Thermoplastic resin compositions and articles
A thermoplastic resin composition with a sea-island structure and siloxane-bonded island structure addresses mechanical and colorability issues, enabling remelting and remolding with improved flexibility and weather resistance.
Patent Information
- Application Number
- JP2022192701
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-01
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2038-09-26
AI Technical Summary
Thermoplastic elastomer compositions face issues with either poor mechanical properties due to partial crosslinking or limited colorability and molding flexibility due to complete crosslinking, and silanol crosslinked resins cannot be remelted and remolded.
A thermoplastic resin composition with a sea-island structure is developed, where the sea structure is made of a thermoplastic resin and the island structure is made of a thermoplastic elastomer crosslinked by siloxane bonds, with a gel fraction of 90% or more, and free radicals are deactivated by a reaction terminator, using a silane coupling agent for dynamic crosslinking.
The composition achieves excellent mechanical properties, colorability, and can be remelted and remolded, with high molding freedom and resistance to weathering deterioration.
Smart Images

Figure 0007583778000002 
Figure 0007583778000003 
Figure 0007583778000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin composition which is excellent in mechanical properties and colorability and which can be molded by remelting, and a method for producing the same. [Background technology]
[0002] Thermoplastic elastomer compositions that can be molded by extrusion molding, injection molding, and the like are used in automobile parts such as weather strips, roof moldings, and mud guards, building materials such as waterproofing materials and joint materials, and industrial components such as hoses. Thermoplastic elastomer compositions include those dynamically crosslinked by blending polypropylene (PP), ethylene propylene diene rubber (EPDM), oil, a crosslinking agent, etc. In the case of complete crosslinking, a phenol-based crosslinking agent is used as the crosslinking agent, and in the case of partial crosslinking, a peroxide crosslinking agent is used as the crosslinking agent (Patent Documents 1 and 2). In addition, there is a silanol cross-linked resin that is produced by mixing a master batch made of polyethylene (PE), a silane coupling agent, and a peroxide (reaction initiator) with a catalyst master batch such as tin, molding the mixture, and then cross-linking with steam or moisture in the air in the subsequent cross-linking process (Patent Document 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-170930 [Patent Document 2] Special Publication No. 58-46138 [Patent Document 3] Japanese Patent Application Publication No. 10-245424 Summary of the Invention [Problem to be solved by the invention]
[0004] However, thermoplastic elastomer compositions (TPVs) dynamically crosslinked using phenolic crosslinking agents have excellent mechanical properties such as compression set due to complete crosslinking, but the molded products have an orange color due to phenol, which reduces coloring freedom. On the other hand, TPVs dynamically crosslinked using peroxide crosslinking agents have a high degree of coloring freedom because the peroxide crosslinking agent itself is colorless and transparent, but they have a problem of poor mechanical properties due to partial crosslinking. In addition, once silanol crosslinking resins are crosslinked, they cannot be remelted or remolded, which reduces the degree of freedom in molding.
[0005] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a thermoplastic resin composition which is excellent in mechanical properties and colorability and can be molded by remelting, and a method for producing the same. [Means for solving the problem]
[0006] First aspect of the invention is a thermoplastic resin composition having an island-in-sea structure, wherein a sea portion of the island-in-sea structure is made of a thermoplastic resin, and an island portion of the island-in-sea structure is made of a thermoplastic elastomer and / or a rubber material crosslinked by a siloxane bond, the island portion has a gel fraction (in accordance with JIS K6769:2004) of 90% or more, and free radicals generated by a reaction initiator contained in the thermoplastic resin composition are deactivated by a reaction terminator contained in the thermoplastic resin composition in a molar ratio of 100% or more relative to the molar ratio of the reaction initiator.
[0007] The second aspect of the invention is the same as the first aspect of the invention. The thermoplastic elastomer and / or rubber material is a thermoplastic elastomer whose main chain and side chain are composed of saturated bonds, and the thermoplastic resin is a thermoplastic resin whose main chain and side chain are composed of saturated bonds.
[0008] The third aspect of the invention is the same as the first or second aspect of the invention. The thermoplastic resin composition is characterized in that it is used as a joint material or a waterproofing material for building materials, an interior material for vehicles, an exterior material for vehicles, or an industrial hose material.
[0009] Aspect of the fourth invention The present invention includes a reaction terminating step of kneading a thermoplastic elastomer and / or rubber material having an alkoxysilyl group, in which an alkoxysilyl group is grafted onto the thermoplastic elastomer and / or rubber material, and a reaction terminator in a molten state in a kneader, and deactivating free radicals derived from a reaction initiator blended to prepare the thermoplastic elastomer and / or rubber material having the alkoxysilyl group with the reaction terminator, thereby preparing a thermoplastic elastomer and / or rubber material having an alkoxysilyl group whose radical activity has been deactivated; and a reaction terminating step of kneading the thermoplastic elastomer and / or rubber material having the alkoxysilyl group, in which an alkoxysilyl group is grafted onto the thermoplastic elastomer and / or rubber material, and a reaction terminating agent in which a free radical derived from a reaction initiator blended to prepare the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated, and and a dynamic crosslinking step of adding a water component to the kneader, converting the alkoxysilyl groups of the thermoplastic elastomer and / or rubber material having alkoxysilyl groups, the radical activity of which has been deactivated, into silanol groups by a hydrolysis reaction with the water component, and then causing a condensation reaction between the silanol groups to form siloxane bonds, wherein the reaction terminator added in the reaction terminating step has a molar ratio of 100% or more to the molar number of the reaction initiator, and the thermoplastic resin composition obtained by the dynamic crosslinking step has an island-sea structure.
[0010] The fifth aspect of the invention is the fourth aspect of the invention. In the dynamic crosslinking step, when the alkoxysilyl group of the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated forms the siloxane bond via the silanol group, the viscosity of the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated becomes greater than the viscosity of the thermoplastic resin, the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated undergoes phase transition to an island structure portion of the sea-island structure, and the thermoplastic resin undergoes phase transition to a sea structure portion of the sea-island structure.
[0011] The sixth aspect of the invention is the fourth or fifth aspect of the invention.The present invention is characterized in that the gel fraction of the island structure portion of the sea-island structure (based on JIS K6769:2004) is 90% or more.
[0012] The seventh aspect of the invention is any one of the fourth to sixth aspects of the invention. In order to prepare a thermoplastic elastomer and / or rubber material having an alkoxysilyl group, the method includes a grafting step of adding the thermoplastic elastomer and / or rubber material, a silane coupling agent, and a reaction initiator, and kneading them in a molten state in the kneader, thereby grafting the silane coupling agent to the thermoplastic elastomer and / or rubber material, and is characterized in that the grafting step, the reaction terminating step, the kneading step, and the dynamic crosslinking step are carried out continuously in the kneader.
[0013] The eighth aspect of the invention is any one of the fourth to seventh aspects of the invention. The present invention is characterized in that the sea structure portion of the sea-island structure is made of the thermoplastic resin and is remeltable.
[0014] The ninth aspect of the invention is any one of the fourth to eighth aspects of the invention. The thermoplastic resin composition has a color difference value ΔE*ab (in accordance with JIS Z8781-4:2013) of 1.5 or more when 0.01 part by weight of a colorant is blended with 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0015] The tenth aspect of the invention is any one of the fourth to ninth aspects of the invention. The thermoplastic resin is a crystalline thermoplastic resin.
[0016] The eleventh aspect of the invention is any one of the fourth to tenth aspects of the invention. The thermoplastic elastomer and / or rubber material is a thermoplastic elastomer whose main chain and side chain are composed of saturated bonds, and the thermoplastic resin is a thermoplastic resin whose main chain and side chain are composed of saturated bonds.
[0017] The twelfth aspect of the invention is the eleventh aspect of the invention. The thermoplastic resin having a main chain and a side chain each composed of a saturated bond is an olefin resin.
[0018] The thirteenth aspect of the invention is the twelfth aspect of the invention. The olefin resin is a polypropylene resin.
[0019] The fourteenth aspect of the present invention is the twelfth or thirteenth aspect of the present invention. The thermoplastic elastomer having a main chain and a side chain each composed of a saturated bond is a polyethylene / α-olefin copolymer.
[0020] The fifteenth aspect of the invention is any one of the twelfth to fourteenth aspects of the invention. The thermoplastic resin composition has a color difference value after weathering degradation: ΔE*ab (based on JIS Z8781-4:2013) of 0 to 3.
[0021] The sixteenth aspect of the invention is any one of the fourth to fifteenth aspects of the invention. The thermoplastic resin composition is characterized in that it is used as a joint material or a waterproofing material for building materials, an interior material for vehicles, an exterior material for vehicles, or an industrial hose material. Effect of the Invention
[0022] Aspects of the first and third inventions According to the method, the sea portion of the sea-island structure is composed of a thermoplastic resin, the island portion of the sea-island structure is composed of a thermoplastic elastomer and / or a rubber material crosslinked by siloxane bonds, the gel fraction of the island portion is 90% or more (based on JIS K6769:2004), and the free radicals generated by a reaction initiator contained in the thermoplastic resin composition have their radical activity inactivated by a reaction terminator, so that a thermoplastic resin composition having good mechanical properties and colorability, which can be remelted and remolded, and which has little deterioration in physical properties and high molding freedom can be obtained.
[0023] Aspects of the second and third aspects of the invention According to the method, a thermoplastic elastomer in which the main chain and side chain are composed of saturated bonds and a thermoplastic resin in which the main chain and side chain are composed of saturated bonds are used as raw materials, and dynamic crosslinking is performed using a silane coupling agent, so that a thermoplastic resin composition can be obtained which is excellent in mechanical properties and colorability, can be remelted and remolded, has a high degree of molding freedom, and is not prone to weather deterioration.
[0024] Aspects of the fourth to sixteenth aspects of the invention According to the method, dynamic crosslinking is carried out using a silane coupling agent, and further, the radical activity of free radicals generated by a reaction initiator is inactivated by a reaction terminator, so that a thermoplastic resin composition having good mechanical properties and colorability and capable of being remelted and remolded and having a high degree of molding freedom can be obtained.
[0025] Aspects of the 12th to 16th aspects of the invention According to the method, a thermoplastic elastomer in which the main chain and side chain are composed of saturated bonds and a thermoplastic resin in which the main chain and side chain are composed of saturated bonds are used as raw materials, and dynamic crosslinking is performed using a silane coupling agent, so that a thermoplastic resin composition can be obtained which is excellent in mechanical properties and colorability, can be remelted and remolded, has a high degree of molding freedom, and is not prone to weather deterioration. [Brief description of the drawings]
[0026] [Figure 1] This is the reaction behavior when an alkoxysilyl group changes into a siloxane bond via a silanol group. [Diagram 2] FIG. 1 is a schematic diagram of a kneader that continuously performs a grafting step, a reaction terminating step, a kneading step, and a dynamic crosslinking step. [Diagram 3] 1 is a table showing the compositions and physical property measurement results of Examples and Comparative Examples. [Figure 4] 1 is a table showing ΔE*ab in NBS units and in terms of color difference. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, embodiments of the thermoplastic composition and the method for producing the same of the present invention will be described. The thermoplastic resin composition of the present invention is a thermoplastic composition having an island-in-sea structure, wherein a sea portion of the island-in-sea structure is composed of a thermoplastic resin, and an island portion of the island-in-sea structure is composed of a thermoplastic elastomer and / or a rubber material crosslinked by a siloxane bond, and the island portion has a gel fraction (in accordance with JIS K6769:2004) of 90% or more, and the radical activity of free radicals generated by a reaction initiator contained in the thermoplastic resin composition is inactivated by a reaction terminator contained in the thermoplastic resin composition in a molar ratio of 100% or more relative to the molar number of the reaction initiator.
[0028] In addition, it is preferable that the thermoplastic elastomer and / or rubber material in the thermoplastic composition of the present invention is a thermoplastic elastomer whose main chain and side chain are composed of saturated bonds, and that the thermoplastic resin is a thermoplastic resin whose main chain and side chain are composed of saturated bonds.
[0029] The thermoplastic composition of the present invention has an island-in-sea structure in which the sea portion is made of a thermoplastic resin, the island portion is made of a thermoplastic elastomer and / or a rubber material crosslinked by a siloxane bond, and the island portion has a gel fraction (in accordance with JIS K6769:2004) of 90% or more. Free radicals generated by a reaction initiator contained in the thermoplastic resin composition have their radical activity inactivated by a reaction terminator, and therefore the thermoplastic composition has good mechanical properties and colorability, can be remelted and remolded, and has a high degree of molding freedom, and is therefore suitable for use as a joint material or water-stopping material for building materials, interior materials for vehicles, exterior materials for vehicles, and industrial hose materials.
[0030] The method for producing the thermoplastic resin composition includes a reaction terminating step, a kneading step, and a dynamic crosslinking step. In the reaction terminating step of the present invention, when a grafting step described later is performed, a reaction terminator is added to the kneader after the grafting step is completed and before the kneading step, while when the grafting step is not performed, the reaction terminator is added to the kneader and kneaded in a molten state before the kneading step, and the free radicals derived from the reaction initiator blended to graft the alkoxysilyl group to the thermoplastic elastomer and / or rubber material are deactivated by the reaction terminator. If the reaction terminator is blended in the kneader before the grafting step is completed, the amount of alkoxysilyl group grafted to the thermoplastic elastomer and / or rubber material decreases, and the gel fraction of the island structure cannot be made 90% or more. On the other hand, if the reaction terminator is blended after blending the thermoplastic resin in the kneader (during the kneading step), the thermoplastic resin may be decomposed by the free radicals present in the kneader to reduce its molecular weight, resulting in a decrease in mechanical properties.
[0031] Reaction stopper (radical capture Agents) include phenolic antioxidants, hindered amine light stabilizers, and radical capture The hindered amine light stabilizer is a colorless compound itself and has a radical- capture It is more preferable because it has excellent coloring and excellent coloring. When using a phenol-based antioxidant, some grades are colored by the phenol-based antioxidant itself, and some grades are colored when processed in a kneader or the like, even if they are not colored, so it is preferable to select a grade that does not become colored even when processed in a kneader or the like. If a colored grade or a grade that becomes colored during processing is used, it is preferable to use an amount that does not affect the coloring property of the thermoplastic resin composition. The reaction stopper may be mixed into the kneader by either mixing the raw materials as they are or mixing them as a master batch.
[0032] The amount of the reaction terminator to be added is preferably 0.01 to 3 parts by weight based on 100 parts by weight of the thermoplastic elastomer and / or rubber material. In order to effectively deactivate the free radicals generated by the reaction initiator, the ratio of the amount (number of moles) of the reaction terminator added to the amount (number of moles) of the reaction initiator added, i.e., the value obtained by the formula [reaction terminator (number of moles) / reaction initiator (number of moles)×100] is preferably 100% or more, and more preferably 100 to 200%.
[0033] The thermoplastic elastomer (TPE) used in the present invention is not limited, and examples thereof include styrene-based thermoplastic elastomers (TPS), hydrogenated styrene-based thermoplastic elastomers (e.g., hydrogenated styrene-ethylene propylene copolymers (SEP), hydrogenated styrene-ethylene propylene styrene copolymers (SEPS), hydrogenated styrene-ethylene butadiene copolymers (SEBS), etc.), olefin-based thermoplastic elastomers (TPO), polymerization type thermoplastic polyolefin-based elastomers (R-TPO), vinyl chloride-based thermoplastic elastomers (TPVC), polyurethane-based thermoplastic elastomers (TPU), polyester-based thermoplastic elastomers (TPC), polyamide-based thermoplastic elastomers (TPA), polybutadiene-based thermoplastic elastomers, and fluorine-based thermoplastic elastomers (TPF), which may be used alone or in combination of two or more.
[0034] The thermoplastic elastomer includes a thermoplastic elastomer in which the main chain and the side chain are saturated bonds, and the thermoplastic elastomer in which the main chain and the side chain are saturated bonds is a thermoplastic elastomer that does not contain unsaturated bonds such as double bonds in the main chain and the side chain. Examples of the thermoplastic elastomer in which the main chain and the side chain are saturated bonds include a polymerized thermoplastic polyolefin elastomer (R-TPO), a polyvinyl chloride thermoplastic elastomer (TPVC), a fluorine-based thermoplastic elastomer (TPF), etc., and one or more types can be used in combination. In particular, a polymerized thermoplastic polyolefin elastomer is preferable, and specifically, an ethylene / α-olefin copolymer elastomer can be mentioned. The copolymer portion of the ethylene / α-olefin copolymer may be either a random copolymer or a block copolymer.
[0035] The rubber material used in the present invention is not limited, and for example, natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene butadiene rubber (SBR), butyl rubber (IIR), nitrile rubber (NBR), ethylene propylene rubber (EPM), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), acrylic rubber (ACM), etc. can be used alone or in combination of two or more. Among the rubber materials, rubber materials that do not contain unsaturated bonds such as double bonds in the main chain are preferred, and examples of such materials include ethylene propylene-based rubbers (EPM, EPDM) and acrylic rubbers (ACM), and these can be used alone or in combination of two or more.
[0036] In the present invention, either the thermoplastic elastomer or the rubber material is used alone, or both are used in combination.
[0037] In addition, when preparing the thermoplastic elastomer having an alkoxysilyl group (when using a thermoplastic elastomer whose main chain and side chain are composed of saturated bonds, a thermoplastic elastomer composed of saturated bonds having an alkoxysilyl group; the same applies below) and / or a rubber material, a grafting process is carried out before the reaction terminating process. In the grafting process, the thermoplastic elastomer and / or rubber material, a silane coupling agent, a reaction initiator, and appropriate additives are added and kneaded in a molten state in a kneader to produce a thermoplastic elastomer consisting of a thermoplastic elastomer and / or rubber material having the alkoxysilyl group.
[0038] The silane coupling agent is used as a crosslinking agent, and a silane coupling agent having an alkoxysilyl group is preferred. Examples of the silane coupling agent having an alkoxysilyl group include an alkoxysilyl compound having a vinyl group, an alkoxysilyl compound having an epoxy group, and an alkoxysilyl compound having an acrylic group or a methacrylic group, and one or more of them can be used in combination. In particular, an alkoxysilyl compound having a vinyl group is more preferred because it has good reactivity with a thermoplastic elastomer and / or a rubber material and is inexpensive. Specific examples of the alkoxysilyl compound having a vinyl group include vinyltrimethoxysilane and vinyltriethoxysilane. The amount of the silane coupling agent to be blended is preferably 0.1 to 3 parts by weight based on 100 parts by weight of the thermoplastic elastomer and / or the rubber material.
[0039] Examples of the reaction initiator include dialkyl peroxides, diacyl peroxides, and alkyl peresters, and one or more of them can be used in combination. In particular, dialkyl peroxides are preferred from the viewpoints of reactivity with the thermoplastic resin composition and cost, and specific examples include dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane. The amount of the reaction initiator is preferably 0.01 to 0.5 parts by weight based on 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0040] Furthermore, it is preferable to add a silanol crosslinking catalyst. Examples of the silanol crosslinking catalyst include dibutyltin and fatty acid amide, and one or more of these can be used in combination. The amount of the silanol crosslinking catalyst added is preferably 0.001 to 0.5 parts by weight per 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0041] Examples of the appropriate additives include synthetic resin stabilizers such as light stabilizers and antioxidants, processing aids such as lubricants and release agents, softeners, colorants, fillers, conductive agents, flame retardants, etc., and can be blended within a range that does not affect the properties of the thermoplastic resin composition. The silanol crosslinking-accelerating catalyst and the appropriate additives may be blended appropriately in a kneader in each of the steps of the grafting step, the kneading step, and the dynamic crosslinking step. The blending of the appropriate additives in the kneader may be performed by blending the raw materials as they are or as a master batch, or by any blending method.
[0042] Examples of synthetic resin stabilizers such as light stabilizers and antioxidants include phenol-based antioxidants and hindered amine-based light stabilizers, and one or more of these can be used in combination. By blending a synthetic resin stabilizer, the stability (weather resistance deterioration, etc.) of the thermoplastic resin composition can be further improved. The same compound as the reaction terminator can be used as the synthetic resin stabilizer. The blending amount of the synthetic resin stabilizer is preferably 0.01 to 3 parts by weight per 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0043] Examples of processing aids such as lubricants and mold release agents include metal soaps such as erucic acid amide and calcium stearate, and these can be used alone or in combination of two or more. By adding the processing aid, the discharge of the thermoplastic resin composition can be stabilized at the outlet of a kneader such as an extruder, and melt fracture can be prevented. The amount of the processing aid to be added is preferably 0.01 to 1 part by weight based on 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0044] Examples of the softener include paraffinic oil, olefinic oil, naphthenic oil, aromatic oil, etc., and one or more of them can be used in combination. Naphthenic oil and aromatic oil are colored light yellow, etc., so it is more preferable to use colorless paraffinic oil or olefinic oil. The amount of the softener can be appropriately adjusted depending on the desired hardness, and is preferably 0 to 150 parts by weight per 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0045] The coloring agent may be a coloring material such as a pigment of various colors, and one or more types may be used in combination to adjust the color. The coloring agent may be directly mixed into the kneader, but it is preferable to use a master batch, which has excellent dispersibility and uniformity and does not scatter or soil the kneader. The amount of the coloring agent to be mixed depends on the desired color, but is preferably 0.001 to 3 parts by weight per 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0046] In the kneading step of the present invention, the thermoplastic elastomer and / or rubber material having an alkoxysilyl group whose radical activity has been deactivated, a thermoplastic resin, and appropriate additives are added and kneaded in a molten state in the kneader.
[0047] The thermoplastic resin (TP) blended in the kneading step may be either crystalline or amorphous, or both may be used in combination. Examples of crystalline thermoplastic resins include olefin resins (PO), polyacetal resins (POM), polyamide resins (PA), and polyester resins (polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.), and examples of amorphous thermoplastic resins include polystyrene resins (PS), polycarbonate resins (PC), and polyvinyl chloride resins (PVC), and one or more of these may be used in combination. The blending amount of the thermoplastic resin is preferably 30 to 300 parts by weight, more preferably 50 to 200 parts by weight, based on 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0048] The thermoplastic resin includes a thermoplastic resin whose main chain and side chain are composed of saturated bonds, and the thermoplastic resin whose main chain and side chain are composed of saturated bonds is a thermoplastic resin that does not contain unsaturated bonds such as double bonds in the main chain and side chain. Examples of the crystalline thermoplastic resin whose main chain and side chain are composed of saturated bonds include olefin resins and polyacetal resins, and examples of the amorphous thermoplastic resin whose main chain and side chain are composed of saturated bonds include polyvinyl chloride resins.
[0049] The thermoplastic resin to be mixed in the kneading step is preferably a crystalline thermoplastic resin, because in the kneading step, the thermoplastic elastomer and / or rubber material having an alkoxysilyl group and the thermoplastic resin are in a molten state, and in the next dynamic crosslinking step, when the alkoxysilyl group of the thermoplastic elastomer and / or rubber material forms a siloxane bond, a crystalline thermoplastic resin having a clear melting point (Tm) generates a viscosity difference and is more likely to undergo a phase transition than an amorphous thermoplastic resin having no clear melting point.
[0050] When a crystalline thermoplastic resin having a main chain and a side chain composed of saturated bonds is used as the thermoplastic resin blended in the kneading step, the thermoplastic resin does not deteriorate, such as hydrolysis, even when the thermoplastic resin comes into contact with the water component blended in the dynamic crosslinking step. Furthermore, since the main chain and the side chain do not contain unsaturated bonds such as double bonds, a thermoplastic resin composition that is less susceptible to weather deterioration can be obtained. Examples of crystalline thermoplastic resins having a main chain and a side chain composed of saturated bonds include olefin resins and polyacetal resins, and one or more of these can be used in combination. Examples of the olefin resin (PO) include polyethylene resin (PE), polypropylene resin (PP), polybutene resin (PB), etc. Among the olefin resins, polypropylene resins are particularly preferred from the viewpoint of the heat resistance and moldability of the thermoplastic resin composition, and may be either a homopolymer (homo PP) or a copolymer (random PP, block PP).
[0051] In the dynamic crosslinking step of the present invention, a water component is added and kneaded. The water component may be directly added as a liquid in the kneader, or may be mixed with a filler, a water-absorbent polymer, or the like to prepare a mixture containing the water component, and the prepared mixture may be added. In addition, a compound containing crystal water (organic compound, inorganic compound, mixture of organic compound and inorganic compound, etc.), a hydroxide, or a compound that releases a water component from the compound by heating, etc. may be added. These may be used alone or in combination of two or more. Note that when the water component is added to a heated kneader, the water component evaporates, so it is preferable to add about 1 to 10 times the theoretical amount at which the alkoxysilyl group is converted to a silanol group. The amount of the water component is preferably 0.1 to 10 parts by weight per 100 parts by weight of the thermoplastic elastomer and / or rubber material.
[0052] In the dynamic crosslinking step, the alkoxysilyl groups of the thermoplastic elastomer and / or rubber material having the alkoxysilyl groups whose radical activity has been deactivated, which had previously formed the sea portion of the island-in-sea structure, come into contact with water, causing a hydrolysis reaction, and the alkoxysilyl groups are converted into silanol groups. Next, the silanol groups undergo a condensation reaction (dehydration condensation reaction) to form siloxane bonds. The alkoxysilyl groups are converted into silanol groups by a hydrolysis reaction, and the silanol groups are further subjected to a condensation reaction to form siloxane bonds, so that the viscosity of the thermoplastic elastomer and / or rubber material having the alkoxysilyl groups whose radical activity has been deactivated becomes higher than that of the thermoplastic resin, and a phase transition occurs to the island portion. Meanwhile, the thermoplastic resin that had previously formed the island portion of the island-in-sea structure undergoes a phase transition to the sea portion. In the dynamic crosslinking step, the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated undergoes a phase transition from the sea structure to the island structure, and the thermoplastic resin undergoes a phase transition from the island structure to the sea structure, whereby the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated and the thermoplastic resin undergo phase inversion to obtain the thermoplastic resin composition. Figure 1 shows the reaction behavior up to the formation of a siloxane bond from the alkoxysilyl group via a silanol group in the case of a thermoplastic elastomer consisting of saturated bonds having the alkoxysilyl group whose radical activity has been deactivated.
[0053] The thermoplastic resin composition is pelletized and then processed into automobile parts, waterproofing materials, building materials, industrial members, and the like by known resin molding such as extrusion molding or injection molding.
[0054] The kneader 10 shown in Fig. 2 is capable of continuously carrying out the grafting step, the reaction termination step, the kneading step, and the dynamic crosslinking step in one kneader, and is a kneader suitable for the method for producing a thermoplastic resin composition of the present invention. As the kneader, a single screw extruder, a twin screw extruder, a kneader, etc. can be used. In particular, a twin screw extruder is preferable from the viewpoint of reactive extrusion properties and self-cleaning properties, and the present invention will be described taking a twin screw extruder as an example.
[0055] The kneader 10 is provided with, from the upstream side to the downstream side, a first zone in which the grafting process is performed, a second zone in which the reaction termination process is performed, a third zone in which the kneading process is performed, and a fourth zone in which the dynamic crosslinking process is performed. A screw provided inside a cylinder is rotated by a motor M, and the kneaded material is sequentially sent downstream (first zone → second zone → third zone → fourth zone). In the cylinder, a first zone where the grafting step is performed is provided with a first supply port 11, a second zone where the reaction terminating step is performed is provided with a second supply port 12, a third zone where the kneading step is performed is provided with a third supply port 13, and a fourth zone where the dynamic crosslinking step is performed is provided with a fourth supply port 14.
[0056] The production of a thermoplastic resin composition using the kneader 10 will be described. The thermoplastic elastomer and / or rubber material, the silane coupling agent, the reaction initiator, the silanol crosslinking promotion catalyst that is appropriately mixed, and appropriate additives are supplied into a cylinder from the first supply port 11, and melt-kneaded in the first zone where the grafting step is performed. By kneading in the first zone, alkoxysilyl groups are grafted onto the thermoplastic elastomer and / or rubber material, and a thermoplastic elastomer and / or rubber material having the alkoxysilyl groups is produced, and sent to the next second zone.
[0057] In the second zone where the reaction terminating step is carried out, the reaction terminator is supplied from the second supply port 12 into the cylinder and melt-kneaded, and the kneaded product is sent to the next third zone. The timing for supplying the reaction terminator from the second supply port 12 into the kneader 10 is after the grafting step (before the kneading step). In the reaction terminating step, the free radicals derived from the reaction initiator blended to graft an alkoxysilyl group to the thermoplastic elastomer and / or rubber material are deactivated by the reaction terminator.
[0058] In the third zone where the kneading step is carried out, the thermoplastic resin and appropriate additives are fed into a cylinder from the third feed port 13 and melt-kneaded, and the kneaded mixture is sent to the next fourth zone.
[0059] In the fourth zone where the dynamic crosslinking step is carried out, a water component is supplied into the cylinder from the fourth supply port 14 and melt-kneaded. In the kneading in the fourth zone, the alkoxysilyl groups of the thermoplastic elastomer and / or rubber material having the alkoxysilyl groups whose radical activity has been deactivated and the water component are hydrolyzed to form silanol groups, and then the silanol groups are subjected to a dehydration condensation reaction to form siloxane bonds. The alkoxysilyl group of the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated is converted into a siloxane bond, so that the viscosity of the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated becomes higher than that of the thermoplastic resin, and the thermoplastic elastomer and / or rubber material having the alkoxysilyl group whose radical activity has been deactivated, which had previously formed the sea part of the sea-island structure, undergoes phase transition to the island part, and the thermoplastic resin which had previously formed the island part of the sea-island structure, undergoes phase inversion to obtain the thermoplastic resin composition. The thermoplastic resin composition extruded from the kneader 10 is then pelletized by a pelletizer and used for resin molding such as extrusion molding and injection molding.
[0060] The grafting step may be carried out in advance, and the obtained thermoplastic elastomer and / or rubber material having an alkoxysilyl group whose radical activity has been deactivated may be stored. At a later date, the thermoplastic resin composition having an island-sea structure may be produced by carrying out the kneading step and the dynamic crosslinking step using the stored thermoplastic elastomer and / or rubber material having an alkoxysilyl group whose radical activity has been deactivated. EXAMPLES
[0061] The thermoplastic resin compositions of Examples 1 to 6 and Comparative Examples 1 to 4 having the composition shown in Fig. 3 were produced in a kneader using the following raw materials. The numbers for each component in the composition shown in Fig. 3 are parts by weight. For Comparative Examples 1 and 2, the product name: Santoprene 201-64: manufactured by ExxonMobil Corporation was used. The kneader used was the above-mentioned kneader 10 consisting of a twin-screw extruder (L / D = 72) having first to fourth zones.
[0062] The production conditions using the kneader 10 were as follows: temperature in the first zone: 230° C., temperatures in the second to fourth zones: 200° C., screw rotation speed: 400 rpm, and discharge rate at the outlet: 30 kg / hr. The temperature of the first zone is set appropriately depending on the melting point of the raw materials (thermoplastic elastomer, rubber material, etc.) used and the decomposition temperature of the reaction initiator used, so the temperature range is preferably 200 to 250°C. The temperatures of the second to fourth zones are preferably set 10 to 30°C higher than the melting point of the raw materials (thermoplastic resin, etc.) used. The temperature range is preferably 180 to 230°C when the thermoplastic resin is a polypropylene-based resin or a polystyrene-based resin.
[0063] TPE (olefin-based): Ethylene / 1-octene copolymer, manufactured by Dow Chemical Company, product name: ENGAGE 8842 Rubber: Ethylene propylene diene rubber (EPDM), manufactured by Dow Chemical Japan, product name: NORDEL IP 4760P Crosslinking agent (silane coupling agent): Vinyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd., Product name: KBM-1003 Reaction initiator: Aliphatic organic peroxide, manufactured by NOF Corporation, product name: Perhexa 25B, generates two radicals from one molecule. Reaction stopper-1: Hindered phenol antioxidant, manufactured by ADEKA, product name: Adeka STAB AO-80, captures two free radicals with one molecule. Reaction stopper-2: Hindered phenol antioxidant, manufactured by ADEKA, product name: Adeka STAB AO-20, captures three free radicals with one molecule. Reaction stopper-3: Hindered phenol antioxidant, manufactured by ADEKA, product name: Adeka STAB AO-60, captures four free radicals with one molecule. Silanol crosslinking catalyst: Octyltin compound, manufactured by ADEKA, product name: Adeka STAB OT-1 TP: Polypropylene resin (block type), manufactured by Japan Polypropylene Corporation, product name: Novatec EC7 Colorant: Color masterbatch, manufactured by Tokyo Ink Co., Ltd., Product name: PEX3162 BLUE
[0064] Examples 1 and 2 are examples in which the grafting step, the reaction terminating step, the kneading step, and the dynamic crosslinking step were performed continuously, and the amount of reaction terminator-1 (ratio of reaction terminator-1 to the reaction initiator) was changed. In addition, both Examples 1 and 2 contain TPE, and no rubber or colorant is contained. In Example 1, the amount of reaction terminator-1 is 0.26 parts by weight, and the ratio of reaction terminator-1 to the reaction initiator (ratio of moles) is 102%, while in Example 2, the amount of reaction terminator-1 is 0.50 parts by weight, and the ratio of reaction terminator-1 to the reaction initiator (ratio of moles) is 196%.
[0065] Example 3 is an example in which rubber was compounded in place of the TPE of Example 1, and the rest was the same as Example 1. Example 4 is an example in which a colorant is added to Example 1, and the rest is the same as Example 1. Example 5 is an example in which 0.22 parts by weight of reaction stopper-2 was used instead of reaction stopper-1 in Example 1, and the ratio (molar ratio) of reaction stopper-2 to the reaction initiator was 122%, and the rest was the same as Example 1. Example 6 is an example in which 0.30 parts by weight of reaction stopper-3 was used instead of reaction stopper-1 in Example 1, and the ratio (molar ratio) of reaction stopper-3 to the reaction initiator was 148%, and the rest was the same as Example 1.
[0066] Comparative Example 1 is an example of phenol crosslinking (complete crosslinking), Comparative Example 2 is an example in which a colorant was added to Comparative Example 1, Comparative Example 3 is an example in which the reaction stopper-1 in Example 1 was 0 parts by weight, and Comparative Example 4 is an example in which the reaction stopper-1 in Example 1 was 0.23 parts by weight, and the ratio (proportion by mole) of reaction stopper-1 to the reaction initiator was 90%.
[0067] For each Example and Comparative Example, the phase transition, sea-island structure, maximum value (theoretical value) (parts by weight) of gel component (insoluble matter) in the island structure, measured value (parts by weight) of gel component (insoluble matter) in the island structure, gel fraction (%) of the island structure, tensile strength (MPa), compression set (%), color difference value due to weather resistance degradation (ΔE*ab), color difference value due to coloring (ΔE*ab), and remeltability were investigated. The results are shown in Figure 3. Note that color difference value due to weather resistance degradation (ΔE*ab) was not measured for Example 3.
[0068] The presence or absence of phase transition and the presence or absence of a sea-island structure was confirmed by preparing a thin film using an ultramicrotome (FC6: manufactured by Leica) and observing it with a transmission electron microscope (H-7650: manufactured by Hitachi High-Technologies Corporation). The maximum value of the gel component (insoluble matter) in the island structure is the compounded amount (100 parts by weight) of the TPE and / or rubber. The gel fraction of the island structure was measured in accordance with JIS K6769:2004.
[0069] The gel fraction (%) of the island structure portion was calculated by [(measured gel fraction of the island structure portion / maximum gel fraction of the island structure portion)×100]. The tensile strength (MPa) was measured in accordance with JIS K6251:2010 (dumbbell-shaped No. 3 × thickness 2 mm). The compression set (%) was measured in accordance with JIS K6262:2013 Method A (small diameter test piece (diameter 13 mm × thickness 2 mm, three sheets stacked together) 70°C × 22h, 25% compression).
[0070] The color difference value (ΔE*ab) due to weathering degradation conforms to JIS Z8781-4:2013, and the color difference value (ΔE*ab) due to weathering degradation measured with a color difference meter (SM Color Computer SM-T: manufactured by Suga Test Instruments Co., Ltd.) is the color difference of the thermoplastic resin composition before and after weathering degradation. The weathering degradation test conforms to JIS K7350-2:2008 B method, and is performed using a light resistance tester (SC-700FP: manufactured by Suga Test Instruments Co., Ltd.) with a xenon lamp at an irradiance of 150 W / m 2 (Wavelength range 300-400 nm) and cumulative irradiation dose: 300 MJ / m 2 The test was performed under the following conditions: black panel temperature: 63±3°C.
[0071] The color difference value due to coloring was measured in accordance with JIS Z8781-4:2013 for the colorability (color development) with or without the incorporation of a colorant, in the same manner as the color difference value due to weathering deterioration described above. The color difference value due to coloring (ΔE*ab) is the color difference value of the thermoplastic resin composition with the incorporation of a colorant, and was measured for Example 4 and Comparative Example 2, in which a colorant was incorporated. The color difference value due to coloring in Example 4 was measured for Example 1 (no colorant incorporated), and the color difference value due to coloring in Comparative Example 2 was measured for Comparative Example 1 (no colorant incorporated). The larger the ΔE*ab value, the better the colorability.
[0072] The color difference value: ΔE*ab is defined as the Euclidean distance between coordinates in the CIE1976 L*a*b* color space, and indicates the color difference between two color stimuli calculated by the following formula. ΔE*ab=[(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 )] 1 / 2 The color difference value: ΔE*ab can be expressed in NBS units defined by the National Bureau of Standards and in color difference sensation (evaluation of the degree of sensory color difference) as shown in Figure 4. The values in the NBS unit column in Figure 4 are the values of ΔE*ab calculated by the above formula.
[0073] The remeltability was evaluated by heat pressing each of the Examples and Comparative Examples at 180° C. for 3 minutes to confirm whether or not the sample melted. If the sample melted, it was marked as “Good” and if it did not melt, it was marked as “Poor.”
[0074] In Examples 1 to 6, phase transition is "present", sea-island structure is "present", and gel fraction of island structure is 96 to 98%. In addition, in Examples 1 to 6, tensile strength is 10.6 to 13.3 MPa, compression set is 26 to 30%, mechanical properties are good, and remeltability is "○". When used for automobile parts, water-stopping materials, building materials, industrial members, etc., tensile strength is preferably 7 MPa or more, more preferably 10 MPa or more, and compression set is preferably 50% or less, more preferably 40% or less. In Examples 1 to 6, gel fraction of island structure is 96 to 98%, compression set is low at 26 to 30% because of complete crosslinking using silane coupling agent, and free radicals generated by reaction initiator are deactivated by reaction terminator, so mechanical strength is sufficiently high at 10.6 to 13.3 MPa, and it can be suitably used for automobile parts, water-stopping materials, building materials, industrial members, etc.
[0075] Comparing the colorability of Example 1 and Example 4, when 0.01 parts by weight of colorant was mixed with 100 parts by weight of TPE, the color difference value (Δ*abE) due to coloring was 5, and the NBS unit was between 3.0 and 6.0. The sense of color difference was at a level that was noticeable, and the colorability was excellent.
[0076] In Examples 1 to 2 and Examples 4 to 6, which used a thermoplastic elastomer whose main chain and side chain are composed of saturated bonds and a thermoplastic resin whose main chain and side chain are composed of saturated bonds, the color difference value (ΔE*ab) due to weather resistance degradation was 2.4 to 2.6, which was small.
[0077] Comparative Example 1 is an example in which a rubber having double bonds in the side chains (EPDM) was cross-linked with phenol, and a phase transition was present, a sea-island structure was present, the gel fraction of the island structure was 99%, the tensile strength was 6.4 MPa, the compression set was 33%, and the remeltability was good. Comparative Example 1 has low tensile strength and the color difference value (ΔE*ab) due to weathering deterioration is large at 13.2 because the rubber is crosslinked with phenol.
[0078] Comparative Example 2 is an example in which a colorant was added to Comparative Example 1, and the phase transition was "present", the sea-island structure was "present", the gel fraction of the island structure was 99%, the tensile strength was 6.5 MPa, the compression set was 35%, and the remeltability was "good". Comparing Comparative Example 1 and Comparative Example 2, the color difference value (ΔE*ab) due to coloring when 0.01 parts by weight of the colorant was added to 100 parts by weight of Santoprene 201-64 was 0.8, the NBS unit was between 0.5 and 1.5, and the color difference was at a level that was barely noticeable, which was inferior to the color difference value (ΔE*ab) of 5 due to coloring in Example 4. This shows that the phenol used for phenol crosslinking itself has a color tone, and the colorability is low even when a colorant is added. If the amount of the colorant added is increased, the color difference value (ΔE*ab) due to coloring of the phenol crosslinked thermoplastic resin composition can be increased, but it becomes difficult to color it to a light color. In particular, it is extremely difficult to color a phenol-crosslinked thermoplastic resin composition with a light color that is the polar opposite to the color tone of the phenol-based crosslinking agent itself in the CIE1976L*a*b* color space. This shows that the thermoplastic resin composition of the present invention can be colored with a light color that is difficult to color with a phenol-crosslinked thermoplastic resin composition, and has excellent freedom in coloring. Comparative Example 2 has low tensile strength and the color difference value (ΔE*ab) due to weathering deterioration is large at 14.2 because the rubber is crosslinked with phenol.
[0079] Comparative Example 3 is an example in which the reaction terminator-1 in Example 1 was not blended, and showed a phase transition "present", a sea-island structure "present", a gel fraction of the island structure was 98%, a tensile strength of 4.1 MPa, a compression set of 52%, a color difference value (ΔE*ab) due to weathering deterioration of 2.7, and a remeltability of "good". Since the reaction terminator-1 in Example 1 was not blended in Comparative Example 3, the mechanical strength of the tensile strength and compression set was significantly inferior to that of Example 1.
[0080] Comparative Example 4 is an example in which the amount of reaction terminator-1 in Example 1 was 0.23 parts by weight, and the ratio (molar ratio) of reaction terminator-1 to the reaction initiator was 90%, and the phase transition was "present", the sea-island structure was "present", the gel fraction of the island structure was 98%, the tensile strength was 6.8 MPa, the compression set was 43%, the color difference value (ΔE*ab) due to weathering deterioration was 2.7, and the remeltability was "good". In Comparative Example 4, the tensile strength and compression set are slightly improved compared to Comparative Example 1 in which reaction terminator-1 is not blended. However, in Comparative Example 4, the amount of reaction terminator-1 blended is less than in Example 1, and the ratio (molar ratio) of reaction terminator-1 to the reaction initiator is low at 90%, so the mechanical strength of the tensile strength and compression set is significantly inferior to that of Example 1.
[0081] As described above, the thermoplastic resin composition obtained by the present invention has excellent colorability and mechanical properties, and can be remolded by remelting, and is therefore suitable for automobile parts, waterproofing materials, building materials, industrial components, etc. Furthermore, by using a thermoplastic elastomer in which the main chain and side chain are composed of saturated bonds, weather resistance deterioration can be suppressed.
[0082] The present invention aims to provide a thermoplastic resin composition which is excellent in mechanical properties and colorability, can be molded by remelting, and is not prone to weather deterioration in applications requiring weather resistance, such as automobile parts, water stoppers, building materials, and industrial components. It can be said that the present invention has the following characteristics as technical means for achieving this aim. <Feature 1> A thermoplastic resin composition having an island-in-a-sea structure, the sea structure portion of the sea-island structure is composed of a thermoplastic resin whose main chain and side chain are formed of saturated bonds, the island structure portion of the sea-island structure is composed of a thermoplastic elastomer in which the main chain and the side chain are formed of saturated bonds and are crosslinked by siloxane bonds, The gel fraction of the island structure (based on JIS K6769:2004) is 90% or more, A thermoplastic resin composition, characterized in that the radical activity of free radicals generated by a reaction initiator contained in the thermoplastic resin composition is deactivated by a reaction terminator contained in the thermoplastic resin composition in a ratio of 100% or more relative to the reaction initiator. <Feature 2> a reaction terminating step of kneading a thermoplastic elastomer having saturated bonds and alkoxysilyl groups, in which alkoxysilyl groups are grafted onto a thermoplastic elastomer whose main chain and side chains are saturated bonds, and a reaction terminator in a molten state in a kneader, and deactivating free radicals derived from a reaction initiator blended to prepare the thermoplastic elastomer having saturated bonds and alkoxysilyl groups with the reaction terminator, thereby preparing a thermoplastic elastomer having saturated bonds and alkoxysilyl groups whose radical activity has been deactivated; a kneading step of kneading the thermoplastic elastomer having a saturated bond and an alkoxysilyl group whose radical activity has been deactivated and a thermoplastic resin whose main chain and side chains are saturated bonds in a molten state in a kneader; a dynamic crosslinking step of adding water to the kneader, converting the alkoxysilyl groups of the thermoplastic elastomer having saturated bonds and alkoxysilyl groups whose radical activity has been deactivated in the kneader into silanol groups by hydrolysis reaction with the water, and then condensing the silanol groups to form siloxane bonds; having The reaction terminator added in the reaction terminating step has a molar ratio of 100% or more to the molar ratio of the reaction initiator, The method for producing a thermoplastic resin composition, wherein the thermoplastic resin composition obtained by the dynamic crosslinking step has an island-in-a-sea structure.
Claims
1. A thermoplastic resin composition having an islands-in-a-sea structure, comprising: a thermoplastic elastomer crosslinked by a siloxane bond and / or a rubber material crosslinked by a siloxane bond, a thermoplastic resin, and at least one radical scavenger selected from the group consisting of a phenolic antioxidant and a hindered amine light stabilizer, wherein an island structural portion of the islands-in-a-sea structure has a structural portion crosslinked by a siloxane bond, and has a tensile strength (in accordance with JIS K6251:2010) of 10.6 MPa or more and / or a compression set (in accordance with JIS K6262:2013 Method A) of 30% or less, The thermoplastic elastomer is a polyethylene / α-olefin copolymer, The rubber material is ethylene propylene diene rubber (EPDM), The thermoplastic resin is an olefin-based resin (PO), The blending amount of the thermoplastic resin is 30 to 300 parts by weight per 100 parts by weight of the thermoplastic elastomer and / or rubber material. Thermoplastic resin composition.
2. A thermoplastic resin composition having an island-in-a-sea structure, the island-in-a-sea structure including a structural portion crosslinked by a siloxane bond, the siloxane bond including the following structure, the composition having a tensile strength (in accordance with JIS K6251:2010) of 10.6 MPa or more and / or a compression set (in accordance with JIS K6262:2013 Method A) of 30% or less, an island structure portion of the sea-island structure contains the thermoplastic elastomer crosslinked by a siloxane bond and / or the rubber material crosslinked by a siloxane bond, and a sea structure portion of the sea-island structure contains a thermoplastic resin, The thermoplastic elastomer is a polyethylene / α-olefin copolymer, The rubber material is ethylene propylene diene rubber (EPDM), The thermoplastic resin is an olefin-based resin (PO), The blending amount of the thermoplastic resin is 30 to 300 parts by weight per 100 parts by weight of the thermoplastic elastomer and / or rubber material. Thermoplastic resin composition. [Case 1]
3. The thermoplastic resin composition described in claim 1, wherein the thermoplastic resin is a polypropylene-based resin.
4. The thermoplastic resin composition described in claim 2, wherein the thermoplastic resin is a polypropylene-based resin.
5. An article comprising the thermoplastic resin composition according to claim 1 , wherein the article is selected from the group consisting of automobile parts, water-stopping materials, building materials, and industrial components.
Citation Information
Patent Citations
Hot roller apparatus
JP1983046138A
Production of thermoplastic elastomer composition
JP1993170930A
Thermoplastic elastomer having low creep property and low-temperature impact resistance
JP1996283492A
Production of silane-crosslinked polyolefin
JP1998245424A
Thermoplastic elastomer composition and method for producing the same
JP2007138020A