Ferritic stainless steel plates and welded structures
The high Al-based ferritic stainless steel plate with specific Al and Cr content and bead width ratio addresses the challenge of poor weld penetration, achieving improved weld penetration and joint strength for high-temperature applications.
Patent Information
- Application Number
- JP2020062545
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Conventional techniques have not effectively improved the weld penetration of high Al-containing stainless steel, particularly in applications requiring excellent oxidation resistance and corrosion resistance, such as heating equipment and exhaust system members.
A high Al-based ferritic stainless steel plate with specific chemical compositions and a welded structure, where the Al and Cr content satisfy the relationship Al≧0.024Cr^2 -1.444, and a bead width ratio (W1/W2) of 0.6 to 1.0, ensuring improved weld penetration and joint strength.
The solution provides ferritic stainless steel sheets and welded structures with enhanced weld penetration and joint strength, suitable for high-temperature members like heating equipment and exhaust system members, while maintaining excellent corrosion resistance and oxidation resistance.
Smart Images

Figure 0007584230000001 
Figure 0007584230000002 
Figure 0007584230000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic stainless steel sheet and welded structure having excellent weld penetration properties and suitable for use in combustion appliance members and high-temperature components such as heating appliances and kitchen appliances, and exhaust system members for automobiles, motorcycles, and the like. [Background technology]
[0002] Ferritic stainless steels are used in a wide range of fields, including home appliances, electronic devices, automobiles, etc. In particular, stainless steels used in fields where materials are exposed to high temperatures, such as heating equipment, kitchen equipment, and the automobile industry, are required to have oxidation resistance and corrosion resistance.
[0003] The oxidation resistance of stainless steels is improved by adding large amounts of Cr, Si, and Al, but the addition of large amounts of these elements leads to a decrease in weld penetration.
[0004] To deepen the penetration of the weld, it is important that the surface tension of the weld metal at the center of the bead in the width direction is higher than the surface tension at the ends of the bead in the width direction. When the surface tension of the weld metal at the center of the bead in the width direction is high, the convection of the weld metal flows from the outside to the inside in the bead in the width direction, and at the center of the weld metal in the width direction, the convection of the weld metal that collides flows in the depth direction, deepening the penetration of the weld. This results in a sound weld.
[0005] O (oxygen) and S (sulfur) are known to be elements that increase the surface tension at the center of the weld metal bead width direction. O has a particularly large effect. On the other hand, Cr, Al, Si, Ti, etc., which tend to form slag on the weld metal surface, form oxides with O, lowering the O concentration in the weld metal and reducing the penetration depth of the weld. Cr and Al in particular are very susceptible to forming slag, so stainless steels containing Al tend to have poor weld penetration.
[0006] Patent Document 1 describes a steel sheet containing, by mass%, C: 0.001-0.020%, Si: 0.01-4.00%, Mn: 0.01-3.00%, P: 0.010-0.040%, S: 0.0001-0.0100%, Cr: 10.0-15.0%, N: 0.001-0.020%, Al: 0.50-10.0%, and further containing at least one of Ti: 0.05-0.40% and Nb: 0.05-0.40%, with the balance being Fe and unavoidable impurities, with Cr / (Si+Al) being 10.0 or less, and a specific gravity of 7.6 g / cm. 3 A low-density ferritic stainless steel sheet characterized by the following is disclosed. Although stainless steel with a low specific gravity due to the addition of Al and Si is mentioned, there is no mention of weld penetration.
[0007] Patent Document 2 describes a steel containing, by mass%, C: 0.001-0.100%, Si: 0.01-5.00%, Mn: 0.01-2.00%, P: 0.050% or less, S: 0.0100% or less, Cr: 9.0-25.0%, Ti: 0.001-1.00%, Al: 0.001-5.000%, N: 0.001-0.050%, and further, Ni: 0-1.00%, Mo: 0-3.00%, Sn: 0-1.000%, Cu: 0-2.00%, B: 0-0.0050%, Nb: 0-0.500%, W: 0-1.000%, V: 0-0.500%, Sb: 0-0.100%, Co: 0-0.500%, %, Ca: 0-0.0050%, Mg: 0-0.0050%, Zr: 0-0.0300%, Ga: 0-0.0100%, Ta: 0-0.050%, REM: 0-0.100%, with the balance being Fe and impurities, there is a passive film on the steel surface, and in a region from the steel surface to a depth of 5 nm (but not exceeding the thickness of the passive film), the total of Al and Si is 1.0 atomic % or more, Cr is 10.0 atomic % or more, and Fe is 85.0 atomic % or less in cationic fractions. The passive film of stainless steel with added Al and Si is specified, but there is no mention of weld penetration.
[0008] Patent Document 3 discloses an Al-containing heat-resistant ferritic stainless steel sheet having excellent workability and oxidation resistance, which contains, by mass%, C: 0.002-0.02%, N: 0.02% or less, Si: 0.05-1.0%, Mn: 3.0% or less, P: 0.04% or less, S: 0.02% or less, Cr: 10-25%, Al: less than 1.0-3.0%, Ti: 3×(C+N)-20×(C+N)%, the balance being Fe and unavoidable impurities, and has an oxide film on its surface with an Al content of 15% or more and a thickness of 0.03-0.5 μm. Although the oxidation resistance is improved by increasing the Al content, the steels examined are mainly 18Cr and high Cr stainless steels. In addition, no reference is made to weld penetration.
[0009] Patent Document 4 describes a steel sheet containing, in mass %, C: 0.001-0.015%, N: 0.002-0.02%, C+N: 0.003-0.02%, Si: 0.3-0.8%, Mn: 1.0% or less, P: 0.04% or less, S: 0.02% or less, Cr: 13-20%, Al: 1.5-less than 2.5%, Cu: 0.5% or less, Ti: 3×(C+N)-20×(C+N)%, and the remainder being Fe and An Al-containing heat-resistant ferritic stainless steel sheet with excellent workability and oxidation resistance is disclosed, which is characterized in that it is made of unavoidable impurities, has a grain size number of 7 to 10 in its microstructure, and has the minimum elongation Elmin [%] in the directions at 0°, 45°, and 90° to the rolling direction and the minimum r-value rmin satisfying Elmin≧25% and rmin≧1.0, respectively. The grain size number and r-value are specified, but no reference is made to weld penetration.
[0010] Patent Document 5 discloses a high Al-containing ferritic stainless steel with excellent high-temperature oxidation resistance and manufacturability, characterized by a composition consisting of, in weight percent, C: 0.10% or less, Si: 0.3 to 1.5%, Mn: 1.0% or less, P: 0.04% or less, S: 0.003% or less, Cr: 13.0 to 25.0%, Ni: 0.60% or less, Al: 2.0 to 5.0%, N: 0.10% or less, B: 0.002 to 0.02%, and the balance being Fe and unavoidable impurities. Although the oxidation resistance is improved by increasing the Al content, the steels examined are mainly high Cr stainless steels with 18 to 20 Cr. In addition, no mention is made of weld penetration. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2018-168457 A [Patent Document 2] JP 2019-178364 A [Patent Document 3] Patent No. 4986975 [Patent Document 4] Patent No. 4236503 [Patent Document 5] Japanese Patent Application Publication No. 10-158791 Summary of the Invention [Problem to be solved by the invention]
[0012] As described above, the conventional techniques have not been able to improve the weld penetration of high Al-content stainless steels.
[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a high-Al ferritic stainless steel sheet and welded structure having improved weld penetration properties. [Means for solving the problem]
[0014] The means for solving the above problems has the following configuration. [1] In weight percent: C: 0.001 to 0.100%, Si: 0.01 to 2.00%, Mn: 0.01 to 2.00%, P:≦0.050%, S:≦0.0100%, Ni: 0.01 to 3.00%, Cr: 9.5-15.0%, Al: 1.0-5.0%, B: 0.0001~0.0100%, O: 0.0001 to 0.0100%, N: Contains 0.001 to 0.050% The ferritic stainless steel sheet further contains one or two of Ti: 0.01-1.00% and Nb: 0.001-1.00%, with the balance being Fe and impurities, and is characterized in that it satisfies the following formula (1): [Al]≧0.024[Cr] 2 -1.444 …(1) In the formula (1), [Al] and [Cr] are the mass percentages of the respective elements. [2] By weight, C: 0.001 to 0.100%, Si: 0.01 to 2.00%, Mn: 0.01 to 2.00%, P:≦0.050%, S:≦0.0100%, Ni: 0.01 to 3.00%, Cr: 9.0-15.0%, Al: 1.0-5.0%, B: 0.0001~0.0030%, O: 0.0001 to 0.0100%, N: Contains 0.001 to 0.050% Further, it contains one or both of Ti: 0.01 to 1.00% and Nb: 0.001 to 1.00%, Furthermore, Mo: 0.01 to 3.00%, Sn: 0.001 to 3.00%, Cu: 0.01~0.44 %, W: 0.001 to 1.00%, V: 0.001 to 1.00%, Sb: 0.001 to 0.100%, Co: 0.001 to 0.500%, Ca: 0.0001 to 0.0050%, Mg: 0.0001 to 0.0050%, Zr: 0.0001 to 0.0300%, Ga: 0.0001 to 0.0100%, Ta: 0.001 to 0.050%, REM: Contains 0.001 to 0.100% of one or more types, A ferritic stainless steel sheet, the balance of which is Fe and impurities, which satisfies the following formula (1): [Al]≧0.024[Cr] 2 -1.444 …(1) In the formula (1), [Al] and [Cr] are the mass percentages of the respective elements. [3] A method for manufacturing a steel sheet having a ferritic stainless steel plate according to the above [1] or [2], and a weld formed at a joint between the base materials, A welded structure, wherein a ratio (W1 / W2) of a weld bead width W1 on a back side of the weld to a weld bead width W2 on a front side of the weld is 0.6 or more and 1.0 or less. Effect of the Invention
[0015] According to the present invention, it is possible to provide a high-Al ferritic stainless steel sheet and welded structure with improved weld penetration. In particular, it is possible to provide a ferritic stainless steel sheet and welded structure with excellent weld penetration suitable for combustion equipment members or high-temperature members such as heating equipment and kitchen equipment, and exhaust system members for automobiles, motorcycles, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present inventors have conducted extensive research with the aim of providing an Al-containing ferritic stainless steel sheet with improved weld penetration, and as a result have discovered the following two points.
[0017] First, in stainless steels with a relatively low Cr content of 9-15%, the O (oxygen) concentration in the weld metal decreases with increasing Al content when the Al content is less than 0.5%, but when the Al content is 0.5% or more, the O concentration in the weld metal increases. In particular, the lower the Cr content of the steel, the better the weld penetration with a small Al content, and further, when [Al] ≥ 0.024 [Cr] 2 It was discovered that by satisfying the relationship of -1.444 ([Al] and [Cr] indicate the mass percentage concentrations of each element), weld penetration equal to or better than that of non-Al-containing stainless steel (Al content 0.01% or less) can be obtained.
[0018] It was also discovered that, as an index for ensuring the joint strength of a weld, it is desirable for the ratio (W1 / W2) of the weld bead width W1 on the back side of the weld to the weld bead width W2 on the front side of the weld to be 0.6 or more and 1.0 or less. If W1 / W2 is less than 0.6, the penetration depth in the weld is insufficient, and the joint strength decreases. Conversely, if W1 / W2 exceeds 1.0, the weld will deform and thin due to excessive heat input, and the joint strength will also decrease. The factor that has the greatest effect on W1 / W2 is basically the welding conditions, but when Al≧0.024Cr 2 It was found that steels satisfying the -1.444 ratio have a very wide range of welding conditions in which the bead width ratio of the weld falls within the above range, and therefore have a significant advantage in terms of weldability.
[0019] The chemical composition of the ferritic stainless steel sheet of this embodiment will be described below, where % means mass %.
[0020] C: 0.001 to 0.100% C reduces intergranular corrosion resistance and workability, so its content must be kept low. Therefore, the upper limit of the C content is set to 0.100% or less. However, excessively lowering the C content increases refining costs, so the lower limit of the C content is set to 0.001% or more. The C content is preferably in the range of 0.002 to 0.050%, more preferably 0.003 to 0.030%.
[0021] Silicon: 0.01 to 2.00% Silicon dramatically improves oxidation resistance at low to medium temperatures (500 to 700°C) and high temperatures (700°C or higher). It is also a very beneficial element that not only suppresses corrosion by concentrating on the surface, but also reduces the corrosion rate of the base material. Therefore, the lower limit of the silicon content is set to 0.01% or more. However, since excessive silicon content reduces weld penetration, the upper limit of the silicon content is set to 2.00% or less. The preferred range of silicon content is 0.30 to 1.50%, and the more preferred range is 0.80 to 1.20%.
[0022] Mn: 0.01 to 2.00% Mn is useful as a deoxidizing element, but excessive Mn content deteriorates corrosion resistance. Therefore, the Mn content is set to 0.01 to 2.00%. The Mn content is preferably in the range of 0.05 to 1.00%, and more preferably in the range of 0.02 to 0.50%.
[0023] P:0.050% or less Since P is an element that deteriorates workability and weldability, its content must be limited. Therefore, the P content is set to 0.050% or less. The preferred range of the P content is 0.030% or less. However, since an excessively low P content increases refining costs, the lower limit of the P content may be set to 0.0001% or more.
[0024] S: 0.0100% or less Since S is an element that deteriorates corrosion resistance, its content must be limited. Therefore, the S content is set to 0.0100% or less. The preferred range of the S content is 0.0070% or less. However, excessively lowering the S content increases refining costs, so the lower limit of the S content may be set to 0.0001% or more.
[0025] Ni: 0.01 to 3.00% Ni content of 0.01% or more is necessary to improve corrosion resistance. However, since a large content leads to an increase in alloy cost, the upper limit of Ni content is set to 3.00% or less. The Ni content is preferably in the range of 0.05 to 1.00%, and more preferably in the range of 0.10 to 0.50%.
[0026] Cr: 9.0~15.0% Cr is an important element in this embodiment. Cr must be contained in an amount of 9.0% or more to ensure oxidation resistance and corrosion resistance in salt damage environments. The higher the Cr content, the better the oxidation resistance and corrosion resistance, but the worse the weld penetration, thermal conductivity, workability, and manufacturability. Since the present invention is a low Cr stainless steel that improves weld penetration, the upper limit of the Cr content is set to 15.0% or less. The preferred range of the Cr content is 9.5 to 14.0%, and more preferably 10.5 to 13.0%.
[0027] Al: 1.0-5.0% Al is an important element in this embodiment. When Al is contained in steel at 0.5% or more, it increases the O concentration in the weld metal of the welded part. It also dramatically improves oxidation resistance, especially at high temperatures (700°C or more). In addition, it is a very useful element that not only suppresses corrosion by concentrating on the steel surface but also reduces the corrosion rate of the base material. This effect is particularly noticeable in low Cr stainless steel. Therefore, the lower limit of the Al content is set to 1.0% or more. However, since an excessive content of Al causes a decrease in the elongation of the material and reduces the workability, the upper limit of the Al content is set to 5.0% or less. The preferred range of the Al content is 1.0 to 3.0%, and more preferably 1.0 to 2.0%.
[0028] B: 0.0001 to 0.0100% B is an element useful for improving secondary workability, and must be contained in an amount of 0.0100% or less. The lower limit of the B content is set to 0.0001% or more, at which a stable effect can be obtained. The preferred range of the B content is 0.0005 to 0.0050%, and the more preferred range is 0.0010 to 0.0030%.
[0029] O: 0.0001 to 0.0100% O is an element useful for weld penetration, but it reduces corrosion resistance and workability. Therefore, it is necessary to suppress the O content to a low level. Therefore, the upper limit of the O content is set to 0.0100% or less. However, excessively lowering the O content increases refining costs, so the lower limit of the O content is set to 0.0001% or more. The preferred range of the O content is 0.002 to 0.020%.
[0030] N: 0.001 to 0.050% N is an element useful for pitting corrosion resistance, but it reduces intergranular corrosion resistance and workability. Therefore, it is necessary to keep the N content low. Therefore, the upper limit of the N content is set to 0.050% or less. However, excessively lowering the N content increases refining costs, so the lower limit of the N content is set to 0.001% or more. The preferred range of the N content is 0.002 to 0.020%.
[0031] One or both of Ti: 0.01-1.00% and Nb: 0.001-1.00% In order to prevent sensitization of stainless steel, Ti and Nb must be contained at 0.01% or more and Nb at 0.001% or more. However, since a large content leads to an increase in alloy cost, a decrease in toughness, a decrease in corrosion resistance due to an increase in inclusions in the steel, and a decrease in manufacturability, the upper limit of the Ti content or Nb content is set to 1.00% or less. The preferable range of the Ti content and Nb content is 0.03 to 0.25%, and the more preferable range is 0.10 to 0.17%, respectively.
[0032] Regarding formula (1) In this embodiment, it is preferable that the Al content and the Cr content in the steel satisfy the relationship of the following formula (1). This can improve the weld penetration. It is more preferable that the Al content and the Cr content satisfy the following formula (2), and it is even more preferable that the Al content and the Cr content satisfy the following formula (3).
[0033] [Al]≧0.024[Cr] 2 -1.444 …(1) [Al]≧0.024[Cr] 2 -1.194 …(2) [Al]≧0.024[Cr] 2 -0.944 …(3) In the formulas (1) to (3), [Al] and [Cr] are the mass percentages of the respective elements.
[0034] The above is the basic chemical composition of the stainless steel of this embodiment, but in this embodiment, the following elements may further be contained as necessary.
[0035] Mo, Sn, Cu, W, V, Sb, Co, Ca, Mg, Zr, Ga, Ta, and REM may be contained alone or in combination depending on the purpose. The lower limit of these elements is 0% or more, and preferably more than 0%.
[0036] Mo: 0.01 to 3.00% Mo can be contained in an amount of 0.01% or more to improve corrosion resistance. However, excessive content of Mo deteriorates workability and is expensive, leading to increased costs. Therefore, the upper limit of the Mo content is set to 3.00% or less. The preferred range of the Mo content is 0.05 to 1.00%.
[0037] Sn: 0.001 to 3.00% Sn can be contained in an amount of 0.001% or more in order to improve corrosion resistance. However, excessive content leads to increased costs. Therefore, the upper limit of the Sn content is set to 3.00% or less. The preferred range of the Sn content is 0.005 to 1.00%, and more preferably 0.010 to 1.00%.
[0038] Cu: 0.01-3.00% Cu can be contained in an amount of 0.01% or more to improve corrosion resistance. However, excessive content leads to increased costs. Therefore, the upper limit of the Cu content is set to 3.00% or less. The Cu content is preferably in the range of 0.02 to 1.00%, and more preferably in the range of 0.05 to 0.09%.
[0039] W: 0.001 to 1.00% W can be contained in an amount of 1.00% or less in order to improve corrosion resistance. In order to obtain a stable effect, the lower limit of the W content is set to 0.001% or more. The preferred range of the W content is 0.005 to 0.80%.
[0040] V: 0.001 to 1.00% V can be contained in an amount of 1.00% or less in order to improve corrosion resistance. In order to obtain a stable effect, the lower limit of the V content is set to 0.001% or more. The preferred range of the V content is 0.005 to 0.50%.
[0041] Sb: 0.001 to 0.100% Sb can be contained in an amount of 0.100% or less in order to improve general corrosion resistance. In order to obtain a stable effect, the lower limit of the Sb content is set to 0.001% or more. The preferred range of the Sb content is 0.010 to 0.080%.
[0042] Co: 0.001 to 0.500% Co can be contained in an amount of 0.500% or less in order to improve secondary workability and toughness. In order to obtain a stable effect, the lower limit of the Co content is set to 0.001% or more. The preferred range of the Co content is 0.010 to 0.300%.
[0043] Ca: 0.0001 to 0.0050% Ca is contained for desulfurization, but if contained in excess, water-soluble inclusions CaS are formed, which reduces corrosion resistance. Therefore, Ca can be contained in the range of 0.0001 to 0.0050%. The preferred range of Ca content is 0.0005 to 0.0030%.
[0044] Mg: 0.0001 to 0.0050% Mg is useful for refining the structure and improving workability and toughness. Therefore, Mg can be contained in the range of 0.0050% or less. In order to obtain a stable effect, the lower limit of the Mg content is set to 0.0001% or more. The preferred range of the Mg content is 0.0005 to 0.0030%.
[0045] Zr: 0.0001 to 0.0300% Zr can be contained in an amount of 0.0300% or less in order to improve corrosion resistance. In order to obtain a stable effect, the lower limit of the Zr content is set to 0.0001% or more. The preferred range of the Zr content is 0.0010 to 0.0100%.
[0046] Ga: 0.0001 to 0.0100% Ga can be contained in an amount of 0.0100% or less in order to improve corrosion resistance and hydrogen embrittlement resistance. In order to obtain a stable effect, the lower limit of the Ga content is set to 0.0001% or more. The Ga content is preferably in the range of 0.0005 to 0.0050%.
[0047] Ta: 0.001 to 0.050% Ta can be contained in an amount of 0.050% or less in order to improve corrosion resistance. In order to obtain a stable effect, the lower limit of the Ta content is set to 0.001% or more. The preferred range of the Ta content is 0.005 to 0.030%.
[0048] REM: 0.001 to 0.100% REM has a deoxidizing effect and is therefore a useful element in refining, so it may be contained in an amount of 0.100% or less. In order to obtain a stable effect, the lower limit of the REM content is set to 0.001% or more. The preferred range of the REM content is 0.003 to 0.050%. Here, REM (rare earth elements) is a general term for two elements, scandium (Sc) and yttrium (Y), and 15 elements (lanthanides) from lanthanum (La) to lutetium (Lu), as generally defined. REM refers to one or more elements selected from these rare earth elements, and the amount of REM refers to the total amount of rare earth elements.
[0049] The ferritic stainless steel sheet of this embodiment is composed of Fe and impurities (including unavoidable impurities) other than the elements described above. In addition to the elements described above, other elements may be contained within a range that does not impair the effects of the present invention. In this embodiment, for example, Bi, Pb, Se, H, etc. may be contained, but in this case, it is preferable to reduce the amount as much as possible. On the other hand, the content ratio of these elements is controlled to the extent that the problem of the present invention is solved, and Bi may be contained in an amount of 0.01% or less, Pb in an amount of 0.01% or less, Se in an amount of 0.01% or less, and H in an amount of 0.01% or less, as necessary.
[0050] The method for producing a ferritic stainless steel sheet of this embodiment comprises the steps of steelmaking-hot rolling-annealing / pickling-cold rolling-annealing, and the production conditions for each step are not particularly specified.
[0051] In steelmaking, a suitable method is to melt steel containing the above-mentioned essential components and components added as necessary in a converter, followed by secondary refining. The melted steel is cast (continuous casting) to form a slab. The slab is heated to a predetermined temperature and hot rolled to a predetermined plate thickness by continuous rolling. Considering the grain size of the final product, the slab thickness is preferably 3.0 mm or more. The annealing process after hot rolling may be omitted, and the cold rolling after pickling may be performed using either a normal Sendzimir mill or a tandem mill, but tandem mill rolling is preferable considering the workability of the steel sheet.
[0052] In cold rolling, the roll roughness, roll diameter, rolling oil, number of rolling passes, rolling speed, rolling temperature, etc. may be appropriately selected within the general range. Intermediate annealing may be performed during cold rolling, and the intermediate and final annealing may be batch annealing or continuous annealing. The annealing atmosphere may be bright annealing in a non-oxidizing atmosphere such as hydrogen gas or nitrogen gas, or annealing in air, if necessary.
[0053] The stainless steel welded structure of this embodiment includes base materials made of ferritic stainless steel plates having the above-mentioned chemical composition, and a welded portion formed at the butt joint between the base materials. The welded portion is formed by welding the ends of the steel plates together by TIG welding, laser welding, MIG welding, or the like. The welding method may be selected as appropriate. The size and shape of the welded structure may also be determined according to the application.
[0054] It is preferable that the ratio (W1 / W2) of the weld bead width W1 on the back side of the weld to the weld bead width W2 on the front side of the weld is 0.6 or more and 1.0 or less. By making W1 / W2 in the range of 0.6 to 1.0, the penetration depth in the weld is sufficient, and deformation and thinning of the weld due to excessive heat input can be prevented, improving the joint strength. In particular, Al≧0.024Cr 2 Ferritic stainless steels that satisfy the -1.444 standard have a very wide range of welding conditions over which the bead width ratio of the weld falls within the above range, making them significantly superior in terms of weldability.
[0055] The thickness of the ferritic stainless steel plate in this embodiment is 3.0 mm or less, preferably 2.0 mm or less, and more preferably 1.5 mm or less. The ratio (W1 / W2) of the weld bead widths W1 and W2 is preferably established when a steel plate having a thickness of 3.0 mm or less is used as the base material.
[0056] The stainless steel plate and welded structure of this embodiment further improve the weld penetration by satisfying a thermal conductivity of 20 W / (m K) or less at 25°C and a thermal conductivity of 28 W / (m K) or less at 800°C. This is to make it difficult to remove heat during welding, thereby achieving deeper weld penetration.
[0057] The ferritic stainless steel plate and welded structure of this embodiment can provide a ferritic stainless steel with excellent weld penetration properties that is suitable for use in combustion equipment components and high-temperature components such as heating equipment and kitchen appliances, and exhaust system components for automobiles, motorcycles, etc. EXAMPLES
[0058] The present invention will now be described in more detail with reference to examples.
[0059] Steels having the compositions shown in Tables 1A to 2B were melted in a converter, followed by secondary refining to produce molten steel, which was then continuously cast into slabs. The resulting slabs were hot-rolled to produce hot-rolled sheets with a thickness of 4 mm. Shot and pickling were then performed. The sheets were then cold-rolled to a thickness of 1.2 mm, annealed at 920°C for 1 minute, and then salt-treated and pickled. The pickling was performed by electrolytic pickling in a solution with a nitric acid concentration of 150 g / L. In this manner, ferritic stainless steel sheets were produced.
[0060] Test pieces measuring 100 mm in length and 50 mm in width were cut out from the prepared steel plate and TIG welded parallel to the rolling direction. The welding current was 90 A, the arc voltage was 8.5-9.5 V, the welding speed was 50 cm / min, and Ar was used as the shielding gas, with the torch shielding gas flow rate being 10 L / min, the back shielding gas flow rate being 15 L / min, and the after shielding gas flow rate being 30 L / min. The penetration depth of the obtained welded structure was evaluated.
[0061] The penetration depth was evaluated by measuring the bead width on the back side of the welded surface, and if the bead width was between 2.4mm and 3.6mm, the weld penetration depth was evaluated as "◎", if it was between 1.8mm and 2.4mm or between 3.6mm and 4.8mm, the weld penetration depth was evaluated as "〇", and if it was less than 1.8mm or more than 4.8mm, the weld penetration depth range was evaluated as "×". Note that under these welding conditions, no steel plates showed values outside the above penetration depth range but greater than the above penetration depth range. "◎" and "〇" were evaluated as passing.
[0062] In addition, two test pieces with a length of 100 mm and a width of 50 mm were cut out from the prepared steel plate, and both test pieces were subjected to TIG butt welding parallel to the rolling direction. The welding was performed by butting the ends of the steel plate together. The welding current was 50 to 150 A, the arc voltage was 8.5 to 10.7 V, and the welding speed was 20 to 100 cm / min, and TIG welding was performed under the four conditions shown in Tables 3A and 3B. Ar was used as the shielding gas during welding, and the flow rate of the torch shielding gas was 10 L / min, the flow rate of the back shielding gas was 15 L / min, and the flow rate of the after shielding gas was 30 L / min. The joint strength of the welded parts of the obtained welded structures was evaluated.
[0063] The joint strength was evaluated by measuring the bead width W1 on the front and back sides of the welded surface, and the bead width W2 on the front side. If W1 / W2 was in the range of 0.6 to 1.0, it was evaluated as "○", and if it was less than 0.6, it was evaluated as "×". Note that under these welding conditions, no steel plates showed a value greater than 1.0. "○" was considered to be acceptable.
[0064] In addition, a disk-shaped test piece with a diameter of 10 mm was cut out from the prepared steel plate, and the thermal diffusivity was measured by the laser flash method using a thermal constant measuring device LFA-502 manufactured by Kyoto Electronics Manufacturing Co., Ltd. The measurement temperatures were room temperature and 800°C, and the atmosphere was air at room temperature and vacuum at 800°C.
[0065] In addition, disk-shaped test pieces with a diameter of 5 mm were cut out from the prepared steel plates and the specific heat was measured. The measurement method was the DSC method, the measurement equipment was a NETZSCH DSC3500 Sirius at room temperature and a NETZSCH DSC404F1 Pegasus at 800°C, the measurement temperatures were room temperature and 800°C, and the atmosphere was Ar.
[0066] The thermal conductivity was calculated by multiplying the thermal diffusivity by the specific heat and the density. The density was calculated by the bulk density at room temperature, which was calculated from the sample dimensions and mass.
[0067] As shown in Tables 1A to 3B, when formula (1) is satisfied, the weld penetration improves and the TIG welding evaluation result is ◎ or ○. In particular, when the thermal conductivity at 25°C is 20 W / (m·K) or less and the thermal conductivity at 800°C is 28 W / (m·K) or less, the weld penetration improves greatly and the evaluation is ◎. In addition, W2 / W1 is also ○, indicating high weld strength and excellent weldability.
[0068] Comparative Examples B1 to B9 did not satisfy formula (1), and the evaluations of the weld penetration and W2 / W1 were all "x".
[0069] In addition, in Comparative Examples B1 to B9, the evaluation of W2 / W1 when the welding conditions were changed was "x" under all welding conditions, so further attempts were made to change the welding conditions in various ways. However, no welding conditions were found that gave a W2 / W1 evaluation of "o", or even if they were found, the range of conditions was very narrow, and the weldability was significantly reduced. On the other hand, the steel plates of Inventive Examples A1 to A25 were able to be welded to a W2 / W1 evaluation of "o" even under welding conditions that gave a W2 / W1 evaluation of "x" in B1 to B9, and therefore had excellent weldability. However, A4 and A13 are examples for reference only.
[0070] [Table 1A]
[0071] [Table 1B]
[0072] [Table 2A]
[0073] [Table 2B]
[0074] [Table 3A]
[0075] [Table 3B] [Industrial Applicability]
[0076] According to the present invention, it is possible to provide a ferritic stainless steel sheet and welded structure having excellent weld penetration properties suitable for use in combustion appliance members and high-temperature members such as heating appliances and kitchen appliances, and exhaust system members for automobiles, motorcycles, etc. In other words, the present invention is extremely useful industrially.
Claims
1. In mass percent, C: 0.001-0.100%, Si: 0.01-2.00%, Mn: 0.01 to 2.00%, P:≦0.050%, S:≦0.0100%, Ni: 0.01 to 3.00%, Cr: 9.5-15.0%, Al: 1.0-5.0%, B: 0.0001 to 0.0100%, O: 0.0001 to 0.0100%, N: 0.001 to 0.050%; The ferritic stainless steel sheet further contains one or two of Ti: 0.01 to 1.00% and Nb: 0.001 to 1.00%, with the balance being Fe and impurities, and is characterized in that it satisfies the following formula (1): [Al]≧0.024[Cr] 2 -1.444 …(1) In the formula (1), [Al] and [Cr] are the mass percentages of the respective elements.
2. In mass percent, C: 0.001-0.100%, Si: 0.01-2.00%, Mn: 0.01 to 2.00%, P:≦0.050%, S:≦0.0100%, Ni: 0.01 to 3.00%, Cr: 9.0-15.0%, Al: 1.0-5.0%, B: 0.0001 to 0.0030%, O: 0.0001 to 0.0100%, N: 0.001 to 0.050%; Further, it contains one or two of Ti: 0.01 to 1.00% and Nb: 0.001 to 1.00%, Furthermore, Mo: 0.01 to 3.00%, Sn: 0.001 to 3.00%, Cu: 0.01 to 0.44%, W: 0.001 to 1.00%, V: 0.001 to 1.00%, Sb: 0.001 to 0.100%, Co: 0.001 to 0.500%, Ca: 0.0001 to 0.0050%, Mg: 0.0001 to 0.0050%, Zr: 0.0001 to 0.0300%, Ga: 0.0001 to 0.0100%, Ta: 0.001 to 0.050%, REM: 0.001 to 0.100%. A ferritic stainless steel sheet, the balance of which is Fe and impurities, and which satisfies the following formula (1): [Al]≧0.024[Cr] 2 -1.444 …(1) In the formula (1), [Al] and [Cr] are the mass percentages of the respective elements.
3. A welding method comprising the steps of: a base material made of the ferritic stainless steel plate according to claim 1 or 2; and a weld portion formed at a joint between the base materials, A welded structure, characterized in that a ratio (W1 / W2) of a weld bead width W1 on a back side of the weld to a weld bead width W2 on a front side of the weld is 0.6 or more and 1.0 or less.
Citation Information
Patent Citations
JP1974086975A
Magnetic stainless steel
JP1994049606A
Ferritic stainless steel sheet excellent in penetration at welding
JP1998102212A
Aluminum-containing ferritic stainless steel excellent in high temperature oxidation resistance and producibility
JP1998158791A
Electromagnetic stainless steel and production method therefor
JP2002302747A