of acid resistance. A mass change per unit area of 1.0 mg / cm 2 Less than 1.0mg / cm 2 The above was marked as “X.” The firing temperature was set to the softening point + 20°C.
[0046] As is clear from Table 1, samples Nos. 1 to 4 have a thermal expansion coefficient of 39×10 -7 / ℃~43×10 -7 The firing temperature was 820 to 850° C., and the acid resistance was also evaluated as good. Therefore, Samples Nos. 1 to 4 are considered to be suitable for covering semiconductor elements.
[0047] On the other hand, sample No. 5 showed strong phase separation and did not vitrify. Sample No. 6 was fired at a high temperature. Samples No. 7 and 8 had poor acid resistance.
Claims
1. The glass composition is, in mol%, SiO 2 20-36%, ZnO 8-40%, B 2 O 3 10-24%, Al 2 O 3 10-20%, MgO+CaO 8-22%, Bi 2 O 3 0-3%, and the molar ratio is SiO 2 4. A glass for covering a semiconductor element, characterized in that the glass has a ZnO ratio of 0.6 or more to less than 3.3 and is substantially free of lead components.
2. 2. The glass for covering a semiconductor element according to claim 1, which contains, in mol %, 8 to 22% of CaO.
3. A material for covering a semiconductor element, comprising 75 to 100 mass % of a glass powder made of the glass for covering a semiconductor element according to claim 1 or 2, and 0 to 25 mass % of a ceramic powder.
4. The thermal expansion coefficient in the temperature range of 30 to 300°C is 20 x 10 -7 / ℃~55×10 -7 4. The semiconductor element coating material according to claim 3, wherein the temperature is 100° C. / ° C.
Citation Information
Patent Citations
JP1973043275A
JP1975129181A
Nonnlinear resistor and method of manufacturing same
JP1981013702A
Dot matrix type printer
JP1989049653A