Resin fine particles and their uses

Resin fine particles with enhanced heat resistance and reduced residual monomer content are achieved through copolymerization with polyfunctional thiols, addressing compounding issues and maintaining optical transparency.

JP7585595B2Active Publication Date: 2024-11-19SEKISUI PLASTICS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020207851
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-15
Publication Date
2024-11-19
Estimated Expiration
2040-12-15

AI Technical Summary

Technical Problem

Existing resin fine particles, particularly organic ones, lack sufficient heat resistance during resin compounding and have high residual unreacted monomer content, leading to issues like resin smear and decreased yield.

Method used

The development of resin fine particles through copolymerization with a polyfunctional thiol antioxidant, incorporating monofunctional vinyl and alkyl (meth)acrylate monomers, and polyfunctional (meth)acrylate monomers to enhance heat resistance and reduce residual monomer content.

Benefits of technology

The resulting resin fine particles exhibit improved heat resistance, reduced residual monomer levels, and maintain optical transparency, minimizing resin smear and yield loss during compounding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585595000001
    Figure 0007585595000001
Patent Text Reader

Abstract

To provide resin fine particles useful as an antiblocking agent or the like which have sufficient resistance to thermal load in resin compounding, in which a residual amount of an unreacted monomer can sufficiently be reduced, and further which have a color tone imparting no influence to an optical property (colorless transparency) even when used for an optical member or the like requiring an extremely high optical property.SOLUTION: Resin fine particles comprise a copolymer including: one or more monofunctional vinyl-based monomer (A) units having a cyclic structure; one or more monofunctional alkyl (meth)acrylate-based monomer (B) units; one or more multifunctional (meth)acrylate-based monomer (C) units; and one or more multifunctional thiol (D) units in the molecular structure, in which a glass-transition temperature of a polymer formed of the monofunctional alkyl (meth)acrylate-based monomer (B) only is 50°C or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to resin fine particles. Specifically, the present invention relates to resin microparticles that are useful as antiblocking agents, have sufficient resistance to the thermal load applied during resin compounding, have a sufficiently reduced amount of unreacted monomer remaining in the resin microparticles, and have a color tone that does not affect the optical properties even when used in optical components, etc., that require extremely high optical properties (colorless transparency). [Background technology]

[0002] Resin films have been widely used for a long time as packaging materials and other applications. In recent years, their applications have expanded, and in particular, the properties required of resin films for optical components and electronic devices have become more advanced. The current challenge is to increase productivity while maintaining the high quality.

[0003] Resin films are often stored in rolls, but at the overlapping parts, the resin films can stick to each other (blocking), which can lead to poor slippage and peelability. Among them, COP (cyclic polyolefin) films have excellent optical properties and moisture absorption resistance, but are more susceptible to the above problems than PMMA (polymethyl methacrylate) films and TAC (triacetyl cellulose) films. To address this issue, it is known to use various fillers such as inorganic and organic fine particles as anti-sticking agents (anti-blocking agents). Representative fillers include inorganic fine particles such as silica, and organic fine particles such as (meth)acrylic resin fine particles.

[0004] The advantage of inorganic fine particles is that they are highly hard, and adding a small amount can provide anti-sticking properties. However, due to the nature of the material, there is a disadvantage that a difference in refractive index occurs between the inorganic fine particles and the resin film, which can cause a loss of transparency. On the other hand, organic fine particles have the advantage that they can be used in resin films that require high quality because they can maintain the transparency of the resin film and impart anti-sticking properties.

[0005] Patent Document 1 discloses organic microparticles characterized by having a base including a copolymer having alkyl(meth)acrylate monomer units whose alkyl group has 4 or more carbon atoms, crosslinkable monomer units, and alkyl(meth)acrylate monomer units whose alkyl group has 1 to 3 carbon atoms, and an outer layer provided on the surface of the base and including a copolymer having alkyl(meth)acrylate monomer units whose alkyl group has 4 or more carbon atoms, and crosslinkable monomer units. Patent Document 2 discloses resin microparticles containing a copolymer having an alkyl(meth)acrylate monomer unit having an alkyl group with 1 or more and 3 or less carbon atoms, an alkyl(meth)acrylate monomer unit having an alkyl group with 4 or more carbon atoms, and a crosslinkable (meth)acrylic monomer unit, and an antioxidant. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-057280 A [Patent Document 2] JP 2017-66362 A Summary of the Invention [Problem to be solved by the invention]

[0007] Organic fine particles, especially resin fine particles, are inferior in hardness to inorganic fine particles, so the amount of organic fine particles added must be increased to improve anti-sticking performance. An issue with increasing the amount of organic fine particles added is that it has a greater effect on film haze, etc. Another issue is that resin scum may be generated due to the heat load applied during resin compounding and unreacted monomers in the resin fine particles, which may result in a decrease in yield. Therefore, there is a demand for resin fine particles that are resistant to heat loads and have as little residual unreacted monomer as possible. According to the present inventors, the organic fine particles described in the above patent documents do not have sufficient heat resistance to the thermal load applied during resin compounding, and it is believed that the amount of remaining unreacted monomers cannot be sufficiently reduced.

[0008] An object of the present invention is to provide fine resin particles which have heat resistance sufficient to withstand the thermal load applied during resin compounding and in which the amount of remaining unreacted monomer in the fine resin particles is sufficiently reduced. [Means for solving the problem]

[0009] As a result of research conducted by the inventors to solve the above-mentioned problems, they discovered that by copolymerizing a specific monomer with a multifunctional thiol, which is an antioxidant, it is possible to impart heat resistance capable of withstanding the above-mentioned thermal load, thereby obtaining resin microparticles in which the amount of remaining unreacted monomer in the resin microparticles is sufficiently reduced, and thus they have completed the present invention. The present invention includes, but is not limited to, the following inventions. [1] Resin microparticles comprising a copolymer having one or more monofunctional vinyl monomer (A) units having a cyclic structure in the molecular structure, one or more monofunctional alkyl (meth)acrylate monomer (B) units, one or more polyfunctional (meth)acrylate monomer (C) units, and one or more polyfunctional thiol (D) units, wherein the glass transition temperature of the polymer consisting only of the monofunctional alkyl (meth)acrylate monomer (B) is 50°C or lower. [2] Resin microparticles according to [1], which are produced by seed polymerization in which seed particles are swelled with a monomer in a medium and then polymerized, the monomer comprising one or more monofunctional vinyl monomers (A) having a cyclic structure in the molecular structure, one or more monofunctional alkyl (meth)acrylate monomers (B), one or more polyfunctional (meth)acrylate monomers (C), and one or more polyfunctional thiols (D). [3] Resin microparticles according to [1] or [2], having a 5% thermal decomposition onset temperature of 345°C or higher in a nitrogen atmosphere and / or a weight loss rate of 30% or less after being held at 270°C for 40 minutes in an air atmosphere. [4] Resin microparticles according to any one of [1] to [3], in which the total residual monomer amount of the monofunctional vinyl monomer (A), the monofunctional alkyl (meth)acrylate monomer (B), and the polyfunctional (meth)acrylate monomer (C) having a cyclic structure in the molecular structure in the resin microparticles is 300 ppm by mass or less. [5] The resin fine particles according to any one of [1] to [4], wherein the content of elemental sulfur in the resin fine particles is 0.20 parts by mass or more. [6] The resin fine particles according to any one of [1] to [5], wherein the amount of residual surfactant in the resin fine particles is 10,000 ppm by mass or more and 30,000 ppm by mass or less. [7] The resin fine particles according to any one of [1] to [6], having a volume average primary particle diameter of 100 nm or more and 5,000 nm or less, and / or a coefficient of variation of the volume average primary particle diameter of 25% or less. [8] The resin fine particles according to any one of [1] to [7], wherein the polyfunctional (meth)acrylate monomer (C) is a bifunctional (meth)acrylate monomer. [9] The resin microparticles according to any one of [1] to [8], wherein the amount of the polyfunctional thiol (D) units is 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the total of the monofunctional vinyl monomer (A) units having a cyclic structure in the molecular structure, the monofunctional alkyl (meth)acrylate monomer (B) units, and the polyfunctional (meth)acrylate monomer (C) units.

[10] A granule formed by agglomerating multiple resin microparticles according to any one of [1] to [9].

[11] The resin microparticles or granules thereof according to any one of [1] to [9], which are used as an anti-sticking agent for resin films.

[12] The resin microparticles or granules thereof according to

[11] , wherein the resin film is a cyclic olefin resin film. Effect of the Invention

[0010] According to the present invention, there are provided fine resin particles which have heat resistance sufficient to withstand the thermal load applied during resin compounding and in which the amount of unreacted monomer remaining in the fine resin particles is sufficiently reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Resin fine particles] The resin microparticles according to the present invention are resin microparticles that contain a copolymer having one or more monofunctional vinyl monomer (A) units having a cyclic structure in the molecular structure, one or more monofunctional alkyl (meth)acrylate monomer (B) units, one or more polyfunctional (meth)acrylate monomer (C) units, and one or more polyfunctional thiol (D) units, and the glass transition temperature of the polymer consisting only of the monofunctional alkyl (meth)acrylate monomer (B) is 50°C or lower.

[0012] <Monofunctional vinyl monomer (A) having a cyclic structure in the molecular structure> The monofunctional vinyl monomer (A) having a cyclic structure in its molecular structure includes a monofunctional vinyl monomer having a cyclic structure such as an aromatic ring or an alicyclic ring in its molecular structure. For example, styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, ethylvinylbenzene, p-tert-butylstyrene, p-methoxystyrene, p-phenylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, vinylnaphthalene, styrenesulfonic acid, styrenesulfonates (sodium styrenesulfonate, ammonium styrenesulfonate, etc.), vinylbenzoic acid, hydroxystyrene, and other styrene monomers; vinylcycloolefin monomers such as vinylcyclohexane, vinylcycloheptane, and vinylcyclooctane; Examples of the cyclic olefin include cycloolefin monomers such as cyclohexene and 2-norbornene; (meth)acrylic acid esters having a cyclic structure in the ester portion, such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, and phenoxyethyl (meth)acrylate, 2-(meth)acryloyloxyethyl phthalate, and 2-(meth)acryloyloxyethyl hexahydrophthalate. In the present invention, monofunctional alkyl (meth)acrylate monomers having a cyclic structure in the molecular structure, such as benzyl (meth)acrylate and cyclohexyl (meth)acrylate, are treated as monofunctional vinyl monomers (A) having a cyclic structure in the molecular structure. Among these, styrene, α-methylstyrene, and sodium styrenesulfonate are preferred. These monofunctional vinyl monomers (A) having a cyclic structure in the molecular structure may be used alone or in combination of two or more.

[0013] <Monofunctional alkyl (meth)acrylate monomer (B)> The monofunctional alkyl(meth)acrylic monomer (B) is not particularly limited as long as the glass transition temperature Tg of a polymer consisting only of the monofunctional alkyl(meth)acrylate monomer (B) is 50° C. or lower. Here, the polymer consisting of only the monofunctional alkyl (meth)acrylic monomer (B) refers to a (co)polymer obtained by extracting only the monofunctional alkyl (meth)acrylic monomer from the monomers constituting the resin microparticles and polymerizing them while maintaining the mass ratio between the monomers. When only one type of monofunctional alkyl (meth)acrylic monomer (B) is used, this (co)polymer becomes a homopolymer, and when two or more types of monofunctional alkyl (meth)acrylic monomer (B) are used, this (co)polymer becomes a copolymer.

[0014] In the present invention, as the monofunctional alkyl (meth)acrylic monomer (B), one or more monofunctional alkyl (meth)acrylate monomers having a homopolymer glass transition temperature Tg of 50° C. or less may be used. In addition, one or more monofunctional alkyl (meth)acrylate monomers having a homopolymer glass transition temperature Tg of 50° C. or less may be used in combination with one or more monofunctional alkyl (meth)acrylate monomers having a homopolymer glass transition temperature Tg of more than 50° C., resulting in a combination of monomers having a copolymer glass transition temperature of 50° C. or less. Among these, it is preferable to use one or more monofunctional alkyl (meth)acrylate monomers having a homopolymer glass transition temperature Tg of 50° C. or less as the monofunctional alkyl (meth)acrylic monomer (B).

[0015] The present inventors speculate that if a monofunctional alkyl (meth)acrylate monomer (B) whose polymer consists solely of the monomer has a glass transition temperature Tg of 50° C. or less is used, the frequency of contact between the growing polymer chain and the unreacted monomer increases from the viewpoint of polymer chain driveability, and the amount of residual monomer can be reduced. However, the present inventors are not bound by this speculation.

[0016] In the present invention, the glass transition temperature Tg means a value obtained by converting the glass transition temperature Tga in absolute temperature obtained by the following formula (1) into Celsius temperature.

[0017] 1 / Tga = Σ(Wi / Tgi) (1) (In formula (1), Tga is the glass transition temperature (unit: absolute temperature) of a polymer consisting only of monofunctional alkyl (meth)acrylic monomer (B). Wi is the mass proportion of each monofunctional alkyl (meth)acrylic monomer i in a polymer consisting only of monofunctional alkyl (meth)acrylic monomer (B). Tgi is the glass transition temperature (unit: absolute temperature) of a homopolymer formed only from each monofunctional alkyl (meth)acrylic monomer i.

[0018] The above formula (1) is a formula called the FOX formula, which is a formula for calculating the glass transition temperature Tga of a polymer based on the glass transition temperature Tgi of a homopolymer of each monomer constituting a polymer, and details thereof are described in Bulletin of the American Physical Society, Series 2, Vol. 1, No. 3, p. 123 (1956). In addition, the glass transition temperatures (Tgi) of homopolymers of various monomers for calculation by the FOX formula can be, for example, numerical values ​​described in Painting and Paints (Paint Publishing Company, 10 (No. 358), 1982). In addition, the glass transition temperature of a homopolymer of a monomer whose glass transition temperature is unknown is an actual measured value for a homopolymer having a weight average molecular weight of about 20,000 to 50,000. This actual measurement is performed by vacuum suctioning the sample placed in the measurement cup to remove volatile components such as the solvent, and then using a differential scanning thermal analyzer "DSC-50Q" (product name, manufactured by Shimadzu Corporation) to measure the change in heat quantity in the range of -50°C to +150°C at a heating rate of 3°C / min, and using the first baseline change point on the low temperature side.

[0019] The glass transition temperature Tg of the polymer consisting of only the monofunctional alkyl(meth)acrylic monomer (B), which is calculated by converting the glass transition temperature calculated by the FOX formula into Celsius temperature, is 50° C. or lower, preferably 40° C. or lower, and more preferably 20° C. or lower. The lower limit of Tg is, for example, −50° C. or higher, and preferably −30° C. or higher.

[0020] Examples of the monofunctional alkyl (meth)acrylic monomer (B) include methyl (meth)acrylate (methyl methacrylate, methyl acrylate), ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, (meth) Examples of the alkyl (meth)acrylate ester include (meth)acrylic acid alkyl esters having 1 to 20 carbon atoms in the alkyl group bonded to the ester, such as nonyl acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isostearyl (meth)acrylate, and eicosyl (meth)acrylate, such as nonadecyl (meth)acrylate. Among these, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, and decyl (meth)acrylate are versatile and preferred, in which the number of carbon atoms in the alkyl group bonded to the ester is 1 to 10. In particular, in applications requiring heat resistance, it is preferred to include methyl methacrylate and n-butyl acrylate in terms of versatility, cost, and handling. These monofunctional alkyl (meth)acrylate monomers (B) may be used alone or in combination of two or more, so long as the glass transition temperature Tg of a polymer consisting only of the monofunctional alkyl (meth)acrylate monomers (B) is 50°C or lower.

[0021] Among these monofunctional alkyl (meth)acrylic monomers (B), examples of those having a homopolymer glass transition temperature Tg of 50° C. or less include 2-ethylhexyl acrylate (−70° C.), n-octyl acrylate (−65° C.), n-lauryl methacrylate (−65° C.), isodecyl acrylate (−60° C.), isooctyl acrylate (−58° C.), isononyl acrylate (−58° C.), n-butyl acrylate (−55° C.), tridecyl acrylate (−55° C.), isodecyl methacrylate (−41° C.), tridecyl methacrylate (−41° C.), and 2-ethylhexyl acrylate (−70° C.). Examples include acrylate (-40°C), isobutyl acrylate (-26°C), n-lauryl acrylate (-23°C), ethyl acrylate (-20°C), isostearyl acrylate (-18°C), 2-ethylhexyl methacrylate (-10°C), methyl acrylate (10°C), n-butyl methacrylate (20°C), n-stearyl acrylate (30°C), propyl methacrylate (35°C), n-stearyl methacrylate (38°C), and isobutyl methacrylate (48°C) (the temperatures in parentheses indicate the glass transition temperature Tg of the homopolymer.).

[0022] <Polyfunctional alkyl (meth)acrylate monomer (C)> Examples of the polyfunctional (meth)acrylic monomer (C) include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, decaethylene glycol di(meth)acrylate, pentadecaethylene glycol di(meth)acrylate, pentacontahexaethylene glycol di(meth)acrylate, 1,3-butylene di(meth)acrylate, allyl (meth)acrylate (allyl methacrylate, allyl acrylate), trimethylolpropane tri(meth)acrylate, pentaerythritol tetraacrylate, dipentaerythritol hexa(meth)acrylate, etc. Among these, bifunctional (meth)acrylate monomers such as ethylene glycol di(meth)acrylate (ethylene glycol dimethacrylate) and allyl (meth)acrylate (allyl methacrylate) are preferred. These polyfunctional (meth)acrylic monomers (C) may be used alone or in combination of two or more.

[0023] <Multifunctional thiol (D)> The polyfunctional thiol (D) is not particularly limited as long as it is a compound having two or more thiol groups in the molecule. For example, 1,2-ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,2-cyclohexanedithiol, decanedithiol, ethylene glycol bisthioglycolate, ethylene glycol bisthiopropionate, ethylene glycol bisthioglycolate (EGTG), 1,4-butanediol bisthiopropionate (BDTG), trimethylolpropane tristhioglycolate (TMTG), trimethylol Examples of the monomer include polyfunctional thiol group-containing monomers such as propane tristhiopropionate, pentaerythritol tetrakisthioglycolate (PETG), pentaerythritol tetrakisthiopropionate, dipentaerythritol hexathiopropionate, trimercaptopropionic acid tris(2-hydroxyethyl)isocyanurate, 1,4-dimethylmercaptobenzene, 2,4,6-trimercapto-s-triazine, and 2-(N,N-dibutylamino)-4,6-dimercapto-s-triazine. Among these, examples include one or more selected from the group consisting of ethylene glycol bisthioglycolate (EGTG), 1,4-butanediol bisthiopropionate (BDTG), trimethylolpropane tristhioglycolate (TMTG), and pentaerythritol tetrakisthioglycolate (PETG). These polyfunctional thiols (D) may be used alone or in combination of two or more.

[0024] <Other Monomers (E)> The resin microparticles of the present invention may contain other monomer (E) units other than the monofunctional vinyl monomer (A) units having a cyclic structure in the molecular structure, the monofunctional alkyl (meth)acrylate monomer (B) units, the polyfunctional (meth)acrylate monomer (C) units, and the polyfunctional thiol (D) units. Examples of the other monomer (E) include one or more selected from the group consisting of unsaturated carboxylic acid monomers such as (meth)acrylic acid and maleic acid, hydroxyalkyl (meth)acrylate monomers such as hydroxyethyl (meth)acrylate, (meth)acrylamide monomers, (meth)acrylonitrile monomers, halogenated vinyl monomers such as vinyl chloride, vinyl carboxylate monomers such as vinyl acetate, olefin monomers such as ethylene, unsaturated imide monomers, vinyl alcohol, divinyl monomers such as m-divinylbenzene, p-divinylbenzene and divinylnaphthalene, and the like. These other monomers (E) may be used alone or in combination of two or more.

[0025] <Quantity ratio of each unit> In the resin microparticles of the present invention, the quantitative ratio of each unit of the monofunctional vinyl monomer (A) unit having a cyclic structure in the molecular structure, the monofunctional alkyl (meth)acrylate monomer (B) unit, the polyfunctional (meth)acrylate monomer (C) unit, the polyfunctional thiol (D) unit, and the other monomer (E) unit is not particularly limited, but for example, the following quantitative ratios are preferred.

[0026] The amount of the monofunctional vinyl monomer (A) unit having a cyclic structure in the molecular structure can be, for example, 5 to 80 parts by mass, preferably 10 to 70 parts by mass, and more preferably 15 to 60 parts by mass, relative to 100 parts by mass in total of the units (A) to (E). If the amount of the (A) unit is less than 5 parts by mass, the difference in refractive index with respect to the film-forming binder resin may become large, which may result in a decrease in transparency when a film containing the resin fine particles is formed. If the amount of the (A) unit exceeds 80 parts by mass, the amount of residual monomer in the resin fine particles may not be reduced sufficiently.

[0027] The monofunctional alkyl (meth)acrylate monomer (B) unit can be, for example, 5 to 80 parts by mass, preferably 10 to 70 parts by mass, and more preferably 15 to 60 parts by mass, per 100 parts by mass of the total of the (A) to (E) units. If the amount of the (B) unit is less than 5 parts by mass, the amount of residual monomer in the resin fine particles may not be reduced sufficiently. If the amount of (B) units exceeds 80 parts by mass, the resin fine particles will have excessive softness, and the desired effects may not be obtained.

[0028] The amount of the polyfunctional (meth)acrylate monomer (C) unit relative to 100 parts by mass of the total of the (A) to (E) units can be, for example, 5 to 50 parts by mass, preferably 7 to 40 parts by mass, more preferably 10 to 30 parts by mass, and even more preferably 15 to 24 parts by mass. When the amount of the (C) unit is within this range, the solvent resistance of the particles is improved, and deformation of the particles when incorporated into a film can be prevented. If the amount of the polyfunctional (meth)acrylate monomer (C) unit is less than 5 parts by mass, the degree of crosslinking of the resin microparticles will be low, and when a resin composition in which the resin microparticles are mixed with a binder resin is used as a coating liquid, the resin microparticles will swell, causing an increase in the viscosity of the coating liquid and reducing the workability of the coating. As a result of the low degree of crosslinking of the resin microparticles, when the resin microparticles are heated in applications in which the resin microparticles are mixed with a binder and molded (so-called kneading applications), the resin microparticles are likely to dissolve or deform. If the amount of the polyfunctional (meth)acrylate monomer (C) unit is 50 parts by mass or more, the improvement in effect commensurate with the amount used may not be achieved, and the production cost may increase.

[0029] The polyfunctional thiol (D) unit can be, for example, 0.05 to 20 parts by mass, preferably 0.1 to 15 parts by mass, and more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the total of the (A) to (E) units. If the (D) unit is less than 0.05 parts by mass, the heat resistance of the resin fine particles against the heat load during resin compounding may decrease, and if it exceeds 20 parts by mass, the resin fine particles may emit a sulfur odor, reducing the commercial value.

[0030] The amount of the other monomer units (E) may be, for example, 0 to 70 parts by mass, preferably 0 to 50 parts by mass, and more preferably 0 to 25 parts by mass, relative to 100 parts by mass of the total of the units (A) to (E). If the amount of the units (E) exceeds 70 parts by mass, there is a risk of a decrease in heat resistance and an increase in the amount of unreacted monomer remaining in the resin fine particles.

[0031] <Thermal decomposition temperature and weight loss rate> The thermal decomposition starting temperature of the resin fine particles of the present invention in a nitrogen atmosphere is preferably 300° C. or higher, and more preferably 330° C. or higher. If the thermal decomposition starting temperature is lower than 300° C., the resin fine particles cannot withstand the heat load during resin compounding, and resin scum is generated, which may cause a decrease in yield. In the present invention, a thermogravimetric and differential thermal analyzer is used to thermally decompose resin fine particles according to the methods and conditions described in the Examples below, and the thermal decomposition onset temperature is determined from the obtained TG / DTA curve using analysis software provided with the apparatus.

[0032] In order to ensure heat resistance, the resin fine particles of the present invention have a weight loss rate due to decomposition of the organic components of the polymer after being kept in an air atmosphere at 270° C. for 40 minutes of 30% or less, preferably 20% or less, and more preferably 15% or less. If the weight loss rate exceeds 30%, the heat resistance of the resin fine particles decreases, and the resin fine particles cannot withstand the heat load during resin compounding, which may cause resin scumming and reduced yield. In the present invention, a thermogravimetric and differential thermal analyzer is used to hold the resin particles at 270° C. for 40 minutes under the conditions described in the Examples below, and the heat loss is measured to determine the weight loss rate.

[0033] <Residual monomer amount> The resin microparticles of the present invention have a reduced amount of residual monomers, and the total amount of residual monomers of the monofunctional vinyl monomer (A), the monofunctional alkyl (meth)acrylate monomer (B), and the polyfunctional (meth)acrylate monomer (C) in the resin microparticles can be, for example, 300 mass ppm or less, preferably 200 mass ppm or less, and more preferably 100 mass ppm or less. If the total amount of residual monomers of the monofunctional vinyl monomer (A), the monofunctional alkyl (meth)acrylate monomer (B), and the polyfunctional (meth)acrylate monomer (C) in the resin microparticles exceeds 300 mass ppm, resin scum may occur when compounding a resin composition containing the resin microparticles.

[0034] In the present invention, the total residual monomer amount of the monofunctional vinyl monomer (A), the monofunctional alkyl (meth)acrylate monomer (B), and the polyfunctional (meth)acrylate monomer (C) in the resin microparticles can be determined, for example, by the following method. 5 mL of methanol is added to 0.01 g of resin microparticles, thoroughly mixed, and then allowed to stand for 24 hours to obtain a dispersion. The dispersion is then centrifuged for 30 minutes at a stirring speed of 18,500 rpm to precipitate insoluble matter. The amount of residual monomer relative to the resin microparticles is measured by analyzing 2 μL of the resulting supernatant using an ultra-high performance liquid chromatogram La Chrom Ultra (Hitachi High-Technologies Corporation). The measurement conditions are as follows: La Chrom Ultra C18 2 μm column, column temperature 40° C., solvent 0.05% trifluoroacetic acid aqueous solution and acetonitrile mixture (50 / 50 w / w), flow rate 0.6 mL / min.

[0035] <Amount of residual monomer in gas generated when resin particles are heated to 300℃> The resin microparticles of the present invention have a reduced amount of residual monomers, and the total amount of residual monomers, which is the monofunctional vinyl monomer (A) having a cyclic structure in its molecular structure, the monofunctional alkyl (meth)acrylate monomer (B), and the polyfunctional (meth)acrylate monomer (C) in the gas generated when the resin microparticles are heated to 300°C, can be, for example, 5000 ppm by mass or less, preferably 4000 ppm by mass or less, and more preferably 3000 ppm by mass or less. When the resin microparticles are heated to 300°C, the gas generated contains monofunctional vinyl monomer (A) having a cyclic structure in its molecular structure, monofunctional alkyl (meth)acrylate monomer (B), and polyfunctional (meth)acrylate monomer (C). If the total amount of residual monomers exceeds 5,000 ppm by mass, resin scum may be generated when compounding a resin composition containing the resin microparticles.

[0036] In the present invention, the total amount of remaining monomers, that is, the monofunctional vinyl monomer (A) having a cyclic structure in its molecular structure, the monofunctional alkyl (meth)acrylate monomer (B), and the polyfunctional (meth)acrylate monomer (C) in the gas generated when the resin microparticles are heated to 300°C, can be obtained using a thermal desorption-gas chromatograph / mass spectrometer (TD-GC / MS). The total amount of residual monomers, which are monofunctional vinyl monomer (A) having a cyclic structure in its molecular structure, monofunctional alkyl (meth)acrylate monomer (B), and polyfunctional (meth)acrylate monomer (C) in the gas generated when resin microparticles are heated to 300°C, can be measured by TD-GC / MS using, for example, the method described in the Examples and Comparative Examples below.

[0037] <Sulfur content> The resin fine particles of the present invention contain sulfur element derived from the polyfunctional thiol and the seed particles, etc. The content of sulfur element in the present invention is determined by fluorescent X-ray analysis. The content of the sulfur element is not particularly limited and is appropriately set according to the purpose and use. For example, it can be 0.20 parts by mass or more, preferably 0.25 parts by mass or more. Also, for example, it can be 0.75 parts by mass or less. If the content of sulfur element in the resin microparticles is less than 0.20 parts by mass, the ratio of polyfunctional thiol present in the copolymer will be low, and the desired heat resistance may not be obtained. If the content is more than 0.75 parts by mass, the odor of the resin microparticles may become strong. The sulfur element content can be measured by fluorescent X-ray analysis, for example, by the method described in the Examples and Comparative Examples below.

[0038] <Residual surfactant amount> The amount of residual surfactant contained in the resin microparticles of the present invention is not particularly limited, and is appropriately set according to the purpose and use. For example, it can be 10000 mass ppm or more, preferably 15000 mass ppm or more, more preferably 20000 mass ppm or more with respect to the resin microparticles. When the amount of residual surfactant is 10000 mass ppm or more, it is considered that the residual surfactant contributes to the dispersibility of the resin microparticles during resin compounding, and the dispersibility of the resin microparticles in the resin composition becomes good. In addition, when the amount of residual surfactant is less than 100 mass ppm, the manufacturing process of the resin microparticles becomes complicated, which may be disadvantageous in terms of cost and the like. When the amount of residual surfactant exceeds 100000 mass ppm, foaming may occur when the resin microparticles are dispersed in a medium.

[0039] The amount of the remaining surfactant in the present invention can be determined, for example, as follows. The resin particles were extracted with a solvent and measured using a liquid chromatograph linear ion trap mass spectrometer (LC / MS / MS device). As the LC / MS / MS device, "UHPLC ACCELA" manufactured by Thermo Fisher Scientific and "Linear Ion Trap LC / MSnLXQ" manufactured by Thermo Fisher Scientific can be used.

[0040] The surfactant content is measured by the following method. Approximately 0.01 g of resin microparticles were precisely weighed into a centrifuge tube, the extraction liquid was poured in, and the resin microparticles and the extraction liquid were thoroughly mixed. After ultrasonic extraction, the mixture was mixed again and centrifuged, and the resulting supernatant was filtered to prepare the test liquid. The concentration of the surfactant in this test solution was measured using an LC / MS / MS device, and the content was calculated from the peak area value on the obtained chromatogram using a calibration curve prepared in advance.The surfactant content in the resin microparticles was then calculated using the following formula from the measured surfactant concentration in the test solution, the weight of the resin microparticles used as a sample (sample weight), and the amount of the extracted solution.

[0041] Surfactant content = surfactant concentration in test solution x volume of extract ÷ sample weight The method for creating the calibration curve is as follows. After preparing an intermediate standard solution (methanol solution) of the surfactant at approximately 1000 ppm by mass, the solution was further diluted stepwise with methanol to prepare standard solutions for creating a calibration curve at 20 ppm by mass, 10 ppm by mass, 5 ppm by mass, and 2.5 ppm by mass. The standard solutions for creating a calibration curve at each concentration were measured under the following conditions, and the peak area values ​​on the chromatogram of the monitor ion m / z=730 to 830 were obtained. Each concentration and the area value were plotted to obtain an approximation curve (quadratic curve) by the least squares method, and this was used as the calibration curve for quantification.

[0042] <Volume average primary particle size / Variation coefficient of volume average primary particle size> The volume average primary particle diameter of the resin fine particles of the present invention is not particularly limited and is appropriately set depending on the purpose and use. For example, it can be 100 nm or more and 5000 nm or less, preferably 100 nm or more and 3000 nm or less, and more preferably 100 nm or more and 1000 nm or less. The coefficient of variation of the volume average primary particle diameter of the resin fine particles of the present invention is not particularly limited and is appropriately set depending on the purpose and use. For example, it can be 25% or less, preferably 20% or less, and more preferably 15% or less.

[0043] The volume average primary particle size and the coefficient of variation can be measured using a laser scattering / diffraction particle size distribution analyzer LS230 (manufactured by Beckman Coulter). Water was used as the dispersion medium for the sample, and the refractive index of the polymer was used as the refractive index of the sample. The volume average particle size here is a value calculated by arithmetic average. The coefficient of variation is a value calculated from the following formula (2), and represents the distribution width of the data. Coefficient of variation (%) = standard deviation × 100 / volume average primary particle size (2)

[0044] [Method of manufacturing resin particles] The method for producing the resin fine particles of the present invention (polymerization method) is not particularly limited as long as it is a known polymerization method, for example, seed polymerization, emulsion polymerization, suspension polymerization, dispersion polymerization, etc. In the method for producing resin fine particles (polymerization method) of the present invention, a polymerization initiator, a surfactant (emulsifier), a dispersant, etc. can be used as necessary.

[0045] <Polymerization method> Seed polymerization is a method in which polymer fine particles obtained by polymerizing a monomer are used as seed particles, the seed particles are made to absorb the monomer in a medium, the seed particles are swollen with the monomer, and then the monomer is polymerized within the seed particles. In seed polymerization, by growing the seed particles, resin fine particles having a particle size larger than that of the original seed particles can be obtained. Emulsion polymerization is a polymerization method in which an aqueous medium, a monomer that is poorly soluble in the medium, and a surfactant (emulsifier) ​​are mixed, and a polymerization initiator that is soluble in the aqueous medium is added to the mixture to carry out polymerization. Emulsion polymerization is characterized by the fact that the particle size of the resulting resin microparticles is small. Suspension polymerization is a polymerization method in which a monomer and an aqueous medium are mechanically stirred to suspend the monomer in the aqueous medium and polymerize it. The particles produced by suspension polymerization have a larger particle size and a broader particle size distribution than those produced by the above-mentioned emulsion polymerization. In addition, it is possible to obtain particles having a relatively sharp particle size distribution by using a fine emulsifier such as a homogenizer, an ultrasonic processor, or a Nanomizer (registered trademark). Dispersion polymerization is a method in which a monomer is dispersed in a polymerization solvent that may contain a dispersion stabilizer, a polymerization initiator is added, and the monomer is polymerized. In order to prevent the particles from adhering to each other during polymerization, it is preferable to carry out the polymerization under stirring by ultrasonic irradiation and / or stirring by a mechanical stirring device such as a magnetic stirrer. Dispersion polymerization is characterized by the fact that the particle size is easy to control and resin fine particles can be easily obtained. In the present invention, a method of obtaining resin fine particles by seed polymerization is preferably used.

[0046] <Polymerization initiator> The polymerization initiator used in producing the resin fine particles of the present invention is not particularly limited and may be any known polymerization initiator. When a non-nitrile azo-based polymerization initiator is used, the resin particles may be colored yellow. Therefore, when the resin particles are used in applications requiring extremely high optical properties, such as optical components, the color tone of the resin particles may not meet the requirements.

[0047] The polymerization initiator is preferably a radical polymerization initiator, particularly a thermal polymerization initiator, such as persulfates (e.g., ammonium persulfate, potassium persulfate, sodium persulfate, etc.), hydrogen peroxide, organic peroxides, and nitrile-azo compounds. For example, organic peroxides such as cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, benzoyl peroxide, lauroyl peroxide, dimethylbis(tert-butylperoxy)hexane, dimethylbis(tert-butylperoxy)hexyne-3, bis(tert-butylperoxyisopropyl)benzene, bis(tert-butylperoxy)trimethylcyclohexane, butyl-bis(tert-butylperoxy)valerate, tert-butyl 2-ethylhexaneperoxy acid, dibenzoyl peroxide, paramenthane hydroperoxide, and tert-butyl peroxybenzoate; 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-isopropylbutyronite), aryl), 2,2'-azobis(2,3-dimethylbutyronitrile), 2,2'-azobis(2,4-dimethylbutyronitrile), 2,2'-azobis(2-methylcapronitrile), 2,2'-azobis(2,3,3-trimethylbutyronitrile), 2,2'-azobis(2,4,4-trimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-meth Examples of the nitrile-azo compounds include 2,2'-azobis(4-ethoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(4-n-butoxy-2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2-(carbamoylazo)isobutyronitrile, and 4,4'-azobis(4-cyanopentanoic acid).

[0048] Furthermore, a redox initiator obtained by combining the above-mentioned persulfate and organic peroxide polymerization initiator with a reducing agent such as sodium sulfoxylate formaldehyde, sodium hydrogen sulfite, ammonium hydrogen sulfite, sodium thiosulfate, ammonium thiosulfate, hydrogen peroxide, sodium hydroxymethanesulfinate, L-ascorbic acid and its salts, cuprous salts, and ferrous salts may be used as the polymerization initiator.

[0049] Among these, there may be mentioned one or more selected from the group consisting of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 4,4'-azobis(4-cyanopentanoic acid), cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, benzoyl peroxide, and lauroyl peroxide. These polymerization initiators may be used alone or in combination of two or more.

[0050] In the present invention, the amount of the polymerization initiator used varies depending on the type thereof, but can be in the range of 0.1 to 5.0 parts by mass, more preferably 0.2 to 3.0 parts by mass, and even more preferably 0.3 to 1.0 parts by mass, relative to 100 parts by mass of the total amount of all monomers used in the polymerization.

[0051] <Surfactant> The surfactant that can be used in the preparation of seed particles used in preparing the resin fine particles of the present invention by seed polymerization is not particularly limited, but it is preferable to use one or more reactive surfactants. Examples of the anionic reactive surfactant include styrenesulfonic acid metal salts such as Spinomer (registered trademark) Nass (manufactured by Tosoh Finechem Corporation), Eleminol (registered trademark) JS-20 and RS-3000 manufactured by Sanyo Chemical Industries, Aqualon (registered trademark) KH-10, KH-1025, KH-05, HS-10, HS-1025, BC-0515, BC-10, BC-1025, BC-20, BC-2020, AR-1025, and AR-2025 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., Latemul (registered trademark) S-120, S-180A, S-180, and PD-104 manufactured by Kao Corporation, and Adeka Reasoap (registered trademark) SR-1025 and SE-10N manufactured by ADEKA Corporation. These anionic reactive surfactants may be used alone or in combination of two or more.

[0052] Examples of nonionic reactive surfactants include alkyl ether surfactants (commercially available products include ADEKA ADEKA REASOAP ER-10, ER-20, ER-30, and ER-40, and Kao LATEMURU PD-420, PD-430, and PD-450); alkyl phenyl ether surfactants or alkyl phenyl ester surfactants (commercially available products include Aqualon RN-10, RN-20, RN-30, RN-50, AN-10, AN-20, AN-30, and AN-5065, and ADEKA ADEKA REASOAP NE-10, NE-20, NE-30, and NE-40, and (meth)acrylate sulfate surfactants (commercially available products include Nippon Nyukazai RMA-564, RMA-568, and RMA-1114, and the like). These nonionic reactive surfactants may be used alone or in combination of two or more.

[0053] In preparing the resin fine particles of the present invention, at least one surfactant selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants and nonionic surfactants is used.

[0054] Examples of anionic surfactants include sodium oleate; fatty acid soaps such as castor oil potassium soap; alkyl sulfate ester salts such as sodium lauryl sulfate and ammonium lauryl sulfate; alkyl benzene sulfonates such as sodium dodecylbenzene sulfonate; alkyl naphthalene sulfonates; alkanesulfonates; dialkyl sulfosuccinates; alkyl phosphate ester salts; naphthalenesulfonate-formaldehyde condensates; polyoxyethylene alkyl phenyl ether sulfate ester salts; polyoxyethylene sulfonated phenyl ether phosphate; polyoxyethylene alkyl sulfate ester salts, and the like.

[0055] Examples of nonionic surfactants include polyoxyalkylene branched decyl ethers, polyoxyethylene tridecyl ethers, polyoxyalkylene alkyl ethers, polyoxyalkylene tridecyl ethers, polyoxyethylene isodecyl ethers, polyoxyalkylene lauryl ethers, polyoxyalkylene alkyl ethers, polyether polyols, polyoxyethylene styrenated phenyl ethers, polyoxyethylene naphthyl ethers, polyoxyethylene phenyl ethers, polyoxyethylene polyoxypropylene glycols, polyoxyethylene lauryl ethers, polyoxyethylene oleyl cetyl ethers, polyoxyethylene glyceryl isostearate, polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxysorbitan fatty acid esters, polyoxyethylene alkylamines, glycerin fatty acid esters, and oxyethylene-oxypropylene block polymers.

[0056] Examples of the cationic surfactant include alkylamine salts such as laurylamine acetate and stearylamine acetate; and quaternary ammonium salts such as lauryltrimethylammonium chloride. Examples of the zwitterionic surfactant include lauryl dimethylamine oxide, phosphate surfactants, and phosphite surfactants.

[0057] These surfactants may be used alone or in combination of two or more. The type of surfactant is appropriately selected and the amount used is appropriately adjusted in consideration of the particle size of the resulting resin microparticles and the dispersion stability of the monomer during polymerization.

[0058] The amount of the surfactant used may be in the range of preferably 0.01 to 20 parts by mass, more preferably 0.05 to 15 parts by mass, and even more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of all the monomers.

[0059] <Dispersant> The dispersant that can be used in the method for producing resin microparticles of the present invention is not particularly limited. When an aqueous medium is used during polymerization, the dispersant can be used to stabilize the dispersibility of monomer droplets and seed particles. Examples of the dispersant include organic dispersants such as partially saponified polyvinyl alcohol, polyacrylates, polyvinylpyrrolidone, carboxymethylcellulose, and methylcellulose, and inorganic dispersants such as magnesium pyrophosphate, calcium pyrophosphate, calcium phosphate, calcium carbonate, magnesium phosphate, magnesium carbonate, and magnesium oxide. When an inorganic dispersant is used, it is preferable to use a surfactant in combination.

[0060] These dispersants may be used alone or in combination of two or more. The type of dispersant is appropriately selected and the amount used is appropriately adjusted in consideration of the particle size of the resulting resin microparticles and the dispersion stability of the monomer during polymerization.

[0061] <Polymerization medium> The polymerization medium that can be used in the method for producing resin microparticles of the present invention is not particularly limited. It may be an aqueous medium or an organic medium (organic solvent). In the present invention, it is preferable to use an aqueous medium. As the aqueous medium, for example, water alone or a mixture of water and a water-soluble organic solvent such as a lower alcohol (methanol, ethanol, isopropyl alcohol, etc.) can be used. From the viewpoint of waste liquid treatment, water alone is preferred. The amount of the aqueous medium used can be within the range of 200 to 2000 parts by mass, preferably within the range of 300 to 1500 parts by mass, based on 100 parts by mass of the total amount of all monomers used in polymerization. By setting the amount of the aqueous medium used to be equal to or higher than the lower limit of the above range, the stability of the monomer particles during polymerization can be maintained, and the generation of aggregates of resin fine particles after polymerization can be suppressed. By setting the amount of the aqueous medium used to be equal to or lower than the upper limit, productivity tends to be good.

[0062] (Seed polymerization) The method for polymerizing a monomer to obtain seed particles to be used in seed polymerization is not particularly limited, but dispersion polymerization, emulsion polymerization, soap-free emulsion polymerization (emulsion polymerization without using a surfactant as an emulsifier), seed polymerization, suspension polymerization, etc. can be used. In order to obtain resin microparticles with a substantially uniform particle size by seed polymerization, it is necessary to first use seed particles with a substantially uniform particle size and grow these seed particles substantially uniformly. The seed particles with a substantially uniform particle size that serve as the raw material can be produced by polymerization using a polymerization method such as soap-free emulsion polymerization of monomers (emulsion polymerization without using a surfactant), polymerization using a surfactant, and dispersion polymerization. The surfactant is not particularly limited, but it is preferable to use a reactive surfactant. Therefore, as a polymerization method for obtaining seed particles by polymerizing a monomer, emulsion polymerization, soap-free emulsion polymerization, seed polymerization, and dispersion polymerization are preferable.

[0063] In the polymerization for obtaining seed particles, a polymerization initiator is used as necessary. The polymerization initiator is not particularly limited, but a water-soluble radical polymerization initiator is preferably used. The amount of the polymerization initiator used is preferably within the range of 0.1 to 2 parts by mass relative to 100 parts by mass of the monomer used for obtaining the seed particles. If the amount is less than 0.1 parts by mass, the reaction rate is slow and the efficiency is poor, and if the amount is more than 2.0 parts by mass, there is a risk of excessive initiator residue.

[0064] When polymerization is performed to obtain seed particles, a molecular weight regulator may be used to adjust the weight average molecular weight of the resulting seed particles. As the molecular weight regulator, for example, mercaptans such as n-octyl mercaptan and tert-dodecyl mercaptan; α-methylstyrene dimer; terpenes such as γ-terpinene and dipentene; halogenated hydrocarbons such as chloroform and carbon tetrachloride can be used. The weight average molecular weight of the resulting seed particles can be adjusted by adjusting the amount of the molecular weight regulator used. The volume average particle size of the seed particles can be appropriately adjusted depending on the average particle size of the resin fine particles, and is preferably in the range of 1 to 2000 nm.

[0065] In the seed polymerization, seed particles are first added to an emulsion containing a monomer and an aqueous medium. The emulsion can be prepared by a known method. For example, an emulsion can be obtained by adding a monomer to an aqueous medium and dispersing the monomer with a microemulsifier such as a homogenizer, an ultrasonic processor, or a Nanomizer (registered trademark).

[0066] In the seed polymerization, it is preferable to use 0.3 to 15 parts by mass of a surfactant per 100 parts by mass of the monomer absorbed in the seed particles. The above-mentioned surfactants can be used as the surfactant. If the amount of the surfactant used is less than the above range, the polymerization stability may be reduced. If the amount of the surfactant used is more than the above range, the amount of the surfactant remaining in the resin fine particles becomes excessive, and foaming may occur when the resin fine particles are dispersed in a medium.

[0067] The seed particles may be added to the emulsion as they are, or may be added to the emulsion in a form dispersed in an aqueous medium. After the seed particles are added to the emulsion, the monomer is absorbed into the seed particles. This absorption can usually be carried out by stirring the emulsion at room temperature (about 25°C) for 1 to 12 hours. In addition, in order to promote the absorption of the monomer into the seed particles, the emulsion may be heated to about 30 to 50°C.

[0068] The seed particles swell by absorbing the monomer. The mixing ratio of the monomer to the seed particles is preferably within the range of 1 to 100 parts by mass of the monomer per 1 part by mass of the seed particles, more preferably within the range of 5 to 50 parts by mass. If the mixing ratio of the monomer is smaller than the above range, the increase in particle size due to polymerization is small, and the production efficiency decreases. On the other hand, if the mixing ratio of the monomer is larger than the above range, the monomer is not completely absorbed into the seed particles, and may be independently emulsion-polymerized in the aqueous medium, resulting in the production of resin microparticles with an abnormal particle size that is not intended. The end of the absorption of the monomer into the seed particles can be determined by confirming the expansion of the particle size by observation with an optical microscope.

[0069] Next, the monomer absorbed in the seed particles is polymerized to obtain a resin particle dispersion liquid. The resin particle dispersion liquid may be obtained by repeating the process of absorbing the monomer in the seed particles and polymerizing the monomer several times. When the monomer absorbed in the seed particles is polymerized, a polymerization initiator may be added as necessary. After mixing the polymerization initiator with the monomer, the resulting mixture may be dispersed in an aqueous medium, or the polymerization initiator and the monomer may be separately dispersed in an aqueous medium and then mixed. The particle size of the droplets of the monomer present in the resulting emulsion is preferably smaller than the particle size of the seed particles, since the monomer is efficiently absorbed by the seed particles.

[0070] As the polymerization initiator, the above-mentioned polymerization initiators can be used. The polymerization initiator is preferably used in an amount of 0 to 3 parts by mass relative to 100 parts by mass of the monomer.

[0071] The polymerization temperature for the seed polymerization can be appropriately selected depending on the type of monomer and the type of polymerization initiator used as necessary, and can be, for example, 25 to 110°C, and preferably 50 to 100°C. The polymerization time for seed polymerization can be appropriately selected depending on the type of monomer and the type of polymerization initiator used as necessary, and can be, for example, 1 to 12 hours. The seed polymerization may be carried out under an atmosphere of a gas inert to the polymerization (eg, nitrogen). In the seed polymerization, it is preferable to carry out the polymerization at an elevated temperature after the monomer and the polymerization initiator, which is used if necessary, are completely absorbed into the seed particles.

[0072] In the seed polymerization, in order to improve the dispersion stability of the resin particles, the above-mentioned dispersant may be added to the polymerization reaction system as a dispersion stabilizer. Among these dispersion stabilizers, polyvinyl alcohol and polyvinylpyrrolidone are preferred. The amount of the dispersion stabilizer added is preferably within the range of 1 to 10 parts by mass per 100 parts by mass of the monomer.

[0073] In order to suppress the generation of emulsion polymerization products (resin fine particles having too small a particle size) in the aqueous medium during the polymerization reaction, a water-soluble polymerization inhibitor such as nitrites such as sodium nitrite, sulfites, hydroquinones, ascorbic acids, water-soluble vitamin B, citric acid, polyphenols, etc. may be added to the aqueous medium. The amount of the polymerization inhibitor added can be within a range of, for example, 0.002 to 0.2 parts by mass per 100 parts by mass of the monomer.

[0074] A preferred embodiment of the method for producing resin microparticles of the present invention is a method for producing resin microparticles, which includes a first polymerization step in which an emulsion containing a monomer, an aqueous medium, and a surfactant is polymerized with a water-soluble polymerization initiator in a nitrogen-substituted polymerization vessel to obtain seed particles, and a second polymerization step in which the emulsion containing the monomer, the aqueous medium, and the surfactant is absorbed into the seed particles and then polymerized.

[0075] <Cleaning, drying, crushing and classification of resin particles> After the polymerization is completed, the resin fine particles can be washed, dried, crushed, classified, etc., as necessary. For example, after the polymerization is completed, the resin fine particles can be made into a cake containing an aqueous medium (water-containing cake) by a method such as suction filtration, centrifugation, pressure separation, etc., and after a washing step with water and / or a solvent as necessary, the cake can be dried in a drying step, and if necessary, a crushing step and a classification step can be performed to isolate the cake as a dry powder.

[0076] The washing method in the washing step is not particularly limited. For example, the aqueous dispersion obtained after polymerization can be washed by centrifugal washing, cross-flow filtration washing, etc. Alternatively, after forming a cake, it can be immersed in water and / or a solvent and then dehydrated. Note that, when a reactive emulsifier is used, the washing of the aqueous dispersion obtained after polymerization can be omitted. The drying method in the drying step is not particularly limited, and may be, for example, a spray drying method using a spray dryer, a freeze drying method, or a drying method in which the mixture is attached to a heated rotating drum such as a drum dryer. The classification method in the classification step is not particularly limited. For example, the resin fine particles or granules can be classified by a known means using a sieve or the like. The classification step preferably includes at least one of a first classification step for classifying the resin fine particles obtained in the second polymerization step and a classification step for classifying the resin fine particles obtained in the crushing step. In addition, a classification step may be used in which the aqueous dispersion obtained after polymerization is dispersed in an organic solvent such as alcohol, toluene, or ketone as necessary, and the dispersed state is passed through a sieve to remove coarse particles.

[0077] [Granules] The resin fine particles of the present invention can be formed into granules constituted by agglomeration of a plurality of resin fine particles. The granules can be obtained by a spray drying step in which the resin fine particles obtained in the polymerization step are spray-dried to obtain granules under conditions of, for example, an inlet temperature of 80 to 220° C. and an outlet temperature of 50 to 100° C. The obtained granules are easier to handle than the resin fine particles themselves.

[0078] In the present invention, a crushing step may be included in which the obtained granules are crushed to disperse the resin fine particles. For example, in the dry type, a crushing step using a mechanical crusher such as a blade mill or a super rotor, or an airflow type crusher such as a nanogrinding mill (jet mill) can be used, and in the wet type, a crushing step using a bead mill, a ball mill, a hammer mill, etc. The resin fine particles dispersed by crushing have good dispersibility in a solvent. In the present invention, it is preferable to include a classification step of classifying the granules. Classification can be carried out by known means. The volume average particle size of the granules of the present invention can be, for example, from 5 to 200 μm, and preferably from 10 to 100 μm.

[0079] [Applications of resin particles] The resin microparticles or granules thereof of the present invention have very high optical properties (colorless transparency), are resistant to heat load, and have a minimal amount of remaining unreacted monomer. Therefore, even if the amount of the resin is increased when forming a resin composition, the effect on the haze of the film can be suppressed. In addition, the occurrence of resin scum due to the heat load applied during resin compounding or the unreacted monomer in the resin microparticles is suppressed, and there is little risk of the yield being deteriorated.

[0080] Taking advantage of these characteristics, the resin microparticles or granules thereof of the present invention can be used for various applications, such as anti-sticking agents (anti-blocking agents) for resin molded products (resin films), modifiers for various resin molded products, optical members such as light diffusion plates, additives for paints, spacers between minute parts of various electronic devices, pore-forming agents for various battery members, and core particles for conductive microparticles that perform electrical connection. For example, the resin fine particles themselves can be mixed with a resin as an anti-sticking agent (anti-blocking agent) for a resin film to form a resin composition, and a resin molded product such as a film can be formed. In particular, the resin fine particles of the present invention have very high optical properties (colorless transparency) and are useful as an anti-sticking agent (anti-blocking agent) for a cyclic olefin resin film. For example, a resin composition containing resin fine particles and a resin binder can be formed, and this can be used to obtain optical members such as optical films, such as antiglare films and light diffusion films, and light diffusion plates, particularly antiglare members. For example, a coating material can be obtained from the resin fine particles themselves or a mixture of the resin fine particles with a binder resin, additives, and the like. For example, the resin particles themselves or a mixture of the resin particles and a resin can be molded to obtain a resin molded product. EXAMPLES

[0081] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited thereto. The volume average particle size, CV value (coefficient of variation of particle size on a volume basis), and thermal decomposition starting temperature of the obtained resin fine particles were determined by the following methods.

[0082] [5% thermal decomposition start temperature] The thermal weight loss of resin particles is measured using a differential thermal and thermogravimetric simultaneous measurement device "TG / DTA6200" (manufactured by SII Nano Technology Co., Ltd.). The sampling method and temperature conditions are as follows. The sample is packed into a platinum measurement container with about 15 mg of sample so that there are no gaps at the bottom, and alumina is used as the reference material under a nitrogen gas flow rate of 230 mL / min. The temperature condition is to obtain a TG / DTA curve when the temperature is raised from 30°C to 800°C at a rate of 10°C / min. The thermal decomposition onset temperature is calculated from the obtained curve using the analysis software attached to the device. The thermal decomposition onset temperature here refers to the mass loss onset temperature described in JIS K7120:1987 "Thermogravimetric measurement method for plastics" (8 "How to read TG curves"), and is the value calculated from the standard.

[0083] [Weight reduction rate] The resin microparticles were held in air at 270°C for 40 minutes, and the heat loss after that was measured using a thermogravimetric and differential thermal analyzer "TG / DTA6200" (manufactured by SII NanoTechnology Co., Ltd.) and used as the weight loss rate. When measuring the heat loss, the temperature was raised from room temperature to 200°C at a rate of about 40°C / min, and the rate of temperature rise was then gradually decreased, the time taken to reach 270°C from room temperature was adjusted to 20 minutes, and the point at which 270°C was reached was set as time 0, and the weight loss was measured after holding the material for 40 minutes.

[0084] [Method for measuring the amount of residual monomer in resin particles] Add 5 mL of methanol to 0.01 g of resin microparticles, mix well, and then let it stand for 24 hours to obtain a dispersion. Next, precipitate the insoluble matter by treating the dispersion with a centrifuge at a stirring rotation speed of 18,500 rpm for 30 minutes. Measure the amount of residual monomer in the vinyl polymer particles by analyzing 2 μL of the obtained supernatant with an ultra-high performance liquid chromatogram "La Chrom Ultra" (manufactured by Hitachi High-Technologies Corporation). The measurement conditions are as follows: use "La Chrom Ultra C18" 2 μm as the column and set the column temperature to 40°C. The solvent used is a mixture of 0.05% trifluoroacetic acid aqueous solution and acetonitrile (50 / 50 w / w), and the flow rate is set to 0.6 mL / min.

[0085] [Method for Measuring the Amount of Residual Monomer in the Gas Generated When Resin Microparticles are Heated to 300°C] (Measurement Method of TD-GC / MS) Using "Multi-shot Pyrolizer 3030D" (manufactured by Frontier Lab) and "GC / MS (7890 / 5977)" (manufactured by Agilent), the amount of residual monomer in the gas generated when resin microparticles are heated to 300°C was measured. Weigh the resin microparticles into a dedicated analysis container, trap the gas generated under the above heating conditions with liquid nitrogen, and perform thermal extraction (Desorp)-GC / MS analysis. Note that toluene (C7H8) was used as the standard substance for quantification, and the quantitative calculation was performed in terms of toluene conversion by comparing the area values of each peak with the area of the standard substance.

[0086] <Thermal Extraction Conditions> Initial temperature = 80°C (held for 0 min) First-stage heating rate = 20°C / min (up to 300°C) Final temperature = 300°C (held for 15 min) <GC / MS Measurement Conditions> Carrier gas = He He flow rate = 1 mL / min Inlet temperature = 280°C Interface temperature = 290°C Ionization energy = 70 eV Detection method = Scan method (m / z = 33 to 600)

[0087] [Method of measuring sulfur content] Using the X-ray fluorescence analyzer "ZSX PrimusIV" (manufactured by Rigaku Corporation), the S-Kα intensity was measured under the following conditions, and C7H 10 The sulfur element content was measured with O3 as the balance. The sample was prepared by weighing 10 mg of sample onto a carbon sample stage (manufactured by Nissin EM Co., Ltd.) and adjusting the sample so that it did not expand beyond 10 mmφ. After that, it was covered with PP film "Cat No. 3399G003" (manufactured by Rigaku Co., Ltd.) and set in the 10 mmφ sample case included with the device, and used as the measurement sample.

[0088] <Equipment conditions> Equipment: Fluorescent X-ray measurement device "ZSX PrimusIV" (manufactured by Rigaku Corporation) X-ray tube = vertical Rh tube (3.0KW) Analysis diameter=10mmφ Spin = No Atmosphere = vacuum Sample form: Metal Balance component = C7H 10 O3 Sample film = PPFilm Set sample weight = thickness

[0089] <Qualitative elemental conditions> S-Kα Tube=Rh(30kV-100mA) 1st filter = OUT Attenuator = 1 / 1 Slit=S4 Analyzing crystal = GeH 2θ=110.830deg (measurement range=107=115deg) PHA=150~300 Step=0.05deg Time=0.15sec

[0090] [Method for measuring the amount of residual surfactant] The resin particles were extracted with a solvent (methanol) and measured using a liquid chromatograph linear ion trap mass spectrometer (LC / MS / MS device) "ACCELA UHPLC" (manufactured by Thermo Fisher Scientific). The surfactant content was measured by the following method. Approximately 0.05 g of resin particles were weighed out into a centrifuge tube. After pouring the methanol extract into the centrifuge tube, the resin particles and the extract were thoroughly mixed. After ultrasonic extraction for approximately 15 minutes, the mixture was mixed again and centrifuged at 3500 rpm for 15 minutes. The resulting supernatant was filtered to prepare the test solution. The concentration of the surfactant in this test solution was measured by using the liquid chromatograph linear ion trap mass spectrometer (LC / MS / MS device), and the content was calculated from the peak area value on the obtained chromatogram using a calibration curve prepared in advance.Then, the surfactant content in the resin microparticles was calculated from the measured surfactant concentration in the test solution, the weight of the resin microparticles used as a sample (sample weight), and the amount of the extracted solution using the following calculation formula. Surfactant content = surfactant concentration in test solution x volume of extract ÷ sample weight

[0091] The method for preparing calibration curves for the three surfactants used (sodium dioctyl sulfosuccinate, nonylphenol ethoxylate, and polyoxyalkylene styrenated phenyl ether) is as follows. After preparing an intermediate standard solution (methanol solution) of about 1000 mass ppm of the surfactant, it was further diluted stepwise with methanol to prepare standard solutions for creating a calibration curve of 20 mass ppm, 10 mass ppm, 5 mass ppm, and 2.5 mass ppm. The standard solutions for creating a calibration curve of each concentration were measured under the following conditions, and the peak area values ​​on the chromatogram of the monitor ions m / z = 421.3 → 227.2 (sodium dioctyl sulfosuccinate), 502.3 → 485.2 (nonylphenol ethoxylate), and 587.6 → 526.7 (polyoxyalkylene styrenated phenyl ether) were obtained. Each concentration and the area value were plotted to obtain an approximation curve (quadratic curve) by the least squares method, and this was used as the calibration curve for quantification.

[0092] <LC measurement conditions> Apparatus = "ACCELA UHPLC" (manufactured by Thermo Fisher Scientific) Column = "Hypersil GOLD C18" 1.9 μm (2.1 mm I.D. × 100 mm L) (manufactured by Thermo Fisher Scientific) Column temperature = 40 °C Mobile phase = (A: 10 mM ammonium acetate / B: acetonitrile) Mobile phase conditions = (0 min = B conc. 90%, 0 → 0.5 min = B conc. 90% → 100%, 0.5 → 1.0 min = B conc. 100%, 1.0 → 1.1 min = B conc. 100 → 90%, 1.1 min → 3.5 min = B conc. 90%) Flow rate = 0.3 mL / min Pump temperature = room temperature Injection volume = 2 μL

[0093] <MS / MS measurement conditions> Apparatus = "LXQ" Linear Ion Trap LC / MS / MS (manufactured by Thermo Fisher Scientific) Ionization = ESI / negative Sheath Gas / AUX Gas / Sweep Gas = 30 / 10 / 0 arb Spray Voltage = 5.0 kV Capillary Temp = 350 °C Capillary voltage / Tube Lens = -20 / -100 V Monitoring Mass (m / z) = Sodium dioctyl sulfosuccinate (421.3 → 227.2), Nonylphenol ethoxylate (502.3 → 485.2), Polyoxyalkylene styrenated phenyl ether (587.6 → 526.7)

[0094] [Volume average particle diameter] The volume average particle size and number average particle size of the resin microparticles were measured using a laser diffraction scattering particle size distribution analyzer "LS230" (manufactured by Beckman Coulter). Specifically, 0.1 g of the resin microparticle water dispersion (20% solid content) and 20 ml of 2% by mass anionic surfactant solution were placed in a test tube. Then, the mixture was dispersed for 5 minutes using a test tube mixer "Test Tube Mixer TRIO HM-1N" (manufactured by AS ONE Corporation) and an ultrasonic cleaner "ULTRASONIC CLEANER VS-150" (manufactured by AS ONE Corporation) to obtain a dispersion. The volume average particle size and number average particle size of the resin microparticles in the dispersion were measured using a laser diffraction scattering particle size distribution analyzer while irradiating the dispersion with ultrasonic waves. The measurement conditions for the laser diffraction scattering particle size distribution analyzer are as follows.

[0095] <Measurement conditions for laser diffraction / scattering particle size distribution analyzer> medium = water Refractive index of medium = 1.333 Refractive index of solid = Refractive index of resin particles PIDS relative concentration: 40-55% The optical model used in the measurement was adjusted to the refractive index of the resin microparticles produced. In the present invention, in which multiple types of monomers are used to produce the resin microparticles, the refractive index of the resin microparticles was determined as an average value obtained by weighting the refractive index of the homopolymer of each monomer by the amount (parts by mass) of each monomer used. From the measurement results, a volumetric particle size distribution of the resin fine particles was obtained, and the arithmetic mean of the volumetric particle size distribution was taken as the volumetric average particle diameter of the resin fine particles.

[0096] [CV value (coefficient of variation of particle size based on volume)] The coefficient of variation (CV value) of the volume-based particle size of the resin fine particles was calculated by the following formula. Coefficient of variation of volume-based particle size of resin microparticles=[(Standard deviation of volume-based particle size distribution of resin microparticles) / (Volume average particle size of resin microparticles)]×100

[0097] [Seed particle production example] In a polymerization vessel equipped with a stirrer, a thermometer, and a cooling mechanism, 270 parts by mass of ion-exchanged water and 0.07 parts by mass of sodium styrenesulfonate were mixed to prepare an aqueous phase. 120 parts by mass of methyl methacrylate and 2.4 parts by mass of 1-octanethiol were mixed in another vessel and poured into the aqueous phase in the polymerization vessel. After purging the polymerization vessel with nitrogen for 5 minutes, the temperature was raised to 80°C, and when the temperature reached 80°C, 0.05 parts of potassium persulfate dissolved in 10 parts by mass of ion-exchanged water was poured in. Thereafter, nitrogen purging was carried out again for 5 minutes, and the mixture was stirred at 80°C for 5 hours to cause an emulsion polymerization reaction. After this, the mixture was heated to 100°C, held for 3 hours, and then cooled to prepare a slurry containing resin fine particles. This was used as a seed particle.

[0098] [Example 1] In a polymerization vessel equipped with a stirrer, a thermometer, and a cooling mechanism, 260 parts by mass of ion-exchanged water, 0.13 parts by mass of Rapisol (registered trademark) A-80 (manufactured by NOF Corporation), 0.13 parts by mass of Phosphanol LO-529 (manufactured by Toho Chemical Industry Co., Ltd.), 0.13 parts by mass of Noigen EA-167 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 0.022 parts by mass of sodium nitrite were mixed to prepare an aqueous phase. In a separate container, 52 parts by mass of methyl methacrylate, 39 parts by mass of styrene, 39 parts by mass of ethylene glycol dimethacrylate, 0.65 parts by mass of pentaerythritol tetrakisthioglycolate, 0.65 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile), and 0.2 parts by mass of benzoyl peroxide were thoroughly mixed to prepare an oil phase. The oil phase was added to the aqueous phase in the polymerization vessel, and the mixture was stirred at 8000 rpm for 10 minutes with a TK homomixer (manufactured by Primix Corporation) to obtain a monomer mixture. 21.7 parts by mass of seed particles A produced in Production Example 1 were added to this monomer mixture, and the mixture was stirred for 3 hours to cause swelling. After that, nitrogen was purged for 5 minutes, and the mixture was heated to 55°C, and stirred at 55°C for 5 hours to cause a polymerization reaction. After adding 0.066 parts by mass of sulfamic acid, the mixture was heated to 100°C, held for 3 hours, and then cooled to produce a resin fine particle-containing slurry. The slurry containing fine resin particles was passed through a 400 Mesh screen to classify the fine resin particles, thereby obtaining a classified fine resin particle slurry. The volume average primary particle diameter of the obtained resin fine particles was 0.489 μm (489 nm), and the coefficient of variation (CV value) of the volume average primary particle diameter was 13.9%. Table 1 also shows the 5% thermal decomposition starting temperature [°C], weight loss rate [%], residual monomer amount [ppm by mass], sulfur element content [parts by mass] and residual surfactant amount [ppm by mass] of the obtained resin microparticles.

[0099] The classified resin microparticle slurry was spray-dried under the following equipment conditions using a spray dryer (manufactured by Sakamoto Giken Co., Ltd., machine name: spray dryer, type: atomizer take-up type, model number: TRS-3WK) to obtain a granulated resin microparticle.

[0100] <Equipment conditions> Slurry supply rate containing resin particles: 25mL / min Atomizer rotation speed: 12000 rpm Air volume: 2m 3 / min Inlet temperature (temperature of the slurry inlet containing resin fine particles, which is provided in the spray dryer and through which the slurry containing resin fine particles is sprayed and introduced): 150°C Outlet temperature (the temperature of the powder outlet from which the resin fine particle granules are discharged from the spray dryer): 70°C

[0101] [Examples 2 and 3 and Comparative Examples 1 and 2] Table 1 shows the monomer, polyfunctional thiol, polymerization initiator, and their amounts (mass ratio) used in the polymerization of the resin microparticles according to Examples 2 and 3 and Comparative Examples 1 and 2. Table 1 also shows the 5% thermal decomposition starting temperature [°C], weight loss rate [%], remaining monomer amount [ppm by mass], sulfur element content [parts by mass], remaining surfactant amount [ppm by mass], volume average primary particle size [μm], and CV value [%] of the obtained resin microparticles.

[0102] [Comparative Example 3] In a polymerization vessel equipped with a stirrer, a thermometer, and a cooling mechanism, 2 parts by mass of magnesium pyrophosphate and 0.03 parts by mass of Rapisol (registered trademark) A-80 (manufactured by NOF Corporation) as suspension stabilizers were added to 100 parts by mass of ion-exchanged water to prepare an aqueous phase. An oil phase was prepared by thoroughly mixing 20 parts by mass of methyl methacrylate, 15 parts by mass of styrene, 15 parts by mass of ethylene glycol dimethacrylate, 2.5 parts by mass of pentaerythritol tetrakisthioglycolate, 2.5 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile), and 1.0 part by mass of benzoyl peroxide. The oil phase was added to the aqueous phase in the polymerization vessel and stirred at 8000 rpm for 10 minutes with a TK homomixer (manufactured by Primix Corporation) to obtain a monomer mixture. After purging with nitrogen for 5 minutes, the temperature was raised to 55°C and the mixture was stirred at 55°C for 5 hours to cause a polymerization reaction. After adding 0.01 parts by mass of sulfamic acid, the mixture was heated to 100°C, held for 3 hours, and then cooled to produce a slurry containing resin fine particles. Hydrochloric acid was added to the resulting slurry containing resin particles to decompose the magnesium pyrophosphate, and the resin particles were extracted by suction filtration. After repeated washing with water and purification, the resin particles were dried in a vacuum oven at 60°C to obtain resin particles. The 5% thermal decomposition onset temperature [°C], weight loss rate [%], residual monomer amount [ppm by mass], sulfur element content [parts by mass], residual surfactant amount [ppm by mass], volume average primary particle diameter [μm] and CV value [%] of the obtained resin microparticles are also shown in Table 1.

[0103] [Table 1]

[0104] In Table 1, the rows from MMA to BPO indicate the parts by mass (mass ratio) of the compounds used in producing the resin microparticles, and the compounds represented by each abbreviation are as follows. MMA: Methyl methacrylate BA: Butyl acrylate St: styrene EGDMA: Ethylene glycol dimethacrylate PETG: Pentaerythritol tetrakisthioglycolate ABN-V: 2,2'-azobis(2,4-dimethylvaleronitrile) BPO: Benzoyl peroxide

[0105] The present invention can be embodied in various other forms without departing from its spirit or main characteristics. Therefore, the above-described embodiments are merely illustrative in all respects and should not be interpreted as being limiting. The scope of the present invention is defined by the claims and is not limited to the text of the specification. Furthermore, all modifications and changes within the scope of the claims are within the scope of the present invention.

Claims

1. The copolymer includes one or more monofunctional vinyl monomer (A) units having a cyclic structure in the molecular structure, one or more monofunctional alkyl (meth)acrylate monomer (B) units, one or more polyfunctional (meth)acrylate monomer (C) units, and one or more polyfunctional thiol (D) units, the amount of the monofunctional vinyl monomer (A) unit having a cyclic structure in its molecular structure is 5 to 80 parts by mass, the amount of the monofunctional alkyl (meth)acrylate monomer (B) unit is 5 to 80 parts by mass, the amount of the polyfunctional (meth)acrylate monomer (C) unit is 5 to 50 parts by mass, and the amount of the polyfunctional thiol (D) unit is 0.05 to 20 parts by mass, relative to 100 parts by mass of the total of all units of the copolymer; The glass transition temperature of the polymer consisting only of the monofunctional alkyl (meth)acrylate monomer (B) is 50° C. or lower, The 5% thermal decomposition starting temperature in a nitrogen atmosphere is 345°C or higher, and / or the weight loss rate after being held at 270°C for 40 minutes in an air atmosphere is 30% or less. Resin fine particles.

2. The resin microparticles according to claim 1, which are produced by seed polymerization in which seed particles are swelled with a monomer in a medium and then polymerized, and the monomer comprises one or more monofunctional vinyl monomers (A) having a cyclic structure in the molecular structure, one or more monofunctional alkyl (meth)acrylate monomers (B), one or more polyfunctional (meth)acrylate monomers (C), and one or more polyfunctional thiols (D).

3. 3. The resin microparticle according to claim 1, wherein the total residual monomer amount of the monofunctional vinyl monomer (A) having a cyclic structure in its molecular structure, the monofunctional alkyl (meth)acrylate monomer (B), and the polyfunctional (meth)acrylate monomer (C) in the resin microparticle is 300 mass ppm or less.

4. 4. The resin fine particles according to claim 1, wherein the amount of residual surfactant in the resin fine particles is 10,000 ppm by mass or more and 30,000 ppm by mass or less.

5. 5. The resin fine particles according to claim 1, having a volume average primary particle diameter of 100 nm or more and 5000 nm or less, and / or a coefficient of variation of the volume average primary particle diameter of 25% or less.

6. The resin fine particles according to any one of claims 1 to 5, wherein the polyfunctional (meth)acrylate monomer (C) is a bifunctional (meth)acrylate monomer.

7. The resin microparticles according to any one of claims 1 to 6, wherein the amount of the polyfunctional thiol (D) unit is 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the total of the monofunctional vinyl monomer (A) unit having a cyclic structure in its molecular structure, the monofunctional alkyl (meth)acrylate monomer (B) unit, and the polyfunctional (meth)acrylate monomer (C) unit.

8. A granule formed by agglomerating a plurality of the resin fine particles according to any one of claims 1 to 7.

9. The resin fine particles according to any one of claims 1 to 7, which are used as an anti-sticking agent for a resin film.

10. The resin fine particles according to claim 9 , wherein the resin film is a cyclic olefin resin film.

11. The granule described in claim 8, used as an anti-sticking agent for resin films.

12. The granule described in claim 11, wherein the resin film is a cyclic olefin resin film.

Citation Information

Patent Citations

  • Toner and binder resin for toner

    JP2006337395A

  • Crosslinked (METH)acrylic polymer particle, method for producing it, and light diffusible resin composition

    JP2009161600A

  • Polymer fine particles and their manufacturing method

    JP2010095598A

  • Porous resin particle, method for producing the porous resin particle, and use thereof

    JP2013227535A

  • Organic polymer particle

    JP2017057280A