Thermoplastic polyurethane resin composition and molded article using said resin composition

A thermoplastic polyurethane resin composition with a specific polyol blend of aliphatic polyisocyanate, polycarbonate polyol, and cyclic polyol addresses wear and hydrolysis resistance issues, ensuring durability and transparency.

JP7583514B2Active Publication Date: 2024-11-14TOSOH CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2018022780
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-02-13
Publication Date
2024-11-14
Estimated Expiration
2038-02-13

AI Technical Summary

Technical Problem

Thermoplastic polyurethane resins formed from aliphatic diisocyanate lack wear resistance under harsh mechanical loads and exhibit insufficient hydrolysis resistance, while those containing aromatic rings suffer from yellowing and hydrolysis issues.

Method used

A thermoplastic polyurethane resin composition is developed as a reaction product of an aliphatic polyisocyanate, a chain extender, and a polyol component comprising polycarbonate polyol and a polyol with a cyclic structure, with a specific mass ratio, enhancing mechanical properties, hydrolysis resistance, and abrasion resistance.

Benefits of technology

The composition achieves improved mechanical properties, hydrolysis resistance, transparency, and abrasion resistance, maintaining durability over time and preventing yellowing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583514000001
    Figure 0007583514000001
  • Figure 0007583514000002
    Figure 0007583514000002
  • Figure 0007583514000003
    Figure 0007583514000003
Patent Text Reader

Abstract

To provide a thermoplastic resin composition that can form an article having improved wear resistance, mechanical properties, hydrolysis resistance, transparency, and blooming resistance and required durability.SOLUTION: A thermoplastic polyurethane resin composition is a reaction product of an isocyanate component (A), a chain extender (B), and a polyol component (C). The isocyanate component (A) has an aliphatic polyisocyanate, The polyol component (C) has a polycarbonate polyol (C1), and a polyol (C2) having a cyclic structure. A mass ratio between the polycarbonate polyol (C1) and the polyol (C2) having the cyclic structure,(C1) / (C2), is 10 / 90 or more and 90 / 10 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic polyurethane resin composition and a molded article using the resin composition. [Background technology]

[0002] Thermoplastic polyurethane resin (hereinafter referred to as TPU) has excellent strength, flexibility and abrasion resistance, and is therefore used in a variety of components that require mechanical durability. TPUs that use aromatic isocyanates are commonly used. However, TPUs that use aromatic isocyanates tend to yellow over time, which reduces their design. Therefore, when design is important, TPUs that are made from aliphatic or alicyclic diisocyanates are often used.

[0003] Patent Document 1 discloses a thermoplastic polyurethane elastomer containing, as main components, a polymeric diol containing an aromatic ring and an aliphatic diisocyanate. Patent Document 2 discloses a polyurethane molding material containing as main components: a mixed polyol composed of a polycarbonate diol and a polyester diol made from adipic acid as a starting material; and 1,6-hexamethylene diisocyanate. Patent Document 3 discloses a TPU using an aliphatic isocyanate, a polycarbonate polyol, and a diol having 6 or more carbon atoms as a chain extender. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Unexamined Patent Publication No. 63-110211 [Patent Document 2] Japanese Patent Application Publication No. 6-206973 [Patent Document 3] Japanese Patent Application Publication No. 6-116355 Summary of the Invention [Problem to be solved by the invention]

[0005] However, even TPUs formed from alicyclic diisocyanates lack abrasion resistance in a usage environment where severe mechanical loads are applied, and are insufficient for maintaining design. Therefore, the TPUs obtained from the polyurethane molding material disclosed in Patent Document 2 and the TPUs disclosed in Patent Document 3 do not have sufficient abrasion resistance, and further improvement is required. Furthermore, the thermoplastic polyurethane elastomer disclosed in Patent Document 1 lacks hydrolysis resistance because the polymer diol containing an aromatic ring in the molecule is a polyester polyol.

[0006] The present inventors have conducted intensive research to solve the above problems, and have found that a thermoplastic polyurethane resin, which is a reaction product of an aliphatic polyisocyanate and a polyol component, and which contains a polycarbonate polyol and a polyol having a cyclic structure in a specific ratio, exhibits better abrasion resistance than the case where these polyols are used alone. As a result of further intensive research on this specific TPU, the inventors have completed a thermoplastic polyurethane resin composition that achieves various properties at a high level and can be used in practical applications, and a molded product using the same.

[0007] Therefore, one embodiment of the present invention is directed to providing a thermoplastic polyurethane resin composition that has excellent mechanical properties, hydrolysis resistance, transparency, bloom resistance, and abrasion resistance and can suppress deterioration of durability over a long period of time. Another embodiment of the present invention is directed to providing a molded article made of the thermoplastic polyurethane resin composition. [Means for solving the problem]

[0008] A thermoplastic polyurethane resin composition according to one embodiment of the present invention is a reaction product of an isocyanate component (A), a chain extender (B), and a polyol component (C), The isocyanate component (A) contains an aliphatic polyisocyanate, The polyol component (C) A polycarbonate polyol (C1), A polyol (C2) having a cyclic structure, The mass ratio (C1) / (C2) of the polycarbonate polyol (C1) to the polyol having a cyclic structure (C2) is 10 / 90 or more and 90 / 10 or less. A molded article according to another embodiment of the present invention is made of the above thermoplastic polyurethane resin composition. Effect of the Invention

[0009] According to the thermoplastic polyurethane resin composition of the present invention, it is possible to provide a thermoplastic polyurethane resin composition having excellent mechanical properties, hydrolysis resistance, transparency, bloom resistance, and abrasion resistance, and capable of suppressing deterioration of durability over a long period of time. Also, according to the molded article of another embodiment of the present invention, it is possible to provide a molded article made of the thermoplastic polyurethane resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Exemplary embodiments for carrying out the present invention are described in detail below.

[0011] [Thermoplastic polyurethane resin composition] A thermoplastic polyurethane resin composition according to one embodiment of the present invention is a reaction product of an isocyanate component (A), a chain extender (B), and a polyol component (C), The isocyanate component (A) contains an aliphatic polyisocyanate, The polyol component (C) A polycarbonate polyol (C1), A polyol (C2) having a cyclic structure, The mass ratio (C1) / (C2) of the polycarbonate polyol (C1) to the polyol having a cyclic structure (C2) is 10 / 90 or more and 90 / 10 or less.

[0012] <Isocyanate component (A)> The isocyanate component (A) contains an aliphatic polyisocyanate. Examples of the aliphatic polyisocyanate include linear aliphatic diisocyanates such as 1,6-hexamethylene diisocyanate, 1,12-dodecane diisocyanate, 3-methyl-1,5-pentane diisocyanate, and trimethyl-hexamethylene diisocyanate; and alicyclic diisocyanates having an alicyclic structure such as cyclohexane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, and norbornane diisocyanate. In addition, examples of the aliphatic polyisocyanate include isocyanate-terminated compounds obtained by the reaction of these isocyanates with active hydrogen group-containing compounds, and polyisocyanate modified products obtained by the reaction of these compounds themselves, such as uretdione reaction, isocyanurate reaction, and carbodiimide reaction. Among these isocyanates, 1,6-hexamethylene diisocyanate is preferred from the standpoint of improving toughness and flexibility.

[0013] <Chain extender (B)> Examples of the chain extender (B) include low molecular weight diols and bifunctional low molecular weight glycol ethers.

[0014] Examples of low molecular weight diols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2,2-diethyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 1,4-cyclohexanedimethanol, and 1,4-bis(2-hydroxyethoxy)benzene, and mixtures of two or more of these. In addition, as long as the properties of the thermoplastic resin are not impaired, active hydrogen compounds having one functional group, such as 1-decanol, 1-dodecanol, stearyl alcohol, 1-docosanol, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, diethylene glycol monohexyl ether, and triethylene glycol monomethyl ether, and active hydrogen compounds having more than two functional groups, such as glycerin, trimethylolpropane, pentaerythritol, diglycerin, and sorbitol, can also be used in combination.

[0015] Examples of difunctional low molecular weight glycol ethers include glycol ethers of 2,2-bis(4-polyoxyethylene-oxyphenyl)propane, 2,2-bis(4-polyoxypropylene-oxyphenyl)propane, dimethylolheptane ethylene oxide adduct, dimethylolheptane propylene oxide adduct, etc. These may be used alone or in combination of two or more.

[0016] The number average molecular weight of the chain extender (B) is preferably 60 or more and 300 or less in order to make the most of the inherent properties of thermoplastic resins, such as softness and flexibility. If the number average molecular weight of the chain extender (B) is less than 60, the concentration of urethane groups in the TPU will be relatively too high, resulting in the generation of unmelted material, or the viscosity of the molten TPU will increase, causing molding defects during processing and a poor appearance. Also, if the number average molecular weight is less than 60, although the hardness, 100% modulus, tensile strength, and tear strength will be high, elongation will decrease, and it may become difficult to utilize the inherent properties of thermoplastic resin, such as flexibility and malleability. On the other hand, if the number average molecular weight of the chain extender (B) exceeds 300, the urethane group concentration becomes relatively too low, so that the desired physical properties may not be obtained, and the molded article of the thermoplastic polyurethane resin composition obtained by using this TPU may have insufficient mechanical properties.

[0017] Of these, the chain extender (B) is preferably at least one selected from the group consisting of 1,4-butanediol and 1,6-hexanediol.

[0018] <Polyol component (C)> The polyol component (C) contains a polycarbonate polyol (C1) and a polyol having a cyclic structure (C2).

[0019] <<Polycarbonate polyol (C1)>> Examples of the polycarbonate polyol (C1) include polycarbonate diols obtainable by dealcoholization reaction, dephenolization reaction, etc. of diols including 2-methyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,4-cyclohexanedimethanol, etc., with dimethyl carbonate, diethyl carbonate, diphenyl carbonate, diethylene carbonate, etc. Two or more kinds of polycarbonate diols can be used in combination. Among these, polycarbonate diols are preferred from the viewpoint of improving durability such as hydrolysis resistance. In order to further improve abrasion resistance, polycarbonate diols whose reaction residues are composed only of linear alkylene groups are more preferred. In other words, polycarbonate diols that do not have a cyclic structure or a branched alkyl group are more preferred.

[0020] <<Polyol having a cyclic structure (C2)>> The polyol (C2) having a cyclic structure is a polyol having a cyclic structure such as an aromatic ring structure or an alicyclic structure in the molecule, and examples thereof include polyester diols, polycarbonate diols, polylactone diols, and polyether diols, and these can be used alone or in combination of two or more. The polyol (C2) having a cyclic structure is preferably a polyether diol containing a structural unit derived from isophthalic acid. Among these polyols, polyester diols comprising a component derived from isophthalic acid and a component derived from 1,6-hexanediol are particularly preferred from the standpoints of transparency, compatibility with bloom-causing substances such as cyclic oligomers contained as by-products in TPU and stabilizers, hydrolysis resistance, and economy.

[0021] <<Number average molecular weight of polyol component (C)>> The number average molecular weight of the polyol component (C) is preferably 750 or more and 3,000 or less, more preferably 800 or more and 2,000 or less, and even more preferably 1,000 or more and 2,000 or less. When the number average molecular weight is 750 or more and 3,000 or less, the moldability during processing of the thermoplastic polyurethane resin is improved, and the mechanical properties and transparency of the molded article of the resin composition can be further improved. The number average molecular weight of the polyol component (C) can be measured in accordance with JIS K 7252-3 (Plastics - Determination of average molecular weight and molecular weight distribution of polymers by size exclusion chromatography - Part 3: Method at about room temperature).

[0022] <<Mass ratio (C1) / (C2)>> The mass ratio (C1) / (C2) of the polycarbonate polyol (C1) to the polyol (C2) having a cyclic structure is 10 / 90 or more and 90 / 10 or less, more preferably 30 / 70 or more and 70 / 30 or less. By mixing and using the polycarbonate polyol (C1) and the polyol (C2) having a cyclic structure, it is possible to exhibit better abrasion resistance than when each polyol is used alone. However, when the mass ratio of the polycarbonate polyol (C1) or the polyol (C2) having a cyclic structure is less than 10 / 90, it causes insufficient abrasion resistance and deterioration of appearance.

[0023] <<Other polyol components>> Note that, as long as the gist of the present disclosure is not impaired, polycarbonate polyol (C1) and polyol (C2) having a cyclic structure may be further used in combination with polylactone diols and polyether diols.

[0024] <<R' value: number of moles of active hydrogen groups of chain extender (B) / number of moles of active hydrogen groups of polyol component (C)>> The blending ratio of the chain extender (B) and the polyol component (C) is the ratio of the number of moles of active hydrogen groups of the chain extender (B) to the number of moles of active hydrogen groups of the polyol component (C) ([number of moles of active hydrogen groups of chain extender (B)] / [number of moles of active hydrogen groups of polyol component (C)] = R' value), which is an index of the amount of hard segments of TPU and affects the expression of physical properties. From this viewpoint, the R' value is preferably 0.1 or more and 15 or less, more preferably 0.3 or more and 12 or less.

[0025] <<<R value: total number of moles of isocyanate groups / total number of moles of active hydrogen groups>>> The ratio of the total number of moles of isocyanate groups of the isocyanate component to the total number of moles of active hydrogen groups obtained by summing the number of moles of active hydrogen groups of the chain extender (B) and the number of moles of active hydrogen groups of the polyol component (C) ([total number of moles of isocyanate groups] / [total number of moles of active hydrogen groups] = R value) is preferably 0.7 or more and 1.3 or less, more preferably 0.8 or more and 1.2 or less, from the viewpoint of adjusting the molecular weight and viscosity of TPU to a preferable range.

[0026] <Stabilizer> The thermoplastic polyurethane resin composition may further contain at least one stabilizer selected from the group consisting of UV (Ultraviolet) absorbers, light stabilizers, and antioxidants.

[0027] As the UV absorbent, a conventionally known one can be used. Representative examples include Tinuvin-328: 2-(2H-1,2,3-benzotriazol-2-yl)-4,6-di-tert-pentylphenol (manufactured by BASF), JF-83: 2-[2-hydroxy-5-(1,1,3,3-tetramethylbutyl)phenyl]benzotriazole (manufactured by Johoku Chemical Industry Co., Ltd.), Tinuvin-326: 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole (manufactured by BASF), Adekas TabLA-46: 2-ethylhexanoic acid = 2-[3-hydroxy-4-(4,6-diphenyl-1,3,5-triazin-2-yl)phenoxy]ethyl (ADEKA), Tinuvin-1577: 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)phenol (BASF), Hostavin-VSU: N-(2-ethylphenyl)-N'-(2-ethoxyphenyl) oxalic acid diamide (Clariant), etc. These may be used alone or in combination of two or more.

[0028] As the light stabilizer, a conventionally known light stabilizer can be used. Representative examples include Chimassorb-944: poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}] (manufactured by BASF), Tinuvin-622: dimethyl succinate·1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate (manufactured by BASF), Tinuvin-770: bis(2,2,6,6-tetramethylpiperidin-4-yl)=decanedioate (manufactured by BASF), and Tinuvin-765: bis(1,2,2,6,6-pentamethyl-4-piperidyl)=decanedioate (manufactured by BASF). These may be used alone or in combination of two or more.

[0029] The antioxidant may be a conventionally known one. Representative examples include IRGANOX-1010: pentaerythritol tetrakis[3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate] (manufactured by BASF), Sumilizer GA-80: 2,2'-dimethyl-2,2'-(2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diyl)dipropane-1,1'-diyl bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propanoate] (manufactured by Sumitomo Chemical Co., Ltd.). These may be used alone or in combination of two or more.

[0030] <Other additives> In addition to the above-mentioned components, various additives that are commonly used in the production of TPU, such as heat stabilizers, antioxidants, ultraviolet absorbers, flame retardants, hydrolysis inhibitors, heat resistance improvers, weather resistance improvers, reactivity retarders, lubricants, plasticizers, antistatic agents, conductivity imparting agents, antibacterial agents, antifungal agents, colorants, inorganic and organic fillers, fiber reinforcing materials, and crystal nucleating agents, can also be added appropriately to the thermoplastic polyurethane resin composition as needed.

[0031] <Method of producing thermoplastic polyurethane resin composition> The thermoplastic polyurethane resin composition can be prepared by mixing raw materials (TPU, stabilizer, other additives) blended in an appropriate ratio in a kneader, Henschel mixer, or the like, feeding them into an extruder, melt-kneading them at a temperature at which normal TPU is extruded (about 150°C to 220°C), and then cutting them into pellets by strand cutting or underwater cutting. Note that the stabilizer and other additives are all optional components, so when mixing, one or more selected from them may be added in appropriate amounts as necessary.

[0032] Alternatively, the optional components can be blended with the raw materials used in producing the TPU, such as the polyol component (C) or the isocyanate component (A), mixed uniformly, and then reacted to prepare a thermoplastic polyurethane resin composition.

[0033] As a method for adding optional components such as stabilizers, in addition to adding them directly to TPU, a method can also be used in which a masterbatch containing the optional components at a high concentration is prepared in advance, and the masterbatch is converted to a desired concentration and then mixed with TPU.

[0034] The TPU constituting the thermoplastic polyurethane resin composition can be obtained by known TPU production methods, such as the one-shot method, prepolymer method, batch reaction method, continuous reaction method, kneader method, extruder method, and the like.

[0035] The thermoplastic polyurethane resin composition can be obtained by the above-mentioned production method in the form of flakes, pellets, powder, granules, rods, sheets, blocks, etc.

[0036] The powder or block-like solid material obtained as described above can be pulverized to obtain flakes, which can then be fed into an extruder and melt-kneaded at a temperature at which ordinary TPU is extruded (approximately 150°C or higher and 220°C or lower), after which pellets can be obtained by strand cutting or underwater cutting.

[0037] In the kneader method, the polyol component (C), the chain extender (B), and optional components such as a stabilizer are charged into a kneader, and the mixture is heated to 100°C under stirring, and then the isocyanate component (A) is added, reacted for 10 to 120 minutes, and cooled to produce a powdered or block-shaped thermoplastic polyurethane resin composition. In these methods, a catalyst can be added as necessary.

[0038] <<Catalyst>> Examples of catalysts used in the production of the TPU include amines such as triethylamine, triethylenediamine, N-methylimidazole, N-ethylmorpholine, and 1,8-diazabicyclo[5,4,0]-7-undecene (DBU); organic metals such as potassium acetate, stannous octoate, dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin diacetate, titanic acid esters, zirconium compounds, bismuth compounds, and iron compounds; phosphorus compounds such as tributylphosphine, phospholene, and phospholene oxide; and the like. These compounds can be used alone or in combination of two or more. Of these, organometallic compounds, particularly titanate, iron, tin, zirconium and bismuth compounds are preferred. The total amount of catalyst used is preferably about 5% by mass or less, more preferably 0.001% by mass to 2% by mass, based on the TPU.

[0039] The thermoplastic polyurethane resin composition can be molded by any of the commonly used molding methods for TPU, such as extrusion molding, injection molding, inflation molding, blow molding, vacuum molding, centrifugal molding, rotational molding, calendar processing, roll processing, and press processing.

[0040] [Molded body] The above-mentioned thermoplastic polyurethane resin composition can be suitably used as various molded articles. Accordingly, a molded article according to one embodiment of the present invention is made of the above-mentioned thermoplastic polyurethane resin composition. Examples of the molded article include interior and exterior materials for houses, communication cables, industrial cables, automobiles, interior and exterior materials for various vehicles, home appliances, decorations, wind turbines for wind power generation, protective films, etc. These can be used in a wide range of fields, both indoors and outdoors.

[0041] [1]: A thermoplastic polyurethane resin composition according to a first embodiment of the present invention is a thermoplastic polyurethane resin composition which is a reaction product of an isocyanate component (A), a chain extender (B), and a polyol component (C), The isocyanate component (A) contains an aliphatic polyisocyanate, The polyol component (C) A polycarbonate polyol (C1), A polyol (C2) having a cyclic structure, The mass ratio (C1) / (C2) of the polycarbonate polyol (C1) to the polyol having a cyclic structure (C2) is 10 / 90 or more and 90 / 10 or less. [2]: A thermoplastic polyurethane resin composition according to a second embodiment of the present invention, the thermoplastic polyurethane resin composition according to the first embodiment, wherein the mass ratio (C1) / (C2) is 30 / 70 or more and 70 / 30 or less. [3]: A thermoplastic polyurethane resin composition according to a third embodiment of the present invention, the thermoplastic polyurethane resin composition according to the first or second embodiment, wherein the aliphatic polyisocyanate is 1,6-hexamethylene diisocyanate. [4]: A thermoplastic polyurethane resin composition according to a fourth embodiment of the present invention is the thermoplastic polyurethane resin composition according to any one of the items 1 to 3, characterized in that the chain extender (B) is at least one selected from the group consisting of 1,4-butanediol and 1,6-hexanediol. [5]: A thermoplastic polyurethane resin composition according to a fifth embodiment of the present invention is the thermoplastic polyurethane resin composition according to any one of the first to fourth embodiments, characterized in that the polycarbonate polyol (C1) is a polycarbonate diol. [6]: A thermoplastic polyurethane resin composition according to a sixth embodiment of the present invention is the thermoplastic polyurethane resin composition according to any one of the first to fifth aspects, characterized in that the polyol (C2) having a cyclic structure is a polyester diol containing a structural unit derived from isophthalic acid. [7]: A thermoplastic polyurethane resin composition according to a seventh embodiment of the present invention is the thermoplastic polyurethane resin composition according to any one of the items 1 to 6, characterized in that the polycarbonate polyol (C1) is a polycarbonate diol whose reaction residues are composed only of linear alkylene groups. [8]: A thermoplastic polyurethane resin composition according to an eighth embodiment of the present invention is the thermoplastic polyurethane resin composition according to any one of items 1 to 7, further comprising at least one stabilizer selected from the group consisting of a UV absorber, a light stabilizer, and an antioxidant. [9]: A molded article according to a ninth embodiment of the present invention is made of the thermoplastic polyurethane resin composition according to any one of the first to eighth aspects.

[0042] According to the thermoplastic polyurethane resin composition of one embodiment of the present invention, the abrasion resistance of an aliphatic TPU, which has high resistance to yellowing over time, is improved, and further, by specifying the TPU composition, good mechanical properties, hydrolysis resistance, and appearance are achieved, making it possible to achieve both designability and durability. EXAMPLES

[0043] The present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these in any way. Among the following Examples 1 to 12, Examples 1 and 2 are examples for reference that do not belong to the scope of the present invention.

[0044] <Examples 1 to 12 and Comparative Examples 1 to 5> (Sample Preparation) The polyol component (C) and the chain extender (B) were charged in the amounts (parts by mass) shown in Tables 1 to 3 into a reaction vessel equipped with a stirrer and a thermometer, and mixed uniformly to obtain a mixed liquid. The resulting mixture was heated to 100°C, and the amount (parts by mass) of isocyanate component (A) shown in Tables 1 to 3 was added to carry out a urethane reaction. When the reaction mixture reached 90°C, it was poured onto a tray and solidified to obtain a solid. The resulting solid was aged in an electric furnace at 80°C for 16 hours, cooled to room temperature, and then pulverized to obtain flake-shaped TPU. The obtained flake-like TPU was pelletized in an extruder, and the obtained pellets were subjected to T-die extrusion molding or injection molding at 180 to 220°C to produce a 0.15 mm thick film (extrusion molding) or a 2 mm thick sheet (injection molding), which were used as samples (thermoplastic polyurethane resin compositions) of Examples 1 to 12 and Comparative Examples 1 to 5.

[0045] [Table 1]

[0046] [Table 2]

[0047] [Table 3]

[0048] The raw materials used and shown in Tables 1 to 3 are as follows. <Isocyanate component (A)> HDI: 1,6-hexamethylene diisocyanate, manufactured by Tosoh Corporation <Chain extender (B)> 1,4-BG: 1,4-butanediol (number average molecular weight = 90), manufactured by Mitsubishi Chemical Corporation 1,6-HG: 1,6-hexanediol (number average molecular weight = 118), manufactured by Mitsubishi Chemical Corporation <Polycarbonate diol (C1) whose reactive residues consist only of linear alkyl groups> PCD(HG / MPD=10 / 0)-1000: Polyhexamethylene carbonate diol (number average molecular weight=1000), manufactured by Tosoh Corporation <Polycarbonate diol (C1) in which the reactive residue contains an alkyl group having a side chain> PCD(HG / MPD=1 / 9)-1000: Polycarbonate diol (number average molecular weight=1000) with a molar ratio of hexamethylene residues and 3-methyl-pentamethylene residues of 1 / 9, manufactured by Tosoh Corporation <Polyol having a cyclic structure (C2)> iPA / HG-1000: polyester diol (number average molecular weight = 1000) containing structural units derived from isophthalic acid and structural units derived from 1,6-hexanediol, manufactured by Tosoh Corporation <Polyester diol> BA-1000: polyester diol (number average molecular weight = 1000) containing adipic acid-derived structural units and 1,4-butanediol-derived structural units, manufactured by Tosoh Corporation

[0049] (Characteristics test) The T-die extrusion film or injection molded sheet as the molded product produced by the above procedure were evaluated for various properties as shown below. The obtained results are shown in Tables 1 to 3.

[0050] (1) Physical properties (mechanical properties) Using a T-die extrusion molded film, measurements were made according to the measurement method described in JIS K 7311 (Testing method for polyurethane-based thermoplastic elastomers). Note that, for the hardness measurement and Taber abrasion measurement, an injection molded sheet was used. [Hardness (JIS-A hardness)] Anything above 56 is sufficient. [100% modulus (tensile stress, MPa)] It can be said that 3.0 MPa or more is sufficient. [Tensile strength (MPa)] It can be said that 12 MPa or more is sufficient. [stretch(%)] Anything over 400% is considered sufficient. [Tear strength (kN / m)] Anything over 60kN / m is sufficient. [Taber abrasion amount (mg)] Less than 130mg is considered sufficient, and less than 50mg is considered good. Therefore, those over 130mg were rated D, those less than 130mg and 50mg or more were rated B, and those less than 50mg were rated A.

[0051] (2) Transparency The haze was measured using a T-die extrusion film (thickness 0.15 mm) as a test piece. A haze of less than 3% was rated as A, and a haze of 3% or more was rated as D. The haze was measured using a haze meter (NDH2000, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0052] (3) Bloom resistance A T-die extrusion film (thickness 0.15 mm) was used as a test piece, and the change in haze was measured after immersion in pure water at 45°C for two days. A change in haze ("haze % after test" - "haze % before test") of less than 4% was rated A, 4% to less than 6% was rated B, and 6% or more was rated D. Haze was measured using the same method as for transparency evaluation.

[0053] (4) Hydrolysis resistance Using a T-die extrusion film (thickness 0.15 mm), a dumbbell shape (No. 3) as specified in JIS K7311 (Testing method for polyurethane-based thermoplastic elastomers) was punched out to prepare a test specimen. The test specimen was immersed in 85°C warm water for 21 days, and the tensile strength was measured using a tensile tester (UTA-500, manufactured by Orientec Co., Ltd.). The hydrolysis resistance was evaluated according to the retention rate by comparing with the film physical properties (tensile strength) before the test, with a retention rate of 60% or more being rated as A, and a retention rate of less than 60% being rated as D.

Claims

1. A thermoplastic polyurethane resin composition which is a reaction product of an isocyanate component (A), a chain extender (B), and a polyol component (C), comprising: The isocyanate component (A) contains an aliphatic polyisocyanate, The polyol component (C) is Polycarbonate polyol (C1), and a polyol (C2) having a cyclic structure, the polyol (C2) having a cyclic structure is a polyester diol containing a structural unit derived from unsubstituted isophthalic acid and a structural unit derived from 1,6-hexanediol, the mass ratio (C1) / (C2) of the polycarbonate polyol (C1) to the polyol having a cyclic structure (C2) is 10 / 90 or more and 70 / 30 or less; A thermoplastic polyurethane resin composition for use in heat extrusion molding or heat injection molding, comprising:

2. 2. The thermoplastic polyurethane resin composition for heat extrusion molding or heat injection molding according to claim 1, wherein the mass ratio (C1) / (C2) is 30 / 70 or more and 70 / 30 or less.

3. 3. The thermoplastic polyurethane resin composition for heat extrusion molding or heat injection molding according to claim 1, wherein the aliphatic polyisocyanate is 1,6-hexamethylene diisocyanate.

4. The thermoplastic polyurethane resin composition for heat extrusion molding or heat injection molding according to any one of claims 1 to 3, characterized in that the chain extender (B) is at least one selected from the group consisting of 1,4-butanediol and 1,6-hexanediol.

5. 5. The thermoplastic polyurethane resin composition for hot extrusion molding or hot injection molding according to claim 1, wherein the polycarbonate polyol (C1) is a polycarbonate diol.

6. The thermoplastic polyurethane resin composition for hot extrusion molding or hot injection molding according to any one of claims 1 to 5, wherein the polycarbonate polyol (C1) is a polycarbonate diol having reaction residues consisting only of linear alkylene groups.

7. 7. The thermoplastic polyurethane resin composition for heat extrusion molding or heat injection molding according to claim 1, further comprising at least one stabilizer selected from the group consisting of a UV absorber, a light stabilizer, and an antioxidant.

8. A molded article comprising the thermoplastic polyurethane resin composition for hot extrusion molding or hot injection molding according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Thermoplastic polyurethane elastomer

    JP1988110211A

  • Production of polyurethane resin and molding

    JP1994116355A

  • Thermoplastically processable polyurethane molding material for producing embossed sintered sheet

    JP1994206973A

  • Polyester urethaneurea resin composition

    JP2011046887A

  • Antifouling resin composition

    JP2014218577A