Hydrogenated polymer composition containing hydrogenated conjugated diene modified polymer having boron-containing functional group and method for producing same

The method of anionic polymerization and boric acid reaction with specific steric parameters addresses the reactivity and dispersibility issues of hydrogenated conjugated diene-modified polymers, achieving high yield and effective modification of thermoplastic polymers.

JP7583840B2Active Publication Date: 2024-11-14KURARAY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022580636
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-12
Filing Date
2022-02-08
Publication Date
2024-11-14
Estimated Expiration
2042-02-08

AI Technical Summary

Technical Problem

Existing methods for producing hydrogenated conjugated diene-modified polymers with boronic acid groups suffer from insufficient reactivity and high content of unmodified polymers, leading to issues such as low grafting efficiency and poor dispersibility in thermoplastic resins.

Method used

A method involving anionic polymerization of conjugated dienes followed by reaction with boric acid compounds having specific steric parameters, and subsequent hydrogenation to produce hydrogenated polymers with boron-containing functional groups, ensuring high yield and reactivity.

Benefits of technology

The resulting hydrogenated polymers exhibit high reactivity towards polar functional groups and excellent dispersibility in thermoplastic polymers, particularly vinyl alcohol-based polymers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583840000001
    Figure 0007583840000001
  • Figure 0007583840000002
    Figure 0007583840000002
  • Figure 0007583840000003
    Figure 0007583840000003
Patent Text Reader

Abstract

Provided are: a method for producing, at a high yield, a hydrogenated conjugated-diene modified polymer that has a boron-containing functional group suitable for property modification of polar materials and property modification of various materials, such as dispersing of inorganic materials; and a hydrogenated polymer composition that contains a hydrogenated conjugated-diene modified polymer having a boron-containing functional group that achieves both high reactivity with respect to various polar functional groups and dispersibility in thermoplastic polymers, representatively, vinyl alcohol-based polymers. The method is for producing a hydrogenated polymer composition containing a hydrogenated conjugated-diene modified polymer that has a boron-containing functional group, and comprises: a step (1) for producing a reactive terminal polymer (Z) through anionic polymerization of a monomer including a conjugated diene in the presence of a reactive metal compound or a reactive metal capable of causing anionic polymerization; a step (2) for obtaining an unhydrogenated conjugated-diene modified polymer having a boron-containing functional group by causing a reaction between the reactive terminal polymer (Z) obtained in step (1) and a borate compound which has at least two partial structures represented by formula (I) and in which at least one R bound to the oxygen atom in said partial structure (I) has a Taft's steric parameter Es not more than -0.30; and a step (3) for hydrogenating at least a portion of carbon-carbon double bonds included in a conjugated diene unit included in the unhydrogenated conjugated-diene modified polymer obtained in step (2). Formula (I): B-O-R (in formula (I), B represents a boron atom, O represents an oxygen atom, and R represents an organic group.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydrogenated polymer composition containing a hydrogenated conjugated diene modified polymer having a boron-containing functional group, and a method for producing the same. [Background technology]

[0002] Methods for synthesizing polymers having various functional groups at their ends by anionic polymerization have been studied. For example, a method for introducing a boronic acid group, which is an example of a boron-containing functional group, into the end of a polymer has been studied, and it has been revealed that polymers having a boronic acid group or a borinic acid group, which is a boron-containing functional group, at their ends are useful as resin modifiers such as compatibilizers for thermoplastic resins having hydroxyl groups in their side chains, such as ethylene-vinyl alcohol copolymers (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-25918 Summary of the Invention [Problem to be solved by the invention]

[0004] Specifically, in Patent Document 1, the inventors have studied a method for obtaining a hydrogenated conjugated diene-modified polymer having boronic acid at the end by reacting the end of an anionic polymerized active end polymer having a structural unit derived from a conjugated diene (hereinafter also referred to as a "conjugated diene unit") with trimethyl borate and then hydrogenating (hereinafter also referred to as "hydrogenation") at least a part of the carbon-carbon double bonds contained in the conjugated diene unit. However, according to the study by the present inventors, although a hydrogenated conjugated diene-modified polymer having boronic acid at the end can be obtained by the production method of Patent Document 1, it was found that the reactivity of the boric acid ester is insufficient in the production method, and a large amount of unmodified polymer not having a boronic acid group may be contained. Therefore, even if resin modification is performed using the polymer obtained in Patent Document 1, since the proportion of polymers having boronic acid groups is small, there are many polymers that cannot react with polymers having groups reactive with boronic acid groups, and problems such as insufficient grafting efficiency, insufficient dispersibility in the resin, and an increase in bleed-out components may occur.

[0005] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a production method for obtaining, in high yield, a hydrogenated conjugated diene-modified polymer having a boron-containing functional group suitable for modifying various materials, such as modifying polar materials and dispersing inorganic materials, and a hydrogenated polymer composition containing a hydrogenated conjugated diene-modified polymer having a boron-containing functional group that has high reactivity with various polar functional groups and excellent dispersibility in a thermoplastic polymer, typically a vinyl alcohol-based polymer. [Means for solving the problem]

[0006] As a result of intensive research by the present inventors, it has been found that in a process for producing a hydrogenated conjugated diene modified polymer having a boron-containing functional group, a desired hydrogenated conjugated diene modified polymer can be obtained in high yield by modifying a functional group using an anionically polymerizable terminal polymer containing a specific conjugated diene unit and a boric acid compound satisfying specific parameters, and further hydrogenating at least a part of the carbon-carbon double bonds contained in the conjugated diene unit. Furthermore, it has been found that a specific hydrogenated polymer composition containing a hydrogenated conjugated diene modified polymer containing a specific boronic acid ester group and a hydrogenated conjugated diene modified polymer containing a specific boric acid group has excellent reactivity to polar functional groups and excellent dispersibility in a thermoplastic polymer, typically a vinyl alcohol-based polymer, and has thus completed the present invention.

[0007] That is, the present invention provides the following [1] to [5]. [1] A method for producing a hydrogenated polymer composition containing a hydrogenated conjugated diene-modified polymer having a boron-containing functional group, the method comprising: a step (1) of anionically polymerizing a monomer containing a conjugated diene in the presence of an anionically polymerizable active metal or active metal compound to produce an active end polymer (Z); a step (2) of reacting the active end polymer (Z) obtained in the step (1) with a boric acid compound having at least two or more partial structures represented by the following formula (I) and having a Taft steric parameter Es value of at least one of R bonded to an oxygen atom contained in the partial structures of −0.30 or less to obtain an unhydrogenated conjugated diene-modified polymer having a boron-containing functional group; and a step (3) of hydrogenating at least a part of the carbon-carbon double bonds contained in the conjugated diene units contained in the unhydrogenated conjugated diene-modified polymer obtained in the step (2). BOR (I) (In formula (I), B represents a boron atom, O represents an oxygen atom, and R represents an organic group.) [2] The method for producing a hydrogenated polymer composition according to [1], wherein in the step (2), a polar compound is mixed with the boric acid compound, and then the mixture is added to the active terminal polymer (Z) for reaction. [3] A hydrogenated polymer composition comprising 65 to 99 mass% of at least one boronic acid-based hydrogenated conjugated diene-modified polymer (A) selected from the group consisting of a hydrogenated conjugated diene-modified polymer containing a boronic acid group represented by the following formula (II), a hydrogenated conjugated diene-modified polymer containing a boronic acid ester group represented by the following formula (III), and a hydrogenated conjugated diene-modified polymer containing a boronic acid salt group represented by the following formula (IV), and 1 to 35 mass% of at least one borinic acid-based hydrogenated conjugated diene-modified polymer (B) selected from the group consisting of a hydrogenated conjugated diene-modified polymer containing a borinic acid group represented by the following formula (V) or (VI), a hydrogenated conjugated diene-modified polymer containing a borinic acid ester group represented by the following formula (VII) or (VIII), and a hydrogenated conjugated diene-modified polymer containing a borinic acid salt group represented by the following formula (IX) or (X).

[0008] [ka] (In the above formula, P 1 , P 2 and P 3 represents a polymer chain containing hydrogenated conjugated diene units, and R 1 and R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms; R 1 and R 2 At least one of R is an alkyl group having 1 to 12 carbon atoms, or R 1 and R 2 are bonded to form an alkylene chain having 2 to 24 carbon atoms, and R 3 , R 4 and R 5 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a polymer chain containing a hydrogenated conjugated diene unit; R 3 , R 4 and R 5 At least one of R is an alkyl group having 1 to 12 carbon atoms or a polymer chain containing a hydrogenated conjugated diene unit, or R 3 and R 4 , R 3 and R 5 , or R 4 and R 5may be bonded to form an alkylene chain having 2 to 24 carbon atoms, R 3 , R 4 and R 5 may be bonded to form a trivalent saturated hydrocarbon chain having 3 to 36 carbon atoms. M represents one alkali metal or 1 / 2 an alkaline earth metal.

[0009] [ka] (In the above formula, P 4 , P 5 , P 6 , P 7 , P 8 , P 9 , P 10 , P 11 and P 12 represents a polymer chain containing hydrogenated conjugated diene units, and R 6 , R 7 , R 8 and R 9 each independently represents an alkyl group having 1 to 12 carbon atoms; R 10 and R 11 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, R 10 and R 11 At least one of R is an alkyl group having 1 to 12 carbon atoms, or R 10 and R 11 are bonded to form an alkylene chain having 2 to 24 carbon atoms, and R 12 represents an alkyl group having 1 to 12 carbon atoms; R 13 and R 14 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, R 13 and R 14 At least one of R is an alkyl group having 1 to 12 carbon atoms, or R 13 and R 14 are bonded to form an alkylene chain having 2 to 24 carbon atoms, and M represents one alkali metal or 1 / 2 alkaline earth metal. [4] A resin composition comprising a vinyl alcohol polymer and the hydrogenated polymer composition according to [3]. [5] The resin composition according to [4], wherein the vinyl alcohol-based polymer is an ethylene-vinyl alcohol copolymer. Effect of the Invention

[0010] According to the present invention, there are provided a hydrogenated polymer composition comprising a hydrogenated conjugated diene-modified polymer containing a boronic acid ester group, which has high reactivity to polar functional groups and excellent dispersibility in a thermoplastic polymer, typically a vinyl alcohol-based polymer, and a hydrogenated conjugated diene polymer containing a borinic acid group, and a method for producing the hydrogenated polymer composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The hydrogenated polymer composition of the present invention comprises 65 to 99 mass % of at least one boronic acid-based hydrogenated conjugated diene modified polymer (A) selected from the group consisting of a hydrogenated conjugated diene modified polymer containing a boronic acid group represented by the following formula (II), a hydrogenated conjugated diene modified polymer containing a boronic acid ester group represented by the following formula (III), and a hydrogenated conjugated diene modified polymer containing a boronic acid salt group represented by the following formula (IV), a hydrogenated conjugated diene modified polymer containing a boronic acid salt group represented by the following formula (V) or (VI), a hydrogenated conjugated diene modified polymer containing a borinic acid group represented by the following formula (VII) or (VIII), and a hydrogenated conjugated diene modified polymer containing a borinic acid ester group represented by the following formula (IX) or (X), Bolin The composition contains 1 to 35 mass % of at least one borinic acid-based hydrogenated conjugated diene modified polymer (B) selected from the group consisting of acid- and salt-group-containing hydrogenated conjugated diene modified polymers.

[0012] In the present invention, the hydrogenated conjugated diene modified polymer containing a boronic acid group is represented by the following formula (II).

[0013] [ka]

[0014] In formula (II), P 1 indicates a polymer chain containing hydrogenated conjugated diene units.

[0015] In the present invention, the hydrogenated conjugated diene modified polymer containing a boronic acid ester group is represented by the following formula (III).

[0016] [ka]

[0017] In formula (III), P 2 represents a polymer chain containing hydrogenated conjugated diene units, and R 1 and R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms; R 1 and R 2 At least one of R is an alkyl group having 1 to 12 carbon atoms, or R 1 and R 2 are bonded to form an alkylene chain having 2 to 24 carbon atoms. Above R 1 and R 2 At least one of the above preferably has a Taft steric parameter Es value of -0.30 or less, more preferably -3.00 to -0.30, and even more preferably -1.55 to -0.39. 1 and R 2 In one embodiment, all of the above R satisfies the above Es value. 1 and R 2 At least one of the R is preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and even more preferably an isopropyl group. 1 and R 2 are preferably n-propyl, isopropyl, n-butyl, sec-butyl, i-butyl or cyclohexyl, more preferably isopropyl or n-butyl, and further preferably isopropyl. The Taft steric parameter Es value will be described below in the section of step (2) of the preferred method for producing a hydrogenated polymer composition.

[0018] In the present invention, the hydrogenated conjugated diene modified polymer containing a boronate group is represented by the following formula (IV).

[0019] [ka]

[0020] In formula (IV), P 3 represents a polymer chain containing hydrogenated conjugated diene units, and R 3 , R 4 and R 5 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a polymer chain containing a hydrogenated conjugated diene unit; R 3 , R 4 and R 5 At least one of R is an alkyl group having 1 to 12 carbon atoms or a polymer chain containing a hydrogenated conjugated diene unit, or R 3 and R 4 , R 3 and R 5 , or R 4 and R 5 may be bonded to form an alkylene chain having 2 to 24 carbon atoms, R 3 , R 4 and R 5 may be bonded to form a trivalent saturated hydrocarbon chain having 3 to 36 carbon atoms. Above R 3 , R 4 and R 5 At least one of the above preferably has a Taft steric parameter Es value of -0.30 or less, more preferably -3.00 to -0.30, and even more preferably -1.55 to -0.39. 3 , R 4 and R 5 In one embodiment, all of the above R satisfies the above Es value. 3 , R 4 and R 5At least one of the R is preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and even more preferably an isopropyl group. 3 , R 4 and R 5 are preferably n-propyl, isopropyl, n-butyl, sec-butyl, i-butyl, or cyclohexyl, more preferably isopropyl or n-butyl, and even more preferably isopropyl. M is one alkali metal or 1 / 2 alkaline earth metal, preferably lithium, sodium, or potassium, and more preferably lithium. Note that "1 alkali metal" means that, for one monovalent anion group shown in parentheses in formula (IV), the cation of the alkali metal is monovalent, so that there is one alkali metal corresponding to the valence of the anion group. Similarly, "1 / 2 alkaline earth metal" means that, for one monovalent anion group shown in parentheses in formula (IV), the cation of the alkaline earth metal is divalent, so that there is 1 / 2 alkaline earth metal corresponding to the valence of the anion group.

[0021] In the present invention, the hydrogenated conjugated diene modified polymer containing a borinic acid group is represented by the following formula (V) or formula (VI).

[0022] [ka]

[0023] In formula (V), P 4 and P 5 indicates a polymer chain containing hydrogenated conjugated diene units.

[0024] [ka]

[0025] In formula (VI), P 6represents a polymer chain containing hydrogenated conjugated diene units, and R 6 represents an alkyl group having 1 to 12 carbon atoms. 6 is preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and further preferably an isopropyl group.

[0026] In the present invention, the hydrogenated conjugated diene modified polymer containing a borinic acid ester group is represented by the following formula (VII) or formula (VIII).

[0027] [ka]

[0028] In formula (VII), P 7 and P 8 represents a polymer chain containing hydrogenated conjugated diene units, and R 7 represents an alkyl group having 1 to 12 carbon atoms. 7 The Taft steric parameter Es value is preferably −0.30 or less, more preferably −3.00 to −0.30, and even more preferably −1.55 to −0.39. 7 is preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and further preferably an isopropyl group.

[0029] [ka]

[0030] In formula (VIII), P 9 represents a polymer chain containing hydrogenated conjugated diene units, and R 8 is an alkyl group having 1 to 12 carbon atoms, and R 9 is an alkyl group having 1 to 12 carbon atoms. 9The Taft steric parameter Es value is preferably −0.30 or less, more preferably −3.00 to −0.30, and even more preferably −1.55 to −0.39. 9 is preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and further preferably an isopropyl group. Above R 8 is preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and further preferably an isopropyl group.

[0031] In the present invention, the hydrogenated conjugated diene modified polymer containing a borinic acid group is represented by the following formula (IX) or formula (X).

[0032] [ka]

[0033] In formula (IX), P 10 and P 11 represents a polymer chain containing hydrogenated conjugated diene units, and R 10 and R 11 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, R 10 and R 11 At least one of R is an alkyl group having 1 to 12 carbon atoms, or R 10 and R 11 are bonded to form an alkylene chain having 2 to 24 carbon atoms, and M represents one alkali metal or 1 / 2 an alkaline earth metal. Above R 10 and R 11At least one of the above preferably has a Taft steric parameter Es value of -0.30 or less, more preferably -3.00 to -0.30, and even more preferably -1.55 to -0.39. 10 and R 11 In one embodiment, all of the above R satisfies the above Es value. 10 and R 11 At least one of the R is preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and even more preferably an isopropyl group. 10 and R 11 are preferably n-propyl, isopropyl, n-butyl, sec-butyl, i-butyl, or cyclohexyl, more preferably isopropyl or n-butyl, and even more preferably isopropyl. M is one alkali metal or 1 / 2 an alkaline earth metal, preferably lithium, sodium, or potassium, and more preferably lithium.

[0034] [ka]

[0035] In formula (X), P 12 represents a polymer chain containing hydrogenated conjugated diene units, and R 12 represents an alkyl group having 1 to 12 carbon atoms; R 13 and R 14 are each independently a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, R 13 and R 14 At least one of R is an alkyl group having 1 to 12 carbon atoms, or R 13 and R 14 are bonded to form an alkylene chain having 2 to 24 carbon atoms, and M represents one alkali metal or 1 / 2 an alkaline earth metal. Above R 13 and R 14At least one of the above preferably has a Taft steric parameter Es value of -0.30 or less, more preferably -3.00 to -0.30, and even more preferably -1.55 to -0.39. 13 and R 14 In one embodiment, all of the above R satisfies the above Es value. 13 and R 14 At least one of the R is preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and even more preferably an isopropyl group. 13 and R 14 are preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and further preferably an isopropyl group. Above R 12 is preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and further preferably an isopropyl group. The above M is preferably lithium, sodium, or potassium, and more preferably lithium.

[0036] As described above, the above formulas (II) to (X) include P 1 ~P 12 The polymer chain includes a hydrogenated conjugated diene unit represented by the formula:

[0037] P 1 ~P 12The hydrogenated conjugated diene unit contained in the above is obtained by polymerizing a conjugated diene to obtain a polymer chain containing the conjugated diene unit, and then hydrogenating (hydrogenating) the carbon-carbon double bond of the conjugated diene unit contained in the polymer chain. Examples of the conjugated diene include butadiene, isoprene, 2,3-dimethylbutadiene, 2-phenylbutadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,3-octadiene, 1,3-cyclohexadiene, 2-methyl-1,3-octadiene, 1,3,7-octatriene, myrcene, farnesene, and chloroprene. Among these conjugated dienes, butadiene and isoprene are preferred, and butadiene is more preferred. The above conjugated dienes may be used alone or in combination of two or more. Details of hydrogenation will be described below in the section on the production method.

[0038] P 1 ~P 12 may contain unhydrogenated conjugated diene units other than the hydrogenated conjugated diene units and structural units derived from other monomers. A preferred embodiment of the structural units derived from other monomers is a structural unit derived from an aromatic vinyl compound (hereinafter also referred to as an "aromatic vinyl compound unit"). P 1 ~P 12Examples of aromatic vinyl compounds that can be included in the aromatic vinyl compound unit include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-t-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 2,4,6-trimethylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, vinylanthracene, N,N-diethyl-4-aminoethylstyrene, vinylpyridine, 4-methoxystyrene, monochlorostyrene, dichlorostyrene, and divinylbenzene. Among these aromatic vinyl compounds, styrene, α-methylstyrene, and 4-methylstyrene are preferred. The aromatic vinyl compounds that can be included in the aromatic vinyl compound unit may be used alone or in combination of two or more.

[0039] P 1 ~P 12 In one preferred embodiment, 30% by mass or more of all monomer units constituting the polymer chain are unhydrogenated conjugated diene units derived from at least one conjugated diene selected from the group consisting of butadiene and isoprene, or hydrogenated conjugated diene units obtained by hydrogenating such conjugated diene units. The total content of the conjugated diene units derived from at least one monomer selected from the group consisting of butadiene and isoprene and the hydrogenated conjugated diene units of such conjugated diene is P 1 ~P 12 It is preferably 30 to 100 mass%, more preferably 40 to 100 mass%, even more preferably 50 to 100 mass%, even more preferably 60 to 100 mass%, and particularly preferably 70 to 100 mass%, based on all monomer units in the polymer chain.

[0040] P 1 ~P 12Of all the monomer units constituting the polymer chain, the content of other monomer units than unhydrogenated conjugated diene units derived from at least one conjugated diene selected from the group consisting of butadiene and isoprene and hydrogenated conjugated diene units of such conjugated dienes is preferably 70 mass% or less, more preferably 60 mass% or less.

[0041] P 1 ~P 12 Examples of the polymer chain that satisfies the above formula include a homopolymer chain or copolymer chain (random copolymer chain, block copolymer chain) of at least one conjugated diene, or a polymer chain in which at least a part of the carbon-carbon double bonds contained in a conjugated diene unit contained in a copolymer chain (random copolymer chain, block copolymer chain) of a conjugated diene and a monomer other than the conjugated diene are hydrogenated.

[0042] P 1 ~P 12 In one embodiment, the weight average molecular weight (Mw) of the polymer chain is preferably 1,000 or more and 1,000,000 or less, more preferably 2,000 or more and 500,000 or less, and even more preferably 3,000 or more and 100,000 or less. The weight average molecular weight (Mw) of the hydrogenated polymer composition of the present invention is also preferably within the above range. When the Mw of the polymer chain is within the above range, the processability during production tends to be excellent and the economic efficiency tends to be good. In the present invention, unless otherwise specified, Mw is the weight average molecular weight calculated in terms of standard polystyrene as determined by gel permeation chromatography (GPC).

[0043] P 1 ~P 12The molecular weight distribution (Mw / Mn) of the polymer chain is preferably 1.0 to 20.0, more preferably 1.0 to 10.0, even more preferably 1.0 to 5.0, even more preferably 1.0 to 2.0, particularly preferably 1.0 to 1.5, and even more particularly preferably 1.0 to 1.2. When Mw / Mn is in the above range, the viscosity variation of the obtained hydrogenated conjugated diene modified polymer is small, which is preferable. In addition, the molecular weight distribution (Mw / Mn) of the hydrogenated polymer composition of the present invention is also preferably in the above range in terms of the viscosity variation being small. In the present invention, Mn means number average molecular weight, and Mn is the number average molecular weight calculated in terms of standard polystyrene obtained by GPC measurement. In addition, the molecular weight distribution (Mw / Mn) means the ratio (Mw / Mn) of the weight average molecular weight (Mw) and the number average molecular weight (Mn) calculated in terms of standard polystyrene obtained by GPC measurement.

[0044] P 1 ~P 12 The vinyl content of the polymer chain is not particularly limited, but is preferably 0.01 to 90 mol%, more preferably 0.1 to 80 mol%, and even more preferably 1 to 80 mol%. The vinyl content of the hydrogenated polymer composition of the present invention is also preferably within the above range. In the present invention, the "vinyl content" refers to the total mol% of conjugated diene units bonded via 1,2-bonds, 3,4-bonds (in the case of other than farnesene), and 3,13-bonds (in the case of farnesene) (conjugated diene units bonded via bonds other than 1,4-bonds (in the case of other than farnesene) and 1,13-bonds (in the case of farnesene)) out of a total of 100 mol% of conjugated diene units contained in the polymer chain or polymer before hydrogenation. The vinyl content is 1 Using H-NMR, it is calculated from the area ratio of the peaks derived from conjugated diene units bonded via 1,2-bonds, 3,4-bonds (in the case of compounds other than farnesene), and 3,13-bonds (in the case of farnesene) to the peaks derived from conjugated diene units bonded via 1,4-bonds (in the case of compounds other than farnesene) and 1,13-bonds (in the case of farnesene).

[0045] P 1 ~P 12The vinyl content of the polymer in the polymer chain can be designed according to the purpose. For example, when the vinyl content is less than 70 mol%, the glass transition temperature (Tg) of the polymer becomes low, and the fluidity and low-temperature properties of the obtained hydrogenated polymer composition tend to be excellent. In an embodiment in which the fluidity and / or low-temperature properties of the obtained hydrogenated polymer composition are important, P 1 ~P 12 The vinyl content of the polymer in the polymer chain is preferably 1 to 60 mol%, more preferably 2 to 55 mol%, and even more preferably 3 to 50 mol%. In a preferred embodiment, the hydrogenated polymer composition of the present invention can be used in combination with a polymer (β) other than the hydrogenated polymer composition (details will be described later). In this case, the other polymer (β) is more preferably a thermoplastic polymer (β1). When the (β1) contains, for example, a vinyl alcohol polymer and polypropylene, from the viewpoint of improving the dispersibility of the hydrogenated polymer composition with these thermoplastic polymers (β1), it is preferable to use a polymer having a vinyl content of 1 to 60 mol%, more preferably 2 to 55 mol%, and even more preferably 3 to 50 mol%. 1 ~P 12 The vinyl content of the polymer in the polymer chain is preferably from 45 to 90 mol %, more preferably from 50 to 85 mol %, and further preferably from 55 to 80 mol %.

[0046] When the hydrogenated polymer composition of the present invention is produced by the method described later, the vinyl content can be adjusted to a desired value by controlling the type of solvent used in the step (1), the polar compound used as necessary, the polymerization temperature, etc.

[0047] P 1 ~P 12The glass transition temperature (Tg) of the polymer chain may vary depending on the vinyl content of hydrogenated butadiene units, hydrogenated isoprene units and hydrogenated butadiene units, hydrogenated conjugated diene units other than hydrogenated isoprene units, the type of hydrogenated conjugated diene units, the content of structural units derived from monomers other than hydrogenated dienes, etc., but is preferably -150 to 50°C, more preferably -130 to 50°C, and even more preferably -130 to 30°C. When Tg is in the above range, for example, the viscosity can be prevented from increasing, making handling easy. In addition, the glass transition temperature (Tg) of the polymer composition of the present invention is also preferably in the above range from the viewpoint of ease of handling. In the present invention, Tg is the peak top value of DDSC (differential curve of DSC) obtained by differential scanning calorimetry (DSC) measurement.

[0048] The hydrogenated polymer composition of the present invention is characterized by comprising, relative to the mass of the total polymer contained in the composition, 65 to 99 mass% of at least one boronic acid-based hydrogenated conjugated diene modified polymer (A) selected from the group consisting of a hydrogenated conjugated diene modified polymer containing a boronic acid group represented by the above formula (II), a hydrogenated conjugated diene modified polymer containing a boronic acid ester group represented by the above formula (III), and a hydrogenated conjugated diene modified polymer containing a boronic acid group represented by the following formula (IV), and 1 to 35 mass% of at least one borinic acid-based hydrogenated conjugated diene modified polymer (B) selected from the group consisting of a hydrogenated conjugated diene modified polymer containing a borinic acid group represented by the above formula (V) or (VI), a hydrogenated conjugated diene modified polymer containing a borinic acid ester group represented by the above formula (VII) or (VIII), and a hydrogenated conjugated diene modified polymer containing a borinic acid group represented by the above formula (IX) or (X). By containing the boronic acid-based hydrogenated conjugated diene-modified polymer (A) and the borinic acid-based hydrogenated conjugated diene-modified polymer (B) in the above-mentioned ratio in the hydrogenated polymer composition of the present invention, the reactivity to polar functional groups and dispersibility in a thermoplastic polymer, typically a vinyl alcohol-based polymer, can be improved.

[0049] The hydrogenated polymer composition of the present invention typically means a mixture of a polymer modified with a boron-containing functional group and an unmodified polymer that is not modified by the functional group modification. Therefore, a preferred embodiment of the hydrogenated polymer composition of the present invention is composed only of a mixture of a polymer modified with a boron-containing functional group and an unmodified polymer that is not modified by the functional group modification.

[0050] The content of the boronic acid-based hydrogenated conjugated diene modified polymer (A) and the borinic acid-based hydrogenated conjugated diene modified polymer (B) in the hydrogenated polymer composition is determined based on the boron concentration in the hydrogenated polymer composition. 11 The boron concentration can be determined from the B-NMR spectrum. The boron concentration can be determined by ICP emission spectrometry. 11 The contents of (A) and (B) are calculated from the area ratio of the signals in the B-NMR spectrum. When a boric acid ester compound is used to obtain a hydrogenated polymer composition, the molecular weight of (B) is larger than that of (A), so the contents of (A) and (B) are also calculated from the area ratio of the GPC chart. When the degree of separation of the peaks is low, the peaks are separated as Gaussian distribution peaks to calculate the area ratio.

[0051] From the viewpoint of further enhancing excellent dispersibility in a thermoplastic polymer, typically a vinyl alcohol-based polymer, the content ratio of the boronic acid-based hydrogenated conjugated diene modified polymer (A) and the borinic acid-based hydrogenated conjugated diene modified polymer (B) in the hydrogenated polymer composition of the present invention is preferably 65 to 99 mass% of the boronic acid-based hydrogenated conjugated diene modified polymer (A) and 1 to 35 mass% of the borinic acid-based hydrogenated conjugated diene modified polymer (B), and more preferably 80 to 99 mass% of the boronic acid-based hydrogenated conjugated diene modified polymer (A) and 1 to 35 mass% of the borinic acid-based hydrogenated conjugated diene modified polymer (B). Hydrogenated conjugated dienes The content of the modified polymer (B) is more preferably 1 to 20% by mass.

[0052] The contents of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) and the borinic acid-based hydrogenated conjugated diene-modified polymer (B) in the hydrogenated polymer composition of the present invention can be controlled, for example, by the Taft steric parameter Es value, reaction temperature, the amount of polar compound, etc. in the production method of the hydrogenated conjugated diene-modified polymer described later.

[0053] The Mw of the boronic acid-based hydrogenated conjugated diene modified polymer (A) is preferably 2,000 or more and 200,000 or less, and more preferably 4,000 or more and 100,000 or less. The Mw of the borinic acid-based hydrogenated conjugated diene modified polymer (B) is preferably 4,000 or more and 400,000 or less, and more preferably 8,000 or more and 200,000 or less.

[0054] The hydrogenated polymer composition of the present invention may further contain at least one of a boron-crosslinked trimer (C) represented by the following formula (XI) and an unmodified polymer (D) having no boron-containing functional group, within a range that does not impair the reactivity of the hydrogenated polymer composition. The contents of (C) and (D) in the hydrogenated polymer composition are each preferably 20 mass% or less.

[0055] [ka]

[0056] In the above formula (XI), P 13 , P 14 and P 15 , P 1 ~P 12 Similarly, FIG. 1 shows a polymer chain containing hydrogenated conjugated diene units.

[0057] The content of the hydrogenated conjugated diene modified polymer having a boron-containing functional group (typically a hydrogenated conjugated diene modified polymer having a boron-containing functional group at its terminal) in the hydrogenated polymer composition is preferably 60 mass% or more, more preferably 65 mass% or more, based on the mass of the total polymer contained in the composition.

[0058] The boron content in the hydrogenated polymer composition can be determined by quantifying the boron content per weight of the hydrogenated polymer composition by ICP (inductively coupled plasma) emission spectrometry.

[0059] From the viewpoints of reactivity to polar functional groups and excellent dispersibility in a thermoplastic polymer, typically a vinyl alcohol-based polymer, the boron content in the polymer composition is preferably 0.001 to 5 mass%, and more preferably 0.003 to 2 mass%.

[0060] In the boronic acid-based hydrogenated conjugated diene-modified polymer (A) and the borinic acid-based hydrogenated conjugated diene-modified polymer (B) contained in the hydrogenated polymer composition of the present invention, as well as the boron-bridged trimer (C) represented by the above formula (XI) and the unmodified polymer (D) having no boron atom at its terminal, which may be contained in some cases, at least a part of the carbon-carbon double bonds contained in the conjugated diene units contained in these polymers are hydrogenated. In these polymers of the hydrogenated polymer composition of the present invention, from the viewpoint of heat resistance and weather resistance, the hydrogenation rate (hydrogenation rate) of the carbon-carbon double bonds contained in the conjugated diene units in the polymer before hydrogenation (unhydrogenated) is preferably 50 mol % or more, more preferably 80 mol % or more, and even more preferably 90 mol % or more. The hydrogenation rate is usually 100 mol % or less. Furthermore, the hydrogenation rate may be substantially 100 mol % (i.e., substantially complete hydrogenation). The hydrogenation rate is, 1 The content of carbon-carbon double bonds contained in the conjugated diene units in the polymer was calculated using H-NMR before and after hydrogenation, and the value was determined from these contents.

[0061] The method for producing the hydrogenated polymer composition containing the hydrogenated conjugated diene modified polymer having a boron-containing functional group of the present invention is preferably a production method including the following steps (1), (2) and (3).

[0062] Step (1): A step of producing an active end polymer (hereinafter also referred to as active end polymer (Z)) by anionically polymerizing a monomer containing a conjugated diene in the presence of an anionically polymerizable active metal or active metal compound.

[0063] Specific examples and preferred embodiments of the monomers which are structural units derived from the monomers constituting the active terminal polymer (Z), and specific examples and preferred embodiments of the structural units derived from the monomers contained in the active terminal polymer (Z) are described in the above-mentioned hydrogenated polymer composition, P 1 ~P 12 and a non-hydrogenated conjugated diene unit contained as necessary, and a structural unit derived from a monomer other than a conjugated diene, such as an aromatic vinyl compound unit.

[0064] The active terminal polymer (Z) having an anionically polymerizable active terminal can be produced by a known polymerization method. For example, the active terminal polymer (Z) can be obtained by anionically polymerizing a monomer in a solvent inactive to the polymerization terminal, using an anionically polymerizable active metal or active metal compound as an initiator, and optionally in the presence of a polar compound.

[0065] As the anionically polymerizable active metal or active metal compound, an organic alkali metal compound is preferred, and an organic lithium compound is more preferred.

[0066] Examples of the anionically polymerizable active metal include alkali metals such as lithium, sodium, potassium, etc., alkaline earth metals such as beryllium, magnesium, calcium, strontium, barium, etc., lanthanoid rare earth metals such as lanthanum, neodymium, etc. Among these, alkali metals and alkaline earth metals are preferred, and alkali metals are more preferred.

[0067] The organic alkali metal compounds preferably used as the anionically polymerizable active metal compound include, for example, organic monolithium compounds such as methyl lithium, ethyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, pentyl lithium, hexyl lithium, phenyl lithium, and stilbene lithium; polyfunctional organic lithium compounds such as dilithiomethane, dilithionaphthalene, 1,4-dilithiobutane, 1,4-dilithio-2-ethylcyclohexane, and 1,3,5-trilithiobenzene; sodium naphthalene, potassium naphthalene, and the like. Among these organic alkali metal compounds, organic lithium compounds are preferred. The organic lithium compounds include, for example, methyl lithium, ethyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, and pentyl lithium.

[0068] Examples of the solvent include aliphatic hydrocarbons such as n-butane, n-pentane, isopentane, n-hexane, n-heptane, and isooctane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; and aromatic hydrocarbons such as benzene, toluene, and xylene.

[0069] In the anionic polymerization, a polar compound may be added. In anionic polymerization, a polar compound is usually used to adjust the microstructure (vinyl content) of the conjugated diene unit without deactivating the reaction. Examples of the polar compound include ether compounds such as dibutyl ether, tetrahydrofuran, and ethylene glycol diethyl ether; tertiary amines such as tetramethylethylenediamine and trimethylamine; alkali metal alkoxides, and phosphine compounds. The polar compound is usually used in an amount of 0.01 to 1000 moles per mole of the organic alkali metal compound.

[0070] The temperature of the anionic polymerization is usually in the range of −80 to 150° C., preferably in the range of 0 to 100° C., and more preferably in the range of 10 to 90° C. The polymerization may be carried out in a batchwise or continuous manner.

[0071] Step (2): A step of reacting the active terminal polymer (Z) with a boric acid compound having at least two partial structures represented by the following formula (I) (hereinafter, the structure is also referred to as partial structure (I)), and in which at least one of R bonded to an oxygen atom contained in the partial structure (I) has a Taft steric parameter Es value of -0.30 or less, to obtain an unhydrogenated conjugated diene modified polymer having a boron-containing functional group. BOR (I) (In formula (I), B represents a boron atom, O represents an oxygen atom, and R represents an organic group.)

[0072] Here, the Taft steric parameter Es value is a relative rate based on the substituent effect of the methyl group in the esterification reaction rate of a substituted carboxylic acid under acidic conditions, and is a general index that indicates the steric bulkiness of a substituent. In the present invention, the Es(Taft) value described in Table 1 in Tetrahedron, 1978, Vol. 34, pp. 3553-3562, and a value measured by a method based on the method described in the above literature are included. For example, the value of a hydrogen atom is 1.24, the value of a methyl group is 0.0, the value of an ethyl group is -0.08, the value of an n-propyl group is -0.36, the value of an isopropyl group is -0.47, the value of an n-butyl group is -0.39, the value of a sec-butyl group is -1.13, the value of an i-butyl group is -0.93, the value of a t-butyl group is -1.54, and the value of a cyclohexyl group is -0.79.

[0073] The Taft steric parameter Es value is preferably from -3.00 to -0.30, and more preferably from -1.55 to -0.39.

[0074] A bulky boric acid compound in which at least one of the R's contained in the partial structure (I) has a Taft steric parameter Es value of -0.30 or less is unlikely to form a cluster structure made of the boric acid compound due to steric hindrance, and therefore has high electrophilicity, improves the reaction rate with the active terminal, and ultimately makes it possible to obtain a polymer composition having a high content of the boronic acid-based hydrogenated conjugated diene modified polymer (A). From the viewpoint of further improving the reaction rate, it is a preferred embodiment that all of the R's bonded to the oxygen atom contained in the partial structure (I) satisfy the above Es value.

[0075] As R satisfying the above Es value, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group is preferable, an isopropyl group or an n-butyl group is more preferable, and an isopropyl group is even more preferable.

[0076] The boric acid compound is a boric acid compound having reactivity with the active terminal of the active terminal polymer (Z) obtained by anionic polymerization. Among these, boric acid esters represented by the following formula (XII) are preferred.

[0077] [ka]

[0078] In the above formula (XII), R 16 , R 17 and R 18 represents a hydrocarbon group having 1 to 12 carbon atoms. Above R 16 , R 17 and R 18 At least one of the above preferably has a Taft steric parameter Es value of -0.30 or less, more preferably -3.00 to -0.30, and even more preferably -1.55 to -0.39. 16 , R 17 and R 18 In one embodiment, all of the above R satisfies the above Es value. 16 , R 17 and R 18At least one of the R is preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and even more preferably an isopropyl group. 16 , R 17 and R 18 are preferably an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, or a cyclohexyl group, more preferably an isopropyl group or an n-butyl group, and further preferably an isopropyl group.

[0079] Examples of the boric acid ester represented by the above formula (XII) include boric acid tri-n-propyl ester, boric acid tri-n-butyl ester, boric acid triisopropyl ester, boric acid tri-sec-butyl ester, boric acid tri-i-butyl ester, boric acid tricyclohexyl ester, etc. Among these, boric acid tri-n-propyl ester, boric acid tri-n-butyl ester, and boric acid triisopropyl ester are preferred.

[0080] In the step (2), the boric acid compound is used in an amount of preferably 0.5 to 10 mol, more preferably 1 to 5 mol, per 1 mol of the active end polymer (Z).

[0081] In the step (2), it is preferable to mix a polar compound with the boric acid compound and then react this mixture with the active terminal polymer (Z).

[0082] Examples of the polar compound include ether compounds such as dibutyl ether, tetrahydrofuran, and ethylene glycol diethyl ether; tertiary amines such as tetramethylethylenediamine and trimethylamine; alkali metal alkoxides, and phosphine compounds. The polar compound is usually used in an amount of 0.01 to 1000 moles relative to the boric acid compound used in step (2). By adding the polar compound, the molecular association of the boric acid compound can be dissociated, and the reactivity can be increased.

[0083] The reaction temperature of the active terminal polymer (Z) with the boric acid compound in the above step (2) is usually in the range of -80 to 150°C, preferably in the range of 0 to 100°C, and more preferably in the range of 10 to 90°C.

[0084] After the active terminal polymer (Z) in the above step (2) is reacted with a boric acid compound to obtain an unhydrogenated conjugated diene modified polymer having a boron-containing functional group, a polymerization terminator for the active terminal polymer (Z) may be further added. By adding a polymerization terminator in this manner, it is possible to reliably suppress side reactions originating from the active terminals contained in the active terminal polymer (Z) remaining after the reaction with the boric acid compound. Examples of the polymerization terminator include alcohols such as methanol, ethanol, n-propanol, and isopropanol.

[0085] The reaction in step (2) may be carried out either batchwise or continuously.

[0086] Step (3): A step of hydrogenating (hydrogenating) at least a portion of the carbon-carbon double bonds contained in the conjugated diene units contained in the unhydrogenated conjugated diene modified polymer obtained in step (2).

[0087] By this step (3), hydrogen is added to at least a portion of the carbon-carbon double bonds contained in the conjugated diene units. To obtain the hydrogenated polymer composition of the present invention, the method of hydrogenating the unhydrogenated conjugated diene modified polymer is not particularly limited, and for example, a known method can be used. The hydrogenation may be performed successively after the above steps (1) and (2), or the composition containing the unhydrogenated conjugated diene modified polymer having a boron-containing functional group obtained in step (2) may be isolated once and then hydrogenated. The method of isolating the composition containing the unhydrogenated conjugated diene modified polymer is the same as the method of recovering the hydrogenated polymer composition from the reaction product obtained in step (3) described below.

[0088] Process ( 3As the catalyst used in the hydrogenation reaction of (1), a catalyst capable of hydrogenating the carbon-carbon double bonds contained in olefin compounds, etc., can be used. Such catalysts usually include heterogeneous catalysts and homogeneous catalysts.

[0089] The heterogeneous catalyst is not particularly limited, and specific examples thereof include sponge metal catalysts such as sponge nickel, sponge cobalt, and sponge copper; and supported metal catalysts such as nickel silica, nickel alumina, nickel zeolite, nickel diatomaceous earth, palladium silica, palladium alumina, palladium zeolite, palladium diatomaceous earth, palladium carbon, palladium calcium carbonate, platinum silica, platinum alumina, platinum zeolite, platinum diatomaceous earth, platinum carbon, platinum calcium carbonate, ruthenium silica, ruthenium alumina, ruthenium zeolite, ruthenium diatomaceous earth, ruthenium carbon, ruthenium calcium carbonate, iridium silica, iridium alumina, iridium zeolite, iridium diatomaceous earth, iridium carbon, iridium calcium carbonate, cobalt silica, cobalt alumina, cobalt zeolite, cobalt diatomaceous earth, cobalt carbon, and cobalt calcium carbonate. These heterogeneous catalysts may be modified with iron, molybdenum, magnesium, etc. for the purpose of improving activity, selectivity, and stability. Furthermore, these heterogeneous catalysts may be used alone or in combination of two or more kinds.

[0090] The homogeneous catalyst is not particularly limited, but specific examples thereof include Ziegler catalysts, such as a catalyst composed of a transition metal compound and an alkylaluminum or an alkyllithium; and metallocene catalysts, such as a catalyst composed of a bis(cyclopentadienyl) compound of a transition metal such as titanium, zirconium, hafnium, etc., and an organometallic compound of a metal such as lithium, sodium, potassium, aluminum, zinc, or magnesium. Specific examples of the transition metal compound used in the Ziegler catalyst include nickel salts such as nickel acetate, nickel octylate, nickel neodecanoate, nickel naphthenate, and nickel acetylacetonate; cobalt salts such as cobalt acetate, cobalt octylate, cobalt neodecanoate, cobalt naphthenate, and cobalt acetylacetonate; titanocene dichloride, and zirconocene dichloride. Specific examples of alkylaluminum used in Ziegler catalysts include trimethylaluminum, triethylaluminum, triisobutylaluminum, and trioctylaluminum. Specific examples of the alkyl lithium used in the Ziegler catalyst include methyl lithium, ethyl lithium, n-butyl lithium, sec-butyl lithium, and t-butyl lithium. These homogeneous catalysts may be used alone or in combination of two or more. The homogeneous catalyst may be used in combination with a heterogeneous catalyst.

[0091] Among these catalysts, from the viewpoint of reactivity, homogeneous catalysts are preferred, Ziegler catalysts are more preferred, Ziegler catalysts comprising a transition metal compound and an alkylaluminum are even more preferred, and Ziegler catalysts comprising titanocene dichloride and an alkylaluminum are particularly preferred. On the other hand, the process ( 3 In the hydrogenation reaction of (1), since a polymer is hydrogenated, the reaction activity is generally low with respect to low molecular weight compounds. For this reason, relatively high temperature and high pressure conditions are often preferred as reaction conditions. In this case, in an embodiment in which the thermal stability of the catalytic activity is important, it is preferred to carry out the hydrogenation reaction using a heterogeneous catalyst having high thermal stability as the catalyst used in the hydrogenation reaction. In terms of hydrogenation activity, it is preferred to use nickel or palladium as a metal having hydrogenation activity. In addition, in order to suppress undesirable side reactions during the hydrogenation reaction, it is preferred to use calcium carbonate or a carbon support as a support, and it is even more preferred to use a carbon support.

[0092] The hydrogenation reaction is usually carried out in a solvent. The solvent is not particularly limited, and for example, the solvents used in the anionic polymerization exemplified in the above step (1) can be used.

[0093] The hydrogenation reaction may be carried out, for example, in the state where the unhydrogenated conjugated diene modified polymer having a boron-containing functional group is present in the solvent used in the above step (1) without any particular treatment of the solvent, or may be carried out in the remaining solvent after removing a part of the solvent by a method such as distillation, or may be carried out in a separate solvent after diluting the polymer with the separate solvent. 2 After completion of the above reaction, the composition containing the unhydrogenated conjugated diene modified polymer having a boron-containing functional group may be temporarily removed, and the composition containing the unhydrogenated conjugated diene modified polymer may be placed in a solvent to carry out the hydrogenation reaction in the solvent.

[0094] When the hydrogenation reaction is carried out in a solvent, the amount of the solvent used is determined based on the process temperature of the reaction solution ( 2 The concentration of the hydrogenated polymer in the entire polymer including the unhydrogenated conjugated diene modified polymer that has been subjected to the above-mentioned step (1) is preferably 1% by mass or more and 30% by mass or less. If the hydrogenation reaction is carried out at less than 1% by mass, the productivity may be significantly reduced, whereas if the concentration exceeds 30% by mass, the viscosity may be significantly increased, resulting in a reduction in mixing efficiency.

[0095] The reaction pressure of the hydrogenation reaction may be appropriately set depending on the catalyst used and the like, and is usually 0.1 MPa to 20 MPa, preferably 0.5 MPa to 15 MPa, and more preferably 0.5 MPa to 5 MPa, as the total pressure.

[0096] The hydrogenation reaction is carried out in the presence of hydrogen gas, but may be carried out in the presence of a gas mixed with a gas other than hydrogen gas that is inert to the hydrogenation reaction. Specific examples of the gas that is inert to the hydrogenation reaction include nitrogen, helium, argon, and carbon dioxide. Depending on the reaction conditions, the solvent used in the reaction may have a significant partial pressure as a gas component, but as long as the hydrogenation reaction proceeds, such a situation is usually not a problem.

[0097] The reaction temperature of the hydrogenation reaction may be appropriately set depending on the catalyst used, but is usually 20° C. to 250° C., preferably 50° C. to 180° C., and more preferably 60° C. to 180° C. In general, it may be desirable to react at a higher temperature with a heterogeneous catalyst than with a homogeneous catalyst. The reaction time of the hydrogenation reaction may be appropriately set depending on the type of catalyst used, the amount of catalyst, and the reaction temperature, but is usually 0.1 to 100 hours, preferably 1 to 50 hours. If the reaction time is too short, the desired hydrogenation rate may not be obtained. If the reaction time is too long, the undesired side reaction may progress significantly, and a composition containing a hydrogenated conjugated diene-modified polymer with the desired physical properties may not be obtained.

[0098] The reaction mode of the hydrogenation reaction is not particularly limited and may be appropriately set depending on the type of catalyst used in the reaction. Examples of the reaction mode include a batch reaction mode, a semi-continuous reaction mode (semi-batch reaction mode), and a continuous reaction mode. Suitable continuous reaction modes include a plug flow mode (PFR) and a continuous flow stirring mode (CSTR). When a heterogeneous catalyst is used, the hydrogenation reaction can be carried out in a fixed bed reactor. When the hydrogenation reaction is carried out under active mixing conditions, the mixing method may be a mixing method using stirring or a mixing method in which the reaction liquid is circulated in a loop. When a heterogeneous catalyst is used under mixed conditions, the reaction takes place in a suspended bed, which results in a gas-liquid-solid reaction field, whereas when a homogeneous catalyst is used under mixed conditions, the reaction takes place in a gas-liquid two-phase field. The hydrogenation reaction may be carried out in a reaction mode in which the hydrogenation reaction in the reaction tank is temporarily terminated, the reaction liquid is extracted, and at least a portion of the extracted reaction liquid is charged into the same or a different reaction tank for further hydrogenation. By carrying out the hydrogenation reaction in such a reaction mode, localization of heat generation accompanying the hydrogenation reaction can be avoided, and the hydrogenation rate may be improved. The hydrogenation reaction may be carried out in one reaction mode alone, or in a combination of two or more reaction modes which may be the same or different. When a higher hydrogenation rate is desired, a hydrogenation reaction step including a step of carrying out the reaction in a plug flow mode using a fixed bed reactor may be desirable.

[0099] The amount of catalyst used in the hydrogenation reaction depends on the type of catalyst used and the process ( 2 ) may be appropriately set depending on the concentration of the whole polymer including the unhydrogenated conjugated diene modified polymer, the reaction type, etc., but when the hydrogenation reaction is carried out using a suspension bed with a heterogeneous catalyst, the step ( 2 The amount of catalyst used per 100 parts by mass of the reaction liquid containing the unhydrogenated conjugated diene modified polymer that has been subjected to step () is usually 0.01 to 20 parts by mass, preferably 0.05 to 15 parts by mass, and more preferably 0.1 to 10 parts by mass. If the amount of catalyst used is too small, the hydrogenation reaction may take a long time, and if the amount of catalyst used is too large, more power may be required to mix the heterogeneous catalyst. In addition, when the hydrogenation reaction is carried out in a fixed bed, 2 It is difficult to specify the amount of catalyst used per reaction solution containing the unhydrogenated conjugated diene modified polymer that has been subjected to the above steps, and the amount may be appropriately set depending on the type of reaction vessel to be used, etc. When a Ziegler catalyst or a metallocene catalyst is used as a homogeneous catalyst, 2 The concentration of the transition metal compound in the reaction liquid containing the unhydrogenated conjugated diene modified polymer that has been subjected to step (1) is usually 0.001 mmol / L to 100 mmol / L, and preferably 0.01 mmol / L to 10 mmol / L.

[0100] The catalyst used in the hydrogenation reaction may be separated from the liquid containing the hydrogenated conjugated diene modified polymer having a boron-containing functional group after the hydrogenation reaction is completed, if necessary. The method of separation is not particularly limited as long as the catalyst can be separated. When a heterogeneous catalyst is used, the catalyst can be separated, for example, by continuous or batch filtration, centrifugation, settling by standing, and decantation. When a homogeneous catalyst is used, the catalyst can be separated, for example, by coagulation settling, adsorption, washing, and aqueous phase extraction. Even if the catalyst after use is separated by these separation methods, a trace amount of metal components derived from the catalyst may remain in the liquid containing the hydrogenated conjugated diene modified polymer having a boron-containing functional group. In this case, the metal components remain in the liquid, so that the remaining metal components can be separated by separation methods such as coagulation precipitation, adsorption, washing and aqueous phase extraction, as described above. The catalyst recovered by separation can be reused in the hydrogenation reaction after, if necessary, part of it is removed or new catalyst is added.

[0101] The hydrogenated polymer composition obtained by the production method of the present invention is recovered from the reaction product obtained in the above step (3). There is no particular restriction on the method for recovering the hydrogenated polymer composition. When the reaction product is obtained in step (3) as a solution containing the hydrogenated polymer composition, the hydrogenated polymer composition can be recovered, for example, by pouring the obtained solution into a poor solvent such as methanol to precipitate the hydrogenated polymer composition; pouring the obtained solution into hot water together with steam to remove the solvent by azeotropy (steam stripping); or by washing the polymer solution with water, separating it, and then drying it to isolate the polymer composition. In this case, the washing efficiency can be further improved by using an acidic aqueous solution for washing. Examples of the acid to be used include strong monovalent or polyvalent acids such as hydrochloric acid, nitric acid, and sulfuric acid; monovalent or polyvalent carboxylic acids such as acetic acid, propionic acid, succinic acid, and citric acid; and weak monovalent or polyvalent acids such as carbonic acid and phosphoric acid.

[0102] The resin composition of the present invention includes a hydrogenated polymer composition (hereinafter also referred to as hydrogenated polymer composition (α)) that contains a boronic acid-based hydrogenated conjugated diene modified polymer (A) and a borinic acid-based hydrogenated conjugated diene modified polymer (B), and optionally contains a boron-bridged trimer (C) and an unmodified polymer (D) that does not have a boron atom at its terminal. The resin composition of the present invention may contain another polymer (β) other than the polymer contained in the hydrogenated polymer composition (α). The other polymer (β) may be a thermoplastic polymer (β1) or a curable polymer (β2).

[0103] Examples of the thermoplastic polymer (β1) include acrylic resins such as polymethyl methacrylate and (meth)acrylic acid ester polymers or copolymers; olefin resins such as polyethylene, ethylene-vinyl acetate copolymer, polypropylene, polybutene-1, poly-4-methylpentene-1, and polynorbornene; ethylene ionomers; styrene resins such as polystyrene, styrene-maleic anhydride copolymer, high impact polystyrene, AS resin, ABS resin, AES resin, AAS resin, ACS resin, and MBS resin; styrene-methyl methacrylate copolymer; styrene-methyl methacrylate-maleic anhydride copolymer; polyethylene terephthalate, poly Polyester resins such as butylene terephthalate and polylactic acid; polyamides such as nylon 6, nylon 66, and polyamide elastomers; polycarbonate; polyvinyl chloride; polyvinylidene chloride; polyvinyl acetate; vinyl alcohol-based polymers such as partially saponified polyvinyl alcohol, polyvinyl alcohol, and ethylene-vinyl alcohol copolymers; polyacetal; polyvinylidene fluoride; polyurethane; modified polyphenylene ether; polyphenylene sulfide; silicone rubber-modified resins; acrylic rubber; silicone rubber; styrene-based thermoplastic elastomers such as SEPS, SEBS, and SIS; and olefin-based rubbers such as IR, EPR, and EPDM. Among these, vinyl alcohol-based polymers are preferred because of their excellent dispersibility in the hydrogenated polymer composition (α) obtained by the present invention, and partially saponified polyvinyl alcohol, polyvinyl alcohol, and ethylene-vinyl alcohol copolymers are more preferred, and ethylene-vinyl alcohol copolymers are even more preferred. The thermoplastic polymer (β1) may be used alone or in combination of two or more kinds.

[0104] The ethylene-vinyl alcohol copolymer is a saponification product of an ethylene-vinyl ester copolymer containing a structural unit derived from ethylene (ethylene unit) and a structural unit derived from a vinyl ester (vinyl ester unit). The content of the ethylene unit in the ethylene-vinyl alcohol copolymer is not particularly limited, but is usually in the range of 10 to 99 mol%, preferably 15 to 60 mol%, more preferably 20 to 60 mol%, and further preferably 25 to 55 mol%. The degree of saponification of the vinyl ester unit of the ethylene-vinyl alcohol copolymer is not particularly limited, but is usually in the range of 10 to 100 mol%, preferably 50 to 100 mol%, more preferably 80 to 100 mol%, further preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%. If the degree of saponification is too low, the crystallization degree may decrease and the thermal stability during melt molding may deteriorate, so a high degree of saponification is preferable. Here, vinyl acetate is a representative example of the vinyl ester, but other examples include vinyl esters such as vinyl propionate, vinyl pivalate, vinyl valerate, vinyl caprate, and vinyl benzoate. These vinyl esters may be used alone or in combination of two or more. Furthermore, as the ethylene-vinyl alcohol copolymer, a mixture of two or more different ethylene-vinyl alcohol copolymers may be used.

[0105] The ethylene-vinyl alcohol copolymer may contain structural units derived from other monomers than the above-mentioned ethylene unit, vinyl ester unit, and saponified vinyl ester unit, within the scope of not impairing the object of the present invention. Examples of such other monomers include olefin monomers such as propylene, 1-butene, and isobutene; acrylamide monomers such as acrylamide, N-methylacrylamide, N-ethylacrylamide, and N,N-dimethylacrylamide; methacrylamide monomers such as methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, and N,N-dimethylmethacrylamide; vinyl ether monomers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether, t-butyl vinyl ether, and dodecyl vinyl ether; allyl alcohol; vinyltrimethoxysilane; and N-vinyl-2-pyrrolidone.

[0106] The melt flow rate (hereinafter sometimes simply abbreviated as "MFR") of the ethylene-vinyl alcohol copolymer according to JIS K 7210:2014 (temperature 210°C, load 2160g) is preferably 0.1g / 10min or more, more preferably 0.5g / 10min or more, and even more preferably 1g / 10min or more. On the other hand, the MFR of the ethylene-vinyl alcohol copolymer is preferably 50g / 10min or less, more preferably 30g / 10min or less, and even more preferably 15g / 10min or less. By setting the MFR of the ethylene-vinyl alcohol copolymer to a value within this range, the melt moldability is improved.

[0107] Examples of the curable polymer (β2) include epoxy resins, unsaturated polyester resins, epoxy (meth)acrylate resins, ester (meth)acrylate resins, phenolic resins, urea resins, melamine resins, thermosetting urethane resins, silicon resins, imide resins, furan resins, alkyd resins, allyl resins, and diallyl phthalate resins. Among these, from the viewpoints of availability and basic physical properties of the cured product, and also from the viewpoints of obtaining a resin composition that is more excellent in terms of bubble removal and toughness of the obtained cured product, epoxy resins, unsaturated polyester resins, and epoxy (meth)acrylate resins are preferred, among which epoxy resins and unsaturated polyester resins are more preferred, and epoxy resins are even more preferred. The curable polymer (β2) may be used alone or in combination of two or more types.

[0108] When the resin composition of the present invention contains the above polymer (β), the mass ratio (α) / (β) of the hydrogenated polymer composition (α) to the other polymer (β) is preferably 50 / 50 to 1 / 99, more preferably 40 / 60 to 2 / 98, even more preferably 30 / 70 to 3 / 97, still more preferably 20 / 80 to 3 / 97, and particularly preferably 15 / 85 to 3 / 97.

[0109] In addition, various additives may be added to the resin composition of the present invention to the extent that the effect of the present invention is not impaired. For example, when the other polymer (β) is a thermoplastic polymer (β1), such additives may be, for example, calcium carbonate, silica, carbon black, glass fiber, clay, or other reinforcing or filler, or process oil, polyethylene glycol, glycerin, phthalic acid ester, or other plasticizer. In addition, other additives may be, for example, heat stabilizers, antioxidants, ultraviolet absorbers, colorants, pigments, lubricants, surfactants, and the like. Furthermore, foaming agents may be included as the additives, and foams can be produced from polymer compositions containing the foaming agent and the thermoplastic polymer (β1). For example, when the other polymer (β) is a curable polymer (β2), such additives include curing agents, curing accelerators, known rubbers, thermoplastic elastomers, impact modifiers such as core-shell particles, fillers (inorganic particles such as silica, talc, calcium carbonate, aluminum hydroxide, etc.), flame retardants, defoamers, pigments, dyes, antioxidants, weather resistance agents, lubricants, release agents, etc.

[0110] The hydrogenated polymer composition (α) of the present invention can be mixed with the other polymer (β) by a method for mixing ordinary polymer substances depending on the composition ratio of each component.

[0111] When the other polymer (β) is a thermoplastic polymer (β1), the resin composition of the present invention can be produced by a mixing device such as an extruder, a mixing roll, a Banbury mixer, a kneader, etc. In particular, in the present invention, a method of melt kneading using such a mixing device is a preferred embodiment.

[0112] When the other polymer (β) is a curable polymer (β2), the resin composition of the present invention can be prepared, for example, by thoroughly mixing the polymers in a mixer, melt-kneading the mixture in a mixing roll or extruder, and then cooling and pulverizing the mixture. EXAMPLES

[0113] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, the physical properties of the hydrogenated polymer compositions were evaluated by the following methods.

[0114] (1) Weight average molecular weight (Mw), number average molecular weight (Mn), molecular weight distribution (Mw / Mn) The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) of the polymer were determined in terms of standard polystyrene by gel permeation chromatography (GPC). Equipment: Tosoh Corporation GPC equipment "HLC-8220" Separation column: Tosoh Corporation's "TSKgel SuperMultiporeHZ-M (column diameter = 4.6 mm, column length = 15 cm)" (two columns connected in series) Eluent: Tetrahydrofuran Eluent flow rate: 0.35mL / min Column temperature: 40℃ Detection method: Refractive index (RI) Injection volume: 10μL Concentration: 1mg / 1mL (polymer / THF)

[0115] (2) Vinyl content and hydrogenation rate 1 The vinyl content of the hydrogenated conjugated diene modified polymer and the polymer at each stage of its production was calculated by H-NMR. The vinyl content was calculated for the unhydrogenated polymer before the hydrogenation reaction, and the vinyl content was calculated from the area ratio of the signal of the double bond derived from the vinylated conjugated diene unit to the signal of the double bond derived from the non-vinylated conjugated diene unit in the obtained spectrum. Since the signal derived from the double bond derived from the conjugated diene unit decreases before and after hydrogenation, the hydrogenation rate was calculated by comparing the area ratio of the signal derived from the double bond derived from the conjugated diene unit to an appropriate signal that does not change by hydrogenation (such as the signal of the aromatic ring derived from styrene and the signal of the terminal methyl derived from the initiator) in the polymer before hydrogenation with the area ratio of the same signal in the polymer after hydrogenation. Equipment: Nuclear magnetic resonance equipment "JNM-ECX400" manufactured by JEOL Ltd. Solvent: deuterated chloroform Measurement temperature: 50℃ Number of times accumulated: 1024

[0116] (3) Boron-containing functional group introduction rate (mass%) The introduction rate of boron-containing functional groups into the polymer terminals (boron-containing functional group introduction rate) by the reaction of a boric acid compound and an active terminal polymer was calculated from the boron atom content by ICP (inductively coupled plasma) emission analysis and the component ratio of the polymer components by GPC measurement after decomposing the polymer composition obtained in each of the following examples, etc., in which unreacted boric acid compounds were removed by washing with water. The boron-containing functional group introduction rate was determined from the sum of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) and the boronic acid-based hydrogenated conjugated diene-modified polymer (B) obtained by subtracting the mass of the unmodified product from the mass of the entire polymer composition obtained in each of the examples, etc. <Microwave decomposition> Apparatus: ETHOS UP manufactured by MILESTONE Solvent: Nitric acid Decomposition temperature: 210 °C Decomposition time: 30 minutes <ICP emission analysis> Apparatus: iCAP7400 Duo manufactured by ThermoFisher

[0117] (4) Content (% by mass) of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) and the boronic acid-based hydrogenated conjugated diene-modified polymer (B) in the polymer composition In the polymer composition obtained in each of the following examples, etc., the boronic acid-based hydrogenated conjugated diene-modified polymer (B) has a higher molecular weight than the unmodified polymer that has not been modified with the boronic acid-based hydrogenated conjugated diene-modified polymer (A) and the boric acid compound. Also, the molecular weights of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) and the unmodified polymer are the same. From these facts, first, from the area ratio obtained by GPC, the content (% by mass) of the boronic acid-based hydrogenated conjugated diene-modified polymer (B) in the polymer composition and the content (% by mass) of the combined boronic acid-based hydrogenated conjugated diene-modified polymer (A) and the unmodified polymer were calculated, respectively. Thereafter, from the boron-containing functional group introduction rate obtained as described above and the content obtained from the above GPC results, the content of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) in the polymer composition was calculated as follows. (Content (mass%) of boronic acid-based hydrogenated conjugated diene modified polymer (A))=(Boron-containing functional group introduction rate (mass%))-(Content (mass%) of borinic acid-based hydrogenated conjugated diene modified polymer (B))

[0118] (5) Reactivity The reactivity of the boron-containing functional group of the hydrogenated conjugated diene modified polymer obtained in the examples is as follows: 1 The amount of catechol was evaluated by H-NMR using the following indexes from the change in the signal when catechol was added to a solution of the polymer in a heavy solvent in an amount equivalent to the polymer initiation terminal in step (1) of each Example or Comparative Example. 1 The value was calculated from the integral ratio of the alkyl group derived from alkyllithium and the integral ratio of the double bond signal derived from the conjugated diene unit of the polymer before hydrogenation by H-NMR. A: Signal shifted catechol amount 70 mol % or more B: Amount of catechol with signal shift: 50 mol % or more, less than 70 mol % C: Amount of catechol with signal shift: 25 mol% or more, less than 50 mol% D: Signal shifted catechol amount less than 25 mol%

[0119] (6) Dispersibility The dispersibility of the polymers obtained in the examples and the like in thermoplastic polymers was evaluated as follows: A vinyl alcohol-based polymer was used as the thermoplastic polymer. Dispersibility in vinyl alcohol-based polymers was measured by kneading 95 parts by mass of an ethylene-vinyl alcohol copolymer with an ethylene unit content of 32 mol% and a saponification degree of 99.9 mol% with 5 parts by mass of a hydrogenated polymer composition using a Labo Plastomill (device name 4M150, manufactured by Toyo Seiki Seisakusho Co., Ltd.) under conditions of 200°C, 10 minutes, and 100 rpm, and pressing the resulting resin composition at 200°C to form a film with a thickness of 125 μm, and then checking the dispersion diameter of the dispersed domains in the cross section with an optical microscope. Evaluation was performed using the following indicators. A: The diameter of the largest dispersed domain in the cross section is less than 3 μm B: The diameter of the largest dispersed domain in the cross section is 3 μm or more and less than 5 μm. C: The diameter of the largest dispersed domain in the cross section is 5 μm or more and less than 7 μm. D: The diameter of the largest dispersed domain in the cross section is 7 μm or more.

[0120] (7) Taft's steric parameter Es value The Taft steric parameter Es value of the organic group bonded to the oxygen atom in the boric acid compound used in the following Examples and Comparative Examples was calculated by the method described in the above-mentioned mode for carrying out the invention.

[0121] [Example 1] (Process (1)) A thoroughly dried 5 L autoclave was purged with nitrogen, and 606 g of cyclohexane, 4.51 g of tetrahydrofuran, and 5.40 g of sec-butyllithium (1.3 M cyclohexane solution) were charged and heated to 50° C., and then 140 g of butadiene was gradually added at 10 mL / min under stirring conditions while controlling the polymerization temperature to 50° C. After the addition of butadiene, the polymerization was completed by heating for 1 hour, and a polymerization liquid containing a butadiene polymer having active terminals was obtained.

[0122] (Process (2)) 1.69 g of triisopropyl borate was added to the polymerization solution obtained in step (1) to introduce boronic acid into the polymerization terminal of the butadiene polymer, thereby obtaining a liquid containing a polymer composition. The vinyl content of the obtained polymer composition was 47 mol%.

[0123] (Step (3)) To the liquid containing the polymer composition obtained in step (2), μ-chloro-μ-methylene[bis(cyclopentadienyl)titanium]dimethylaluminum (Tebbe catalyst) was added as a hydrogenation catalyst in an amount of 0.0001 mol% as the amount of Ti in the hydrogenation catalyst relative to the carbon-carbon double bonds contained in the butadiene units of all polymers contained in the polymer composition, and the hydrogenation reaction was carried out at 85°C and under a hydrogen pressure of 1 MPa until the hydrogenation rate reached 96 mol%. The liquid containing the obtained hydrogenated polymer composition was poured into a 5-fold amount of methanol, and the polymer components were precipitated, then recovered and dried. The introduction rate of terminal functional groups in the obtained hydrogenated polymer composition was 90% by mass. In addition, the content of the boronic acid-based hydrogenated conjugated diene modified polymer (A) in the obtained hydrogenated polymer composition was 86% by mass, the content of the borinic acid-based hydrogenated conjugated diene modified polymer (B) was 4% by mass, and the weight average molecular weight of the boronic acid-based hydrogenated conjugated diene modified polymer (A) was 30,000, and Mw / Mn was 1.05.

[0124] [Example 2] (Process (1)) A thoroughly dried 5L autoclave was purged with nitrogen, and 606g of cyclohexane, 5.40g of sec-butyllithium (1.3M cyclohexane solution), and 0.65g of tetramethylethylenediamine (TMEDA) were charged and heated to 40°C. After that, 140g of butadiene was gradually added at 10mL / min under stirring conditions while controlling the polymerization temperature to 40°C. After the addition of butadiene, the polymerization was completed by heating for 1 hour, and a polymerization liquid containing a butadiene polymer having active terminals was obtained.

[0125] (Process (2)) 1.69 g of triisopropyl borate was added to the polymerization solution obtained in step (1) to introduce boronic acid into the polymerization terminal of the butadiene polymer, thereby obtaining a liquid containing a polymer composition. The vinyl content of the obtained polymer composition was 75 mol%.

[0126] (Step (3)) The liquid containing the polymer composition obtained in step (2) was added with a Tebbe catalyst as a hydrogenation catalyst in an amount of 0.0001 mol% as the amount of Ti in the hydrogenation catalyst relative to the carbon-carbon double bonds contained in the butadiene units of all polymers contained in the polymer composition, and hydrogenation reaction was carried out at 85°C and under a hydrogen pressure of 1 MPa until the hydrogenation rate reached 96 mol%. The liquid containing the obtained hydrogenated polymer composition was poured into a 5-fold amount of methanol to precipitate the polymer components, which were then recovered and dried. The introduction rate of terminal functional groups in the obtained hydrogenated polymer composition was 90% by mass. The content of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) in the obtained hydrogenated polymer composition was 88% by mass, the content of the borinic acid-based hydrogenated conjugated diene-modified polymer (B) was 2% by mass, and the weight average molecular weight of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) was 30,000, and Mw / Mn was 1.04.

[0127] [Example 3] (Process (1)) A thoroughly dried 5L autoclave was purged with nitrogen, and 606g of cyclohexane, 5.40g of sec-butyllithium (1.3M cyclohexane solution), and 0.65g of tetramethylethylenediamine (TMEDA) were charged and heated to 40°C. After that, 140g of butadiene was gradually added at 10mL / min under stirring conditions while controlling the polymerization temperature to 40°C. After the addition of butadiene, the polymerization was completed by heating for 1 hour, and a polymerization liquid containing a butadiene polymer having active terminals was obtained.

[0128] (Process (2)) A mixture of 0.65 g of TMEDA and 1.69 g of triisopropyl borate was added to the polymerization solution obtained in step (1) to introduce boronic acid into the polymerization terminal of the butadiene polymer, thereby obtaining a liquid containing a polymer composition. The vinyl content of the obtained polymer composition was 75 mol%.

[0129] (Step (3)) The liquid containing the polymer composition obtained in step (2) was added with a Tebbe catalyst as a hydrogenation catalyst in an amount of 0.0001 mol% as the amount of Ti in the hydrogenation catalyst relative to the carbon-carbon double bonds contained in the butadiene units of all polymers contained in the polymer composition, and hydrogenation reaction was carried out at 85°C and under a hydrogen pressure of 1 MPa until the hydrogenation rate reached 96 mol%. The liquid containing the obtained hydrogenated polymer composition was poured into a 5-fold amount of methanol to precipitate the polymer components, which were then recovered and dried. The introduction rate of terminal functional groups in the obtained hydrogenated polymer composition was 98% by mass. The content of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) in the obtained hydrogenated polymer composition was 95% by mass, the content of the borinic acid-based hydrogenated conjugated diene-modified polymer (B) was 3% by mass, and the weight average molecular weight of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) was 30,000, and Mw / Mn was 1.04.

[0130] [Example 4] The same procedure as in Example 3 was carried out except that the type and amount of the compound added in each step were changed as shown in Table 1, to obtain a hydrogenated polymer composition containing a hydrogenated conjugated diene-modified polymer.

[0131] [Example 5] The same procedure as in Example 1 was carried out except that the type and amount of the compound added in each step were changed as shown in Table 1, to obtain a hydrogenated polymer composition containing a hydrogenated conjugated diene-modified polymer.

[0132] [Example 6] (Process (1)) A thoroughly dried 5 L autoclave was purged with nitrogen, and 606 g of cyclohexane and 4.19 g of sec-butyllithium (1.3 M cyclohexane solution) were charged and heated to 50° C., after which 137 g of isoprene was gradually added at 10 mL / min under stirring conditions while controlling the polymerization temperature to 50° C. After the addition of isoprene, the mixture was heated for 1 hour to complete the polymerization, and a polymerization liquid containing an isoprene polymer having active terminals was obtained.

[0133] (Process (2)) 1.31 g of triisopropyl borate was added to the polymerization solution obtained in step (1) to introduce boronic acid into the polymerization terminal of the isoprene polymer, thereby obtaining a liquid containing a polymer composition. The vinyl content of the obtained polymer composition was 8 mol%.

[0134] (Step (3)) A Ziegler-based hydrogenation catalyst formed from nickel octylate and triethylaluminum was added as a hydrogenation catalyst to the liquid containing the polymer composition obtained in step (2) in an amount of 0.1 mol% of Ni in the hydrogenation catalyst relative to the carbon-carbon double bonds contained in the isoprene units of all polymers contained in the polymer composition, and hydrogenation reaction was carried out at 85°C and under a hydrogen pressure of 1 MPa until the hydrogenation rate reached 96 mol%. The liquid containing the obtained hydrogenated polymer composition was poured into a 5-fold amount of methanol to precipitate the polymer components, which were then recovered and dried. The introduction rate of terminal functional groups in the obtained hydrogenated polymer composition was 85% by mass. The content of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) in the obtained hydrogenated polymer composition was 73% by mass, the content of the borinic acid-based hydrogenated conjugated diene-modified polymer (B) was 12% by mass, and the weight average molecular weight of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) was 30,000, and Mw / Mn was 1.05.

[0135] [Example 7] (Process (1)) A thoroughly dried 5L autoclave was purged with nitrogen, and 606g of cyclohexane, 4.49g of sec-butyllithium (1.3M cyclohexane solution), and 0.54g of TMEDA were charged. After heating to 50°C, 93g of butadiene was added successively at 10mL / min under stirring conditions while controlling the polymerization temperature to 50°C. After the addition of butadiene, the mixture was heated for 1 hour, and then 30g of isoprene was added successively at 10mL / min. After the addition of isoprene, the mixture was heated for 1 hour to complete the polymerization, and a polymerization liquid containing a block copolymer consisting of a butadiene polymer block and an isoprene polymer block having an active terminal was obtained.

[0136] (Process (2)) A mixture of 0.54 g of TMEDA and 1.41 g of triisopropyl borate was added to the polymerization solution obtained in step (1) to introduce boronic acid to the polymerization terminal of the isoprene polymer block, thereby obtaining a liquid containing a polymer composition. The vinyl content of the entire obtained polymer composition was 69 mol%.

[0137] (Step (3)) A Ziegler-based hydrogenation catalyst formed from nickel octylate and triethylaluminum was added as a hydrogenation catalyst to the liquid containing the polymer composition obtained in step (2) in an amount of 0.1 mol% of Ni in the hydrogenation catalyst relative to the carbon-carbon double bonds contained in the butadiene units and isoprene units of all polymers contained in the polymer composition, and the hydrogenation reaction was carried out at 85°C and under a hydrogen pressure of 1 MPa until the hydrogenation rate reached 96 mol%. The liquid containing the obtained hydrogenated polymer composition was poured into a 5-fold amount of methanol to precipitate the polymer components, which were then recovered and dried. The introduction rate of terminal functional groups in the obtained hydrogenated polymer composition was 95% by mass. The content of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) in the obtained hydrogenated polymer composition was 83% by mass, the content of the borinic acid-based hydrogenated conjugated diene-modified polymer (B) in the obtained hydrogenated polymer composition was 12% by mass, and the weight average molecular weight of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) was 30,000, and Mw / Mn was 1.05.

[0138] [Example 8] (Process (1)) A thoroughly dried 5L autoclave was purged with nitrogen, and 606g of cyclohexane, 3.30g of sec-butyllithium (1.3M cyclohexane solution), and 0.39g of TMEDA were charged. After heating to 40°C, 47g of butadiene was added successively at 10mL / min under stirring conditions while controlling the polymerization temperature to 40°C. After the addition of butadiene, the mixture was heated for 1 hour, and then 74g of styrene was added successively at 10mL / min. After the addition of styrene, the mixture was heated for 1 hour to complete the polymerization, and a polymerization liquid containing a block copolymer consisting of a butadiene polymer block and a styrene polymer block having an active terminal was obtained.

[0139] (Process (2)) A mixture of 0.39 g of TMEDA and 1.03 g of triisopropyl borate was added to the polymerization solution obtained in step (1) to introduce boronic acid into the polymerization terminal of the styrene polymer block. The vinyl content of the obtained polymer composition was 76 mol%.

[0140] (Step (3)) The liquid containing the polymer composition obtained in step (2) was added with a Tebbe catalyst as a hydrogenation catalyst in an amount of 0.0001 mol% as the amount of Ti in the hydrogenation catalyst relative to the carbon-carbon double bonds contained in the butadiene units of all polymers contained in the polymer composition, and hydrogenation reaction was carried out at 85°C and under a hydrogen pressure of 1 MPa until the hydrogenation rate reached 96 mol%. The liquid containing the obtained hydrogenated polymer composition was poured into a 5-fold amount of methanol to precipitate the polymer components, which were then recovered and dried. The introduction rate of terminal functional groups in the obtained hydrogenated polymer composition was 95% by mass. The content of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) in the obtained hydrogenated polymer composition was 85% by mass, the content of the borinic acid-based hydrogenated conjugated diene-modified polymer (B) in the obtained hydrogenated polymer composition was 10% by mass, and the weight average molecular weight of the boronic acid-based hydrogenated conjugated diene-modified polymer (A) was 30,000, and Mw / Mn was 1.06.

[0141] [Comparative Example 1] As shown in Table 1, the same procedure as in Example 1 was carried out except that 0.93 g of trimethyl borate was added instead of triisopropyl borate in step (2), to obtain a hydrogenated polymer composition containing a hydrogenated conjugated diene modified polymer.

[0142] [Comparative Example 2] As shown in Table 1, the same procedure as in Example 1 was carried out except that the boric acid compound was not added in the step (2), to obtain a hydrogenated polymer composition.

[0143] [Comparative Example 3] As shown in Table 1, the same procedure as in Example 1 was carried out except that 2.78 g of phenylboronic anhydride was added instead of triisopropyl borate in step (2), to obtain a hydrogenated polymer composition containing a hydrogenated conjugated diene-modified polymer having borinic acid introduced at its terminal.

[0144] [Table 1]

[0145] Table 2 shows the physical properties of the hydrogenated polymer compositions containing the hydrogenated conjugated diene polymers obtained in Examples 1 to 8 and Comparative Examples 1 to 3.

[0146] [Table 2]

[0147] In Table 2, R is an organic group that bonds to the oxygen atom of the boric acid compound used in step (1), and corresponds to R in formula (I).

[0148] From Table 2, it can be seen that by reacting a boric acid compound having a substituent with a Taft steric parameter Es value of -0.30 or less shown in Examples 1 to 8, a hydrogenated diene-based polymer containing a hydrogenated conjugated diene-modified polymer having a boron-containing functional group can be obtained, which has a high terminal functional group introduction rate, excellent reactivity with polar functional groups, and excellent dispersibility in a thermoplastic polymer (vinyl alcohol-based polymer). On the other hand, in Comparative Example 1, in which a boric acid compound having a substituent with a Taft steric parameter Es value of more than -0.30 was reacted, the terminal functional group introduction rate was low, and the reactivity and dispersibility in a thermoplastic polymer (vinyl alcohol-based polymer) were poor. In Comparative Example 2, in which no boric acid compound was reacted, the reaction did not occur with polar functional groups, and the dispersibility in a thermoplastic polymer (vinyl alcohol-based polymer) was also poor. Furthermore, in Comparative Example 3, which contains only a boric acid compound, the reactivity was excellent but the dispersibility in a thermoplastic polymer (vinyl alcohol-based polymer) was poor, making it difficult to achieve both reactivity and dispersibility in a thermoplastic polymer (vinyl alcohol-based polymer). [Industrial Applicability]

[0149] The production method of the present invention provides a boronic acid-based hydrogenated conjugated diene modified polymer (A) in high yield, which is suitable for modifying polar materials and dispersing inorganic materials. In addition, the hydrogenated polymer composition containing the boronic acid-based hydrogenated conjugated diene modified polymer and the borinic acid-based hydrogenated conjugated diene modified polymer in a specific ratio obtained by the present invention has high reactivity with polar functional groups and excellent dispersibility in thermoplastic polymers, typically vinyl alcohol-based polymers. Therefore, the hydrogenated polymer composition of the present invention and a resin composition containing the polymer composition can be effectively used in a wide range of fields, such as automobile interior and exterior parts, electric and electronic parts, packaging materials, sporting goods, daily necessities, laminate materials, elastic materials, various rubber products, medical supplies, various adhesives, and various paint primers.

Claims

1. A step (1) of producing an active terminal polymer (Z) by anionically polymerizing a monomer containing a conjugated diene in the presence of an anionically polymerizable active metal or active metal compound; a step (2) of reacting the active terminal polymer (Z) obtained in the step (1) with a boric acid ester represented by the following formula (XII), which is a boric acid compound, to obtain an unhydrogenated conjugated diene modified polymer having a boron-containing functional group; and a step (3) of hydrogenating at least a portion of the carbon-carbon double bonds contained in the conjugated diene units contained in the unhydrogenated conjugated diene modified polymer obtained in the step (2). 【Chemistry 1】 (In the above formula (XII), R 16 , R 17 and R 18 each represent an isopropyl group or an n-butyl group.)

2. 2. The method for producing a hydrogenated polymer composition according to claim 1, wherein in the step (2), a polar compound is mixed with the boric acid compound, and then the polar compound is added to the active terminal polymer (Z) and reacted.

3. A hydrogenated polymer composition comprising 65 to 99 mass% of at least one boronic acid-based hydrogenated conjugated diene-modified polymer (A) selected from the group consisting of a hydrogenated conjugated diene-modified polymer containing a boronic acid group represented by the following formula (II), a hydrogenated conjugated diene-modified polymer containing a boronic acid ester group represented by the following formula (III), and a hydrogenated conjugated diene-modified polymer containing a boronic acid salt group represented by the following formula (IV), and 1 to 35 mass% of at least one borinic acid-based hydrogenated conjugated diene-modified polymer (B) selected from the group consisting of a hydrogenated conjugated diene-modified polymer containing a borinic acid group represented by the following formula (V) or (VI), a hydrogenated conjugated diene-modified polymer containing a borinic acid ester group represented by the following formula (VII) or (VIII), and a hydrogenated conjugated diene-modified polymer containing a borinic acid salt group represented by the following formula (IX) or (X). 【Chemistry 2】 (In the above formula, P 1 , P 2 and P 3 represents a polymer chain containing hydrogenated conjugated diene units, R 1 and R 2 each independently represents an alkyl group having 1 to 12 carbon atoms and a Taft steric parameter Es value of −0.30 or less; R 3 , R 4 and R 5 each independently represents an alkyl group having 1 to 12 carbon atoms and a Taft steric parameter Es value of -0.30 or less; M represents one alkali metal or 1 / 2 an alkaline earth metal. 【Chemistry 3】 (In the above formula, P 4 , P 5 , P 6 , P 7 , P 8 , P 9 , P 10 , P 11 and P 12 represents a polymer chain containing hydrogenated conjugated diene units, R 6 , R 7 , R 8 and R 9 each independently represents an alkyl group having 1 to 12 carbon atoms and a Taft steric parameter Es value of −0.30 or less; R 10 and R 11 each independently represents an alkyl group having 1 to 12 carbon atoms and a Taft steric parameter Es value of −0.30 or less; R 12 represents an alkyl group having 1 to 12 carbon atoms and a Taft steric parameter Es value of -0.30 or less; R 13 and R 14 each independently represents an alkyl group having 1 to 12 carbon atoms and a Taft steric parameter Es value of -0.30 or less, and M represents one alkali metal or 1 / 2 an alkaline earth metal.

4. The hydrogenated polymer composition according to claim 3, wherein R 1 and R 2, R 3, R 4 and R 5, R 6, R 7, R 8 and R 9, R 10 and R 11, R 12, and R 13 and R 14 are each independently at least one group selected from the group consisting of an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an i-butyl group, and a cyclohexyl group.

5. The hydrogenated polymer composition according to claim 4, wherein R 1 and R 2 , R 3 , R 4 and R 5 , R 6 , R 7 , R 8 and R 9 , R 10 and R 11 , R 12 , and R 13 and R 14 are each independently an isopropyl group or an n-butyl group.

6. A resin composition comprising a vinyl alcohol polymer and the hydrogenated polymer composition according to any one of claims 3 to 5.

7. 7. The resin composition according to claim 6, wherein the vinyl alcohol polymer is an ethylene-vinyl alcohol copolymer.

Citation Information

Patent Citations

  • Reactive polymer

    JP1995025918A

  • Block copolymer and thermoplastic resin composition

    JP2006176788A

  • Curable resin composition

    JP2017137397A

  • Functionalized polymers and improved tires therefrom

    US20090326161A1

  • Polymer having terminal modified with borinic acid group, method for producing same, and rubber composition containing same

    WO2014088092A1