Resin composition, film and molded article

A resin composition with specific acrylic polymers enhances fluorine-based films by addressing fish eyes and chemical resistance issues, achieving fine matte properties and transparency for automotive applications.

JP7585803B2Active Publication Date: 2024-11-19MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021007221
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-20
Publication Date
2024-11-19
Estimated Expiration
2041-01-20

AI Technical Summary

Technical Problem

Existing fluorine-based matte films face issues such as fish eyes, poor chemical resistance, and uneven matte properties, which are not adequately addressed by current manufacturing methods, particularly in applications requiring high quality for automotive interiors.

Method used

A resin composition comprising a fluororesin and specific acrylic polymers with defined reactive and non-reactive groups, including a first polymer with reactive groups, a second polymer with 30% by mass of (meth)acrylic acid alkyl esters with 1-3 carbon atoms, and a third polymer with 30% by mass of (meth)acrylic acid alkyl esters with 4 or more carbon atoms, improves chemical resistance and reduces fish eyes.

Benefits of technology

The composition achieves fine matte properties, transparency, and enhanced chemical resistance, reducing fish eyes and improving film appearance, making it suitable for high-quality automotive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585803000001
    Figure 0007585803000001
  • Figure 0007585803000002
    Figure 0007585803000002
  • Figure 0007585803000003
    Figure 0007585803000003
Patent Text Reader

Abstract

To provide a resin composition which can reduce a fish eye causing poor appearance of a film and is excellent in fine matting properties, transparency and chemical resistance, and to provide a film using the same, and a molding.SOLUTION: A resin composition contains a fluorine-based resin, a first polymer, a second polymer and a third polymer, wherein the first polymer is a polymer having a reactive group; the second polymer is a polymer that has 30 mass% or more of alkyl (meth)acrylate whose ester group has 1 or more and 3 or less carbon atoms as a constitutional unit and does not substantially have a reactive group; the third polymer is a polymer that has 30 mass% or more of alkyl (meth)acrylate whose ester group has 4 or more carbon atoms as a constitutional unit and does not substantially have a reactive group, and the second polymer and the third polymer have different compositions.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a film, and a molded article. [Background technology]

[0002] Fluorine-based films made of fluorine-based resins, such as vinylidene fluoride resins, are excellent in weather resistance, chemical resistance, and stain resistance, and are therefore widely used as protective films laminated onto the surfaces of various substrates such as plastics, glass, slate, rubber, metal plates, wooden boards, etc. In addition, substrates whose surfaces are protected with fluorine-based films are used in many applications, such as interior and exterior materials for buildings, furniture, and interior and exterior materials for automobiles.

[0003] Particularly in recent years, emphasis has been placed on a luxurious appearance, and fluorine-based matte film laminates are increasingly being used.

[0004] The main methods for producing matte films are: (1) a method in which a film surface is roughened by a metal or rubber matte roll, followed by thermoforming; (2) a method in which fine particles of sand or metal are sprayed onto the film surface to create a fine irregularity (sandblasting method); (3) a method in which a film is coated with a matte agent; and (4) a method in which fine organic or inorganic fillers (matte agents) are added to the resin that constitutes the film.

[0005] In the method (1), there are problems such as clogging of the mat roll due to additives such as ultraviolet absorbers added to the fluororesin, and in the case of a thin film, thickness unevenness directly leads to gloss unevenness, making it difficult to obtain a uniform matte film. In the method (2), there is a problem that the treated film stretches or breaks during sandblasting. In the method (3), since the matte agent is non-adhesive (non-bonding) to the fluororesin, it is difficult to coat the surface of the fluororesin with the matte agent.

[0006] As an example of using an inorganic matting agent in the method (4), Patent Document 1 proposes a matte fluorine film in which inorganic fine particles are dispersed in a vinylidene fluoride resin.

[0007] As a case where an organic matting agent is used in the method (4), Patent Document 2 proposes a surface protection film for interior and exterior building materials in which a cross-linked acrylic resin with a specific particle size is contained in a vinylidene fluoride resin. Patent Document 3 discloses a matte fluorine film in which a fluorine resin contains a non-cross-linked acrylic resin. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2002-80674 A [Patent Document 2] JP 2008-7709 A [Patent Document 3] International Publication No. 2011 / 093300 Summary of the Invention [Problem to be solved by the invention]

[0009] The film obtained in Patent Document 1 has excellent chemical resistance and matte finish, but the presence of an inorganic matte agent during melt extrusion accelerates decomposition of the resin, which may cause problems with poor appearance such as foaming and coloring of the obtained film. In addition, the film obtained in Patent Document 2 has excellent weather resistance and matte finish, but its chemical resistance is insufficient. The film obtained in Patent Document 3 has excellent matte finish and chemical resistance, but has the problem of frequent occurrence of foreign matter defects called fisheyes. When fluorine-based films are used for applications such as automotive interior and exterior materials, in addition to chemical resistance and matte finish, higher quality is required, and there are many requests for reducing fisheyes in particular.

[0010] An object of the present invention is to provide a resin composition capable of reducing fish eyes that cause poor appearance of a film and having a fine matte finish, excellent transparency and chemical resistance, and a film and a molded article using the same. [Means for solving the problem]

[0011] Means for Solving the Problems The present inventors have conducted intensive research and have found that, by adding two or more specific acrylic polymers to a resin composition, it is possible to reduce fisheyes that cause poor appearance of a film, and to obtain a resin composition that has a fine matte finish, excellent transparency and chemical resistance, and a fluorine-based film, a fluorine-based laminate film and a laminate molded article using the same.

[0012] That is, the present invention has the following features. [1] A resin composition comprising a fluororesin, a first polymer, a second polymer, and a third polymer, wherein the first polymer is a polymer having a reactive group, the second polymer is a polymer having, as a structural unit, 30% by mass or more of a (meth)acrylic acid alkyl ester having an ester group with a carbon number of 1 to 3 and having substantially no reactive groups, and the third polymer is a polymer having, as a structural unit, 30% by mass or more of a (meth)acrylic acid alkyl ester having an ester group with a carbon number of 4 or more and having substantially no reactive groups, and the second polymer and the third polymer have different compositions. [2] The resin composition according to [1], wherein the third polymer has a mass average molecular weight of 50,000 to 500,000. [3] The resin composition according to [1] or [2], further comprising a fourth polymer having, as structural units, a methacrylic acid alkyl ester having an ester group with 1 to 3 carbon atoms and a (meth)acrylic acid alkyl ester having an ester group with 4 to 18 carbon atoms, and having substantially no reactive groups. [4] The mass average molecular weight of the fourth polymer is 500,000 or more and 5,000,000 or less. [3] The resin composition described above. [5] The fluorine systemThe content of the fluorine atom relative to 100 mass % in total of the resin, the first polymer, the second polymer, and the third polymer is system The resin composition according to any one of [1] to [4], wherein the proportion of the resin is 40% by mass or more and 98% by mass or less. [6] The fluorine system The resin composition according to any one of [1] to [5], wherein a ratio of the first polymer to a total of 100 mass% of a resin, the first polymer, the second polymer, and the third polymer is 1 mass% or more and 20 mass% or less. [7] The fluorine system The resin composition according to any one of [1] to [6], wherein a ratio of the second polymer to a total of 100 mass% of a resin, the first polymer, the second polymer, and the third polymer is 1 mass% or more and 40 mass% or less. [8] The fluorine system The resin composition according to any one of [1] to [7], wherein a ratio of the third polymer to a total of 100 mass% of a resin, the first polymer, the second polymer, and the third polymer is 0.1 mass% or more and 10 mass% or less. [9] The above The resin composition according to any one of [1] to [8], wherein the fluorine-based resin is polyvinylidene fluoride.

[10] The resin composition according to any one of [1] to [9], wherein the first polymer is an acrylic polymer.

[11] The resin composition according to any one of [1] to

[10] , wherein the reactive group of the first polymer is one or more selected from the group consisting of a carboxy group, a hydroxy group, an acid anhydride group, an epoxy group, an isocyanate group, an amide group, an amino group, a cyano group, and an imine group.

[12] A film comprising the resin composition according to any one of [1] to

[11] .

[13] A molded article having the film according to

[12] . Effect of the Invention

[0013] The present invention makes it possible to provide a resin composition that can reduce fisheyes that cause poor appearance of a film and has a fine matte finish, excellent transparency and chemical resistance, and a fluorine-based film, a fluorine-based laminate film and a laminate molded article each using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to these descriptions, and other than the following examples, modifications and variations can be made as appropriate without departing from the spirit of the present invention. In this specification, (meth)acrylic means acrylic or methacrylic, and (meth)acrylic acid ester means acrylic acid ester or methacrylic acid ester. In this specification, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as the lower limit and upper limit.

[0015] The resin composition according to the present embodiment includes at least a fluororesin, a first polymer, a second polymer, and a third polymer. The first polymer is a polymer having a reactive group, the second polymer is a polymer having 30% by mass or more of a methacrylic acid alkyl ester having an ester group carbon number of 1 to 3 as a structural unit and having substantially no reactive group, the third polymer is a polymer having 30% by mass or more of a (meth)acrylic acid alkyl ester having an ester group carbon number of 4 or more as a structural unit and having substantially no reactive group, and the second polymer and the third polymer are polymers of different compositions.

[0016] [Fluorine resin] The fluorine-based resin is not particularly limited, and examples thereof include ethylene-tetrafluoroethylene copolymers, polychlorotrifluoroethylene, polytetrafluoroethylene, polyvinyl fluoride, tetrafluoroethylene-hexafluoropropylene copolymers, tetrafluoroethylene-perfluoro(propyl vinyl ether) copolymers, vinylidene fluoride polymers, etc. These may be used alone or in combination of two or more. Among them, vinylidene fluoride polymers are preferred in terms of the light transmittance of the resulting film, the ability to develop a fine matte finish, and the compatibility of the fluorine-based resin with the first polymer.

[0017] The vinylidene fluoride polymer may be any resin containing vinylidene fluoride units, and examples thereof include homopolymers consisting of vinylidene fluoride units and copolymers containing vinylidene fluoride units. The content of vinylidene fluoride units relative to the total number of repeating units of the vinylidene fluoride polymer is not particularly limited, but in order to improve chemical resistance, it is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and most preferably 100 mol%, i.e., polyvinylidene fluoride.

[0018] Examples of other vinyl monomers copolymerizable with vinylidene fluoride include fluorinated vinyl monomers such as vinyl fluoride, tetrafluoroethylene, trifluorochloroethylene, and hexafluoropropylene; and vinyl monomers such as styrene, ethylene, butadiene, propylene, and (meth)acrylic acid esters.

[0019] In addition, commercially available fluorine-based resins can also be used, such as those available under the trade name KFT manufactured by Kureha Corporation and those available under the trade names Kynar 720 and Kynar 710 manufactured by Arkema Corporation.

[0020] The vinylidene fluoride copolymer may be used alone or in combination of two or more kinds.

[0021] The weight average molecular weight (Mw) of the fluororesin is not particularly limited, but from the viewpoint of chemical resistance, it is preferably 20,000 or more, more preferably 50,000 or more. Further, from the viewpoint of film-forming properties, the weight average molecular weight (Mw) of the fluororesin (A) is preferably 1,000,000 or less, more preferably 700,000 or less. In the present invention, the weight average molecular weight (Mw) of the compound indicates a value obtained by measuring under the following conditions by gel permeation chromatography (GPC).

[0022] <GPC measurement conditions> Equipment used: HLC-8320GPC system manufactured by Tosoh Corporation Column (guard): TGKgel SupaerGuadH-H (manufactured by Tosoh Corporation, trade name) Column (main): 2 pieces of TGKgel SupaerHZM-H (manufactured by Tosoh Corporation, trade name) Eluent: DMF containing 0.01 mmol / L LiCl Column temperature: 40 °C Detector: Differential refractive index (RI)

[0023] The fluororesin is not particularly limited, but preferably has an MFR of 5 g / 10 min or more, more preferably 6 g / 10 min or more, still more preferably 7 g / 10 min or more, when measured under the conditions of a temperature of 230 °C and a load of 49 N. On the other hand, it is preferably 40 g / 10 min or less, more preferably 35 g / 10 min or less, still more preferably 30 g / 10 min or less. If the MFR of the fluororesin (A) is 5 g / 10 min or more, it has excellent moldability, and if it is 40 g / 10 min or less, it has excellent process stability.

[0024] The melting point of the fluororesin is not particularly limited, but from the viewpoint of heat resistance, it is preferably 100 °C or more, more preferably 120 °C or more. On the other hand, from the viewpoint of transparency, it is preferably 190 °C or less, more preferably 180 °C or less.

[0025] The refractive index of the fluororesin is not particularly limited, but is preferably 1.30 or more, more preferably 1.40 or more, and is preferably 1.60 or less, more preferably 1.50 or less, in order to improve transparency. Also, the refractive index of the fluororesin (A) is preferably close to the refractive index of the acrylic resin (C) described later, in order to improve transparency, and specifically, the difference therebetween is preferably 0.25 or less, more preferably 0.15 or less.

[0026] [First polymer] There is no particular limitation on the first polymer as long as it is a polymer having a reactive group. In this way, the first polymer having a reactive group can function as a matting agent that suppresses the gloss of a film or a molded product obtained by using the resin composition according to the present embodiment and improves the appearance.

[0027] The first polymer is not particularly limited, and examples thereof include polystyrene, polyvinyl chloride, AS resin, ABS resin, acrylic resin, polycarbonate, modified polyphenylene ether, etc., each of which has a reactive group. These may be used alone or in combination of two or more.

[0028] The reactive group means a group that enables the first polymer to react with itself, and is not particularly limited. Preferred examples of the reactive group include a carboxy group, a hydroxyl group, an acid anhydride group, an epoxy group, an isocyanate group, an amide group, an amino group, a cyano group, an imine group, a sulfonic acid group, an aziridine group, an amine group, a urea group, a phosphate group, a cyanate group, an imidazole group, and an oxazoline group.

[0029] The reactive group of the first polymer may be present in the monomer portion constituting the polymer. That is, to produce a first polymer having a desired reactive group, it can be obtained by polymerizing a monomer having the desired reactive group. That is, it can be obtained by polymerizing a monomer having a reactive group. The first polymer having a reactive group may be a homopolymer of a monomer having a reactive group, a copolymer of two or more types having a reactive group, or a copolymer of a monomer having a reactive group and a monomer having no reactive group.

[0030] Among these, the first polymer is preferably a copolymer of a monomer having a reactive group and a monomer not having a reactive functional group.

[0031] Among the above, the first polymer is preferably a (meth)acrylic polymer having a reactive group, from the viewpoint of compatibility with the fluorine-based resin.

[0032] The (meth)acrylic polymer is a polymer mainly composed of (meth)acrylic monomer units. The (meth)acrylic monomer units preferably contain 50% by mass or more of (meth)acrylic acid alkyl ester units. In particular, from the viewpoint of compatibility between the fluorine-based resin and the first polymer, the total content of the (meth)acrylic acid alkyl ester units relative to the total amount of the first polymer is more preferably 70% by mass or more.

[0033] When the first polymer is a (meth)acrylic polymer, the (meth)acrylic polymer may be a homopolymer of a (meth)acrylic acid alkyl ester, a copolymer of a plurality of (meth)acrylic acid alkyl esters, or a copolymer of a (meth)acrylic acid ester and another monomer. The other monomer is not particularly limited, but examples thereof include (meth)acrylic acid and styrene.

[0034] Examples of (meth)acrylic monomers having a reactive group include (meth)acrylic acid hydroxyalkyl ester, acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, maleic acid, fumaric acid, crotonic acid, (meth)acrylamide, diethylacrylamide, aminoethyl (meth)acrylate, glycidyl alkyl (meth)acrylate, (meth)acryloyl isocyanate, cyanoethyl acrylate, etc. Among these, in terms of improving the matte appearance of the obtained film or molded article, the first polymer is preferably a polymer containing a hydroxyl group as a reactive group, specifically, a polymer having a (meth)acrylic acid hydroxyalkyl ester as a monomer unit.

[0035] Examples of (meth)acrylic acid hydroxyalkyl esters include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2,3-dihydroxypropyl methacrylate, 2-hydroxyethyl acrylate, and 4-hydroxybutyl acrylate. These may be used alone or in combination of two or more. Among these, the (meth)acrylic acid hydroxyalkyl ester is preferably a (meth)acrylic acid hydroxyalkyl ester having an ester group with 1 or more carbon atoms, while the (meth)acrylic acid hydroxyalkyl ester having an ester group with 8 or less carbon atoms is preferred, the (meth)acrylic acid hydroxyalkyl ester having an ester group with 6 or less carbon atoms is more preferred, and the (meth)acrylic acid hydroxyalkyl ester having an ester group with 4 or less carbon atoms is even more preferred, and 2-hydroxyethyl methacrylate is particularly preferred from the viewpoint of the best matte development.

[0036] The monomer having no reactive functional group is not particularly limited, but may be an alkyl (meth)acrylate having no reactive group.

[0037] The alkyl methacrylate ester having no reactive group is not particularly limited, and examples of the alkyl methacrylate ester having no reactive group include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, i-propyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, and t-butyl methacrylate. These may be used alone or in combination of two or more. Among them, alkyl methacrylate esters having an ester group with 1 or more carbon atoms are preferred, while alkyl methacrylate esters having an ester group with 13 or less carbon atoms are preferred, alkyl methacrylate esters having an ester group with 9 or less carbon atoms are more preferred, and alkyl methacrylate esters having an ester group with 6 or less carbon atoms are even more preferred, and among them, methyl methacrylate is particularly preferred in terms of weather resistance.

[0038] Examples of alkyl acrylates having no reactive groups include methyl acrylate, ethyl acrylate, n-propyl acrylate, i-propyl acrylate, n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, and 2-ethylhexyl acrylate. These may be used alone or in combination of two or more. Among them, alkyl acrylates having an ester group with 1 or more carbon atoms are preferred, while alkyl acrylates having an ester group with 12 or less carbon atoms are preferred, alkyl acrylates having an ester group with 8 or less carbon atoms are more preferred, and alkyl acrylates having an ester group with 6 or less carbon atoms are even more preferred.

[0039] Among these, the first polymer is preferably a copolymer of a (meth)acrylic acid alkyl ester having a reactive group and a (meth)acrylic acid alkyl ester having no reactive group, and more preferably a copolymer of a reactive group and a (meth)acrylic acid alkyl ester, a methacrylic acid alkyl ester having no reactive group, and an acrylic acid alkyl ester having no reactive group. The preferred form of each monomer is as described above.

[0040] When the first polymer is a (meth)acrylic polymer, the proportion of the (meth)acrylic acid alkyl ester having a reactive group relative to 100% by mass of all monomer components constituting the polymer is preferably 5% by mass or more, and more preferably 20% by mass or more, in order to obtain a good matte property of the film obtained, while it is preferably 80% by mass or less, and more preferably 50% by mass or less, in order to obtain good dispersibility of the first polymer in the resin composition and good film formability.

[0041] The proportion of the alkyl methacrylate ester relative to 100% by mass of all monomer components constituting the first polymer is preferably 20% by mass or more, and more preferably 30% by mass or more, in terms of obtaining good weather resistance, while it is preferably 99% by mass or less, and more preferably 90% by mass or less in terms of expressing a matte finish.

[0042] The proportion of the alkyl acrylate ester relative to 100% by mass of all monomer components constituting the first polymer is preferably 0.5% by mass or more, and more preferably 5% by mass or more, in order to achieve good dispersibility of the first polymer in the resin composition, while from the viewpoints of weather resistance and heat resistance, it is preferably 40% by mass or less, and more preferably 25% by mass or less.

[0043] As described above, the (meth)acrylic acid alkyl ester having no reactive group is mentioned as a monomer unit having no reactive group, but the first polymer may further have other vinyl monomer units having no reactive group. Specifically, the other vinyl monomer having no reactive group may be an aromatic vinyl compound such as styrene, chlorostyrene, methylstyrene, or other substituted styrene. These may be used alone or in combination of two or more. The content of these other vinyl monomers having no reactive group relative to 100% by mass of all the structural units constituting the first polymer is not particularly limited, but from the viewpoint of the water whitening resistance of the obtained film or molded product, it is preferably 0% by mass or more, and on the other hand, it is preferably 50% by mass or less.

[0044] The glass transition temperature (Tg) of the first polymer is not particularly limited, but is preferably 120° C. or lower, more preferably 110° C. or lower, in terms of obtaining a good matte appearance in the resulting film or molded article, and good dispersibility in the film or molded article. On the other hand, in terms of obtaining good water whitening resistance, the glass transition temperature (Tg) is preferably 50° C. or higher, particularly preferably 60° C. or higher. The Tg of the first polymer is calculated from the FOX formula using the Tg values ​​of the homopolymers of each monomer component (as described in Polymer Handbook, J. Brandrup, Interscience, 1989).

[0045] The hydroxyl value of the first polymer is not particularly limited, but is preferably 50 mgKOH / g or more, more preferably 60 mgKOH / g or more, and is preferably 230 mgKOH / g or less, more preferably 200 mgKOH / g or less. If the hydroxyl value is 50 mgKOH / g or more, the first polymer is incompatible with the resin mixture of the fluorine-based resin and the second polymer, and the obtained film or molded body exhibits better matte properties. In addition, if the hydroxyl value of the first polymer is 230 mgKOH / g or less, whitening when the obtained film or molded body is exposed to warm water is more suppressed, so it is preferable. The hydroxyl value is calculated by acetylating the hydroxyl groups in 1 g of solid content of the vinyl polymer solution with acetic anhydride and measuring the mg number of potassium hydroxide required to neutralize the acetic acid generated by the acetylation by titration.

[0046] The intrinsic viscosity of the first polymer is not particularly limited, but is preferably 0.3 L / g or less, more preferably 0.15 L / g or less, from the viewpoint of improving the dispersibility of the first polymer in the obtained film or molded article, reducing foreign matter in the film or molded article, and improving the appearance. The intrinsic viscosity of the first polymer is more preferably 0.05 L / g or more, even more preferably 0.06 L / g or more, from the viewpoint of improving the matte property of the obtained film or molded article. The intrinsic viscosity of the first polymer is a value measured at 25°C using a San Denshi Industry AVL-2C automatic viscometer using chloroform as a solvent.

[0047] To adjust the intrinsic viscosity of the first polymer, a polymerization regulator such as mercaptan can be used. Examples of mercaptan include n-octyl mercaptan, n-dodecyl mercaptan, and t-dodecyl mercaptan. The content of mercaptan is preferably 0.01 parts by mass or more relative to 100 parts by mass of the first polymer in order to improve dispersibility. In addition, the content is preferably 1 part by mass or less in order to improve the matte property of the resulting film or molded article.

[0048] The ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the first polymer, Mw / Mn, is preferably 2.3 or less, more preferably 2.2 or less. The smaller this Mw / Mn, the closer the molecular weight distribution of the first polymer is to monodisperse, so the high molecular weight components decrease, and the occurrence of appearance defects due to foreign substances in the film is suppressed. Note that Mw / Mn indicates a value obtained by measurement under the following conditions using gel permeation chromatography (GPC).

[0049] <GPC measurement conditions> Equipment used: HLC-8320GPC system manufactured by Tosoh Corporation Columns: 2 TGKgel SupaerHZM-H (manufactured by Tosoh Corporation, trade name) Eluent: Tetrahydrofuran Column temperature: 40 °C Detector: Differential refractive index (RI)

[0050] The Mw of the first polymer is preferably 30,000 or more, more preferably 50,000 or more. On the other hand, it is preferably 250,000 or less, more preferably 200,000 or less. If the Mw of the first polymer is 30,000 or more, the dispersibility in the resin composition becomes better. On the other hand, if it is 250,000 or less, it is easier to exhibit a fine matte appearance.

[0051] As a method for producing the first polymer, as described above, it can be obtained by selecting monomers to be used so as to have a desired composition and polymerizing them. There is no particular limitation on the polymerization method, and suspension polymerization and emulsion polymerization can be mentioned. Examples of initiators used in suspension polymerization include known organic peroxides and azo compounds. Examples of suspension stabilizers include those obtained by combining known organic colloidal polymer substances, inorganic colloidal polymer substances, inorganic fine particles, and surfactants thereof. As an inorganic suspension stabilizer, those that can be removed by post-treatment of polymerization such as washing are preferred, and for example, tricalcium phosphate can be mentioned.

[0052] Usually, suspension polymerization is carried out using a material in which monomers and the like are suspended in water together with a polymerization initiator in the presence of a suspension stabilizer. Also, when suspension polymerization is carried out, a polymer soluble in the monomer can be dissolved in the monomer and polymerized as necessary. After suspension polymerization, it is preferable to remove cullets, which are components insoluble in chloroform generated during polymerization and cause poor appearance, from the bead-like material obtained by suspension polymerization by sieving. In order to ensure a sufficient yield, the sieve used for sieving is preferably 150 mesh or less, more preferably 50 mesh or less. In order to sufficiently remove cullets, it is preferable to use a sieve of 50 mesh or more, more preferably 150 mesh or more. Cullets refer to lumpy objects that are generated when the polymer adheres to the part in contact with the latex, such as the inner wall surface of the polymerization layer, during polymerization.

[0053] In order to reduce foreign matter in the resulting film or molded article and improve the appearance of the film or molded article, it is preferable that the first polymer does not contain cullets of 300 μm or more, and it is more preferable that the first polymer does not contain cullets of 100 μm or more.

[0054] When an inorganic suspension stabilizer is used, it is preferable to wash the obtained bead-like material of the first polymer with water to reduce the content of inorganic matter in the first polymer in order to suppress the occurrence of fish eyes in the obtained film and suppress printing defects. Examples of the water washing method include a dispersion washing method in which a washing solution such as nitric acid is added to the bead-like material of the thermoplastic resin to disperse it, followed by solid-liquid separation, and a passing washing method in which a washing solution is passed through the bead-like material of the thermoplastic resin. The washing temperature is preferably 10 to 90°C in terms of washing efficiency.

[0055] In the post-treatment such as sieving and water washing after the completion of the polymerization as described above, in order to efficiently remove cullet by sieving without reducing the product yield, and to efficiently remove inorganic matter by washing, the average particle size of the first polymer is preferably 300 μm or less, more preferably 150 μm or less. In addition, in terms of the handleability of the polymer, this average particle size is preferably 10 μm or more, more preferably 20 μm or more. The average particle size of the first polymer can be measured using a laser diffraction scattering type particle size distribution analyzer LA-910 manufactured by HORIBA Co., Ltd.

[0056] [Second polymer] The second polymer is a polymer having 30 mass% or more of (meth)acrylic acid alkyl ester units having 1 to 3 carbon atoms in the ester group and having no reactive group as a constituent unit, and having substantially no reactive group. In the present invention, having substantially no reactive group means that the total ratio of monomers having reactive groups in 100 mass% of the monomer components constituting the polymer is 1.0 mass% or less. By containing the second polymer in the resin composition, it is possible to improve the dispersibility of the first polymer in the obtained film or molded product, reduce foreign matter in the film or molded product, and improve the appearance of the film.

[0057] Examples of methacrylic acid alkyl esters having 1 to 3 carbon atoms in the ester group include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, and i-propyl methacrylate. These may be used alone or in combination of two or more. Among them, methyl methacrylate is preferred from the viewpoint of weather resistance.

[0058] Examples of alkyl acrylates having an ester group with 1 to 3 carbon atoms include methyl acrylate, ethyl acrylate, n-propyl acrylate, and i-propyl acrylate. These may be used alone or in combination of two or more.

[0059] Among the above, the second polymer is preferably a copolymer having, as monomer units, an alkyl methacrylate ester and an alkyl acrylate ester. In this case, the ratio of the alkyl methacrylate ester having 1 to 3 carbon atoms in the ester group to 100% by mass of the monomer components constituting the second polymer is preferably 50% by mass or more, more preferably 85% by mass or more, and even more preferably 92% by mass or more in terms of weather resistance, while being preferably 100% by mass or less, more preferably 99.9% by mass or less in terms of heat resistance.

[0060] The proportion of the acrylic acid alkyl ester having an ester group carbon number of 1 to 3 in 100% by mass of the monomer component is preferably 0% by mass or more, more preferably 0.1% by mass or more, in terms of heat resistance, and preferably 50% by mass or less, more preferably 15% by mass or less, and even more preferably 8% by mass or less, in terms of weather resistance.

[0061] The second polymer may also have other vinyl monomers as monomer units. Specifically, examples of other copolymerizable vinyl monomers include aromatic vinyl compounds such as styrene, chlorostyrene, methylstyrene, and other substituted styrenes, and lower alkoxy acrylates. These may be used alone or in combination of two or more. From the viewpoint of water whitening resistance of the film, the ratio of these vinyl monomers to 100% by mass of all monomer units constituting the second polymer is preferably 0% by mass or more, and is preferably 49% by mass or less.

[0062] The glass transition temperature (Tg) of the second polymer is preferably 80° C. or higher, more preferably 85° C. or higher, from the viewpoint of heat resistance, and is preferably 120° C. or lower, more preferably 110° C. or lower, from the viewpoint of formability of the resulting film or molded article.

[0063] Examples of the polymerization method for the second polymer include suspension polymerization, emulsion polymerization, and bulk polymerization.

[0064] The mass average molecular weight (Mw) of the second polymer is preferably 10,000 or more, more preferably 30,000 or more, from the viewpoint of mechanical properties, while it is preferably 250,000 or less, more preferably 200,000 or less, from the viewpoint of formability of a film or molded article.

[0065] The second polymer may be a commercially available product, such as ACRYPET VH, ACRYPET MD, or ACRYPET MF, available from Mitsubishi Chemical Corporation.

[0066] [Third polymer] The third polymer is a polymer having 30% by mass or more of a (meth)acrylic acid alkyl ester having 4 or more carbon atoms in the ester group as a structural unit, and having substantially no reactive group, and having a composition different from that of the second polymer. When the resin composition contains the third polymer, the film formation stability during molding is improved, and further, fish eyes in the obtained film or molded product can be reduced. The mechanism by which the above effect can be expected by containing the third polymer in the resin composition is not clear, but the following reasons are thought to be the reason.

[0067] The resin composition according to the present embodiment contains a fluororesin and a first polymer for the purpose of improving chemical resistance and improving matte function. However, as described above, since the first polymer has a reactive group, during melt extrusion in producing a film or the like, the first polymers react excessively with each other due to shear heat generation, and when an abnormal polymer with a large particle size is formed, the dispersibility in the fluororesin is reduced, and thermal deterioration of the resin due to retention is caused. As a result, the film formability of the film or molded body is reduced, and further, due to these, spots and foreign matter like fish eyes are formed in the obtained film or molded body. However, as described above, in the present embodiment, since the third polymer having a (meth)acrylic acid alkyl ester with a specific carbon number is contained as a monomer unit, the lubricity of the fluororesin composition can be improved, and as a result, the shear heat generation during melt extrusion is reduced, and the excessive reaction of the first polymer is suppressed, thereby improving the dispersibility of the first polymer in the fluororesin, and it is considered that the film formability stability can be improved and a film or molded body with fewer fish eyes can be obtained.

[0068] Examples of alkyl acrylates having 4 or more carbon atoms in the ester group include n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, phenyl acrylate, and cyclohexyl acrylate. Among these, alkyl acrylates having 18 or less carbon atoms in the ester group are preferred, and alkyl acrylates having 8 or less carbon atoms in the ester group are particularly preferred. These alkyl acrylates may be used alone or in combination of two or more.

[0069] Examples of methacrylic acid alkyl esters having 4 or more carbon atoms in the ester group include n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, stearyl methacrylate, phenyl methacrylate, and cyclohexyl methacrylate. Among these, methacrylic acid alkyl esters having 18 or less carbon atoms in the ester group are preferred, and methacrylic acid alkyl esters having 8 or less carbon atoms in the ester group are particularly preferred. These methacrylic acid alkyl esters may be used alone or in combination of two or more.

[0070] The third polymer may also have other monomer units as monomer units, such as alkyl methacrylates having 1 to 3 carbon atoms.

[0071] Examples of methacrylic acid alkyl esters having 1 to 3 carbon atoms in the ester group include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, and i-propyl methacrylate. These may be used alone or in combination of two or more. Among them, methyl methacrylate is preferred from the viewpoint of weather resistance.

[0072] Among the above, the third polymer is preferably a polymer having at least one monomer selected from n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, and 2-ethylhexyl methacrylate, and methyl methacrylate as monomer units, and among these, a polymer having n-butyl acrylate, n-butyl methacrylate, and methyl methacrylate as monomer units is particularly preferable.

[0073] The total ratio of the (meth)acrylic acid alkyl esters having 4 or more carbon atoms in the ester group to 100% by mass of all monomer units constituting the third polymer is not particularly limited, but as described above, it is 30% by mass or more, and preferably 40% by mass or more, while 70% by mass or less is preferable, and 60% by mass or less is more preferable. If the ratio is 30% by mass or more, the resin composition can provide more lubricity, so that shear heat generation during kneading in the extruder can be suppressed and the occurrence of fish eyes due to thermal deterioration of the resin can be further reduced. In addition, if the ratio is 70% by mass or less, the compatibility with the fluororesin is excellent, and the occurrence of fish eyes due to poor dispersion can be further reduced.

[0074] When the third polymer is composed of both an alkyl acrylate having 4 or more carbon atoms and an alkyl methacrylate having 4 or more carbon atoms as monomer units, the ratio of the alkyl acrylate having 4 or more carbon atoms to the total amount of these is not particularly limited, but is preferably 20 mass% or more, and particularly preferably 30 mass% or more, while being preferably 80 mass% or less, and particularly preferably 70 mass% or less.

[0075] The proportion of the methacrylic acid alkyl ester having an ester group having 1 to 3 carbon atoms relative to 100% by mass of all monomer units constituting the third polymer is not particularly limited, but in order to improve weather resistance, it is preferably 30% by mass or more, and more preferably 40% by mass or more, while in order to improve heat resistance, it is preferably 70% by mass or less, and more preferably 60% by mass or less.

[0076] The third polymer may contain other vinyl monomers. Specific examples include aromatic vinyl compounds such as styrene, chlorostyrene, methylstyrene, and other substituted styrenes, and lower alkoxy acrylates. These may be used alone or in combination of two or more. From the viewpoint of film transparency, the content of these copolymerizable other vinyl monomers is preferably 0% by mass or more, and on the other hand, 20% by mass or less, based on 100% by mass of all monomer units constituting the third polymer.

[0077] The mass average molecular weight (Mw) of the third polymer is not particularly limited, but is preferably 50,000 or more, more preferably 80,000 or more, and even more preferably 120,000 or more. The mass average molecular weight (Mw) of the third polymer is preferably 5,000,000 or less, more preferably 4,000,000 or less, and even more preferably 3,500,000 or less. If the mass average molecular weight (Mw) is 50,000 or more, the resin composition can be given greater lubricity, so that shear heat generation during kneading in an extruder can be suppressed, and the occurrence of fish eyes due to thermal deterioration of the resin can be further reduced, and blooming on the surface of a molded product and plate-out to a mold during molding processing are less likely to occur. On the other hand, if the mass average molecular weight (Mw) is 5,000,000 or less, the compatibility with fluororesins is excellent, and the occurrence of fish eyes due to poor dispersion can be further reduced. In addition, the melt viscosity can be kept lower, and thermal deterioration of the resin due to retention in a molding machine can be suppressed. When the obtained molded article is a film, defects such as a defect called a fish eye caused by thermal degradation that increases over time are less likely to occur, and melt extrusion such as film molding can be performed for a relatively long period of time.

[0078] The third polymer may be a commercially available product, for example, Metablen L (trade name) manufactured by Mitsubishi Chemical Corporation.

[0079] There is no particular limitation on the 5% weight loss temperature of the third polymer, but in order to improve thermal stability, it is preferably 250° C. or higher, more preferably 260° C. or higher, and particularly preferably 270° C. or higher.

[0080] The resin composition may contain two or more types of third polymers.

[0081] The resin composition may contain other components in addition to the fluororesin, the first polymer, the second polymer, and the third polymer. For example, the resin composition may contain a fourth polymer. [Fourth polymer] By including the fourth polymer (D) in the resin composition, when the resin composition is molded, the film formation stability is improved and the generation of gum can be suppressed.

[0082] The fourth polymer is a polymer which contains, as structural units, a methacrylic acid alkyl ester having an ester group with 1 to 3 carbon atoms and a (meth)acrylic acid alkyl ester having an ester group with 4 or more carbon atoms, and which is substantially free of reactive groups.

[0083] Examples of methacrylic acid alkyl esters having 1 to 3 carbon atoms in the ester group include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, and i-propyl methacrylate. These may be used alone or in combination of two or more. Among them, methyl methacrylate is preferred from the viewpoint of weather resistance.

[0084] Examples of alkyl acrylates having an ester group with 4 or more carbon atoms include n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, phenyl acrylate, cyclohexyl acrylate, etc. These may be used alone or in combination of two or more.

[0085] Examples of methacrylic acid alkyl esters having an ester group with 4 or more carbon atoms include n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, stearyl methacrylate, phenyl methacrylate, cyclohexyl methacrylate, etc. These may be used alone or in combination of two or more.

[0086] Although there are no particular limitations on the (meth)acrylic acid alkyl ester having an ester group with 4 or more carbon atoms, it is preferable that the ester group has 18 or less carbon atoms.

[0087] The proportion of the methacrylic acid alkyl ester having an ester group carbon number of 1 to 3 in 100% by mass of the monomer components constituting the fourth polymer is preferably 70% by mass or more, more preferably 75% by mass or more, in terms of weather resistance, and is preferably 90% by mass or less, more preferably 80% by mass or less, in terms of heat resistance.

[0088] The proportion of the (meth)acrylic acid alkyl ester having an ester group having 4 or more carbon atoms in 100% by mass of the monomer components constituting the fourth polymer is preferably 10% by mass or more, more preferably 20% by mass or more, in terms of heat resistance, and is preferably 30% by mass or less, more preferably 25% by mass or less, in terms of weather resistance.

[0089] The fourth polymer may also contain other copolymerizable vinyl monomers. Specific examples include aromatic vinyl compounds such as styrene, chlorostyrene, methylstyrene, and other substituted styrenes, and lower alkoxy acrylates. These may be used alone or in combination of two or more. From the viewpoint of water whitening resistance of the film, the content of these other copolymerizable vinyl monomers is preferably 0 to 50% by mass relative to 100% by mass of the monomer units constituting the fourth polymer.

[0090] The weight average molecular weight (Mw) of the fourth polymer is not particularly limited, but is preferably 500,000 or more, more preferably 1,000,000 or more, while it is preferably 5,000,000 or less, more preferably 4,000,000 or less, and even more preferably 3,500,000 or less. If Mw is 500,000 or more, the swell ratio of the resin composition is increased, the generation of scum during film formation is suppressed, and the appearance is improved. In addition, if Mw is 5,000,000 or less, the transparency of the obtained film is good.

[0091] The fourth polymer may be a commercially available product, such as METABLEN P (trade name) manufactured by Mitsubishi Chemical Corporation, KANEACE PA (trade name) manufactured by Kaneka Corporation, or ACRYLOID (trade name) manufactured by Rohm and Haas Co., Ltd.

[0092] In the resin composition, the content of the fluororesin relative to the total 100% by mass of the fluororesin, the first polymer, and the second polymer is preferably 40% by mass or more, more preferably 47% by mass or more, and even more preferably 54% by mass or more. The content is preferably 98% by mass or less, more preferably 97% by mass or less, and even more preferably 96% by mass or less. If the content of the fluororesin is 40% by mass or more, a film with better chemical resistance can be obtained. If the content of the fluororesin is 98% by mass or less, yellowing of the film due to thermal deterioration of the resin can be further reduced.

[0093] In the resin composition, the content of the first polymer relative to the total 100% by mass of the fluorine-based resin, the first polymer, the second polymer, and the third polymer is preferably 1.0% by mass or more, more preferably 1.5% by mass or more, and even more preferably 2.0% by mass or more. The content is preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 16% by mass or less. If the content of the first polymer is 1.0% by mass or more, the obtained film can be given a good matte appearance. If the content of the first polymer is 20% by mass or less, the fluidity and thermal stability during molding are not too low, and thermal deterioration of the resin can be further suppressed.

[0094] In the resin composition, the content of the second polymer relative to the total 100% by mass of the fluororesin, the first polymer, the second polymer, and the third polymer is preferably 1.0% by mass or more, more preferably 1.5% by mass or more, and even more preferably 2.0% by mass or more. Also, it is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less. If the content of the second polymer is 1.0% by mass or more, the dispersibility of the first polymer in the resin composition is further improved, and the occurrence of fisheyes due to poor dispersion can be further reduced. Also, if the content of the second polymer is 20% by mass or less, the chemical resistance of the obtained film is better.

[0095] In the resin composition, the content of the third polymer relative to the total 100% by mass of the fluorine-based resin, the first polymer, the second polymer, and the third polymer is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more. The content is preferably 10% by mass or less, more preferably 5.0% by mass or less. If the amount of the third polymer added is 0.1% by mass or more, the resin composition can impart lubricity, so that the shear heat generated during kneading in the extruder can be suppressed, and the occurrence of fish eyes due to thermal deterioration of the resin can be further reduced, which is preferable. If the content of the third polymer is 10% by mass or less, the melt viscosity can be further reduced, and the thermal deterioration of the resin due to retention in the molding machine can be further suppressed, which is preferable. When the obtained molded product is a film, defects called fish eyes caused by thermal deterioration are less likely to occur over time, and melt extrusion such as film molding can be performed for a relatively long period of time.

[0096] In the resin composition, the content of the fourth polymer relative to the total 100% by mass of the fluorine-based resin, the first polymer, the second polymer, and the third polymer is not particularly limited, but is 0% by mass or more, preferably 1.0% by mass or more, and more preferably 2.0% by mass or more. The content is preferably 20% by mass or less, and more preferably 10% by mass or less. If the content of the fourth polymer is 1.0% by mass or more, the occurrence of scum on the film is suppressed, and the appearance design of the film is improved, which is preferable. If the content of the fourth polymer is 20% by mass or less, the film thickness variation and appearance defect due to melt fracture do not occur, which is preferable.

[0097] Various additives may be blended into the resin composition of the present invention as necessary, such as antioxidants, heat stabilizers, light stabilizers, plasticizers, lubricants, spreading agents, antistatic agents, flame retardants, fillers, matting agents, processing aids, impact resistance aids, antibacterial agents, antifungal agents, foaming agents, release agents, colorants, ultraviolet absorbers, and thermoplastic polymers.

[0098] These may be known. Examples of the antioxidant include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. Examples of the heat stabilizer include hindered phenol-based heat stabilizers, sulfur-based heat stabilizers, and hydrazine-based heat stabilizers. Examples of the plasticizer include phthalic acid esters, phosphoric acid esters, fatty acid esters, aliphatic dibasic acid esters, oxybenzoic acid esters, epoxy compounds, and polyesters. Examples of the lubricant include fatty acid esters, fatty acids, metal soaps, fatty acid amides, higher alcohols, and paraffins. Examples of the antistatic agent include cationic antistatic agents, anionic antistatic agents, nonionic antistatic agents, and amphoteric antistatic agents. Each of these additives may be used alone or in combination of two or more.

[0099] The resin composition can be produced by a known method such as a single-screw kneading method, a same-direction twin-screw kneading method, or a different-direction twin-screw kneading method using an extruder, which is a general compound processing method. Among them, a method with a large kneading effect, such as a twin-screw kneading method, is preferable. An example of the twin-screw extruder is the TEM series manufactured by Toshiba Machine Co., Ltd. In addition, an example of the screw configuration is a screw configuration having a conveying section for conveying the resin composition and a kneading section for kneading the resin composition, such as a kneading zone or a screw segment in which the feeding direction of the molten material is opposite (a screw segment in which the spiral winding direction is opposite).

[0100] In addition, the extruder preferably has a vent capable of degassing the moisture in the resin composition as the raw material and the volatile gas generated from the melt kneaded molten material. It is preferable to install a decompression pump such as a vacuum pump in the vent. This pump efficiently discharges the generated moisture and volatile gas to the outside of the extruder. In addition, a screen for removing foreign matter mixed in during extrusion reduction can be installed in a zone before the die part of the extruder to remove the foreign matter from the resin composition. Examples of this screen include a filter pack using a wire mesh or a sintered metal nonwoven fabric, a screen changer, and a leaf disk type and pleat type polymer filter.

[0101] In addition, as a method for increasing the kneading effect, it is possible to increase the screw rotation speed as much as possible and reduce the amount of resin composition supplied. The resin composition melt-extruded in this way is prone to shear heat, and the resin temperature at the head tends to be high. The melt kneaded in the extruder is extruded as a strand from a die having a nozzle with a diameter of about 3 to 5 mm installed in the head, and is cut by a cold cut method or a hot cut method and pelletized.

[0102] Furthermore, the number of times the resin composition is kneaded is not limited, and kneading can be carried out in one stage or in multiple stages using a master batch.

[0103] The resin composition may be in the form of, for example, a lump, a powder, or a pellet. Among these, the pellet form is preferred from the viewpoint of the handleability of the resin composition.

[0104] In the present invention, when the MFRs (based on JIS K7210 A method) of the fluororesin, the first polymer, and the second polymer measured at 200°C and a load of 49N for 4 minutes are defined as MFR(A), MFR(B), and MFR(C), respectively, it is preferable to satisfy the relationship of "MFR(A)>MFR(B)≒MFR(C)". By satisfying this relationship, the dispersibility of the first polymer in the resin mixture of the fluororesin and the second polymer during melt extrusion is improved, and the matte stability of the film is improved. Note that MFR(B)≒MFR(C) means that the difference between MFR(B) and MFR(C) is within ±0.5g / 10min. Note that the MFR value is a value measured based on JIS K7210, and can be measured using a product name Melt Indexer manufactured by Techno Seven Co., Ltd.

[0105] [film] A film can be produced by molding the resin composition according to this embodiment. That is, the film contains the resin composition according to this embodiment, and the film has excellent matte properties and chemical resistance. In addition, since the manufacturing variation of the matte appearance during film production is very small, the productivity when obtaining the film is good. Furthermore, since the occurrence of fish eyes during film production can be reduced, the obtained film has the characteristic of having very few appearance defects.

[0106] In the performance evaluation of a film, the 60-degree surface gloss is used as an index of the high-class feeling of the design. In general, it is preferable that the 60-degree surface gloss is low. The 60-degree surface gloss of the film is preferably 5% or more, more preferably 6% or more, and even more preferably 7% or more. In addition, the 60-degree surface gloss is preferably 70% or less, more preferably 50% or less, and even more preferably 30% or less. If the 60-degree surface gloss is 70% or less, the obtained film has a matte property and is excellent in design and decoration such as a high-class feeling and a sense of depth. In addition, if the 60-degree surface gloss is 5% or more, it is not necessary to add a large amount of a matte agent, and the appearance defects of the film such as fish eyes are reduced. The surface gloss of the film is a value measured in accordance with JIS Z8741.

[0107] The standard deviation of the 60 degree surface gloss is preferably 6 or less, more preferably 3 or less, and even more preferably 2 or less, in order to improve production stability and yield.

[0108] The arithmetic mean roughness (Ra) of the film is preferably 0.05 or more, more preferably 0.10 or more, and even more preferably 0.15 or more. Also, it is preferably 0.50 or less, more preferably 0.45 or less, and even more preferably 0.43 or less. If Ra is 0.05 or more, the film has low glare and is excellent in design and decorative properties such as a sense of luxury and depth. If Ra is 0.50 or less, the matte texture is fine and the film has excellent appearance design. The arithmetic mean roughness (Ra) is a value measured in accordance with JIS B0601-2001.

[0109] The average length (Rsm) of the contour curve element of the film is preferably 30 or more, more preferably 35 or more, and even more preferably 40 or more. Also, it is preferably 90 or less, more preferably 85 or less, and even more preferably 80 or less. If Rsm is 30 or more, the film has low glare and is excellent in design and decorativeness such as a sense of luxury and depth. If Rsm is 90 or less, the film has a fine matte texture and is excellent in appearance design. The average length (Rsm) of the contour curve element is a value measured in accordance with JIS B0601-2001.

[0110] The light transmittance of the film is preferably 80% or more, more preferably 83% or more, and even more preferably 85% or more, as measured according to JIS K7361-1. If the total light transmittance is 80% or more, the decorative layer printed on the film looks beautiful when viewed from the side on which the decorative layer is not printed.

[0111] The haze of the film is not particularly limited as long as the total light transmittance is 80% or more. From the viewpoint of the beauty of the appearance as a matte film, the haze is preferably 95% or less, more preferably 90% or less, and even more preferably 85% or less. The haze of the film is a value measured according to JIS K7136.

[0112] From the viewpoint of appearance design, the number of fisheyes in the film is set at 0.05 mm for a 40 μm thick film. 2 Number of fish eyes of size 20 or more per 0.01m 2 Preferably less than 10 pieces / 0.01m 2 It is more preferable that:

[0113] The thickness of the film is preferably 1 μm or more, more preferably 5 μm or more, from the viewpoint of good handling and lamination properties of the film, and is preferably 500 μm or less, more preferably 300 μm or less, from the viewpoint of good film formability and processability when formed into a film.

[0114] Examples of the film manufacturing method include melt extrusion methods such as melt casting, T-die method, and inflation method; and calendar method. Among these, the T-die method is preferred because of its good economic efficiency. After the film is formed by the T-die method using an extruder or the like, it can be wound up on a tubular object such as a paper tube by a winder to form a roll-shaped product. In addition, if necessary, a stretching step such as uniaxial stretching (machine direction or transverse direction (direction perpendicular to the machine direction)) or biaxial stretching (sequential biaxial stretching, simultaneous biaxial stretching) by a known stretching method can be provided during the film formation process. When melt extrusion is performed, it is preferable to extrude the resin composition in a molten state while filtering it through a screen mesh of 200 mesh or more in order to remove nuclei and foreign matter that may cause poor appearance.

[0115] In addition, a fine structure can be formed on the film surface as necessary. Examples of methods for forming a fine structure include a thermal transfer method and an etching method. Among these, a thermal transfer method in which a mold having a fine structure is heated and then the heated mold is pressed against the surface of the film to form a fine structure on the surface of the film is preferred in terms of productivity and economy. Examples of the thermal transfer method include the following methods (1) and (2). (1) A method in which a mold having a microstructure is hot-pressed onto a film cut out from a roll-shaped product, thereby thermally transferring the microstructure sheet by sheet. (2) A continuous shaping method in which a film unwound from a roll-shaped product is sandwiched between a heated belt-shaped mold having a microstructure using a nip roll, and pressure is applied to thermally transfer the microstructure to the surface of the film.

[0116] Methods for producing a mold having the above-mentioned fine structure include, for example, a sandblasting method, an etching method, and an electric discharge machining method.

[0117] The film obtained from the resin composition according to the present embodiment can be combined with other films for lamination. In particular, the film obtained from the resin composition according to this embodiment is preferably used as a laminate film with another acrylic resin layer. A specific form of such a laminate film will be described below. In the following, for convenience, the film obtained from the resin composition according to this embodiment may be referred to as "film (X)" and the other acrylic resin layer may be referred to as "acrylic resin layer (Y)".

[0118] [Laminated film] The laminated film is a laminate of a film (X) and an acrylic resin layer (Y). This laminated film is preferable because it improves the formability of the laminated film and the visibility of the decorative layer. In addition to the acrylic layer, films made of other resins such as ionomer resins, polyolefin resins, silicone resins, epoxy resins, and polyurethane resins can also be used.

[0119] The layer thickness ratio of the film (X) to the acrylic resin layer (Y) (hereinafter referred to as "(X) / (Y)") is preferably 1 / 99 or more, more preferably 2 / 98 or more, from the viewpoints of the solvent resistance, cost, transparency, and matte appearance of the laminated film. In addition, from the viewpoints of surface hardness and printability, the value of (X) / (Y) is preferably 50 / 50 or less, more preferably 20 / 80 or less. The thickness of each film can be calculated by observing a sample obtained by cutting the laminated film to a thickness of 70 nm in the cross-sectional direction with a transmission electron microscope. An example of a commercially available transmission electron microscope is the product name J100S manufactured by JEOL Ltd.

[0120] The 60 degree surface gloss of the laminated film measured from the film (X) side is preferably 5% or more, more preferably 6% or more, and even more preferably 7% or more. The 60 degree surface gloss is preferably 70% or less, more preferably 50% or less, and even more preferably 30% or less. If the 60 degree surface gloss is 70% or less, the resulting film has good matte properties and is excellent in design and decorative properties such as a luxurious feel and a deep feeling. If the 60 degree surface gloss is 5% or more, it is not necessary to add a large amount of a matte agent, and appearance defects of the film such as fish eyes are reduced.

[0121] The standard deviation of the 60 degree surface gloss is preferably 6 or less, more preferably 3 or less, and even more preferably 2 or less, in order to improve production stability and yield.

[0122] The arithmetic mean roughness (Ra) of the laminated film measured from the film (X) side is preferably 0.05 or more, more preferably 0.10 or more, and even more preferably 0.15 or more, while it is preferably 0.50 or less, more preferably 0.45 or less, and even more preferably 0.43 or less. If Ra is 0.05 or more, the film has low glare and is excellent in design and decorativeness such as a sense of luxury and depth. If Ra is 0.50 or less, the matte texture is fine and the external design is excellent. The arithmetic mean roughness (Ra) is a value measured in accordance with JIS B0601-2001.

[0123] The average length (Rsm) of the contour curve element of the laminated film measured from the film (X) side is preferably 30 or more, more preferably 35 or more, and even more preferably 40 or more, while it is preferably 90 or less, more preferably 85 or less, and even more preferably 80 or less. If Rsm is 30 or more, the film has low glare and is excellent in design and decorativeness such as a sense of luxury and depth. If Rsm is 90 or less, the matte texture is fine and the external design is excellent. The average length (Rsm) of the contour curve element is a value measured in accordance with JIS B0601-2001.

[0124] The light transmittance of the laminated film is preferably 80% or more, more preferably 83% or more, and even more preferably 85% or more, as measured according to JIS K7361-1. If the total light transmittance is 80% or more, the decorative layer printed on the film looks beautiful when viewed from the side on which the decorative layer is not printed.

[0125] The haze of the laminated film is not particularly limited as long as the total light transmittance is 80% or more. From the viewpoint of the beauty of the appearance of the film, the haze is preferably 95% or less, more preferably 90% or less, and even more preferably 85% or less.

[0126] Regarding the surface hardness of the laminate film, the pencil hardness (JIS K5400) measured from the film (X) side is preferably higher than B. More preferably, HB or higher, and most preferably F or higher. When a laminate film having a pencil hardness higher than B is used, the laminate film is less likely to be scratched during the process of insert molding or in-mold molding described below, and further has good scratch resistance. When used for vehicle applications, the laminate film preferably has a pencil hardness of HB or higher. When the laminate film has a pencil hardness of HB or higher, the resulting laminate can be suitably used for various vehicle members such as door waist garnishes, front control panels, power window switch panels, and airbag covers. Furthermore, when the pencil hardness is higher than F, scratches are hardly noticeable even when scratched with a rough cloth such as gauze, so that the industrial utility value is high. As described above, the surface hardness of the laminate film can be adjusted by selecting the thickness ratio of the film (X) and the acrylic resin layer (Y) or the acrylic resin composition constituting the acrylic resin layer (Y).

[0127] From the viewpoint of appearance design, the number of fisheyes in the laminated film is set at 0.01 mm for a film with a thickness of 75 μm (film thickness ratio (X) / (Y)=9 / 91). 2 Number of fish eyes of size 100 or more per 0.5m 2 Preferably less than 75 pieces / 0.5m 2More preferably, 50 pieces / 0.5m or less. 2 It is more preferable that the number of fisheyes in the laminated film is equal to or less than 1000. The number of fisheyes in the laminated film can be measured, for example, by using an offline fisheye counter. An example of a commercially available offline fisheye counter is the trade name LSC-4500 manufactured by MEC Co., Ltd.

[0128] The thickness of the laminated film is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 40 μm or more in terms of good handling and lamination properties of the film, and is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less in terms of good film formability and processability when molded into a film.

[0129] [Acrylic resin layer (Y)] The acrylic resin layer (Y) is a layer made of an acrylic resin composition (y). The acrylic resin composition (y) is preferably an acrylic resin composition containing a rubber-containing polymer.

[0130] Examples of the rubber-containing polymer include rubber-containing multi-stage polymers having, as at least the polymer constituents, a known alkyl acrylate and / or alkyl methacrylate, and a graft crosslinking agent. A specific example of a rubber-containing multistage polymer is one formed by polymerizing, in this order, an elastic polymer (S) having as at least a polymer component an acrylic acid alkyl ester having an ester group with 1 to 8 carbon atoms and / or a methacrylic acid alkyl ester having an ester group with 1 to 4 carbon atoms, and a graft crosslinking agent, and a rigid polymer (H) having as at least a polymer component an methacrylic acid alkyl ester having an ester group with 1 to 4 carbon atoms.

[0131] The elastic polymer (S) is, for example, a polymer having as its constituent components an acrylic acid alkyl ester having an ester group carbon number of 1 to 8 and / or a methacrylic acid alkyl ester having an ester group carbon number of 1 to 4 (S1) (hereinafter referred to as "component (S1)"), another monomer (S2) (hereinafter referred to as "component (S2)") used as necessary, a multifunctional monomer (S3) (hereinafter referred to as "component (S3)") used as necessary, and a graft crossing agent (S4) (hereinafter referred to as "component (S4)"), and is the first to be polymerized when polymerizing the rubber-containing multistage polymer.

[0132] Among the components (S1), the alkyl acrylate having 1 to 8 carbon atoms in the ester group may be either linear or branched. Specific examples thereof include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate. These may be used alone or in combination of two or more. Among these, those with a low Tg are preferred, and butyl acrylate is more preferred.

[0133] Among the components (S1), the methacrylic acid alkyl ester having an ester group with 1 to 4 carbon atoms may be either linear or branched. Specific examples thereof include methyl methacrylate, ethyl methacrylate, propyl methacrylate, and butyl methacrylate. These may be used alone or in combination of two or more.

[0134] From the viewpoints of flexibility, transparency and processability, it is preferable to use 60 to 100 mass % of the component (S1) relative to 100 mass % in total of the components (S1) to (S4).

[0135] Examples of the component (S2) include alkyl acrylate monomers such as alkyl acrylates having an ester group with 9 or more carbon atoms, acrylates having an alkoxy group with 4 or less carbon atoms, and cyanoethyl acrylate; acrylamide, (meth)acrylic acid, styrene, alkyl-substituted styrene, and (meth)acrylonitrile.

[0136] From the viewpoint of flexibility, the component (S2) is preferably used in an amount of 0 to 40 mass % relative to 100 mass % in total of the components (S1) to (S4).

[0137] Examples of the component (S3) include alkylene glycol dimethacrylates such as ethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate, and propylene glycol dimethacrylate; and polyvinylbenzenes such as divinylbenzene and trivinylbenzene.

[0138] From the viewpoint of flexibility, the component (S3) is preferably used in an amount of 0 to 10 mass % relative to 100 mass % in total of the components (S1) to (S4).

[0139] Examples of the component (S4) include allyl, methallyl or crotyl esters of copolymerizable α,β-unsaturated carboxylic or dicarboxylic acids, triallyl cyanurate, triallyl isocyanurate, etc. Among these, allyl esters of acrylic acid, methacrylic acid, maleic acid or fumaric acid are preferred, and allyl methacrylate is more preferred. The component (S4) reacts mainly due to the conjugated unsaturated bond of the ester reacting much faster than the allyl group, methallyl group or crotyl group, to form a chemical bond.

[0140] From the viewpoint of flexibility, the component (S4) is preferably used in an amount of 0.1 to 5 mass%, more preferably 0.5 to 2 mass%, based on 100 mass% of the total of the components (S1) to (S4). The lower limit of this range is significant in terms of the effective amount of graft bonding. The upper limit is significant in terms of appropriately suppressing the amount of reaction with the polymer formed next by polymerization, thereby preventing a decrease in the elasticity of the rubber elastomer.

[0141] The content of the elastomeric polymer (S) in the rubber-containing multistage polymer is preferably from 5 to 70% by mass, more preferably from 5 to 50% by mass, from the viewpoints of flexibility, transparency and processability.

[0142] The elastomeric polymer (S) may be polymerized in two or more stages. When the polymer is polymerized in two or more stages, the ratio of the monomer components constituting each stage may be changed.

[0143] The rigid polymer (H) is a component involved in the moldability and mechanical properties of the rubber-containing multistage polymer, and is a polymer composed of an alkyl methacrylate ester (H1) (hereinafter referred to as "component (H1)") having an ester group with 1 to 4 carbon atoms and another monomer (H2) (hereinafter referred to as "component (H2)") used as necessary, which is polymerized last when polymerizing the rubber-containing multistage polymer. Preferable specific examples of the components (H1) and (H2) are the same as those given for the components (S1) and (S2) of the elastic polymer (S), respectively.

[0144] From the viewpoint of transparency, the component (H1) is preferably used in an amount of 51 to 100 mass % relative to 100 mass % in total of the components (H1) and (H2).

[0145] From the viewpoint of mechanical properties, the Tg of the hard polymer (H) alone is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 80° C. or higher. From the viewpoint of film formability, the Tg is preferably 150° C. or lower, and more preferably 130° C. or lower.

[0146] The content of the hard polymer (H) in the rubber-containing multistage polymer is preferably from 30 to 95% by mass, more preferably from 40 to 70% by mass, from the viewpoints of flexibility, transparency and processability.

[0147] The rubber-containing multistage polymer has an elastic polymer (S) and a hard polymer (H) as a basic structure. After polymerizing the elastic polymer (S) and before polymerizing the hard polymer (H), one or more layers of an intermediate polymer (M) may be polymerized. The intermediate polymer (M) has a composition that is intermediate between the composition of the elastic polymer (S) and the composition of the hard polymer (H). By providing the intermediate polymer (M), the transparency of the obtained film can be improved.

[0148] The content of the intermediate polymer (M) in the rubber-containing multistage polymer is preferably from 0 to 35 mass%, more preferably from 0 to 25 mass%, relative to 100 mass% in total of the elastic polymer (S) and the hard polymer (H).

[0149] The average particle size of the rubber-containing polymer is preferably 0.03 μm or more, more preferably 0.07 μm or more, and even more preferably 0.09 μm or more, from the viewpoint of mechanical properties and transparency of the laminated film including the acrylic resin layer (Y) mainly composed of the rubber-containing polymer, and is preferably 0.3 μm or less, more preferably 0.15 μm or less, and even more preferably 0.13 μm or less, from the viewpoint of film transparency.

[0150] The mass average molecular weight (Mw) of the acetone soluble portion of the rubber-containing polymer is preferably 20,000 or more, more preferably 30,000 or more. Also, it is preferably 80,000 or less, more preferably 70,000 or less. If Mw is 20,000 or more, the mechanical strength of the obtained laminated film is improved, and cracks during molding processing can be suppressed. Also, the obtained laminated film exhibits stress whitening resistance. If Mw is 80,000 or less, the obtained laminated film has high flexibility and excellent processability. After the laminated film is bonded to a substrate such as a steel plate, whitening does not occur at the bent portion during bending processing, and the appearance of the obtained various parts is good.

[0151] The gel content of the rubber-containing polymer is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 55% by mass or more. Also, it is preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less. If the gel content of the rubber-containing polymer is 40% by mass or more, the mechanical strength of the obtained molded body can be increased, and handling becomes easier. Also, if the gel content is 99% by mass or less, the fluidity and thermal stability during molding can be increased, the melt viscosity can be reduced, and the retention in the molding machine can be reduced, which is preferable because the thermal deterioration of the resin can be suppressed. When the obtained molded body is a film, problems such as an increase in fish eyes caused by thermal deterioration over time are unlikely to occur, and melt extrusion such as film molding can be performed for a long period of time.

[0152] The gel content of the rubber-containing polymer can be calculated according to the following formula. G = (m / M) x 100 In the formula, G (%) represents the gel content of the rubber-containing polymer, M represents the mass of a given amount of the rubber-containing polymer (also referred to as the mass before extraction), and m represents the mass of the acetone-insoluble portion of the given amount of the rubber-containing polymer (also referred to as the mass after extraction). More specifically, m was obtained by dissolving the rubber-containing polymer in acetone at a concentration of 1 g / 100 mL, refluxing the solution at 65°C for 4 hours and centrifuging the solution, refluxing the remaining solid again, centrifuging the resulting solution and decanting the resulting solid, and drying the resulting solid at 50°C for 24 hours.

[0153] The acrylic resin composition (y) may contain a thermoplastic resin. The thermoplastic resin is not particularly limited, and may be any known thermoplastic resin.

[0154] Examples of the thermoplastic resin include polyethylene resins, polypropylene resins, vinyl chloride resins, polystyrene resins, acrylonitrile-styrene copolymer resins, polyethylene terephthalate resins, acrylic resins, ethylene-vinyl acetate copolymer resins, vinylidene chloride resins, polycarbonate resins, polyamide resins, polyacetal resins, polybutylene terephthalate resins, fluorine resins, thermoplastic elastomers, etc. These may be used alone or in combination of two or more.

[0155] The thermoplastic resin that can be used in the present invention is preferably an acrylic resin that is required to have qualities such as transparency, weather resistance, etc. For example, the above-mentioned second polymer can be mentioned.

[0156] The acrylic resin layer (Y) may contain various additives as required. Examples of additives include antioxidants, heat stabilizers, light stabilizers, plasticizers, lubricants, antistatic agents, flame retardants, fillers, matting agents, processing aids, impact resistance aids, antibacterial agents, antifungal agents, foaming agents, release agents, colorants, ultraviolet absorbers, and thermoplastic polymers. These may be used alone or in combination of two or more.

[0157] When the laminated film is laminated on a substrate for the purpose of protecting the substrate, it is preferable to add an ultraviolet absorber to the acrylic resin layer (Y) to impart weather resistance. The molecular weight of the ultraviolet absorber is preferably 300 or more, more preferably 400 or more. When an ultraviolet absorber with a molecular weight of 300 or more is used, for example, mold contamination due to volatilization of the ultraviolet absorber during vacuum molding or pressure molding in an injection mold can be prevented. In addition, generally, the higher the molecular weight of the ultraviolet absorber, the less likely it is to cause long-term bleed-out after processing into a film state, and the ultraviolet absorbing performance will last for a longer period of time than those with a lower molecular weight.

[0158] Furthermore, when the molecular weight of the UV absorber is 300 or more, the amount of UV absorber that volatilizes during the production of the film is small. Therefore, the amount of UV absorber that remains is sufficient, and good performance is exhibited. In addition, the problem of the volatilized UV absorber recrystallizing and growing over time, adhering to the film and causing defects in appearance is reduced.

[0159] As the ultraviolet absorbent, known ones can be used, but in particular, benzotriazole-based ones having a molecular weight of 400 or more or triazine-based ones having a molecular weight of 400 or more are preferable. Examples of commercially available ultraviolet absorbents include BASF's Tinuvin 234 and Tinuvin 1577, and ADEKA's Adeka STAB LA-31 and Adeka STAB LA-46.

[0160] The amount of the ultraviolet absorber added is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more, based on 100 parts by mass of the resin constituting the acrylic resin composition (y), from the viewpoint of weather resistance. Also, from the viewpoint of preventing process contamination during film formation and the viewpoint of transparency of the molded product, it is preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 3.0 parts by mass or less.

[0161] In addition, it is preferable to add a light stabilizer to the acrylic resin layer (Y). As the light stabilizer, a known one can be used, but a radical scavenger such as a hindered amine light stabilizer is particularly preferable. Examples of commercially available products of such light stabilizers include Adeka STAB LA-57, Adeka STAB LA-67, and Adeka STAB LA-77, both of which are products of ADEKA Corporation, and Chimassorb 2020FDL and Chimassorb 944FDL, both of which are products of BASF Japan.

[0162] The amount of the light stabilizer added is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, based on 100 parts by mass of the resin constituting the acrylic resin composition (y) from the viewpoint of weather resistance. Also, from the viewpoint of thermal stability, it is preferably 2.0 parts by mass or less, more preferably 1.0 parts by mass or less. If it is 2.0 parts by mass or less, the thermal stability during molding can be increased and the increase in melt viscosity due to thermal deterioration of the resin can be suppressed to a lower level, and the retention in the molding machine can be reduced, which is preferable because the thermal deterioration of the resin can be suppressed. When the obtained molded product is a film, defects called fish eyes caused by thermal deterioration are unlikely to occur over time, and melt extrusion such as film molding can be performed for a long period of time.

[0163] It is preferable to add an antioxidant to the acrylic resin layer (Y). As the antioxidant, known ones can be used, but phenol-based antioxidants are particularly preferable. The phenol-based antioxidant is not particularly limited, and may be a known phenol-based antioxidant that is a compound containing a phenolic hydroxyl group. Examples of commercially available products of such phenol-based antioxidants include Adeka STAB AO-50, Adeka STAB AO-60, and Adeka STAB AO-80 from ADEKA Corporation, and Irganox1010, Irganox1035, and Irganox1076 from BASF Japan.

[0164] The amount of the antioxidant added is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 0.8 parts by mass or more, based on 100 parts by mass of the resin constituting the acrylic resin composition (y), from the viewpoints of thermal stability and weather resistance during molding. Also, from the viewpoints of preventing process contamination during film formation and transparency of the molded product, it is preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 3.0 parts by mass or less.

[0165] [Laminated film manufacturing method] A laminated film can be provided by laminating the film (X) and the acrylic resin layer (Y). As a method for producing the laminated film, a co-extrusion method in which the film (X) and the acrylic resin layer (Y) are simultaneously melt-extruded and laminated is preferred, in terms of reducing the number of production steps.

[0166] Methods for laminating multiple molten resin layers include (1) a method for laminating molten resin layers before passing through a die, such as a feed block method, (2) a method for laminating molten resin layers within a die, such as a multi-manifold method, and (3) a method for laminating molten resin layers after passing through a die, such as a multi-slot method.

[0167] When the film (X) and the acrylic resin layer (Y) are laminated while being melt-extruded at the same time, it is preferable to melt-extrude the acrylic resin layer (Y) so that it comes into contact with a cooling roll in terms of the matte surface of the fluorine-based film. Specifically, the laminated film of the present invention can be produced by a production method including the following steps. Two melt extruders are prepared, and their cylinder temperatures and die temperatures are set to 200 to 250°C. In one of the extruders, the resin composition of the film (X) is melt-plasticized. At the same time, in the other extruder, the acrylic resin composition (y) is melt-plasticized. The molten resins extruded from the dies at the tips of both extruders are co-extruded onto a cooling roll set to 50 to 100°C.

[0168] Each of the film (X) and the acrylic resin layer (Y) constituting the laminate film may be composed of a plurality of layers.

[0169] When melt extrusion is performed, it is preferable to extrude the resin composition constituting each layer in a molten state while filtering it through a screen mesh of 200 mesh or more in order to remove nuclei and foreign matter that may cause printing defects.

[0170] The thickness of the laminate film is preferably 500 μm or less. In the case of a film used for a laminate molded product, the thickness is preferably 30 μm or more, more preferably 50 μm or more. Also, it is preferably 400 μm or less, more preferably 300 μm or less. If the thickness is 30 μm or more, sufficient depth can be obtained in the appearance of the molded product. In particular, when molding into a complex shape, sufficient thickness can be obtained by stretching. On the other hand, if the thickness is 400 μm or less, the laminate film has appropriate rigidity, so that lamination properties, secondary processability, etc. are improved. In addition, it is economically advantageous in terms of mass per unit area. Furthermore, the film-forming properties are stable, making it easy to manufacture the film.

[0171] [Decorative film] The film (X) and the laminated film can be used as a decorative film. The decorative film has a pattern layer on at least one surface of the film (X) or the laminated film. In particular, from the viewpoint of printability, it is preferable that the acrylic resin layer has a pattern layer.

[0172] The pattern layer constituting the decorative film can be formed by a known method. In particular, it is preferable to use one or both of a printed layer formed by a printing method and a vapor deposition layer formed by a vapor deposition method as the pattern layer. This printed layer becomes a pattern or letters on the surface of the laminate obtained by insert or in-mold molding, which will be described later. Examples of the printed pattern include patterns consisting of wood grain, stone grain, cloth grain, sand grain, geometric patterns, letters, full solid color, metallic, etc.

[0173] Examples of the method for forming the printed layer include known printing methods such as offset printing, gravure rotary printing, and screen printing, known coating methods such as roll coating and spray coating, and flexographic printing. The thickness of the printed layer may be appropriately determined as needed, and is usually about 0.5 to 30 μm. The thickness of the printed layer may be appropriately selected according to the degree of elongation during molding so that the desired surface appearance can be obtained in the laminate obtained by insert or in-mold molding described later.

[0174] [Laminated molded body] The laminated film is further laminated on a substrate to produce a laminated molded article having the film (X) on the surface thereof. Here, the laminate is laminated so that the surface of the acrylic resin layer (Y) is in contact with the substrate.

[0175] The substrate can be appropriately selected depending on the intended laminated molded product, and examples of the material include resin, wood boards such as wooden veneer, wooden plywood, particle board, and medium density fiberboard (MDF), wood boards such as wood fiberboard, and metals such as iron and aluminum. In the case of resin molded products, examples include thermoplastic resins such as polyvinyl chloride resin, olefin resin, ABS resin, and polycarbonate resin.

[0176] The thickness of the substrate can be appropriately set according to need, and is usually preferably about 20 to 500 μm, more preferably 50 to 300 μm. The thickness of the substrate can maintain the mechanical properties and handling properties of the film.

[0177] When the substrate is two-dimensional and made of a material capable of being thermally fused, the substrate and the laminate film can be laminated by a method such as thermal lamination. For metal members and the like that are difficult to thermally fused, an adhesive may be used or one side of the laminate film may be adhesively processed for lamination. For laminates having a three-dimensional shape, known methods such as insert molding, in-mold molding, and three-dimensional overlay laminate molding can be used.

[0178] The three-dimensional overlay laminate molding method is as follows: First, two sealed spaces separated by a sheet are formed, a molded body is placed in one of the spaces, and the pressure is reduced in both spaces or only in the space where the molded body is placed. Next, the sheet is heated and softened, and while the molded body is pressed against the sheet surface from one space side to the other space side, only the other space where the molded body is not placed is returned to normal pressure, and the sheet is attached to the molded body using the pressure difference.

[0179] In the three-dimensional overlay laminate molding method, the heated sheet is applied with uniform pressure to the surface of the molded body, so that the sheet can be successfully attached to the molded body even if the surface of the molded body is curved. An example of an apparatus for performing three-dimensional overlay laminate molding is "TOM (product name)" manufactured by Fuse Vacuum Co., Ltd. EXAMPLES

[0180] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the following description, "parts" means "parts by mass" and "%" means "% by mass". Abbreviations mean the following: MMA Methyl methacrylate BA n-Butyl acrylate BDMA 1,3-butylene glycol dimethacrylate AMA Allyl Methacrylate MA Methyl acrylate HEMA 2-Hydroxyethyl Methacrylate St Styrene LPO Lauryl Peroxide CHP Cumene Hydroperoxide tBH t-Butyl hydroperoxide RS610 Sodium mono-n-dodecyloxytetraoxyethylene phosphate (Phosphanol RS-610NA: manufactured by Toho Chemical Industry Co., Ltd.) OTP Di-2-ethylhexyl Sodium Sulfosuccinate (Pelex OT-P: manufactured by Kao Corporation) nOM n-Octyl mercaptan EDTA Disodium Ethylenediaminetetraacetate SFS Sodium Formaldehyde Sulfoxylate

[0181] [Evaluation method] (1) Average particle size of the first polymer The mass average particle size of the first polymer was measured using a laser diffraction / scattering particle size distribution analyzer LA-910 manufactured by HORIBA Corporation.

[0182] (2) Intrinsic viscosity of the first polymer The intrinsic viscosity of the first polymer was measured in a chloroform solvent at 25° C. using an AVL-2C automatic viscometer manufactured by San Denshi Kogyo Co., Ltd.

[0183] (3) Average particle size of rubber-containing polymer The mass average particle size of the rubber-containing polymer was measured by dynamic light scattering using a light scattering photometer DLS-700 (trade name) manufactured by Otsuka Electronics Co., Ltd.

[0184] (4) Gel content of rubber-containing polymer The acetone solution in which 0.5 g of rubber-containing polymer was dissolved in 50 mL of acetone as the pre-extraction mass M was refluxed at 65° C. for 4 hours. The obtained extract was centrifuged at 14,000 rpm for 30 minutes at 4° C. using a high-speed cooling centrifuge (manufactured by Hitachi Koki Co., Ltd., product name: CR21G). The solution was removed by decantation to obtain the remaining solid. The reflux, centrifugation, and decantation were repeated for this solid, and the obtained solid was dried at 50° C. for 24 hours, and the mass of the acetone insoluble matter obtained was measured as the post-extraction mass m. The gel content G (%) of the rubber-containing polymer was calculated from the pre-extraction mass M and the post-extraction mass m according to the following formula. Gel content G (%) = (mass after extraction m (g) / mass before extraction M (g)) x 100

[0185] (5) 60 degree surface gloss In accordance with JIS Z8741, the 60 degree surface gloss of the film (X) side of the laminated film was measured using a portable glossmeter (manufactured by Konica Minolta, Inc., product name: GM-268Plus). The measurement points were 14 points in total, 7 points equally spaced in the film production width direction and 2 points in the film production flow direction, and all the measured values ​​were averaged to obtain the measured value.

[0186] (6) Total light transmittance, haze The total light transmittance and haze of the laminated film were measured in accordance with JIS K7361-1 and JIS K7136, respectively, using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name: NDH4000) under conditions of a light source of D65 and a temperature of 25°C.

[0187] (7) Arithmetic mean roughness (Ra) and mean length of profile curve elements (Rsm) Using a surface roughness measuring instrument (Tokyo Seimitsu Co., Ltd., product name: SURFCOM 1400D), the arithmetic mean roughness (Ra) and the mean length of the profile curve element (Rsm) of the film (X) side of the laminated film were measured in accordance with JIS B0601-2001 under the conditions of measurement length 4.0 mm, evaluation length 4.0 mm, cutoff wavelength 0.8 mm, and measurement speed 0.3 mm / s. When measuring a long sample such as a film, it can be measured in either the transverse direction (TD) or the longitudinal direction (MD), but evaluation must be performed in either TD or MD only. The arithmetic mean roughness (Ra) is the value, expressed in micrometers (μm), calculated by the following formula when a reference length is extracted from a roughness curve in the direction of the mean line, the X axis is plotted in the direction of the mean line of this extracted portion, and the Y axis is plotted in the direction of the longitudinal magnification, and the roughness curve is expressed as y = f(x).

[0188]

number

[0189] The average length of a profile element (Rsm) is the average of the lengths Xs of the profile elements in the reference length, and is expressed in micrometers (μm) using the following formula: Xsi is the length of one profile element.

[0190]

number

[0191] (8) Chemical resistance rating 1 A piece of gauze was placed on the surface of the film (X) side of the laminated film (test piece), a drop of suntan lotion (product name: Coppertone Waterbabies SPF50) was placed on top of it, and a 5 cm x 5 cm aluminum plate and a 500 g load were placed on top of that, in that order, and left for 1 hour at 74°C. The test piece was then washed with a neutral detergent and air-dried, and the surface of the test piece was visually observed to evaluate the chemical resistance according to the following criteria. ○: No change on the surface of the test piece. △: Slight traces of solvent remain on the surface of the test piece. ×: Traces of the solvent or gauze are clearly remaining on the surface of the test piece, or the surface that came into contact with the solvent is cloudy.

[0192] (9) Chemical resistance rating 2 A drop of 10% lactic acid aqueous solution was placed on the surface of the film (X) side of the laminated film (test piece) and left for 24 hours at 80° C. The test piece was then washed with a neutral detergent and air-dried, and the surface of the test piece was visually observed to evaluate the chemical resistance according to the following criteria. ○: No change on the surface of the test piece. △: Slight traces of solvent remain on the surface of the test piece. ×: Traces of the solvent are clearly visible on the surface of the test piece, the film surface is swollen, or the surface that came into contact with the solvent is cloudy.

[0193] (10) Number of fisheyes on the film 0.05 mm in a film (X) with a thickness of 40 μm 2 The number of fish eyes of a size of 0.01 m or more was visually observed using a contaminant measurement table (manufactured by Choyokai Co., Ltd.). 2 Five pieces of film cut into the range were measured, and the total number of measurements was averaged to calculate the number of fisheyes.

[0194] (Production Example 1: Production of Hydroxyl-Containing Polymer (1)) The following monomer mixture (1) was charged into a reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen gas inlet, etc. Next, the inside of the vessel was sufficiently replaced with nitrogen gas, and then the monomer mixture (1) in the reaction vessel was heated to 75°C while stirring, and reacted for 3 hours in a nitrogen gas stream. After this, the temperature in the reaction vessel was raised to 90°C, and further maintained at 90°C for 45 minutes to complete the polymerization, and the mixture was sieved through a 100 μm mesh, and the beads that passed through were dehydrated and dried to obtain a hydroxyl group-containing polymer (1). The resulting hydroxyl-containing polymer (1) had a glass transition temperature of 77° C., an intrinsic viscosity of 0.11 L / g, Mw / Mn of 2.1, and an average particle size of 70 μm.

[0195] <Monomer mixture (1)> MA: 10 parts MMA: 60 parts HEMA: 30 copies nOM: 0.18 parts LPO: 1 copy Tricalcium phosphate: 1.8 parts Deionized water: 250 parts

[0196] (Production Example 2: Production of Rubber-Containing Polymer (2-1)) A polymerization vessel equipped with a stirrer, a cooling tube, a thermocouple, and a nitrogen inlet tube was charged with 195 parts of deionized water, and then a premix of 0.3 parts of MMA, 4.5 parts of BA, 0.05 parts of AMA, 0.2 parts of BDMA, 0.025 parts of CHP, and 1.3 parts of RS610 was charged and heated to 75°C. After the temperature was raised, a mixture consisting of 5 parts of deionized water, 0.20 parts of SFS, 0.0001 parts of ferrous sulfate, and 0.0003 parts of EDTA was charged into the polymerization vessel at once to initiate polymerization. After the peak of the temperature rise was confirmed, the temperature was maintained for 15 minutes, and the polymerization of the first elastic polymer (S-1-1) was completed. Next, 9.6 parts of MMA, 14.4 parts of BA, 0.25 parts of AMA, 1.0 parts of BDMA, and 0.016 parts of CHP were dropped into the polymerization vessel over 90 minutes, and the mixture was then held for 60 minutes to complete the polymerization of the second elastic polymer (S-2-1). The first elastomeric polymer (S-1-1) had a Tg of -48°C, and the second elastomeric polymer (S-2-1) had a Tg of -10°C.

[0197] Then, 6.0 parts of MMA, 4.0 parts of BA, 0.075 parts of AMA, and 0.0125 parts of CHP were dropped into the polymerization vessel over 45 minutes. The mixture was then held for 60 minutes to complete the polymerization of the intermediate polymer (M-1). The Tg of the intermediate polymer (M-1) was 60°C.

[0198] Finally, 57.0 parts of MMA, 3.0 parts of MA, 0.075 parts of tBH, and 0.264 parts of nOM were dropped into the polymerization vessel over 140 minutes. The mixture was then held for 60 minutes to complete the polymerization of the hard polymer (H-1). The Tg of the hard polymer (H-1) was 79.3°C. The average particle size of the resulting latex-like rubber-containing polymer (2-1) was 0.11 μm.

[0199] 100 parts of the latex-like rubber-containing polymer (2-1) was filtered using a vibration filter equipped with a SUS mesh with an opening of 62 μm. The latex was then coagulated by dropping it into 100 parts of hot water at 80° C. containing 3.5 parts of calcium acetate. The temperature was then raised to 95° C. and held for 5 minutes to solidify. The obtained coagulated product was separated and washed, and dried at 75° C. for 24 hours to obtain a powder-like rubber-containing polymer (2-1). The gel content of the rubber-containing polymer (2-1) was 70%, and Mw was 58,000.

[0200] [Table 1]

[0201] (Production Example 3: Production of Rubber-Containing Polymer (2-2)) The ratio of each raw material was changed to the ratio shown in Table 1, and a rubber-containing polymer (2-2) was produced by the following method. 244 parts of deionized water was placed in a polymerization vessel equipped with a reflux condenser and heated to 80° C. Next, a mixed aqueous solution of 0.6 parts of SFS, 0.00012 parts of ferrous sulfate, and 0.0003 parts of EDTA was added to the polymerization vessel, and 1 / 15 of the monomer mixture for the first stage was charged while stirring under a nitrogen atmosphere, and the mixture was maintained for 15 minutes. The remaining first-stage monomer mixture was then added dropwise at an increasing rate of 8% / hour relative to the water, and the mixture was held for 60 minutes to obtain a polymer latex. The Tg of the polymer obtained from the first-stage monomer mixture was 4°C.

[0202] 0.6 parts of SFS was added to this polymer latex and held for 15 minutes. Next, under a nitrogen atmosphere, while stirring at 80°C, the second stage monomer mixture was added dropwise at an increase rate of 4% / hour relative to water, and then held for 120 minutes to obtain a polymer latex. The Tg of the polymer obtained from the second stage monomer mixture was -37°C.

[0203] 0.4 parts of SFS was added to the latex of this polymer and kept for 15 minutes. Next, under a nitrogen atmosphere, while stirring at 80°C, the monomer mixture of the hard polymer was dropped at an increasing rate of 10% / hour with respect to water, and then kept for 60 minutes to obtain a latex of rubber-containing polymer (2-2). The Tg of the hard polymer was 99°C.

[0204] The average particle size of the resulting latex-like rubber-containing polymer (2-2) was 0.28 μm. 100 parts of latex-like rubber-containing polymer (2-2) was filtered with a vibration filter equipped with a SUS mesh with a mesh size of 150 μm. Then, it was salted out in an aqueous solution containing 3.5 parts of calcium acetate, washed with water to recover the solid content, and then dried to obtain a powder-like rubber-containing polymer (2-2). The gel content of the obtained rubber-containing polymer (2-2) was 90%, and Mw was 45,000.

[0205] (Production Example 4: Production of acrylic resin composition (y)) 80 parts of the rubber-containing polymer (2-1) obtained in Production Example 2, 10 parts of the rubber-containing polymer (2-2) obtained in Production Example 3, 10 parts of an acrylic resin (manufactured by Mitsubishi Chemical Corporation, product name: ACRYPET MD), and additives such as 1.4 parts of an ultraviolet absorber (manufactured by BASF Japan Ltd., product name: Tinuvin 234), 0.3 parts of a light stabilizer (manufactured by ADEKA Corporation, product name: LA-57), and 0.1 parts of an antioxidant (manufactured by BASF Japan Ltd., product name: Irganox 1076) were added and mixed using a Henschel mixer.

[0206] This mixture was extruded into a strand shape using a degassing extruder (manufactured by Toshiba Machine Co., Ltd., product name: TEM-35B, the same applies below) at a cylinder temperature of 100 to 240°C and a die temperature of 240°C while removing impurities with a screen mesh. The extruded mixture was then cooled through a water bath and cut to obtain pellets of acrylic resin composition (y).

[0207] (Production Example 5: Production of second polymer (1)) A second copolymer (1) was obtained according to the method for producing a rigid (co)polymer (B-1) in Production Example 7 of JP-A No. 2003-313392.

[0208] (Production Example 6: Production of third polymer (1)) A third polymer (1) was obtained according to the production method of the copolymer composition (b-2) in Reference Example 2 of JP-A No. 2000-319516.

[0209] (Production Example 7: Production of Fourth Polymer (1)) A fourth polymer (1) was obtained according to the method for producing a thermoplastic polymer (VII-1) described in JP-A-2005-139416.

[0210] [Example 1] A multi-manifold die was installed at the tip of the 40 mmφ single screw extruder 1 and the 30 mmφ single screw extruder 2. The pellets of the acrylic resin composition (y) obtained in Production Example 4 were fed into a single-screw extruder 1 having a cylinder temperature of 230 to 240° C. and melted and plasticized.

[0211] Separately, 68 parts of PVDF (manufactured by Kureha Corporation, trade name KFT#850) as a fluororesin, 9 parts of a hydroxyl group-containing polymer (1) as a first polymer (1), 18 parts of a second polymer (1), 0.8 parts of a third polymer (1) (Mw=160000), 5 parts of a fourth polymer (1) (Mw=1500000), and 0.8 parts of an antioxidant (manufactured by ADEKA Corporation, trade name: Adeka STAB AO-60) were mixed. The mixture was extruded into strands using a degassing extruder at a cylinder temperature of 100-240°C and a die temperature of 250°C while removing impurities with a screen mesh, and then cut and pelletized after cooling through a water bath. The pellets were fed into a single-screw extruder at a cylinder temperature of 200-230°C and melt-plasticized.

[0212] These molten plasticized materials were fed into a multi-manifold die heated to 240° C. to obtain a laminated film having a film (X) layer with a thickness of 8.7 μm and an acrylic resin layer (Y) with a thickness of 66.3 μm. At that time, the temperature of the cooling roll was set to 80° C., and the acrylic resin layer (Y) was brought into contact with the cooling roll to obtain a laminated film. The evaluation results of the obtained laminated film are shown in Table 2.

[0213] [Example 2] A 75 μm laminated film was obtained in the same manner as in Example 1, except that the composition was changed to that shown in Table 2. The evaluation results of the obtained laminated film are shown in Table 2.

[0214] [Comparative Example 1] A 75 μm laminated film was obtained in the same manner as in Example 1, except that the composition was changed as shown in Table 2. The evaluation results of the obtained laminated film are shown in Table 2.

[0215] [Comparative Example 2] A 75 μm laminated film was obtained in the same manner as in Example 1, except that the composition was changed to that shown in Table 2. The evaluation results of the obtained laminated film are shown in Table 2.

[0216] [Table 2]

[0217] The above examples and comparative examples have revealed the following. The films obtained in Examples 1 and 2 had an arithmetic mean roughness Ra of 0.1 to 1.0 μm, an average length Rsm of a contour curve element of 30 to 100 μm, and had a matte appearance with extremely low glare, and had good design and decorative properties such as a sense of luxury and depth. They also had excellent chemical resistance to sunscreen and 10% lactic acid. 2 Number of fish eyes of size 20 or more per 0.01m 2 The results were as follows: the number of defects was very few and the appearance was good. By adding two or more specific acrylic polymers, it is possible to impart lubricity and long-run properties to the resin composition, thereby preventing thermal deterioration of the resin during extrusion processing and adhesion of resin deterioration products at the die exit, and reducing the occurrence of fisheyes. On the other hand, the films obtained in Comparative Examples 1 and 2 had good matte properties and chemical resistance, but 2 Number of fish eyes of size 20 or more per 0.01m 2 For example, when a printing layer is applied directly or after lamination to a resin sheet, problems such as ink loss may frequently occur.

[0218] The resin composition of the present invention can reduce fish eyes that cause poor appearance of the film, and has a fine matte finish, excellent transparency and chemical resistance. [Industrial Applicability]

[0219] As described above, the matte film, laminate film, decorative film, laminate sheet, and laminate molded product produced from the resin composition of the present invention are particularly suitable for vehicle applications and building material applications. Specific examples include automotive interior applications such as instrument panels, console boxes, meter covers, door lock bezels, steering wheels, power window switch bases, center clusters, and dashboards, automotive exterior applications such as weather strips, bumpers, bumper guards, side mudguards, body panels, spoilers, front grilles, strut mounts, wheel caps, center pillars, door mirrors, center ornaments, side moldings, door moldings, window moldings, windows, headlamp covers, taillamp covers, and windshield parts, and AV equipment and furniture product applications. the like; as surface decorative materials for furniture; as building interior materials for walls, ceilings, floors, etc.; as building exterior materials for exterior walls such as siding, fences, roofs, gates, gable boards, etc.; as surface decorative materials for furniture such as window frames, doors, handrails, thresholds, lintels, etc.; as optical components such as various displays, lenses, mirrors, goggles, window glass, etc.; as interior and exterior decoration materials for various types of vehicles other than automobiles, such as trains, airplanes, ships, etc.; as various packaging containers and materials such as bottles, cosmetic containers, accessory cases, etc.; and as miscellaneous goods for prizes, accessories, etc.

Claims

1. A resin composition containing a fluorine-based resin, a first polymer, a second polymer, and a third polymer, the first polymer is a polymer having a reactive group, the second polymer is a polymer having 30 mass% or more of a (meth)acrylic acid alkyl ester having an ester group having 1 to 3 carbon atoms as a structural unit, and having substantially no reactive group; the third polymer is a polymer having 30% by mass or more of a (meth)acrylic acid alkyl ester having an ester group having 4 or more carbon atoms as a structural unit, and having substantially no reactive group; The resin composition, wherein the second polymer and the third polymer have different compositions.

2. The resin composition according to claim 1, wherein the third polymer has a mass average molecular weight of 50,000 to 500,000.

3. The resin composition according to claim 1 or 2, further comprising a fourth polymer having, as structural units, a methacrylic acid alkyl ester having an ester group with 1 to 3 carbon atoms and a (meth)acrylic acid alkyl ester having an ester group with 4 to 18 carbon atoms, and having substantially no reactive group.

4. The resin composition according to claim 3 , wherein the fourth polymer has a mass average molecular weight of 500,000 or more and 5,000,000 or less.

5. The resin composition according to any one of claims 1 to 4, wherein a ratio of the fluororesin to a total of 100 mass% of the fluororesin, the first polymer, the second polymer, and the third polymer is 40 mass% or more and 98 mass% or less.

6. The resin composition according to any one of claims 1 to 5, wherein a ratio of the first polymer to a total of 100 mass% of the fluororesin, the first polymer, the second polymer, and the third polymer is 1 mass% or more and 20 mass% or less.

7. The resin composition according to any one of claims 1 to 6, wherein a ratio of the second polymer to a total of 100 mass% of the fluororesin, the first polymer, the second polymer, and the third polymer is 1 mass% or more and 40 mass% or less.

8. The resin composition according to any one of claims 1 to 7, wherein a ratio of the third polymer to a total of 100 mass% of the fluororesin, the first polymer, the second polymer, and the third polymer is 0.1 mass% or more and 10 mass% or less.

9. A resin composition described in any one of claims 1 to 8, wherein the fluororesin is polyvinylidene fluoride.

10. The resin composition according to any one of claims 1 to 9, wherein the first polymer is an acrylic polymer.

11. The resin composition according to any one of claims 1 to 10, wherein the reactive group of the first polymer is one or more selected from the group consisting of a carboxy group, a hydroxy group, an acid anhydride group, an epoxy group, an isocyanate group, an amide group, an amino group, a cyano group and an imine group.

12. A film comprising the resin composition according to any one of claims 1 to 11.

13. A molded article having the film according to claim 12.

Citation Information

Patent Citations

  • Thermoplastic resin composition and molded product thereof

    JP2000204222A

  • Auxiliary for processing resin and thermoplastic resin composition using the same

    JP2000319516A

  • Vinylidene fluoride resin composition, production method thereof, and molding comprising the same

    JP2002080674A

  • Surface protective film for innerior / exterior building materials, and method for manufacturing the same

    JP2008007709A