Epoxy resin composition for fiber-reinforced composite materials, prepreg and fiber-reinforced composite material
The epoxy resin composition with controlled ratios of components achieves both high elastic modulus and deflection, addressing the trade-off issue in existing technologies, resulting in improved mechanical properties for fiber-reinforced composites.
Patent Information
- Application Number
- JP2020150249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-09-08
AI Technical Summary
Existing epoxy resin compositions for fiber-reinforced composite materials face a trade-off between elastic modulus and deflection, with improvements in deflection often leading to a decrease in elastic modulus, making it difficult to achieve both mechanical properties simultaneously.
An epoxy resin composition comprising specific ratios of epoxy resin, amine curing agent, phenolic compound, and curing accelerator, with defined XB, XC1, and XB+XC1 ranges, to enhance both elastic modulus and deflection.
The composition achieves a cured resin product with excellent elastic modulus and deflection, suitable for high-performance fiber-reinforced composite materials.
Smart Images

Figure 0007585671000001 
Figure 0007585671000002 
Figure 0007585671000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin composition which is preferably used as a matrix resin for fiber-reinforced composite materials suitable for aerospace applications, sports applications, and general industrial applications, and to a prepreg and a fiber-reinforced composite material using the same as a matrix resin. [Background technology]
[0002] Fiber-reinforced composite materials using carbon fibers, aramid fibers, etc. as reinforcing fibers have excellent specific strength and specific elastic modulus, and are therefore widely used in structural materials for aircraft and automobiles, and in materials for sports such as tennis racket frames, golf shafts, fishing rods, and bicycle frames. Methods for producing fiber-reinforced composite materials include a method in which multiple sheets of prepreg, a sheet-shaped molding material in which reinforcing fibers are impregnated with an uncured resin composition, are laminated and then heated and cured, and a resin transfer molding method in which liquid resin is poured into reinforcing fibers arranged in a mold and then heated and cured. Among these manufacturing methods, the method using prepreg has the advantage that it is easy to obtain high-performance fiber-reinforced composite materials because the orientation of the reinforcing fibers can be strictly controlled and there is a high degree of freedom in designing the laminate structure. As the resin composition used in this prepreg, an epoxy resin composition with excellent mechanical properties, heat resistance, and handling properties is widely used.
[0003] Epoxy resin compositions used in fiber-reinforced composite materials are required to achieve both elastic modulus and deflection after curing. In particular, improved deflection is required to increase the 90° strength, impact resistance, and fatigue properties of fiber-reinforced composite materials. Reducing the crosslink density of the cured epoxy resin is effective for improving deflection, but lowering the crosslink density often results in a decrease in elastic modulus, and there is a trade-off between the deflection and elastic modulus of the cured resin. Therefore, achieving both elastic modulus and deflection of the cured resin has been an extremely difficult task.
[0004] As a method for solving this problem, Patent Document 1 describes a technique for improving the deflection and elastic modulus of a cured resin by using a phenolic compound in combination with a resin composition consisting of an epoxy resin, an amine-based curing agent, and a curing accelerator. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-284852 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, even when the technique described in Patent Document 1 is used, the mechanical properties of the resulting cured resin and fiber-reinforced composite materials are not sufficient, and further improvement in the mechanical properties is required.
[0007] Therefore, an object of the present invention is to provide an epoxy resin composition excellent in elastic modulus and deflection, and a prepreg and a fiber-reinforced composite material each using the epoxy resin composition. [Means for solving the problem]
[0008] The present invention employs the following means to solve the above problems. That is, the epoxy resin composition of the present invention is an epoxy resin composition for fiber-reinforced composite materials, which comprises the following components [A], [B], [C], and [D], and satisfies all of the following conditions (i) to (iii): Component [A]: Epoxy resin Component [B]: Amine-based hardener Component [C]: Phenolic compounds Component [D]: Curing accelerator Condition (i): When the ratio of the number of active hydrogens in the component [B] to the number of epoxy groups in the component [A] is XB, XB is in the range of 0.1 to 0.4. Condition (ii): When the phenol compound represented by formula (1) among the components [C] is defined as [C1] and the ratio of the number of active hydrogens in the component [C1] to the number of epoxy groups in the component [A] is defined as XC1, XC1 is in the range of 0.3 to 0.9.
[0009] [ka]
[0010] (In formula (1), R 1 ~R 5 R represents a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a methoxy group, a hydroxyl group, or a halogen, and may all be the same or different, but at least two are hydroxyl groups. 6 ~R 10 represents a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a methoxy group, or a halogen, and may all be the same or different. X represents no element, SO 2 , C.H. 2 , CH(CH 3 ), C(CH 3 ) 2 , S, O, or C=O.) Condition (iii): XB+XC1 is in the range of 0.4 to 1.0.
[0011] The prepreg of the present invention is a prepreg comprising reinforcing fibers and the above-mentioned epoxy resin composition.
[0012] Furthermore, the fiber-reinforced composite material of the present invention is a fiber-reinforced composite material comprising reinforcing fibers and a cured product of the above-mentioned epoxy resin composition. Effect of the Invention
[0013] According to the present invention, it is possible to obtain an epoxy resin composition excellent in elastic modulus and deflection, as well as a prepreg and a fiber-reinforced composite material using the epoxy resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The epoxy resin composition of the present invention contains, as essential components, [A] an epoxy resin, [B] an amine-based curing agent, [C] a phenolic compound, and [D] a curing accelerator. First, these components will be described.
[0015] (Component [A]) The component [A] in the present invention is an epoxy resin. An epoxy resin is a compound having an epoxy group in the molecule. When [A] is an epoxy resin having two or more epoxy groups in one molecule, it is preferable because the glass transition temperature of the resin cured product obtained by curing the epoxy resin composition is high. A monofunctional epoxy resin having one epoxy group in one molecule may be contained within a range that does not significantly adversely affect the heat resistance and mechanical properties of the prepreg or fiber-reinforced composite material of the present invention.
[0016] Examples of such epoxy resins include bisphenol A type, bisphenol F type, diaminodiphenylmethane type, diaminodiphenylsulfone type, aminophenol type, metaxylenediamine type, 1,3-bisaminomethylcyclohexane type, isocyanurate type, hydantoin type, phenol novolac type, orthocresol novolac type, trishydroxyphenylmethane type, and tetraphenylolethane type epoxy resins, etc. These epoxy resins may be used alone or in combination.
[0017] Commercially available bisphenol A type epoxy resins include jER (registered trademark) 828 (manufactured by Mitsubishi Chemical Corporation), Epicron (registered trademark) 850 (manufactured by DIC Corporation), Epotohto (registered trademark) YD-128 (manufactured by Tohto Kasei Co., Ltd.), and DER-331 and DER-332 (all manufactured by The Dow Chemical Company).
[0018] Commercially available bisphenol F type epoxy resins include "Araldite (registered trademark)" GY282 (manufactured by Huntsman Advanced Materials), "jER (registered trademark)" 806, "jER (registered trademark)" 807, "jER (registered trademark)" 1750 (all manufactured by Mitsubishi Chemical Corporation), "Epicron (registered trademark)" 830 (manufactured by DIC Corporation), and "Epotohto (registered trademark)" YD-170 (manufactured by Tohto Kasei Co., Ltd.).
[0019] Commercially available diaminodiphenylmethane epoxy resins include ELM434 (manufactured by Sumitomo Chemical Co., Ltd.), Araldite (registered trademark) MY720 (manufactured by Huntsman Advanced Materials Co., Ltd.), Araldite (registered trademark) MY721 (manufactured by Huntsman Advanced Materials Co., Ltd.), Araldite (registered trademark) MY9512 (manufactured by Huntsman Advanced Materials Co., Ltd.), Araldite (registered trademark) MY9663 (manufactured by Huntsman Advanced Materials Co., Ltd.), Epotohto (registered trademark) YH-434 (manufactured by Tohto Kasei Co., Ltd.), and jER (registered trademark) 630 (manufactured by Mitsubishi Chemical Corporation).
[0020] Commercially available diaminodiphenylsulfone type epoxy resins include TG3DAS (manufactured by Mitsui Fine Chemicals, Inc.).
[0021] Commercially available aminophenol type epoxy resins include ELM120 (manufactured by Sumitomo Chemical Co., Ltd.), ELM100 (manufactured by Sumitomo Chemical Co., Ltd.), jER (registered trademark) 630 (manufactured by Mitsubishi Chemical Corporation), Araldite (registered trademark) MY0500 (manufactured by Huntsman Advanced Materials Co., Ltd.), Araldite (registered trademark) MY0510 (manufactured by Huntsman Advanced Materials Co., Ltd.), Araldite (registered trademark) MY0600 (manufactured by Huntsman Advanced Materials Co., Ltd.), and Araldite (registered trademark) MY0610 (manufactured by Huntsman Advanced Materials Co., Ltd.).
[0022] The epoxy resin composition of the present invention may contain epoxy resins other than those mentioned above as appropriate, provided that the object of the present invention is not impaired.
[0023] (Component [B]) The component [B] of the present invention is an amine-based curing agent, for example, an aromatic amine such as diaminodiphenylmethane or diaminodiphenylsulfone, or an aliphatic amine such as dicyandiamide, triethylenetetramine, or isophoronediamine.
[0024] The amine-based curing agent preferably contains aromatic amines and / or dicyandiamide, from the viewpoint of excellent storage stability and curing properties of the resulting resin composition. Among these, dicyandiamide is more preferably used, from the viewpoint of excellent storage stability and curing properties.
[0025] As the content of the component [B] in the present invention, when the equivalent ratio of the epoxy resin in the epoxy resin composition to the amine-based curing agent, that is, the ratio of the number of active hydrogens of the amine-based curing agent to the number of epoxy groups of the epoxy resin in the epoxy resin composition (number of active hydrogens of the amine-based curing agent / number of epoxy groups of the epoxy resin) is XB, XB must be in the range of 0.1 to 0.4, and XB is preferably in the range of 0.1 to 0.3. By setting XB in this range, a resin cured product excellent in elastic modulus and deflection can be obtained. Usually, in order to obtain an epoxy resin cured product excellent in deflection, the number of epoxy groups of the epoxy resin and the number of active hydrogens of the curing agent are made equal to each other in order to reduce unreacted functional groups as much as possible, that is, XB is often made close to 1.0, but in the present invention, since the component [C] described later also reacts with the epoxy resin, it is important to reduce the content of the component [B].
[0026] (Component [C]) The component [C] of the present invention is a phenol compound, such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, bisphenol Z, dihydroxynaphthalene, (phenylenediisopropylidene)bisphenol, and halogen- or alkyl-substituted derivatives thereof.
[0027] In the present invention, it is necessary to contain a phenol compound [C1] represented by formula (1) in the epoxy resin composition.
[0028] [ka]
[0029] (In formula (1), R 1 ~R 5 R represents a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a methoxy group, a hydroxyl group, or a halogen, and may all be the same or different, but at least two are hydroxyl groups. 6 ~R 10 represents a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a methoxy group, or a halogen, and may all be the same or different. X represents no element, SO 2 , C.H. 2 , CH(CH 3 ), C(CH 3 ) 2 , S, O, or C=O.) The inventors have found that by including [C1] as a phenolic compound, it is possible to achieve both an extremely high level of elastic modulus and deflection of the resin cured product. It has been known that the use of a compound such as bisphenol A in an epoxy resin composition increases the deflection of the epoxy resin cured product, but there is a problem of a decrease in elastic modulus. This is thought to be due to the fact that a rigid bisphenol compound is inserted between the crosslinking points, creating a small gap. [C1] is a compound that has two aromatic rings in its molecule, and one of the aromatic rings has two or more hydroxyl groups bonded to it. It is believed that when the hydroxyl group reacts with the epoxy group and is incorporated into the crosslinking structure, the aromatic ring that does not have a hydroxyl group fills the gap, thereby improving the elastic modulus compared to compounds that have hydroxyl groups on both aromatic rings, such as bisphenol A.
[0030] Examples of the phenol compound [C1] include 4-benzylresorcinol, 4-(α-methylbenzyl)resorcinol, 2-(phenylsulfonyl)-1,4-benzenediol, phenylhydroquinone, 2,3-dihydroxybiphenyl, 2,4-dihydroxybenzophenone, 2,3,4-trihydroxybenzophenone, 3,4-dihydroxybenzophenone, 2,4-dihydroxy-5-tert-butylbenzophenone, etc. Among these, 2,4-dihydroxybenzophenone is preferably used from the viewpoints of having appropriate solubility in epoxy resins and excellent handling properties.
[0031] Regarding the content of the component [C1] in the present invention, when the equivalent ratio of the epoxy resin to the phenol compound [C1] in the epoxy resin composition, i.e., the ratio of the number of active hydrogens of the phenol compound [C1] to the number of epoxy groups of the epoxy resin in the epoxy resin composition (number of active hydrogens of the phenol compound [C1] / number of epoxy groups of the epoxy resin) is defined as XC1, XC1 must be in the range of 0.3 to 0.9, and preferably in the range of 0.3 to 0.7.
[0032] Furthermore, when the sum of XB and XC1 is taken as XB+XC1, XB+XC1 must be in the range of 0.4 to 1.0, and preferably in the range of 0.5 to 1.0. By setting XC1 and XB+XC1 in such ranges, a cured resin having excellent elastic modulus and deflection can be obtained.
[0033] (Component [D]) The component [D] of the present invention is a curing accelerator, specifically, a curing accelerator for an epoxy resin and a phenolic compound, and promotes the reaction between the component [A] and the component [C]. In order to enhance the reactivity of the epoxy resin and the phenolic compound, it is necessary that the epoxy resin composition contains a curing accelerator. As the curing accelerator, it is preferable to use at least one curing accelerator selected from the group consisting of aromatic urea compounds, imidazole derivatives, and phosphorus compounds, in order to achieve both storage stability and curability of the epoxy resin composition.
[0034] Examples of the aromatic urea compound include 3-phenyl-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, toluenebisdimethylurea, etc. Commercially available aromatic urea compounds include DCMU-99 (manufactured by Hodogaya Chemical Co., Ltd.), "Omicure (registered trademark)" 24 (manufactured by PTI Japan, Inc.), etc.
[0035] Examples of the imidazole derivatives include 1-benzyl-2-methylimidazole, 1-benzyl-2-ethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, etc. Commercially available imidazole derivatives include "Cureduct (registered trademark)" P-0505, 1B2MZ, 1B2PZ, 2MZ-CN, 2E4MZ-CN, 2PZ-CN (all manufactured by Shikoku Chemical Industry Co., Ltd.), etc.
[0036] Examples of the phosphorus compound include triphenylphosphine, tri-o-tolylphosphine, tris(p-methoxyphenyl)phosphine, triphenylphosphine triphenylborane, tetraphenylphosphonium tetraphenylborate, etc. Commercially available phosphorus compounds include "Hokuko TPP (registered trademark)", "TOTP (registered trademark)", "TPP-K (registered trademark)" (all manufactured by Hokko Chemical Industry Co., Ltd.), etc.
[0037] The content of the curing accelerator [D] is preferably 1 to 8 parts by mass, more preferably 1.5 to 6 parts by mass, and further preferably 2 to 4 parts by mass, based on 100 parts by mass of the epoxy resin [A]. By containing the curing accelerator [D] within this range, an epoxy resin composition can be obtained that has an excellent balance between storage stability and curing speed and gives a resin cured product with good physical properties.
[0038] (Component [E]) The epoxy resin composition of the present invention may contain a thermoplastic resin as component [E] within the range that does not impair the effects of the present invention. Although the thermoplastic resin is not an essential component of the present invention, by including it in the epoxy resin composition, it is possible to control the viscoelasticity and impart toughness to the cured product.
[0039] Examples of such thermoplastic resins include polymethyl methacrylate, polyvinyl formal, polyvinyl butyral, polyvinyl acetal, polyvinyl pyrrolidone, polymers having at least two components selected from aromatic vinyl monomers, vinyl cyanide monomers, and rubber-like polymers, polyamides, polyesters, polycarbonates, polyarylene oxides, polysulfones, polyethersulfones, and polyimides. Examples of the polymer include acrylonitrile-butadiene-styrene copolymer (ABS resin), acrylonitrile-styrene copolymer (AS resin), etc. The polysulfone and polyimide may have an ether bond or an amide bond in the main chain.
[0040] Polymethyl methacrylate, polyvinyl formal, polyvinyl butyral, and polyvinyl pyrrolidone are preferred because they have good compatibility with many types of epoxy resins such as bisphenol A type epoxy resins and novolac type epoxy resins, and are highly effective in controlling the fluidity of the epoxy resin composition, with polyvinyl formal being particularly preferred. Commercially available examples of these thermoplastic resins include "Denka Butyral (registered trademark)" and "Denka Formal (registered trademark)" (manufactured by Denki Kagaku Kogyo Co., Ltd.), and "Vinylec (registered trademark)" (manufactured by JNC Corporation).
[0041] In addition, polysulfone, polyethersulfone, and polyimide have excellent heat resistance in themselves, and there are polymers having a resin skeleton that has moderate compatibility with glycidylamine-type epoxy resins such as tetraglycidyldiaminodiphenylmethane, triglycidylaminophenol, triglycidylaminocresol, and tetraglycidylxylenediamine, which are epoxy resins often used in applications requiring heat resistance, such as structural members of aircraft. The use of these polymers is preferable because they have a large effect of controlling the flowability of the epoxy resin composition and have the effect of increasing the impact resistance of fiber-reinforced resin composite materials. Examples of such polymers include polysulfones such as "Radel (registered trademark)" A (manufactured by Solvay Advanced Polymers) and "Sumikaexcel (registered trademark)" PES (manufactured by Sumitomo Chemical Co., Ltd.), and polyimides such as "Ultem (registered trademark)" (manufactured by GE Plastics Co., Ltd.) and "Matrimid (registered trademark)" 5218 (manufactured by Huntsman Co., Ltd.).
[0042] In the epoxy resin composition of the present invention, when a thermoplastic resin is contained, it is preferably contained in an amount of 1 to 60 parts by mass relative to 100 parts by mass of the epoxy resin contained in the epoxy resin composition.
[0043] (Other additives) The epoxy resin composition of the present invention may contain, within the scope of not impairing the effects of the present invention, a coupling agent, thermosetting resin particles, conductive particles such as carbon black, carbon particles, metal-plated organic particles, or inorganic fillers such as silica gel, clay, etc. The addition of these has a viscosity adjusting effect of increasing the viscosity of the epoxy resin composition and reducing resin flow, an effect of improving the elastic modulus and heat resistance of the cured resin, and an effect of improving the abrasion resistance.
[0044] (Method for preparing epoxy resin composition) In preparing the epoxy resin composition of the present invention, the ingredients may be kneaded using a machine such as a kneader, a planetary mixer, a three-roll mill, or a twin-screw extruder, or may be mixed by hand using a beaker and a spatula, etc., so long as uniform kneading is possible.
[0045] (Fiber-reinforced composite materials) The epoxy resin composition of the present invention is excellent in elastic modulus and deflection after curing, and is suitable for use as a matrix resin for fiber-reinforced composite materials. Methods for obtaining fiber-reinforced composite materials include methods in which the resin composition is impregnated into reinforcing fibers in a molding process, such as the hand lay-up method, the RTM method, the filament winding method, and the pultrusion molding method, and methods in which a prepreg in which the resin composition has been previously impregnated into reinforcing fibers is molded by the autoclave method or the press molding method. Among these, it is preferable to prepare a prepreg made of the epoxy resin composition and reinforcing fibers in advance, since the fiber arrangement and the resin ratio can be precisely controlled and the properties of the composite material can be maximized.
[0046] The reinforcing fibers used in the prepreg and fiber-reinforced composite material of the present invention are preferably carbon fiber, graphite fiber, aramid fiber, glass fiber, etc., with carbon fiber being particularly preferred. There are no limitations on the form or arrangement of the reinforcing fibers, and for example, fiber structures such as long fibers aligned in one direction, single tow, woven fabric, knit, and braided cord are used. As the reinforcing fibers, two or more types of carbon fibers, glass fibers, aramid fibers, boron fibers, PBO fibers, high-strength polyethylene fibers, alumina fibers, silicon carbide fibers, etc. may be used in combination.
[0047] Specific examples of carbon fibers include acrylic, pitch and rayon carbon fibers, with acrylic carbon fibers having particularly high tensile strength being preferably used.
[0048] The carbon fiber can be in the form of twisted yarn, untwisted yarn, non-twisted yarn, etc., but in the case of twisted yarn, the filaments that make up the carbon fiber are not oriented parallel to one another, which can cause a decrease in the mechanical properties of the resulting carbon fiber reinforced composite material. Therefore, untwisted yarn or non-twisted yarn, which provide a good balance between the formability and strength properties of the carbon fiber reinforced composite material, are preferably used.
[0049] The prepreg of the present invention can be produced by various known methods. For example, the prepreg can be produced by a hot melt method in which a resin composition is heated to reduce its viscosity without using an organic solvent and then impregnated into reinforcing fibers.
[0050] In the hot melt method, a resin composition whose viscosity has been reduced by heating can be directly impregnated into the reinforcing fibers, or a release paper sheet with a resin film can be first prepared by coating the resin composition on release paper or the like, and then a resin film can be placed on the reinforcing fiber side from both sides or one side of the reinforcing fibers, and the reinforcing fibers can be impregnated with the resin composition by heating and pressurizing.
[0051] The content of reinforcing fibers in the prepreg is preferably 30 to 90% by mass, more preferably 35 to 85% by mass, and even more preferably 65 to 85% by mass. If the fiber mass content is low, the amount of resin is too high, and the advantages of a fiber-reinforced composite material having excellent specific strength and specific elastic modulus may not be obtained. In addition, when molding a fiber-reinforced composite material, the amount of heat generated during curing may be too high. On the other hand, if the fiber mass content is too high, impregnation with the resin may be insufficient, and the resulting composite material may have many voids. In addition, the tackiness of the prepreg may be impaired.
[0052] The fiber-reinforced composite material of the present invention can be produced, for example, by laminating the above-mentioned prepregs of the present invention in a predetermined shape and curing the resin by applying pressure and heat. Methods for applying heat and pressure include press molding, autoclave molding, bagging molding, wrapping tape method, internal pressure molding, etc.
[0053] The fiber-reinforced composite material of the present invention can be widely used in aerospace applications, general industrial applications, and sports applications. More specifically, in general industrial applications, it is preferably used in structures such as automobiles, ships, and railway vehicles. In sports applications, it is preferably used in golf shafts, fishing rods, and tennis and badminton rackets. EXAMPLES
[0054] The present invention will be described in detail below with reference to examples. However, the scope of the present invention is not limited to these examples. The unit "parts" in the composition ratio means parts by mass unless otherwise noted. Furthermore, the measurements of various characteristics (physical properties) were performed in an environment with a temperature of 23°C and a relative humidity of 50% unless otherwise noted.
[0055] <Materials used in the Examples and Comparative Examples>
[0056] (1) [A]: Epoxy resin [A]-1: “jER (registered trademark)” 828 (bisphenol A type epoxy resin, epoxy equivalent: 189 g / eq, manufactured by Mitsubishi Chemical Corporation).
[0057] (2) [B]: Amine-based hardener [B]-1: “jER Cure (registered trademark)” DICY7 (dicyandiamide, active hydrogen equivalent: 21 g / eq, number of active hydrogens: 4, manufactured by Mitsubishi Chemical Corporation).
[0058] (3) [C]: Phenolic compounds Phenol compounds corresponding to [C1] [C1]-1: 2,4-Dihydroxybenzophenone (active hydrogen equivalent: 107 g / eq, number of active hydrogens: 2, manufactured by Tokyo Chemical Industry Co., Ltd.). [C1]-2: 4-Benzylresorcinol (active hydrogen equivalent: 100 g / eq, number of active hydrogens: 2, manufactured by Tokyo Chemical Industry Co., Ltd.). [C1]-3: 2,3-dihydroxybiphenyl (active hydrogen equivalent: 93 g / eq, number of active hydrogens: 2, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). Phenolic compounds not falling under [C1] [C]-4: Bisphenol A (active hydrogen equivalent: 114 g / eq, number of active hydrogens: 2, manufactured by Tokyo Chemical Industry Co., Ltd.).
[0059] (4) [D]: Curing accelerator [D]-1: DCMU-99 (3-(3,4-dichlorophenyl)-1,1-dimethylurea, manufactured by Hodogaya Chemical Industry Co., Ltd.). [D]-2: “Cureduct (registered trademark)” P-0505 (epoxy-imidazole adduct, manufactured by Shikoku Chemicals Corporation). [D]-3: TPP (triphenylphosphine, manufactured by Tokyo Chemical Industry Co., Ltd.).
[0060] <Method for preparing epoxy resin composition> (1) How to make a hardener master [B]-1 ("jER Cure (registered trademark)" DICY7) was added to 10 parts of [A]-1 ("jER (registered trademark)" 828) out of 100 parts, and the mixture was kneaded at room temperature using a kneading device. The mixture was passed between the rolls of a three-roll mill twice to prepare a hardener master.
[0061] (2) Method for preparing epoxy resin composition 90 parts of 100 parts of [A]-1 ("jER (registered trademark)" 828) (excluding the 10 parts of [A]-1 ("jER (registered trademark)" 828) used in (1) above) and the phenol compound [C] were charged into a kneading device, and the temperature was raised to 150°C while kneading, and a transparent viscous liquid was obtained by kneading at 150°C for 30 minutes. Next, while continuing kneading, the temperature was lowered to 60°C, and the hardener master prepared in (1) above and the hardening accelerator [D] were charged, and the mixture was kneaded at 60°C for 30 minutes to obtain an epoxy resin composition.
[0062] The compositions of the epoxy resin compositions of the respective Examples and Comparative Examples are shown in Tables 1 to 3.
[0063] <Method of producing cured resin> The epoxy resin composition prepared according to the above <Preparation method of epoxy resin composition> was degassed in a vacuum, and then heated from 30°C to 130°C at a rate of 2.5°C / min in a mold set to a thickness of 2 mm using a 2 mm thick Teflon (registered trademark) spacer, and cured at 130°C for 90 minutes to obtain a plate-shaped cured resin product with a thickness of 2 mm.
[0064] <Measurement of elastic modulus and bending deflection of cured resin> Test pieces measuring 10 mm in width and 60 mm in length were cut out from the cured resin products prepared according to the above <Method for Preparing Cured Resin Product> and subjected to three-point bending in accordance with JIS K7171 (1994) using an Instron universal testing machine (manufactured by Instron Corp.) with a span of 32 mm, a crosshead speed of 100 mm / min, and sample number n=6. The average values of the elastic modulus and bending deflection were taken as the elastic modulus and bending deflection of the cured resin product, respectively.
[0065] <Example 1> An epoxy resin composition was prepared according to the above <Method for preparing epoxy resin composition> using [A] 100 parts of "jER (registered trademark)" 828 as an epoxy resin, [B] 1.9 parts of "jER Cure (registered trademark)" DICY7 as an amine curing agent, [C] 34.0 parts of 2,4-dihydroxybenzophenone as a phenol compound, and [D] 3 parts of DCMU-99 as a curing accelerator.
[0066] In this epoxy resin composition, XB, which represents the ratio of the number of active hydrogens in the amine curing agent [B] to the number of epoxy groups contained in the epoxy resin [A], was 0.2. Also, XC1, which represents the ratio of the number of active hydrogens in the phenol compound corresponding to [C1] to the number of epoxy groups contained in the epoxy resin [A], was 0.6. XB+XC1, which represents the sum of XB and XC1, was 0.8.
[0067] The obtained epoxy resin composition was cured by the method described above in <Method for producing cured resin> to produce a plate-shaped cured resin. Furthermore, a three-point bending test described in <Measurement of elastic modulus and bending deflection of cured resin> was carried out, and the elastic modulus was 3.6 GPa and the bending deflection was 17 mm, which were excellent values.
[0068] <Examples 2 to 8> Epoxy resin compositions and cured resins were prepared in the same manner as in Example 1, except that the resin compositions were changed as shown in Tables 1 and 2, respectively.
[0069] For the epoxy resin composition of each example, XB, XC1 and XB+XC1 are as shown in Tables 1 and 2, respectively.
[0070] A three-point bending test of the cured resin showed that both the elastic modulus and bending deflection were good.
[0071] <Comparative Examples 1 to 6> An epoxy resin composition was obtained in the same manner as in Example 1 above, using the resin composition in Table 3. The obtained epoxy resin composition was cured by the method described above in <Method for producing cured resin product> to produce a plate-shaped cured resin product.
[0072] For the epoxy resin compositions of each comparative example, XB, XC1 and XB+XC1 are as shown in Table 3.
[0073] Next, the three-point bending test described in <Measurement of elastic modulus and bending deflection of cured resin> was carried out. The evaluation results are shown in Table 3.
[0074] Since Comparative Example 1 did not contain the amine-based curing agent [B], the cured resin was extremely brittle, and it was difficult to prepare a test piece for a three-point bending test of the cured resin, so that evaluation was not possible.
[0075] In Comparative Example 2, since XB was greater than 0.4, the bending deflection of the cured resin was low at 13 mm in a three-point bending test.
[0076] In Comparative Example 3, since XB+XC1 was greater than 1.0, the cured resin was extremely brittle and it was difficult to prepare a test piece for a three-point bending test of the cured resin, so that evaluation was not possible.
[0077] In Comparative Example 4, XC1 was smaller than 0.3, and therefore the cured resin had a low deflection of 12 mm in a three-point bending test.
[0078] Since Comparative Example 5 did not contain the phenol compound (C), the cured resin had a low deflection of 12 mm in a three-point bending test.
[0079] Comparative Example 6 contained bisphenol A as the phenol compound [C] but did not contain a phenol compound corresponding to [C1], and therefore the elastic modulus of the cured resin was low at 2.9 GPa in a three-point bending test.
[0080] [Table 1]
[0081]
Table 2
[0082]
Table 3
Claims
1. An epoxy resin composition for use in a fiber-reinforced composite material, comprising the following components [A], [B], [C] and [D], and satisfying all of the following conditions (i) to (iii): Component [A]: Epoxy resin Component [B]: Amine-based curing agent Component [C]: Phenolic compound Component [D]: Curing accelerator Condition (i): When the ratio of the number of active hydrogens in the component [B] to the number of epoxy groups in the component [A] is XB, XB is in the range of 0.1 to 0.
4. Condition (ii): The constituent element [C] contains 4-benzylresorcinol, 4-(α-methylbenzyl)resorcinol, phenylhydroquinone, 2,3-dihydroxybiphenyl, 2,4-dihydroxybenzophenone, 2,3,4-trihydroxybenzophenone, 3,4-dihydroxybenzophenone or 2,4-dihydroxy-5-tert-butylbenzophenone as the constituent element [C1], and when the ratio of the number of active hydrogens in the constituent element [C1] to the number of epoxy groups in the constituent element [A] is defined as XC1, XC1 is in the range of 0.3 to 0.
9. Condition (iii): XB+XC1 is in the range of 0.4 to 1.
0.
2. An epoxy resin composition for fiber-reinforced composite materials as described in claim 1, characterized in that component [C] contains 4-benzylresorcinol, 2,3-dihydroxybiphenyl or 2,4-dihydroxybenzophenone as component [C1].
3. 3. The epoxy resin composition for fiber-reinforced composite materials according to claim 1 or 2, characterized in that it contains, as the component [D], at least one curing accelerator selected from the group consisting of aromatic urea compounds, imidazole derivatives and phosphorus compounds.
4. 4. The epoxy resin composition for fiber-reinforced composite materials according to claim 1, wherein the component [B] is dicyandiamide.
5. A prepreg comprising the epoxy resin composition for fiber-reinforced composite materials according to any one of claims 1 to 4 and reinforcing fibers.
6. 6. The prepreg according to claim 5, wherein the reinforcing fibers are carbon fibers.
7. A fiber-reinforced composite material comprising a cured product of the epoxy resin composition for fiber-reinforced composite materials according to any one of claims 1 to 4 and reinforcing fibers.
8. 8. The fiber-reinforced composite material according to claim 7, characterized in that the reinforcing fibers are carbon fibers.
Citation Information
Patent Citations
Epoxy resin composition
JP1990124919A
Resin composition for laminate
JP1999147996A
Epoxy resin composition, prepreg, and fiber reinforced composite material
JP2002284852A
Epoxy resin composition for fiber-reinforced composite material and fiber-reinforced composite material
JP2018053065A
Epoxy resin composition, prepreg and fiber-reinforced composite material
WO2018159574A1