Non-calcined agglomerates, manufacturing method thereof, and ironmaking method using non-calcined agglomerates

A non-calcined agglomerate ore using an iron oxide-containing substance and urea bond-containing compound addresses strength and environmental issues in blast furnaces, achieving high strength, reduced CO2 emissions, and improved working conditions.

JP7584119B2Active Publication Date: 2024-11-15HOKKAIDO UNIVERSITY
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020132567
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-04
Publication Date
2024-11-15
Estimated Expiration
2040-08-04

AI Technical Summary

Technical Problem

Existing agglomerate ores used in blast furnaces face challenges in ensuring high strength, leading to difficulties in handling and ventilation, and contribute significantly to CO2 emissions due to the use of coal as a reducing agent, while also posing environmental hazards from dust generation.

Method used

The use of a non-calcined agglomerate ore composed of an iron oxide-containing substance and a urea bond-containing compound, which acts as both a binder and reducing agent, promoting a solid-phase reduction reaction and reducing coal usage.

Benefits of technology

The non-calcined agglomerate ore exhibits high strength, reduces CO2 emissions, suppresses dust generation, and improves working conditions by utilizing urea as a binder that is environmentally friendly and energy-efficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584119000003
    Figure 0007584119000003
  • Figure 0007584119000004
    Figure 0007584119000004
  • Figure 0007584119000005
    Figure 0007584119000005
Patent Text Reader

Abstract

To provide a non-fired agglomerated ore which exhibits high strength, suppresses use of coal and contributes to suppression of generation of CO2 and dust, and is excellent in work environment properties, a method for manufacturing the non-fired agglomerated ore, and an iron manufacturing method using the non-fired agglomerated ore.SOLUTION: A non-fired agglomerated ore contains an iron oxide-containing substance, and an urea bond-containing compound. A method for manufacturing a non-fired agglomerated ore includes: a mixing step of mixing a raw material composition containing an iron oxide-containing substance raw material and an urea bond-containing compound raw material, and obtaining a mixture; and a compression molding step of compressing the mixture and molding it into a lumpy shape.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-sintered agglomerate, a manufacturing method for the non-sintered agglomerate, and a method for making iron using the non-sintered agglomerate. [Background technology]

[0002] The mainstream of iron making methods is the iron making method using a blast furnace. In the iron making method using a blast furnace, lump ore is used as the iron source to be charged into the blast furnace, and agglomerated ore obtained by mixing iron ore powder as the main raw material with other auxiliary raw materials and calcining or not is used. The agglomerated ore is required to be easy to handle, i.e., easy to transport to the blast furnace, and to have a gap sufficient to ensure air flow in the blast furnace when it is piled alternately with coke, etc., in the blast furnace, i.e., to have high strength to withstand the above-mentioned pile-up.

[0003] For example, Patent Document 1 discloses a method for producing raw ore for a blast furnace, which includes sintered powder of 5 mm or less generated during the production of sintered ore, adding a binding material including at least an organic binder to the sintered powder, kneading the mixture, and forming the mixture into a shape. Thereafter, the material is subjected to a two-stage curing process, that is, a preliminary curing process and a steam curing process, to produce a non-sintered agglomerate ore.

[0004] Patent Document 2 discloses a method for producing sintered ore as a raw material for a blast furnace, which comprises adding a binder to a sintering raw material to make the sintering raw material into a lump and give it strength, granulating or molding the lump, and firing the lump. The method is characterized in that at least one of water-soluble phenolic resin, water glass, polyimide, polysiloxane, and colloidal silica is added as the binder in an amount of 2 to 12 parts by mass per 100 parts by mass of the sintering raw material, mixed and stirred with the sintering raw material, and then granulated or molded.

[0005] Furthermore, Patent Document 3 discloses an iron-making method in which iron-making raw materials and ammonia are supplied to a reactor and subjected to a reduction reaction to produce iron. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2009-030113 A [Patent Document 2] JP 2011-047006 A [Patent Document 3] JP 2011-179089 A Summary of the Invention [Problem to be solved by the invention]

[0007] In Patent Document 1, at least an organic binder is used, but it is considered difficult to ensure high strength when the organic binder is used. In Patent Document 2, at least one of water-soluble phenolic resin, water glass, polyimide, polysiloxane, and colloidal silica is used as the binder, but it is also considered difficult to ensure strength in this case.

[0008] Furthermore, although steelmaking technology using blast furnaces is considered to be efficient, there are problems such as a large amount of CO2 emissions, which is one of the causes of global warming, due to the use of a large amount of coal, and a shortage of the above-mentioned coal. Conventional agglomerates contain coal or a carbonaceous material made from coal as a reducing agent, but it is desired to reduce the use of the coal as much as possible. From the viewpoint of reducing the use of the carbonaceous material, the technology of Patent Document 3 has been proposed. However, from the viewpoint of the working environment, it is desired to consider other means.

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a non-sintered agglomerated ore which exhibits high strength, can reduce the use of coal, and as a result, contributes to the reduction of CO2 emissions and dust emissions, and is also excellent in working environment, a method for producing the non-sintered agglomerated ore, and a method for making iron using the non-sintered agglomerated ore. [Means for solving the problem]

[0010] A first embodiment of the present invention is a non-calcined agglomerate containing an iron oxide-containing material and a urea bond-containing compound that is solid at room temperature.

[0011] A second aspect of the present invention is the non-calcined agglomerate according to the first aspect, wherein the urea bond-containing compound is urea.

[0012] A third aspect of the present invention is the non-sintered agglomerate according to the first or second aspect, wherein the iron oxide-containing material is in a fragmentary form, and the equivalent circle diameter thereof is 1.0 mm or less.

[0013] A fourth aspect of the present invention is the non-sintered agglomerate according to any one of the first to third aspects, wherein the proportion of the urea bond-containing compound is 20 to 65 area % in terms of a proportion of the cross-sectional area of ​​the non-sintered agglomerate.

[0014] A fifth aspect of the present invention is the non-sintered agglomerate according to any one of the first to fourth aspects, wherein a mass ratio of the urea bond-containing compound to the iron oxide-containing substance is within a range of 1:1 to 1:24.

[0015] A sixth aspect of the present invention is the unsintered agglomerated ore according to any one of the first to fifth aspects, wherein in an EDS elemental mapping obtained by photographing an arbitrary observation field of 0.4 mm×0.5 mm of a cross section of the unsintered agglomerated ore with a scanning electron microscope at a magnification of 200 times, when an arbitrary measurement line of 0.4 mm or more is drawn, the measurement line has five or more points where the measurement line overlaps with the urea bond-containing compound.

[0016] A seventh aspect of the present invention is the non-sintered agglomerate according to any one of the first to sixth aspects, wherein the iron oxide-containing material has an Fe2O3 content of 50 mass % or more.

[0017] An eighth aspect of the present invention relates to the non-sintered agglomerate according to any one of the first to seventh aspects, wherein a ratio of voids to a cross-sectional area of ​​the non-sintered agglomerate is 5 area % or less.

[0018] A ninth aspect of the present invention is a method for producing a non-sintered agglomerate according to any one of the first to eighth aspects, A mixing step of mixing a raw material composition containing an iron oxide-containing material raw material and a urea bond-containing compound raw material to obtain a mixture; and A compression molding step of compressing the mixture into a block shape. The present invention relates to a method for producing a non-calcined agglomerate, comprising the steps of:

[0019] A tenth aspect of the present invention is the method for producing a non-sintered agglomerate according to the ninth aspect, wherein the compression molding step is performed at a pressure of 40 MPa or less.

[0020] An eleventh aspect of the present invention is the method for producing a non-sintered agglomerate according to the ninth or tenth aspect, wherein in the compression molding step, the compression is performed for 60 minutes or less.

[0021] A twelfth aspect of the present invention is the method for producing a non-sintered agglomerate according to any one of the ninth to eleventh aspects, wherein the mixture is heated after the mixing step and before completion of the compression molding step.

[0022] A thirteenth aspect of the present invention is the method for producing an agglomerate according to the twelfth aspect, wherein the heating temperature is 50°C or more and less than 120°C.

[0023] A fourteenth aspect of the present invention is the method for producing a non-sintered agglomerate according to the twelfth or thirteenth aspect, wherein in the compression molding step, the mixture is compressed while being heated.

[0024] A fifteenth aspect of the present invention is the method for producing a non-sintered agglomerate according to any one of the ninth to fourteenth aspects, wherein the raw iron oxide-containing material is a powder having an undersieve particle size of less than 1 mm.

[0025] A sixteenth aspect of the present invention is the method for producing a non-calcined agglomerate according to any one of the ninth to fifteenth aspects, wherein the urea bond-containing compound raw material is a powder having an undersieve particle size of less than 1 mm.

[0026] A seventeenth aspect of the present invention is a method for making iron using the non-sintered agglomerate ore according to any one of the first to eighth aspects. Effect of the Invention

[0027] According to the present invention, it is possible to provide a non-sintered agglomerate which exhibits high strength, reduces the use of coal, contributes to the suppression of CO2 and dust generation, and is excellent in working environment, a method for producing the non-sintered agglomerate, and a method for making iron using the non-sintered agglomerate. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a schematic diagram of a load measuring device used for measuring the crushing strength in the examples. [Diagram 2] FIG. 2 shows an SEM photograph and EDS (Energy Dispersive x-ray Spectroscopy) element mapping in the example. [Diagram 3] FIG. 3 is an EDS elemental mapping for evaluating the degree of dispersion of urea in the non-calcined agglomerates in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The present inventors have conducted extensive research to obtain a non-calcined agglomerate that has high strength, contributes to suppression of CO2 and dust generation by suppressing the use of coal, and is excellent in working environment. As a result, it has been found that if the non-calcined agglomerate contains a urea bond-containing compound that is solid at room temperature together with an iron oxide-containing substance, the urea bond-containing compound acts as a strong adhesive binder between the iron oxide-containing substances, thereby ensuring high strength, and further, that at the point where the iron oxide-containing substance and the urea bond-containing compound are in direct contact with each other, a solid-phase reaction process (reduction reaction) as described later in detail occurs between the iron oxide-containing substance and the urea bond-containing compound, thereby promoting the reduction of the iron oxide-containing substance. In addition to the suppression of CO2 and dust generation and the excellent working environment, the non-calcined agglomerate of the present invention can be expected to have an energy-saving effect by not calcining. The non-calcined agglomerate of the present invention, a manufacturing method for the non-calcined agglomerate, and an ironmaking method using the non-calcined agglomerate are described below.

[0030] First, the non-sintered agglomerates of the present invention will be described in terms of the urea bond-containing compound and the iron oxide-containing substance that constitute the non-sintered agglomerates.

[0031] (Urea bond-containing compounds contained in uncalcined agglomerates) The non-sintered agglomerated ore of the present invention contains a urea bond-containing compound that is solid at room temperature together with an iron oxide-containing substance. By containing a urea bond-containing compound that is solid at room temperature, the strength of the non-sintered agglomerated ore can be ensured. The urea bond-containing compound has an adhesive effect of binding iron oxide-containing substances, such as iron ore powder, to each other and agglomerating them into pellets, briquettes, etc. By binding them with the urea bond-containing compound in this way, the strength of the non-sintered agglomerated ore is increased, and the contact area between the urea bond-containing compound as a reducing agent and the iron oxide-containing substance is increased, thereby accelerating the reduction reaction. In other words, the urea bond-containing compound plays the role of both a binder and a reducing agent. In addition, since the urea bond-containing compound is solid at room temperature, the workability, including storage, transportation, etc., is good.

[0032] The urea bond-containing compound is represented by the chemical formula R1-NH-CO-NH-R2. The chemical formula has a urea bond (-NH-CO-NH-), and R1 and R2 bonded to the NH group are hydrogen or a chain hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 5 carbon atoms, or an aromatic hydrocarbon group having 6 to 9 carbon atoms, and R1 and R2 may be the same or different. The chain hydrocarbon group includes a linear or branched saturated or unsaturated alkyl group. For example, the urea bond-containing compound includes urea, methylurea, ethylurea, butylurea, pentylurea (N-amylurea), dimethylurea, diethylurea, phenylurea, tolylurea, etc.

[0033] The urea bond-containing compound is preferably urea. Urea ((NH2)2CO) is a compound that contributes sufficiently to the reduction of iron oxide. For example, when the iron oxide is Fe2O3, the reactions of the following formulas (1) to (3) may occur. These reactions are solid-phase reaction processes that occur at higher temperatures in the order of (1), (2), and (3). 9Fe2O3+CH4N2O=6Fe3O4+CO2+2H2O+N2...(1) 3Fe2O3+CH4N2O=6FeO+CO2+2H2O+N2...(2) Fe2O3+CH4N2O=2Fe+CO2+2H2O+N2...(3)

[0034] Urea is a white powder at room temperature, but softens when heated. As it softens, urea is more likely to exhibit its binding properties, and it fully exerts its adhesive effect of binding iron oxide-containing materials, such as iron ore powder, to each other and agglomerating them into pellets, briquettes, etc. By binding with urea in this way, the strength of the non-sintered agglomerates is increased, and the contact area between urea as a reducing agent and the iron oxide-containing materials is sufficiently increased, accelerating the reduction reaction as described above.

[0035] In addition, urea is synthesized from ammonia and CO2, and consumes CO2 during the manufacturing process, which means that unlike the aforementioned cement, it contributes to reducing CO2 emissions, including the preparation of raw materials. It is also harmless to the human body, odorless, and solid at room temperature, making it highly easy to work with.

[0036] Furthermore, urea contains 4 / 60 = approximately 6% by mass of hydrogen, and when heated it decomposes (CH4N2O = 2H2(g) + CO(g) + N2(g)) to generate hydrogen and CO gas. Because hydrogen and CO are both reducing gases and combustible gases, urea can be considered a solid hydrogen reduction material or solid hydrogen fuel. Also, while cement causes an increase in the amount of slag, urea has the advantage that the amount of slag does not increase at all because it decomposes into gas when heated.

[0037] Furthermore, urea is a substance excreted in large quantities by living organisms on Earth, making it an abundant resource. If this urea could be reused as an excreted substance, it would be possible to supply non-calcined agglomerates at low cost.

[0038] From the above, by preferably using urea as the urea bond-containing compound, it is possible to increase the strength of the agglomerated ore without calcining, to suppress the generation of CO2 and dust by reducing the use of coal, and to save energy by not calcining, and it is also possible to contribute to the establishment of an agglomerated ore manufacturing technology that is inexpensive and does not increase the amount of slag.

[0039] The form of the urea bond-containing compound in the non-sintered agglomerates of the present invention is not particularly limited, but from the viewpoint of achieving the above-mentioned high strength and accelerating the solid-phase reaction process by bonding it to the iron oxide-containing material, it is preferable that the urea bond-containing compound is present, for example, surrounding the fragmentary iron oxide-containing material when the cross section of the non-sintered agglomerates is observed under a microscope, as shown in the examples described later. Furthermore, when observed by EDS, the proportion of the urea bond-containing compound in the cross section of the non-sintered agglomerates is preferably 20 area % or more, more preferably 30 area % or more, even more preferably 35 area % or more, and even more preferably 40 area % or more. On the other hand, from the viewpoint of ensuring high strength and supplying more iron oxide-containing material to the blast furnace, the proportion of the urea bond-containing compound in the observation field is preferably 65 area % or less, more preferably 60 area % or less.

[0040] (Iron oxide-containing substances contained in unburned agglomerates) The iron oxide-containing material may be any material that contains iron oxide. From the viewpoint of increasing the contact area with the urea bond-containing compound, increasing the strength, and promoting the reduction reaction, the iron oxide-containing material is preferably in a fragmentary shape. Examples of the fragmentary shape include spherical, elliptical, needle-like, and polygonal shapes.

[0041] For example, when a cross section of the non-sintered agglomerate is observed under a microscope as shown in the Examples below, the circle-equivalent particle size of the iron oxide-containing material within the observation field is preferably 1.0 mm or less, more preferably 0.5 mm or less, even more preferably 0.3 mm or less, still more preferably 0.1 mm (100 μm) or less, and particularly preferably 80 μm or less. The lower limit of the average particle size of the iron oxide-containing material can be, for example, 1 μm.

[0042] The iron oxide-containing material constituting the non-sintered agglomerate of the present invention may be, for example, mainly composed of Fe2O3, i.e., the content of Fe2O3 may be 50 mass% or more, or even 60 mass% or more. Alternatively, the iron oxide-containing material constituting the non-sintered agglomerate of the present invention may be mainly composed of Fe3O4 or FeO, i.e., the content of Fe3O4 may be 50 mass% or more, or the content of FeO may be 50 mass% or more. For example, in the case of iron ore, in addition to the iron oxide, oxides such as Al2O3 and SiO2 may be contained.

[0043] The mass ratio of the urea bond-containing compound to the iron oxide-containing material is preferably within a range of 1:1 to 1:24. By setting the mass ratio of the urea bond-containing compound to the iron oxide-containing material to 1:24 or less, the reduction of iron oxide in the iron oxide-containing material can be promoted, which is preferable. In addition, the adhesive effect between the iron oxide-containing material and the urea bond-containing compound is enhanced, which contributes to achieving high strength. The mass ratio is more preferably 1:20 or less, even more preferably 1:10 or less, and even more preferably 1:5 or less. On the other hand, from the viewpoint of ensuring high strength and increasing the ratio of iron oxide in the non-sintered agglomerates, the mass ratio is preferably 1:1 or more. For example, the mass ratio of the urea bond-containing compound to the iron oxide-containing material may be 3:8 (=1:2.67).

[0044] In the EDS element mapping obtained by photographing an arbitrary observation field of 0.4 mm × 0.5 mm of the cross section of the non-sintered agglomerate at a magnification of 200 times using a scanning electron microscope, when a measurement line of 0.4 mm or more is arbitrarily drawn, it is preferable that there are 5 or more points where the measurement line overlaps with the urea bond-containing compound. The more points where the measurement line overlaps with the urea bond-containing compound, the more sufficiently dispersed the urea bond-containing compound is. If the urea bond-containing compound is sufficiently dispersed, the contact volume between the fragmentary iron oxide-containing material and the urea bond-containing compound increases, the adhesive action increases, contributing to high strength, and the reduction reaction between the iron oxide-containing material and the urea bond-containing compound is promoted, which is preferable. The number of points where the measurement line overlaps with the urea bond-containing compound is preferably 7 or more, more preferably 10 or more.

[0045] (Other components contained in unfired agglomerates) The non-sintered agglomerates of the present invention may contain the iron oxide-containing material and the urea bond-containing compound. In addition to the case where the non-sintered agglomerates of the present invention are composed of the iron oxide-containing material and the urea bond-containing compound, the non-sintered agglomerates of the present invention may further contain small amounts of other components for the purpose of further improving the strength and improving the reducibility without impairing the object of the present invention. Examples of other components include cement (main component 2CaO SiO2) such as Portland cement, alumina cement, and blast furnace cement, carbonizing agents such as coke powder, general coal, anthracite, and coke dust, other inorganic binders, and organic binders.

[0046] The use of the cement makes it easy to produce pellets, briquettes, etc., without firing, but if the cement is used in a large amount, there are problems such as a decrease in iron quality and an increase in the amount of slag. In addition, since the production of cement itself requires a lot of energy, it is difficult to say that the production process of cement is energy-saving. Therefore, from the viewpoint of suppressing the increase in slag and achieving energy saving, it is preferable to suppress the amount of cement as much as possible, and from the viewpoint of preventing the increase in slag and realizing energy saving, it is preferable that the amount of cement is zero.

[0047] The proportion of other components including the cement is preferably 10 area % or less, more preferably 5 area % or less, and particularly preferably 0 area %, in terms of the proportion of the whole of the non-sintered agglomerates, when a cross section of the non-sintered agglomerates is observed under a microscope as shown in the Examples described later. In other words, the proportion of other components is not included.

[0048] If the non-sintered agglomerate of the present invention is made of an iron oxide-containing material and a urea bond-containing compound, it will exhibit sufficiently high strength, the reduction reaction between the iron oxide-containing material and the urea bond-containing compound will be easily promoted, and since it will become gaseous even if it is thermally decomposed by heating, the amount of slag will not increase at all, and furthermore, it will contribute to reducing CO2 and dust by reducing the use of coal. Furthermore, such a beneficial non-sintered agglomerate can be provided at low cost and with reduced energy consumption.

[0049] The non-sintered agglomerate ore of the present invention may be any suitable one as long as it contains the iron oxide-containing material and the urea bond-containing compound as described above, and other conditions are not important.

[0050] For example, the size of the non-sintered agglomerates may be 9 to 30 mm, or even 15 to 30 mm in diameter when a true sphere equivalent to the volume of the agglomerates is simulated. The shape of the agglomerates may be pellets, briquettes, or the like.

[0051] The non-sintered agglomerates of the present invention may have voids. However, from the viewpoint of increasing the crushing strength and from the viewpoint of adhering the iron oxide-containing material and the urea bond-containing compound to promote the reduction reaction, it is preferable that the voids in the non-sintered agglomerates are small, and when observed by SEM photographs or EDS element mapping as described below, the voids are preferably suppressed to, for example, 5 area % or less, more preferably 3 area % or less, and most preferably 0 area %.

[0052] The agglomerate ore of the present invention can ensure a crushing strength of 600N or more at room temperature when the crushing strength is measured by the method described in the Examples below, and further exhibits a strength of 800N or more, further 900N or more, particularly 1000N or more, which is sufficiently applicable for practical use.

[0053] (Method of manufacturing non-calcined agglomerates) The method for producing non-sintered agglomerates of the present invention comprises the steps of: A mixing step of mixing a raw material composition containing a urea bond-containing compound raw material and an iron oxide-containing substance raw material to obtain a mixture; and A compression molding step of compressing the mixture into a block shape. Each step will be described below.

[0054] 1.Raw materials First, a raw material composition containing a raw material of a urea bond-containing compound and a raw material of an iron oxide-containing substance is prepared. Each raw material contained in the raw material composition is described below.

[0055] (Urea bond-containing compound raw material) The raw material of the urea bond-containing compound can be synthesized from ammonia and CO2 at 120°C, in addition to using commercially available products. In this case, CO2 can be consumed during the production of the urea bond-containing compound, which is effective from the viewpoint of reducing CO2. In addition, the waste of living organisms can be recycled and used. The purity of the urea bond-containing compound in the raw material of the urea bond-containing compound is preferably 90% or more, and more preferably 95% or more.

[0056] The urea bond-containing compound raw material is preferably a powder having a sieve particle size of less than 1 mm. The sieve particle size can be, for example, less than 500 μm, and can be even less than 250 μm. The urea bond-containing compound powder has a smaller strength than the iron oxide-containing material powder, and is crushed or melted during the compression process, dispersing around the iron oxide-containing material powder, so it does not need to be strictly controlled. The ratio of particle sizes of the iron oxide-containing material powder and the urea bond-containing compound powder is not particularly important, and for example, the sieve particle size of the urea bond-containing compound powder can be the same as or smaller than the sieve particle size of the iron oxide-containing material powder.

[0057] The content of the urea bond-containing compound raw material in the raw material composition is, for example, preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 50% by mass or less, more preferably 30% by mass or less.

[0058] (iron oxide-containing raw material) The iron oxide-containing raw material may be, for example, a raw material containing Fe2O3 as the main component. Alternatively, the iron oxide-containing raw material may be an iron oxide-containing raw material such as iron ore, which is mainly composed of Fe3O4 or FeO, i.e., in which Fe3O4 or FeO accounts for 50 mass% or more. The iron oxide-containing raw material may be iron ore, iron sand, dust, sludge, ironmaking waste, etc., which are generated in large quantities in the ironmaking process. For example, an iron ore containing 50 mass% or more of Fe2O3 may be riodocose iron ore.

[0059] The iron oxide-containing raw material may be in the form of a lump having an average particle size of, for example, about 1 to 3 mm, but is preferably in the form of a powder having a sieve size of less than 1 mm, more preferably less than 500 μm, and even more preferably less than 250 μm.

[0060] The proportion of the iron oxide-containing raw material in the raw material composition is, for example, preferably 50 mass % or more, more preferably 70 mass % or more, and preferably 96 mass % or less, more preferably 90 mass % or less.

[0061] (Other ingredients) The raw material composition may contain other component raw materials in addition to the urea bond-containing compound raw material and the iron oxide-containing substance raw material. Examples of other component raw materials include the above-mentioned cements such as portland cement, alumina cement, and blast furnace cement, carbon materials such as coke powder, general coal, anthracite, and coke dust, and other inorganic and organic binders. The proportion of these other component raw materials in the raw material composition is preferably controlled to, for example, 10% by mass or less, more preferably 5% by mass or less, even more preferably 3% by mass or less, and particularly 0% by mass.

[0062] The method for producing non-sintered agglomerates of the present invention may include a step of crushing the raw material to have the above-mentioned preferred particle size or a step of sieving the raw material before mixing with other raw materials.

[0063] 2. Manufacturing process The raw materials are weighed and mixed to obtain a mixture. The mixing may be performed using a mixer or a ball mill such as a tumbling ball mill or a planetary ball mill. The mixture obtained by mixing is charged into a compressor and compressed to obtain an agglomerate. In the step of compressing the mixture, it is preferable to compress the mixture at a pressure of 100 MPa or less. From the viewpoint of increasing the adhesive force between the urea bond-containing compound raw material and the iron oxide-containing material raw material to ensure strength, the pressure is more preferably 20 MPa or more. The higher the pressure, the more preferable it is, but if the pressure is too high, the effect of increasing the adhesive force is saturated, so the pressure is more preferably 40 MPa or less as described above. The atmosphere in both the raw material mixing step and the mixture compression step was air.

[0064] The compression is preferably performed for 5 minutes or more to obtain non-sintered agglomerates having sufficient strength. The compression time is more preferably 10 minutes or more. On the other hand, if the compression time is too long, the effect of compression is saturated and productivity is reduced. Therefore, the compression time is preferably 60 minutes or less, more preferably 30 minutes or less. The compression may be performed by a method of compressing and molding from above as shown in the examples described later, or by a method of compressing and molding from both sides using two rolls as in a briquette manufacturing device. Also, a method of compressing and molding by extrusion molding may be used.

[0065] The non-sintered agglomerate of the present invention can be produced by performing the compression without heating after the mixing step. However, from the viewpoint of promoting the adhesive effect of the urea bond-containing compound and obtaining stronger non-sintered agglomerate, it is preferable to perform heating after the mixing step and before the end of the compression molding step.

[0066] As an embodiment of the heating, for example, (a) A method in which, after the step of obtaining the mixture, the temperature is raised before compression, and the mixture is compressed while being maintained at the following preferred temperature: (b) A method in which, after the step of obtaining the mixture, the mixture is heated at the following preferred temperatures before compression, and compression is performed immediately after the heating is terminated. (c) A method in which, after the step of obtaining the mixture, the mixture is heated to the following preferred temperature before compression, and compressed while maintaining the temperature: Preferably, in the step of compressing the mixture as in (a) or (c), the mixture is compressed while being heated.

[0067] The temperature of the mixture is preferably 50°C or higher and lower than 120°C by the heating. By setting the temperature at 50°C or higher, the adhesion promoting effect of the urea bond-containing compound described above can be sufficiently obtained. The heating temperature is more preferably 60°C or higher, and even more preferably 70°C or higher. On the other hand, if the temperature is too high, the urea bond-containing compound is easily decomposed, making it difficult to exert the effect of the urea bond-containing compound. Therefore, when heating is performed, the temperature of the mixture is preferably lower than 120°C, more preferably 100°C or lower, and even more preferably 80°C or lower.

[0068] The time for holding at the above temperature is preferably 5 minutes or more in order to obtain non-sintered agglomerates with sufficient strength. The time for holding at the above temperature is more preferably 10 minutes or more. On the other hand, if the heating time is too long, the effect of heating is saturated and productivity decreases. Therefore, the time for holding at the above temperature is preferably 60 minutes or less, more preferably 30 minutes or less. When the heating is performed together with compression, the time for holding at the above temperature can be the same as the compression time.

[0069] (Ironmaking method using unburned agglomerates) The present invention also includes an ironmaking method using the non-calcined agglomerates of the present invention. When the non-calcined agglomerates of the present invention are applied to a blast furnace process as an ironmaking method, the high strength of the non-calcined agglomerates allows the shape of the agglomerates to be maintained during transportation from the non-calcined agglomerates of the present invention manufacturing site to the blast furnace and during deposition in the blast furnace, thereby improving the ventilation of reducing gases and the like in the blast furnace and promoting the reduction reaction. In addition, the non-calcined agglomerates of the present invention are heated in the blast furnace to promote the reduction reaction between the iron oxide-containing material in the non-calcined agglomerates and the urea bond-containing compound, particularly the reduction reaction by urea as shown in the above formulas (1) to (3). As a result, energy saving, resource saving by suppressing the use of coal raw materials, and reduction in CO2 and dust generation can be achieved. EXAMPLES

[0070] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, and all such modifications are included in the technical scope of the present invention.

[0071] 1. Sample Preparation Raw iron ore (iron ore mainly composed of Fe2O3) with the composition shown in Table 1 was crushed and sieved to obtain iron ore powder with a particle size of less than 106 μm. Urea manufactured by Kishida Chemical Co., Ltd. was also crushed and sieved to obtain urea powder with a particle size of less than 106 μm.

[0072] The iron ore powder and the urea powder were weighed out so as to have a mass ratio of 8:3 (the ratio of urea in the entire composition was 27.3 mass%), and the iron ore powder and the urea powder were mixed in a rolling ball mill at a rotation speed of 100 rpm for 1 hour to obtain a mixture. The mass ratio was determined from the stoichiometric ratio of the following formula (4), in the expectation of reduction to Fe. Fe2O3+CH4N2O=2Fe+N2(g)+2H2O(g)+2(g)...(4)

[0073] The mixture was filled into a die, and powder compaction was performed as follows. FIG. 1 is a schematic diagram of a uniaxial press used for powder compaction of the mixture. 3 g of the mixture was weighed and filled into a space formed by a die 2 and a support stand 3 of a uniaxial press 1, and after an upper punch 4 was attached, it was moved toward the filling (mixture) 5 and pressurized. In this embodiment, the temperature of the filling 5 was raised to 50°C or 80°C under a pressure of 40 MPa, and was maintained for 30 minutes. After a certain time had elapsed, the pressure was stopped, and the heating was immediately terminated. After the heating, the mixture was cooled to obtain a cylindrical powder compact with a height of about 1.3 to 1.5 cm and a diameter of about 10 mm as an agglomerate. In this embodiment, the temperature near the filling was controlled, and the set temperature of the device was almost the temperature of the mixture.

[0074] [Table 1]

[0075] Using the obtained powder compact, the cross section was observed and the crushing strength was measured as follows.

[0076] (Cross-section observation) For each of the green compacts obtained by compressing at 50°C and 80°C, the cylindrical green compacts were cut at approximately the diameter position in the pressure direction, i.e., in the height direction, and the center of the cut surface was observed by SEM-EDS. The photographs are shown in Figure 2. The upper part of Figure 2 shows the SEM photograph, and the lower part of Figure 2 shows the EDS element mapping. In the EDS element mapping, the dark gray part indicates the presence of C (carbon) that constitutes urea, the light gray part indicates the presence of Fe that constitutes iron ore, and the black part indicates other than the urea and iron ore. In Figure 2, the brightness of the SEM photographs at 50°C and 80°C is different, but this is due to automatic brightness adjustment during measurement.

[0077] (Measurement of crushing strength) The crushing strength was measured using a load measuring device (MINEBEA model LTS-1kNB-S50, specifications: maximum test force 1kN, test speed 5mm / min, speed accuracy: ±3% of set speed) and a compression test was performed in which the load was gradually increased from the top of the cylindrical sample until it reached 1000N at room temperature in an air atmosphere, and the load at which one of the above-mentioned green compacts was crushed was calculated as the "maximum load". The results are shown in Table 2. Note that since the maximum load of the load measuring device is 1000N, examples where the value is almost 1000N mean that the sample did not crush even at 1000N. Note that when a similar measurement was performed on industrial sintered ore as a conventional product, it was crushed at 835.7N.

[0078] [Table 2]

[0079] From the above-mentioned crushing strength measurement results, the agglomerates of the present invention are easy to handle, and even after being charged into a blast furnace, a green compact that can sufficiently ensure ventilation in the blast furnace can be obtained. In addition, since the non-sintered agglomerates of the present invention do not use ammonia, they are also excellent in terms of working environment.

[0080] Moreover, from the photograph of Fig. 2, it can be seen that in the non-sintered agglomerates of the present invention, urea surrounds the finely dispersed iron ore powder. Furthermore, Fig. 3 shows EDS element mapping of the green compact obtained by compressing at 80°C in Fig. 2. As shown in Fig. 3, when the non-sintered agglomerates of the present invention are photographed at a magnification of 200 times in a cross-sectional observation field of 0.4 mm x 0.5 mm, even when a measurement line of about 0.4 mm is drawn in an area with relatively little urea, the measurement line overlaps with the urea bond-containing compound at seven points, and urea is sufficiently dispersed in the iron ore powder.

[0081] In the present invention, it is believed that the high strength was obtained because urea acts as a binder to bond the iron ore powder. Also, it is believed that the presence of urea adjacent to the iron ore powder promotes the reduction of the iron ore in the blast furnace. In addition, in this embodiment, only urea is used in addition to the iron oxide-containing material, and the urea is thermally decomposed by heating to become gaseous, so the amount of slag does not increase at all. [Explanation of symbols]

[0082] 1. Uniaxial press device 2 Dice 3 Support stand 4 Upper punch 5 Filling (mixture)

Claims

1. An unsintered agglomerate ore comprising an iron oxide-containing substance and a urea bond-containing compound which is solid at room temperature and has the chemical formula R 1 -NH-CO-NH-R 2 (R 1 and R 2 bonded to the NH group are hydrogen, a chain hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 5 carbon atoms, or an aromatic hydrocarbon group having 6 to 9 carbon atoms, and R 1 and R 2 may be the same or different), and the mass ratio of the urea bond-containing compound to the iron oxide-containing substance is within the range of 1:1 to 1:

24.

2. 2. The non-calcined agglomerate according to claim 1, wherein the urea bond-containing compound is urea.

3. 3. The non-sintered agglomerate according to claim 1, wherein the iron oxide-containing material is in the form of fragments, and the equivalent circle diameter of the fragments is 1.0 mm or less.

4. The non-sintered agglomerates according to any one of claims 1 to 3, wherein a ratio of the urea bond-containing compound to a cross-sectional area of ​​the non-sintered agglomerates is 20 to 65 area %.

5. The non-sintered agglomerate according to any one of claims 1 to 4, wherein in an EDS element mapping obtained by photographing an arbitrary observation field of 0.4 mm × 0.5 mm of a cross section of the non-sintered agglomerate at a magnification of 200 times using a scanning electron microscope, when a measurement line of 0.4 mm or more is arbitrarily drawn, there are five or more points where the measurement line overlaps with the urea bond-containing compound.

6. The iron oxide-containing material is Fe 2 O 3 The non-sintered agglomerate according to any one of claims 1 to 5, wherein the content of is 50 mass% or more.

7. The non-sintered agglomerate according to any one of claims 1 to 6, wherein a ratio of voids to a cross-sectional area of ​​the non-sintered agglomerate is 5 area % or less.

8. The method for producing non-sintered agglomerates according to any one of claims 1 to 7, a mixing step of mixing a raw material composition containing an iron oxide-containing material raw material containing an iron oxide-containing substance and a urea bond-containing compound raw material containing a urea bond-containing compound represented by the chemical formula: R 1 -NH-CO-NH-R 2 (R 1 and R 2 bonded to the NH group are hydrogen, a chain hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 5 carbon atoms, or an aromatic hydrocarbon group having 6 to 9 carbon atoms, and R 1 and R 2 may be the same or different), so that the mass ratio of the urea bond-containing compound to the iron oxide-containing substance is within the range of 1:1 to 1:24 to obtain a mixture; A compression molding step of compressing the mixture into a block shape. A method for producing non-calcined agglomerates comprising the steps of:

9. The method for producing non-sintered agglomerates according to claim 8, wherein the compression molding step is performed at a pressure of 40 MPa or less.

10. The method for producing non-sintered agglomerates according to claim 8 or 9, wherein in the compression molding step, the compression is performed for 60 minutes or less.

11. The method for producing non-sintered agglomerates according to any one of claims 8 to 10, wherein the mixture is heated after the mixing step and before completion of the compression molding step.

12. The method for producing non-sintered agglomerates according to claim 11, wherein the heating temperature is 50°C or more and less than 120°C.

13. The method for producing non-sintered agglomerates according to claim 11 or 12, wherein in the compression molding step, the mixture is compressed while being heated.

14. The method for producing non-sintered agglomerates according to any one of claims 8 to 13, wherein the raw iron oxide-containing material is a powder having an undersieve particle size of less than 1 mm.

15. The method for producing non-sintered agglomerates according to any one of claims 8 to 14, wherein the urea bond-containing compound raw material is a powder having an undersieve particle size of less than 1 mm.

16. A method for making iron using the non-sintered agglomerate ore according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Cold-pressing forming method

    CN104263918A

  • Cold-pressing forming adhesive

    CN104263919A

  • JP1977115601U

  • Method for binding granular iron recovered from slag

    JP1987020835A

  • Method for briquetting granular metal

    JP1991006334A