Ethylene / α-olefin / non-conjugated polyene copolymer composition and its use

The ethylene/α-olefin/non-conjugated polyene copolymer composition addresses weight reduction and mold removal issues by incorporating crystalline olefin polymer and carbon black, resulting in improved injection moldability and mechanical properties.

JP7584233B2Active Publication Date: 2024-11-15MITSUI CHEMICALS INC
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2020069068
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-07
Publication Date
2024-11-15
Estimated Expiration
2040-04-07

AI Technical Summary

Technical Problem

Existing ethylene/α-olefin/non-conjugated polyene copolymers used in automobile parts face challenges with high specific gravity due to filler content, hindering weight reduction and complicate mold removal during injection molding of complex shapes.

Method used

A composition of ethylene/α-olefin/non-conjugated polyene copolymer containing crystalline olefin polymer and carbon black, with specific ratios and additives, enhancing injection moldability and mold removability.

Benefits of technology

The composition achieves excellent injection moldability and mold removability, producing articles with good appearance and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584233000001
    Figure 0007584233000001
  • Figure 0007584233000002
    Figure 0007584233000002
Patent Text Reader

Abstract

To provide an ethylene / α-olefin / non-conjugated polyene copolymer composition that is suitable for obtaining an injection molded product having excellent releasability from a metal mold after injection molding and having excellent rigidity.SOLUTION: The present invention relates to: an ethylene / α-olefin / non-conjugated polyene copolymer (S) that contains ethylene, α-olefin having 3 or more carbon atoms, and non-conjugated polyene as constituent units; an ethylene / α-olefin / non-conjugated polyene copolymer composition that contains a crystalline olefin polymer (G) in a range of 1 to 80 pts.mass and a carbon black (L) in a range of 10 to 300 pts.mass relative to 100 pts.mass of the ethylene / α-olefin / non-conjugated polyene copolymer (S); and a use thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ethylene / α-olefin / non-conjugated polyene copolymer composition, and more particularly to an ethylene / α-olefin / non-conjugated polyene copolymer composition having excellent injection moldability and uses thereof. [Background technology]

[0002] Olefin-based thermoplastic elastomers, which are obtained by crosslinking a composition of an ethylene-α-olefin-non-conjugated polyene copolymer, which is a type of thermoplastic elastomer, and a crystalline olefin polymer, are lightweight and easy to recycle, and therefore are widely used as energy- and resource-saving thermoplastic elastomers, particularly as a replacement for vulcanized rubber, in automobile parts such as hoses, pipes, and boots (blow molded products) for automobiles (for example, Patent Documents 1 and 2).

[0003] However, these automobile parts are always required to be lighter in order to improve fuel efficiency, but the thermoplastic elastomers used contain a large amount of filler, which tends to increase the specific gravity, hindering the weight reduction of the parts. In addition, injection molding is often used for some automobile parts in order to speed up the manufacturing process of the parts, and it is also required to perform injection molding on parts with complex shapes. However, when injection molding parts with complex shapes, it may not be easy to remove the molded product from the mold. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-294714 A [Patent Document 2] JP 2011-202136 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to obtain an ethylene-α-olefin-non-conjugated polyene copolymer composition which is suitable for obtaining injection-molded articles which have excellent demoldability from a mold after injection molding and good rigidity. [Means for solving the problem]

[0006] The present invention relates to an ethylene-α-olefin-non-conjugated polyene copolymer (S) containing ethylene, an α-olefin having 3 or more carbon atoms, and a non-conjugated polyene as constituent units; an ethylene-α-olefin-non-conjugated polyene copolymer composition comprising more than 10 parts by mass and up to 300 parts by mass of a crystalline olefin polymer (G) and 10 to 300 parts by mass of carbon black (L) per 100 parts by mass of the ethylene-α-olefin-non-conjugated polyene copolymer (S); and a crosslinked product of the copolymer composition. Effect of the Invention

[0007] The ethylene-α-olefin-non-conjugated polyene copolymer composition of the present invention has excellent injection moldability and can be used to produce injection molded articles with good appearance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Ethylene-α-olefin-non-conjugated polyene copolymer (S) The ethylene-α-olefin-non-conjugated polyene copolymer (S) (hereinafter also referred to as "copolymer (S)") has structural units derived from ethylene (A), structural units derived from an α-olefin (B) having 3 to 20 carbon atoms, and structural units derived from a non-conjugated polyene (C). The non-conjugated polyene (C) contains, in the molecule, two or more in total of at least one partial structure selected from formulae (I) and (II).

[0009] [ka]

[0010] Examples of the α-olefin (B) having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms such as propylene, 1-butene, 1-hexene, and 1-octene are preferred, and propylene is more preferred.

[0011] The copolymer (S) contains structural units derived from at least one type of α-olefin (B) having 3 to 20 carbon atoms, and may contain structural units derived from two or more types of α-olefins (B) having 3 to 20 carbon atoms.

[0012] Examples of the non-conjugated polyene (C) include 5-vinyl-2-norbornene (VNB), norbornadiene, 1,4-hexadiene, and dicyclopentadiene. Among these, it is preferable that the non-conjugated polyene (C) contains VNB, and it is more preferable that the non-conjugated polyene (C) is VNB, since it is highly available, has good crosslinkability, and is likely to improve the heat resistance of the composition.

[0013] The copolymer (S) contains constitutional units derived from at least one type of non-conjugated polyene (C), and may contain constitutional units derived from two or more types of non-conjugated polyenes (C). The copolymer (S) may further have a constitutional unit derived from a non-conjugated polyene (D) containing only one partial structure selected from the formulae (I) and (II) in the molecule.

[0014] Examples of the non-conjugated polyene (D) include 5-ethylidene-2-norbornene (ENB), 5-methylene-2-norbornene, 5-(2-propenyl)-2-norbornene, 5-(3-butenyl)-2-norbornene, 5-(1-methyl-2-propenyl)-2-norbornene, 5-(4-pentenyl)-2-norbornene, 5-(1-methyl-3-butenyl)-2-norbornene, 5-(5-hexenyl)-2-norbornene, 5-(1-methyl-4-pentenyl)-2-norbornene, 5-(2,3-dimethyl-3-butenyl)-2-norbornene, 5-(2-ethyl-3-butenyl)-2-norbornene, Examples of such compounds include 5-(6-heptenyl)-2-norbornene, 5-(3-methyl-5-hexenyl)-2-norbornene, 5-(3,4-dimethyl-4-pentenyl)-2-norbornene, 5-(3-ethyl-4-pentenyl)-2-norbornene, 5-(7-octenyl)-2-norbornene, 5-(2-methyl-6-heptenyl)-2-norbornene, 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(5-ethyl-5-hexenyl)-2-norbornene, and 5-(1,2,3-trimethyl-4-pentenyl)-2-norbornene. Among these, ENB is preferred because it is highly available and has good mechanical properties. The copolymer (S) can contain constitutional units derived from at least one type of non-conjugated polyene (D), and may contain constitutional units derived from two or more types of non-conjugated polyenes (D).

[0015] As the requirement (i), in the copolymer (S), the molar ratio (structural units derived from ethylene (A) / structural units derived from α-olefin (B) having 3 to 20 carbon atoms) is 40 / 60 to 99.9 / 0.1, preferably 50 / 50 to 90 / 10, more preferably 55 / 45 to 85 / 15, and further preferably 55 / 45 to 78 / 22. Such a copolymer (S) is preferable because it has excellent mechanical strength and flexibility.

[0016] As the requirement (ii), the content of the structural unit derived from the non-conjugated polyene (C) in 100% by mass of the copolymer (S) (i.e., 100% by mass of the total content of all structural units) is 0.07 to 10% by mass, preferably 0.1 to 8.0% by mass, and more preferably 0.5 to 5.0% by mass. Such a copolymer (S) is preferable because the crosslinked product obtained from the composition of the present invention has sufficient hardness and excellent mechanical properties, and is also preferable because it shows a fast crosslinking speed.

[0017] In 100% by mass of the copolymer (S), the content of the constitutional units derived from the non-conjugated polyene (D) is usually 0 to 20% by mass, and preferably 0 to 8% by mass. The content ratio of structural units derived from ethylene (A), α-olefin (B), non-conjugated polyene (C), and non-conjugated polyene (D) in the copolymer (S) is 13 It can be determined by C-NMR.

[0018] Mooney viscosity ML of copolymer (S) at 125°C (1+4) is preferably 5 to 100, more preferably 20 to 95, and further preferably 50 to 90. The copolymer (S) having a Mooney viscosity in the above range has good processability and flowability, exhibits excellent rubber properties, and also tends to exhibit good post-treatment quality (ribbon handleability).

[0019] The Mooney viscosity is measured using a Mooney viscometer (Shimadzu Corporation, Model SMV202) in accordance with JIS K6300 (1994). The copolymer (S) has an intrinsic viscosity [η] measured in decalin at 135° C. of preferably 0.1 to 5 dL / g, more preferably 0.5 to 5.0 dL / g, and even more preferably 0.9 to 4.0 dL / g. The copolymer (S) having an intrinsic viscosity [η] within the above range tends to have excellent moldability.

[0020] Specifically, the intrinsic viscosity [η] is measured as follows: Approximately 20 mg of copolymer (S) is dissolved in 15 mL of decalin, and the specific viscosity η spAdd 5 mL of decalin solvent to this decalin solution to dilute it, and measure the specific viscosity η sp This dilution procedure was repeated two more times, and the η sp The value of / C is taken as the intrinsic viscosity. [η]=lim(η sp / C) (C→0)

[0021] <Production method of ethylene-α-olefin-non-conjugated polyene copolymer (S)> The ethylene-α-olefin-non-conjugated polyene copolymer (S) according to the present invention is obtained by copolymerizing monomers including ethylene (A), an α-olefin (B) having 3 to 20 carbon atoms, a non-conjugated polyene (C), and, if necessary, a non-conjugated polyene (D). The copolymer (S) may be prepared by any method, but is preferably obtained by copolymerizing the monomers in the presence of a metallocene compound, and more preferably obtained by copolymerizing the monomers in the presence of a catalyst system containing a metallocene compound. Specifically, the copolymer (S) can be produced by adopting, for example, the method using a metallocene catalyst described in International Publication No. 2015 / 122495.

[0022] <Crystalline olefin polymer (G)> The crystalline olefin polymer (hereinafter, sometimes referred to as "polymer (G)"), which is one of the components contained in the copolymer composition according to the present invention, is a crystalline polymer which is a homopolymer or copolymer of an α-olefin having 2 to 20 carbon atoms.

[0023] In the present invention, a crystalline polymer is a polymer having a melting point. Specific examples of the α-olefin constituting the crystalline olefin polymer (G) include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-pentene, 4-methyl-1-pentene, and 5-methyl-1-hexene.

[0024] Specific examples of the crystalline olefin polymer (G) according to the present invention include the following (co)polymers. (1) Ethylene homopolymers and copolymers of ethylene with 10 mol% or less of other α-olefins or vinyl monomers such as vinyl acetate and ethyl acrylate, more specifically, ethylene-based polymers such as high-pressure low-density polyethylene (HP-LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene, high-density polyethylene (HDPE), ethylene-vinyl acetate copolymer (EVA), and ethylene-acrylic acid copolymer. (2) Propylene-based polymers such as propylene homopolymers, random copolymers of propylene and up to 10 mol% of other α-olefins, and block copolymers of propylene and up to 30 mol% of other α-olefins, which are generally referred to as homo-, random, or block type polypropylenes. (3) 1-butene polymers such as homopolymers of 1-butene and random copolymers of 1-butene with 10 mol % or less of other α-olefins. (4) Homopolymers of 4-methyl-1-pentene and random copolymers of 4-methyl-1-pentene and 20 mol % or less of other α-olefins.

[0025] These crystalline olefin polymers (G) can be used alone or in combination of two or more kinds. Among these crystalline olefin polymers (G), ethylene polymers are preferred, and high-pressure low-density polyethylene (HP-LDPE) is particularly preferred. The ethylene polymer usually has a melt flow rate (MFR) of preferably 0.1 to 100 g / 10 min, and more preferably 0.5 to 80 g / 10 min.

[0026] Carbon Black (L) Carbon black (L), which is one of the components contained in the copolymer composition of the present invention, is a type of known rubber reinforcing agent that is compounded in rubber compositions, and is an inorganic substance generally known as carbon black.

[0027] Specific examples of the carbon black (L) used in the present invention include Asahi #55G, Asahi #60G, and Asahi #60UG (all manufactured by Asahi Carbon Co., Ltd.), and Seast (V, SO, 116, 3, 6, 9, SP, TA, etc.) carbon blacks (manufactured by Tokai Carbon Co., Ltd.), as well as carbon blacks that have been surface-treated with a silane coupling agent or the like.

[0028] Fatty acid amide (M) The fatty acid amide (M), which is one of the components contained in the copolymer composition of the present invention, is an amide of a higher fatty acid, and specifically, monoamides of higher fatty acids such as stearamide, oxystearamide, oleylamide, erucic acid amide, laurylamide, palmitylamide, behenamide, and methylolamide; diamides of higher fatty acids such as methylene bis-stearamide, ethylene bis-stearamide, ethylene bis-oleylamide, and ethylene bis-laurylamide; complex amides of higher fatty acids such as stearyl oleylamide, N-stearyl erucamide, and N-oleyl palmitamide; and plastrogin. TM (Fujisawa Pharmaceutical Co., Ltd.), Plastrodin S TM Examples of suitable fatty acids include those commercially available under the trade names of 1,2,3-trimethylsiloxyphenyl (manufactured by Fujisawa Pharmaceutical Co., Ltd.).

[0029] <Ethylene / α-olefin / non-conjugated polyene copolymer composition> The copolymer composition of the present invention contains the above-mentioned copolymer (S), the above-mentioned crystalline olefin polymer (G) in an amount of more than 10 to 30 parts by mass, preferably 15 to 25 parts by mass, and more preferably 17 to 23 parts by mass, and the above-mentioned carbon black (L) in an amount of 10 to 300 parts by mass, preferably 30 to 200 parts by mass, and more preferably 50 to 180 parts by mass, relative to 100 parts by mass of the copolymer (S).

[0030] The copolymer composition of the present invention, containing the crystalline olefin polymer (G) and the carbon black (L) in the above-mentioned ranges, has excellent injection moldability and excellent releasability from a mold, and the obtained molded article has a good appearance without cracking in shape.

[0031] The copolymer composition of the present invention may contain, in addition to the crystalline olefin polymer (G) and carbon black (L), the fatty acid amide (M) in an amount of 0.1 to 10 parts by mass, more preferably 0.2 to 8 parts by mass, and even more preferably 0.5 to 6 parts by mass.

[0032] In addition to the copolymer (S), the crystalline olefin polymer (G), the carbon black (L) and the fatty acid amide (M), the copolymer composition of the present invention may contain other components as necessary within a range that does not impair the effects of the present invention. Examples of other components include polymers, crosslinking agents, crosslinking assistants, vulcanization accelerators, vulcanization assistants, and inorganic fillers. At least one selected from softeners, antiaging agents (stabilizers), processing assistants, activators, moisture absorbents, heat stabilizers, weather stabilizers, antistatic agents, colorants, lubricants and thickeners may be contained. Each of the polymers and additives may be used alone or in combination of two or more. Also, known foaming agents, foaming assistants, colorants, dispersants, flame retardants, etc. may be used as other components as necessary.

[0033] <Crosslinking Agent, Crosslinking Coagent, Vulcanization Accelerator, and Vulcanization Coagent> Examples of the crosslinking agent include crosslinking agents generally used when crosslinking rubber, such as organic peroxides, phenolic resins, sulfur-based compounds, hydrosilicone-based compounds, amino resins, quinones or their derivatives, amine-based compounds, azo-based compounds, epoxy-based compounds, isocyanate-based compounds, etc. Among these, organic peroxides and sulfur-based compounds (hereinafter also referred to as "vulcanizing agents") are preferred.

[0034] Examples of organic peroxides include dicumyl peroxide (DCP), di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, ert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.

[0035] When an organic peroxide is used as a crosslinking agent, the amount of the organic peroxide in the copolymer composition is generally 0.1 to 25 parts by mass, preferably 0.2 to 20 parts by mass, and more preferably 0.5 to 15 parts by mass, based on 100 parts by mass of the copolymer (S). When the amount of the organic peroxide is within the above range, the copolymer composition exhibits excellent crosslinking properties without blooming on the surface of the obtained molded article, which is preferable.

[0036] When an organic peroxide is used as a crosslinking agent, it is preferable to use a crosslinking assistant in combination. Examples of the crosslinking assistant include sulfur; quinone dioxime crosslinking assistant such as p-quinone dioxime; acrylic crosslinking assistant such as ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate; allyl crosslinking assistant such as diallyl phthalate and triallyl isocyanurate; maleimide crosslinking assistant; divinylbenzene; and metal oxides such as zinc oxide (e.g., ZnO#1 / zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name; manufactured by Inoue Seki Kogyo Co., Ltd.)).

[0037] When a crosslinking auxiliary is used, the amount of the crosslinking auxiliary in the copolymer composition is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, more preferably 1 to 6 mol, per mol of the organic peroxide.

[0038] Examples of sulfur-based compounds (vulcanizing agents) include sulfur, sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dithiocarbamate.

[0039] When a sulfur-based compound is used as a crosslinking agent, the blending amount in the copolymer composition is usually 0.1 to 10 parts by mass, preferably 0.2 to 7.0 parts by mass, and more preferably 0.5 to 5.0 parts by mass, based on 100 parts by mass of the copolymer (S). When the blending amount of the sulfur-based compound is within the above range, there is no bloom on the surface of the obtained molded article, and the copolymer composition shows excellent crosslinking properties. When a sulfur-based compound is used as the crosslinking agent, it is preferable to use a vulcanization accelerator in combination.

[0040] Examples of the vulcanization accelerator include N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole (e.g., Suncerer M (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), 2-(4-morpholinodithio)benzothiazole (e.g., Noccelaer MDB-P (trade name; manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-dinitrophenyl)mercaptobenzothiazole, Thiazole-based vulcanization accelerators such as ethyl-4-morpholinothio)benzothiazole and dibenzothiazyl disulfide (for example, Sancerer DM (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); guanidine-based vulcanization accelerators such as diphenyl guanidine, triphenyl guanidine, and diorthotolyl guanidine; aldehyde amine-based vulcanization accelerators such as acetaldehyde-aniline condensation product and butyraldehyde-aniline condensation product; imidazoline-based vulcanization accelerators such as 2-mercaptoimidazoline; tetramethylthiuram monosulfide (for example, Sancerer DM (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (e.g., Sancerer TS (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetramethylthiuram disulfide (e.g., Sancerer TT (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetraethylthiuram disulfide (e.g., Sancerer TET (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetrabutylthiuram disulfide (e.g., Sancerer TBT (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), and dipentamethylenethiuram tetrasulfide (e.g., Sancerer TRA (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); zinc dimethyldithiocarbamate, diethyldithio Examples of such vulcanization accelerators include dithioacid salt vulcanization accelerators such as zinc carbamate, zinc dibutyldithiocarbamate (e.g., Sancerar PZ, Sancerar BZ, and Sancerar EZ (trade names; manufactured by Sanshin Chemical Industry Co., Ltd.)) and tellurium diethyldithiocarbamate; thiourea vulcanization accelerators such as ethylenethiourea (e.g., Sancerar BUR (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.), Sancerar 22-C (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), N,N'-diethylthiourea, and N,N'-dibutylthiourea; and xanthate vulcanization accelerators such as zinc dibutylxatogenate.

[0041] When a vulcanization accelerator is used, the blending amount of the vulcanization accelerator in the copolymer composition is generally 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the copolymer (S). When the blending amount of the vulcanization accelerator is within the above range, the copolymer composition exhibits excellent crosslinking properties without blooming on the surface of the obtained molded article. When a sulfur-based compound is used as a crosslinking agent, a vulcanization assistant can be used in combination.

[0042] Examples of the vulcanization aid include zinc oxide (e.g., ZnO#1 and zinc oxide type 2, manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name, manufactured by Inoue Seki Kogyo Co., Ltd.)).

[0043] When a vulcanization aid is used, the blending amount of the vulcanization aid in the ethylene copolymer composition is usually 1 to 20 parts by mass based on 100 parts by mass of the copolymer (S).

[0044] <Softener> Specific examples of the softener according to the present invention include petroleum-based softeners such as process oil, lubricating oil, paraffin oil, liquid paraffin, petroleum asphalt, Vaseline, liquid ethylene-propylene copolymer, and liquid ethylene-1-butene copolymer; coal tar-based softeners such as coal tar; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, soybean oil, and coconut oil; waxes such as beeswax and carnauba wax; and fatty acids or salts thereof such as ricinoleic acid, palmitic acid, stearic acid, barium stearate, and calcium stearate. ; naphthenic acid, pine oil, rosin or derivatives thereof; synthetic polymer substances such as terpene resin, petroleum resin, coumarone-indene resin, etc.; ester-based softeners such as dioctyl phthalate, dioctyl adipate, etc.; others include microcrystalline wax, liquid polybutadiene, modified liquid polybutadiene, hydrocarbon-based synthetic lubricating oil, tall oil, sub(factice), etc., with petroleum-based softeners being preferred, and liquid ethylene-propylene copolymer, liquid ethylene-1-butene copolymer, and process oil being particularly preferred. These softeners may be used alone or in combination of two or more.

[0045] The blending amount of the softener in the copolymer composition is generally 2 to 100 parts by mass, and preferably 10 to 100 parts by mass, based on 100 parts by mass of the copolymer (S).

[0046] <Inorganic fillers> Specific examples of inorganic fillers used in the present invention include one or more of light calcium carbonate, heavy calcium carbonate, talc, clay, etc., and among these, heavy calcium carbonate such as "Whiten SB" (product name; Shiraishi Calcium Co., Ltd.) is preferred.

[0047] When the copolymer composition contains an inorganic filler, the blending amount of the inorganic filler is usually 2 to 50 parts by mass, preferably 5 to 50 parts by mass, based on 100 parts by mass of the copolymer S. When the blending amount is within the above range, the kneading processability of the copolymer composition is excellent.

[0048] <Anti-aging agent (stabilizer)> By blending an antioxidant (stabilizer) with the copolymer composition of the present invention, the life of a molded article formed therefrom can be extended. Examples of such antioxidants include conventionally known antioxidants, such as amine-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants.

[0049] Further examples of the antiaging agent include aromatic secondary amine-based antiaging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine; phenol-based antiaging agents such as dibutylhydroxytoluene and tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane; thioether-based antiaging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based antiaging agents such as nickel dibutyldithiocarbamate; and sulfur-based antiaging agents such as 2-mercaptobenzoylimidazole, 2-mercaptobenzimidazole, zinc salt of 2-mercaptobenzimidazole, dilaurylthiodipropionate, and distearylthiodipropionate.

[0050] These antioxidants can be used alone or in combination of two or more, and the blending amount is usually 0.3 to 10 parts by mass, preferably 0.5 to 7.0 parts by mass, based on 100 parts by mass of the copolymer (S). By setting the blending amount within such a range, no bloom occurs on the surface of a molded article obtained from a crosslinked product of the copolymer composition, and furthermore, the occurrence of crosslinking inhibition can be suppressed.

[0051] <Processing aids> As the processing aid according to the present invention, a wide variety of processing aids that are generally compounded with rubber can be used.

[0052] Specific examples of processing aids include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, esters, etc. Of these, stearic acid is preferred.

[0053] The amount of the processing aid is usually 10 parts by mass or less, and preferably 8.0 parts by mass or less, based on 100 parts by mass of the copolymer (S) contained in the copolymer composition.

[0054] <Activator> Specific examples of the surfactant include amines such as di-n-butylamine, dicyclohexylamine, and monoethanolamine; surfactants such as diethylene glycol, polyethylene glycol, lecithin, triaryl ether mellate, and zinc compounds of aliphatic or aromatic carboxylic acids; zinc peroxide preparations; octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds.

[0055] When an activator is contained, the amount thereof is usually 0.2 to 10 parts by mass, and preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the copolymer (S).

[0056] Moisture absorbent Specific examples of the moisture absorbent include calcium oxide, silica gel, sodium sulfate, molecular sieve, zeolite, and white carbon.

[0057] When the moisture absorbent is contained, the amount of the moisture absorbent is usually 0.5 to 15 parts by mass, and preferably 1.0 to 12 parts by mass, based on 100 parts by mass of the copolymer (S).

[0058] <Crosslinked product of copolymer composition> The crosslinked product of the copolymer composition of the present invention is obtained by crosslinking the above-mentioned copolymer composition of the present invention. In order to crosslink the copolymer composition of the present invention, a crosslinking agent such as an organic peroxide is blended with the copolymer composition, and then crosslinking is carried out.

[0059] As a method for crosslinking the copolymer composition of the present invention, the copolymer composition is mixed with the organic peroxide and the like, and then a conventionally known kneading device, for example, an open-type mixing roll, a non-open-type Banbury mixer, an extruder, a kneader, a continuous mixer, etc., is used. Among these, a non-open-type kneading device is preferred, and kneading is preferably carried out in an atmosphere of an inert gas such as nitrogen gas or carbon dioxide gas.

[0060] <<Uses of the copolymer composition>> The copolymer composition of the present invention can be molded by a commonly used molding method such as injection molding, extrusion molding, blow molding, compression molding, and the like. It is used in a wide range of applications, including automotive parts (weather strips, ceiling materials, interior seats, bumper moldings, side moldings, air spoilers, air duct hoses, cup holders, handbrake grips, shift knob covers, seat adjustment knobs, flapper door seals, wire harness grommets, rack and pinion boots, suspension cover boots, glass guides, inner belt line seals, roof guides, trunk lid seals, molded quarter window gaskets, corner moldings, glass encapsulations, hood seals, glass run channels, secondary seals, clean side ducts, various packings, etc.), civil engineering and building material parts (waterstop materials, joint materials, architectural window frames, etc.), sporting goods (golf clubs, tennis racket grips, etc.), industrial parts (hose tubes, gaskets, etc.), home appliance parts (hoses, packings, etc.), medical equipment parts, electric wires, and miscellaneous goods. EXAMPLES

[0061] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. The ethylene / α-olefin / non-conjugated polyene copolymers (S) used in the examples and comparative examples are shown below.

[0062] [Production Example 1] Production of ethylene-α-olefin-vinylnorbornene copolymer (S-1) Ethylene-propylene-5-vinyl-2-norbornene (VNB) copolymer (S-1) was produced using a continuous polymerization apparatus as follows.

[0063] A 300-liter polymerization reactor was continuously fed with 58.3 L / hr of dehydrated hexane solvent from line 1, 4.5 mmol / hr of triisobutylaluminum (TiBA), 0.150 mmol / hr of (C6H5)3CB(C6F5)4, and 0.030 mmol / hr of di(p-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride from line 2. At the same time, 6.6 kg / hr of ethylene, 9.3 kg / hr of propylene, 18 L / hr of hydrogen, and 340 g / hr of VNB were continuously fed into the polymerization reactor from separate lines, and copolymerization was carried out under the conditions of a polymerization temperature of 87°C, a total pressure of 1.6 MPaG, and a residence time of 1.0 hour.

[0064] The ethylene-propylene-VNB copolymer solution produced in the polymerization reactor was continuously discharged at a flow rate of 88.0 L / hr, heated to 170°C (pressure increased to 4.1 MPaG), and fed to a phase separator. At this time, ethanol, a polymerization inhibitor, was continuously introduced into the discharge line in an amount of 0.1 mol times the amount of TiBA in the liquid component extracted from the polymerization reactor.

[0065] In the phase separator, the ethylene-propylene-vinyl alcohol copolymer solution was separated into a dense phase (lower phase) containing most of the ethylene-propylene-vinyl alcohol copolymer and a dilute phase (upper phase) containing a small amount of the polymer.

[0066] The separated thick phase was introduced into heat exchanger K at a rate of 85.4 L / hr, and then into a hopper where the solvent was evaporated and separated to obtain an ethylene-propylene-VNB copolymer at a rate of 7.8 kg / hr.

[0067] The physical properties of the copolymer (S-1) obtained were measured by the method described above. Mooney viscosity ML of copolymer (S-1) (1+4)The intrinsic viscosity [η] at 125°C was 69, the molar ratio (ethylene unit / propylene unit) was 70 / 30, the content of VNB units was 1.4 mass%, and the intrinsic viscosity [η] measured in decalin at 135°C was 2.8 dL / g. The molecular weight distribution of the obtained copolymer (S-1) was bimodal.

[0068] [Production Example 2] <Polymerization of softener components> The polymerization of the softener component was carried out in a 300L SUS reactor equipped with a stirrer, with the temperature kept at 80°C and the liquid level at 100L, with hexane at 52.0kg / h, ethylene at 12.0kg / h, propylene at 7.7kg / h, and hydrogen at 1600NL / h, using [N-(1,1-dimethylethyl)-1,1-dimethyl-1-[(1,2,3,3A,8A-η)-1,5,6,7-tetrahydro- 2-Methyl-S-indacene-1-yl]silane aminate (2-)-κN][(1,2,3,4-η)-1,3-pentadiene]-titanium was continuously fed to the reactor at a rate of 0.09 mmol per hour, (C6H5)3CB(C6F5)4 as a cocatalyst at a rate of 0.36 mmol per hour, and TIBA as an organoaluminum compound at a rate of 2.0 mmol per hour, to obtain a polymerization liquid of ethylene and propylene copolymer (softener component). The main catalyst was synthesized according to the method described in International Publication No. 98 / 49212. The softener component was obtained from the obtained polymerization liquid by flash drying. The molar ratio of the softener (ethylene unit / propylene unit) was 70 / 30, and the intrinsic viscosity [η] measured in decalin at 135°C was 0.2 dL / g.

[0069] As the crystalline olefin polymer (G) used in the examples and comparative examples, the following high-pressure low-density polyethylene was used. Nippon Unicar Co., Ltd. Product name: DND2450 MFR = 1.30g / 10min, density = 0.920g / cm 3 .

[0070] [Physical Properties of Uncrosslinked Copolymer Composition] (Mooney Viscosity (ML (1+4) 100℃) Mooney viscosity at 100℃ (ML(1+4) 100°C) was measured at 100°C using a Mooney viscometer (SMV202 model, manufactured by Shimadzu Corporation) in accordance with JIS K6300.

[0071] <Physical properties of molded body (crosslinked product)> (Tensile stress at break, tensile elongation at break) The tensile stress at break and the tensile elongation at break of the sheet were measured by the following method. The sheet was punched out to prepare No. 3 dumbbell test pieces described in JIS K 6251 (1993). Using these test pieces, tensile tests were performed according to the method specified in JIS K6251, section 3, at a measurement temperature of 25°C and a tensile speed of 500 mm / min, and the modulus at 100% elongation (M100), tensile stress at break (TB), and tensile elongation at break (EB) were measured.

[0072] (Durometer A hardness) In accordance with JIS K 6253, the sheet hardness (type A durometer, HA) was measured using six 2 mm sheet-like molded products with smooth surfaces, with the flat parts stacked to a thickness of approximately 12 mm.

[0073] (Injection moldability) Using an injection molding die, the ethylene-α-olefin-non-conjugated polyene copolymer composition (Compound 2) obtained in the Examples and Comparative Examples was injected at a die temperature of 170°C and held for 5 or 10 minutes to obtain a boot-shaped molded product with a thickness of 3 mm, in which the large diameter end and the small diameter end of the bellows portion were connected, and the four peaks (diameters: 95 mm, 93 mm, 83 mm, 75 mm) with peaks and valleys alternating in the axial direction, the intervals between the four peaks (25 mm, 30 mm, 15 mm), and three valleys (diameters: 69 mm, 65 mm, 49 mm). When the rubber boot-shaped crosslinked molding was removed from the mold, if the rubber boot-shaped crosslinked molding tore even partially, it was marked with "X", and if it could be removed without tearing, it was marked with "O".

[0074] Example 1 Using a MIXTRON BB MIXER (manufactured by Kobe Steel, BB-4 type, volume 2.95 L, rotor 4WH), 100 parts by mass of the copolymer (S-1) obtained in Production Example 1 and 100 parts by mass of the copolymer (S-1), 115 parts by mass of the mixture containing 15 parts by mass of the softener (liquid ethylene-propylene copolymer) obtained in Production Example 2, 20 parts by mass of the high-pressure low-density polyethylene (DND2450), 5 parts by mass of zinc oxide (ZnO#1) as a crosslinking aid, 2 parts by mass of stearic acid as a processing aid, 133 parts by mass of carbon black (trade name Asahi#60UG, manufactured by Asahi Carbon Co., Ltd.), 82 parts by mass of paraffin-based process oil (trade name Diana Process Oil PW-380, manufactured by Idemitsu Kosan Co., Ltd.) as a softener, and phenol-based antioxidant (trade name Irganox 1010) as an anti-aging agent. 1 part by mass of BASF Japan Ltd., 2 parts by mass of 2-mercaptobenzimidazole (product name: Sandant MB, manufactured by Sanshin Chemical Industry Co., Ltd.) as an anti-aging agent, and 1 part by mass of fatty acid amide (product name: Struktol WB212: calcium soap & saturated fatty acid amide mixture, manufactured by S&S Japan Co., Ltd.) as a lubricant were mixed and kneaded to obtain Compound 1.

[0075] The kneading conditions for preparation of compound 1 were rotor rotation speed of 50 rpm and floating weight pressure of 3 kg / cm 2 The kneading time was 5 minutes, and the kneading discharge temperature was 170°C. Mooney Viscosity ML of Formulation 1 (1+4) The viscosity was measured at 100°C using a Mooney viscometer (Shimadzu Corporation, Model SMV202) in accordance with JIS K6300 (1994).

[0076] Next, after confirming that the temperature of Compound 1 had reached 40°C, 12.5 parts by mass of dicumyl peroxide (trade name: Parkmil D-40 (dicumyl peroxide 40% by mass), manufactured by Nippon Oil & Fats Co., Ltd.) as a crosslinking agent and 3 parts by mass of trimethylolpropane trimethacrylate (trade name: Hi-Cross M, manufactured by Seiko Chemical Co., Ltd.) as a crosslinking aid were added to Compound 1 and kneaded using a 6-inch roll to obtain Compound 2.

[0077] The kneading conditions for preparing compound 2 were as follows: roll temperature: front roll / rear roll = 50°C / 50°C, roll peripheral speed: front roll / rear roll = 18 rpm / 15 rpm, roll gap: 2 mm, and kneading time: 8 minutes to obtain compound 2. Compound 2 was pressed at 170° C. for 10 minutes using a press molding machine to produce a crosslinked sheet having a thickness of 2 mm. The physical properties of the resulting crosslinked sheet were evaluated by the methods described above. The evaluation results are shown in Table 1.

[0078] Comparative Example 1 A crosslinked sheet was obtained in the same manner as in Example 1, except that the high-pressure low-density polyethylene (DND2450) was not used instead of the compound used in Example 1, and the types and amounts of additives were changed to those shown in Table 1. The physical properties of the crosslinked sheet were evaluated by the methods described above. The evaluation results are shown in Table 1.

[0079] Comparative Example 2 A crosslinked sheet was obtained in the same manner as in Example 1, except that the high-pressure low-density polyethylene (DND2450) was not used instead of the compound used in Example 1, and the types and amounts of additives were changed to those shown in Table 1. The physical properties of the crosslinked sheet were evaluated by the methods described above. The evaluation results are shown in Table 1.

[0080] Example 2 The same procedure as in Example 1 was repeated except that the zinc oxide (ZnO#1) was replaced with activated zinc oxide (product name META-Z102, manufactured by Inoue Sekiryo Kogyo Co., Ltd.), the fatty acid amide (product name Struktol WB212: mixture of calcium soap and saturated fatty acid amide, manufactured by S&S Japan Co., Ltd.) was replaced with Struktol WB16 (mixture of calcium soap and saturated fatty acid amide, product name: manufactured by S&S Japan Co., Ltd.) instead of the compounding materials used in Example 1, and the amounts of high-pressure low-density polyethylene and additives were changed to the amounts shown in Table 1. A crosslinked sheet was obtained, and its physical properties were evaluated by the methods described above. The evaluation results are shown in Table 1.

[0081] Example 3 The same procedure as in Example 1 was repeated except that the zinc oxide (ZnO#1) was replaced with activated zinc oxide (product name META-Z102, manufactured by Inoue Sekiryo Kogyo Co., Ltd.), the fatty acid amide (product name Struktol WB212: mixture of calcium soap and saturated fatty acid amide, manufactured by S&S Japan Co., Ltd.) was replaced with Struktol WB16 (mixture of calcium soap and saturated fatty acid amide, product name: manufactured by S&S Japan Co., Ltd.) instead of the compounding materials used in Example 1, and the amounts of high-pressure low-density polyethylene and additives were changed to the amounts shown in Table 1. A crosslinked sheet was obtained, and its physical properties were evaluated by the methods described above. The evaluation results are shown in Table 1.

[0082] Comparative Example 3 The procedure of Example 1 was repeated except that the amounts of additives used in Example 2 were changed to those shown in Table 1, to obtain a crosslinked sheet, and its physical properties were evaluated by the methods described above. The evaluation results are shown in Table 1.

[0083] [Table 1]

Claims

1. An ethylene-α-olefin-non-conjugated polyene copolymer (S) containing ethylene, an α-olefin having 3 or more carbon atoms, and a non-conjugated polyene as structural units, and containing, relative to 100 parts by mass of the ethylene-α-olefin-non-conjugated polyene copolymer (S), more than 10 parts by mass to 30 parts by mass of a crystalline olefin polymer (G), 10 to 300 parts by mass of carbon black (L), and 1 to 10 parts by mass of a fatty acid amide (M), The ethylene / α-olefin / non-conjugated polyene copolymer composition, wherein the crystalline olefin polymer (G) is a high-pressure low-density polyethylene (HP-LDPE).

2. The ethylene / α-olefin / non-conjugated polyene copolymer composition according to claim 1, characterized in that the ethylene / α-olefin / non-conjugated polyene copolymer (S) is an ethylene / α-olefin / non-conjugated polyene copolymer (S) that satisfies the following requirements (i) to (iv): (i) The molar ratio (structural units derived from ethylene (A) / structural units derived from an α-olefin having 3 to 20 carbon atoms (B)) is 40 / 60 to 99.9 / 0.

1. (ii) The content of the constituent units derived from the non-conjugated polyene (C) is in the range of 0.07 to 10 mass %. (iii) Mooney viscosity ML at 125°C (1+4) is in the range of 5 to 100. (iv) The intrinsic viscosity [η] measured in decalin at 135° C. is in the range of 0.1 to 5 dL / g.

3. The ethylene / α-olefin / non-conjugated polyene copolymer composition according to claim 1 or 2, wherein the α-olefin having 3 or more carbon atoms constituting the ethylene / α-olefin / non-conjugated polyene copolymer (S) is propylene.

4. An injection-molded article formed from the ethylene / α-olefin / non-conjugated polyene copolymer composition according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Rubber composition, vulcanized rubber composition, and radiator hose

    JP1994220266A

  • Rubber composition

    JP1996231782A

  • Rubber composition

    JP1998007849A

  • Air bag storage case

    JP1999208404A

  • Crosslinkable rubber composition and its use

    JP2001031809A