Thermoplastic resin composition, its production method and molded article
A thermoplastic resin composition with polycarbonate, specific vinyl copolymers, and acrylic block copolymers addresses the challenges of vibration welding strength, flow marks, and impact resistance, providing improved performance for automotive parts.
Patent Information
- Application Number
- JP2021028568
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-02-25
AI Technical Summary
Existing thermoplastic resin compositions for automotive exterior parts face challenges in achieving excellent vibration welding strength, flow mark resistance, and impact resistance, with previous solutions either compromising on one or more of these properties.
A thermoplastic resin composition comprising polycarbonate resin, specific weight average molecular weight vinyl copolymers, and an acrylic block copolymer, combined in specific ratios, to enhance vibration welding strength, flow mark resistance, and impact resistance.
The composition achieves improved vibration welding strength, reduced flow marks, and enhanced impact resistance in molded products, suitable for automotive applications without painting.
Smart Images

Figure 0007585868000004 
Figure 0007585868000001 
Figure 0007585868000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin composition having excellent vibration welding strength, resistance to tiger stripes and flow marks, and impact resistance, and to a molded article thereof. [Background technology]
[0002] Acrylonitrile-styrene-acrylate (ASA) resin, which is made by polymerizing acrylic rubber polymers, aromatic vinyl monomers, and vinyl cyanide monomers, is a resin with excellent weather resistance because it does not have double bonds in its main chain. PC / ASA resin, which is a blend of ASA resin and polycarbonate (PC) resin, has excellent weather resistance, impact resistance, and moldability, and is used in a wide range of fields including automotive interior and exterior parts, communication device housings, and building materials.
[0003] Conventionally, automotive exterior parts such as spoilers have been manufactured by integrating multiple molded bodies with hot melt adhesives, but in recent years, they are often integrated using vibration welding to increase productivity. Vibration welding is a method in which two thermoplastic resin molded bodies are pressed together and one of the molded bodies is given a reciprocating motion to generate frictional heat and weld them together. On the other hand, in recent years, there have been an increasing number of cases in which the painting process is omitted in automotive exterior parts in order to reduce costs and volatile organic compounds, and there is a demand for thermoplastic resins that have excellent appearance, especially those that do not produce tiger stripe flow marks (hereinafter referred to as flow marks).
[0004] In response to such demands, Patent Document 1 proposes a PC / ASA resin composition that has excellent appearance of melted areas in vibration welding by copolymerizing 1,3-butadiene monomer units during the production of an acrylic rubber polymer.
[0005] Generally, flow marks can be suppressed by lowering the viscosity of PC resin or acrylonitrile-styrene (AS) resin, but this tends to impair impact resistance. Therefore, as in Patent Document 2, a PC / ABS resin composition has been proposed that makes flow marks inconspicuous in molded products by blending a specific diene rubber polymer, an aromatic vinyl copolymer with a specific relative viscosity, and a polycarbonate resin in a specific composition ratio. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2000-302824 A [Patent Document 2] Japanese Patent Application Publication No. 8-253651 [Patent Document 3] International Publication No. 2018 / 116850 [Patent Document 4] JP 2020-164774 A Summary of the Invention [Problem to be solved by the invention]
[0007] The resin composition described in Patent Document 1 has excellent vibration weldability, but the rubber is easily deformed during molding, so flow marks are likely to occur. On the other hand, when an attempt is made to improve this problem by the technology described in Patent Document 2, the vibration weld strength is poor and the compatibility with flow mark resistance is insufficient.
[0008] Furthermore, Patent Document 3 proposes an ABS resin composition that has excellent paintability by containing two types of aromatic vinyl copolymers with different weight-average molecular weights, and Patent Document 4 proposes a resin composition that has excellent impact resistance, fluidity, and the like by adding an acrylic block copolymer to a PC / AS resin, but neither of these proposes any description of vibration weldability or flow marks.
[0009] In view of the above-mentioned problems in the prior art, an object of the present invention is to provide a thermoplastic resin composition which gives a molded product excellent in all of vibration welding strength, flow mark resistance and impact resistance. [Means for solving the problem]
[0010] As a result of extensive investigations to solve the above problems, the inventors have discovered that a resin composition which is excellent in all of vibration welding strength, flow mark resistance and impact resistance can be provided by using a polycarbonate having a specific fluidity, combining two or more types of aromatic vinyl monomers having specific weight-average molecular weights in a specific ratio, and further adding a specific amount of an acrylic block copolymer, thereby completing the present invention.
[0011] That is, the present invention is comprised of the following (1) to (6): (1) A thermoplastic resin composition comprising (A) a polycarbonate resin, (B) a vinyl copolymer obtained by copolymerizing a monomer mixture containing an aromatic vinyl monomer and a vinyl cyanide monomer, and (C) an acrylic graft copolymer obtained by graft copolymerizing a monomer mixture containing at least an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of an acrylic rubber polymer, wherein the melt volume rate of the polycarbonate resin (A) is 14 cm 3 / 10 minutes or more 45cm 3 / 10 minutes or less, the vinyl copolymer (B) includes (B-1) having a weight average molecular weight of 250,000 or more and 400,000 or less and (B-2) having a weight average molecular weight of 80,000 or more and 135,000 or less, (A) is 35 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the total of (A), (B) and (C), (B-1) is 8 parts by mass or more and 13 parts by mass or less, (B-2) is 22 parts by mass or more and 42 parts by mass or less, and (C) is 10 parts by mass or more and 15 parts by mass or less A thermoplastic resin composition comprising: (2) The thermoplastic resin composition according to (1), further comprising (D) an acrylic block copolymer in an amount of 0.5 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the total of (A), (B), and (C). (3) The thermoplastic resin composition according to (2), wherein the (D) acrylic block copolymer is an acrylic block copolymer having a polymer block containing a methacrylic acid ester unit and a polymer block containing an acrylic acid ester unit. (4) The thermoplastic resin composition according to any one of (1) to (3), wherein the glass transition temperature of the acrylic rubber polymer contained in the acrylic graft copolymer (C) is −60° C. or higher. (5) A method for producing a thermoplastic resin composition, comprising melt-kneading a graft copolymer obtained by graft copolymerizing at least a monomer mixture containing an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of (A) a polycarbonate resin, (B) a vinyl copolymer obtained by copolymerizing a monomer mixture containing an aromatic vinyl monomer and a vinyl cyanide monomer, and (C) an acrylic graft copolymer, wherein the melt volume rate of the polycarbonate resin (A) is 14 cm 3 / 10 minutes or more 45cm 3 / 10 minutes or less, the vinyl copolymer (B) includes (B-1) having a weight average molecular weight of 250,000 or more and 400,000 or less and (B-2) having a weight average molecular weight of 80,000 or more and 135,000 or less, (A) is 35 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the total of (A), (B) and (C), (B-1) is 8 parts by mass or more and 13 parts by mass or less, (B-2) is 22 parts by mass or more and 42 parts by mass or less, and (C) is 10 parts by mass or more and 15 parts by mass or less The present invention relates to a method for producing a thermoplastic resin composition comprising the steps of: (6) A molded article obtained by molding the thermoplastic resin composition according to any one of (1) to (4). Effect of the Invention
[0012] According to the present invention, it is possible to obtain a thermoplastic resin composition which, when molded into a molded article, has excellent vibration welding strength, flow mark resistance, and impact resistance. [Brief description of the drawings]
[0013]
Figure 1
[0014] The thermoplastic resin composition and its molded article of the present invention will be specifically described below.
[0015] (1) Polycarbonate resin (A) The polycarbonate resin (A) used in the present invention is obtained by reacting an aromatic dihydroxy compound, typically exemplified by 2,2-bis(4-hydroxyphenyl)propane and 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, with a carbonate precursor, typically exemplified by phosgene.
[0016] Examples of aromatic dihydroxy compounds include 2,2-bis(4-hydroxyphenyl)propane (hereinafter sometimes referred to as bisphenol A), 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(3-tert-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, and the like. bis(hydroxyaryl)alkanes such as 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylpropane, 2,2-bis(3-phenyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, and bis(4-hydroxyphenyl)diphenylmethane; Bis(hydroxyaryl)cycloalkanes such as cyclohexane; bisphenols containing a cardo structure such as 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene; dihydroxydiaryl ethers such as 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether; 4,4'-dihydroxydiphenyl sulfide and 4,4'-dihydroxy-3,3'-dimethyl dihydroxydiaryl sulfides exemplified by 4,4'-dihydroxydiphenyl sulfide and the like; dihydroxydiaryl sulfoxides exemplified by 4,4'-dihydroxydiphenyl sulfoxide and the like; dihydroxydiaryl sulfones exemplified by 4,4'-dihydroxydiphenyl sulfone and the like; hydroquinone, resorcin, 4,4'-dihydroxydiphenyl, etc. These can be used alone or in combination of two or more kinds.Among these, bis(4-hydroxyphenyl)alkanes are preferred, and bisphenol A is more preferred.
[0017] Examples of carbonate precursors include phosgene, carbonyl halides, carbonate esters, and haloformates, and more specifically, phosgene; diaryl carbonates such as diphenyl carbonate and ditolyl carbonate; dialkyl carbonates such as dimethyl carbonate and diethyl carbonate; and dihaloformates of dihydric phenols. These can be used alone or in combination. Among these, phosgene is preferred.
[0018] The melt volume rate of the polycarbonate resin (A) used in the present invention, measured in accordance with ISO 1133-1:2011 under conditions of temperature: 300°C and load: 1.2 kg, is 14 cm from the viewpoint of flow mark resistance. 3 / 10 minutes or more, and from the viewpoint of impact resistance, 45cm 3 / 10 minutes or less, preferably 30 cm 3 / 10 minutes or less. The method for producing the polycarbonate resin (A) used in the present invention is not particularly limited, and any method can be used, such as interfacial polymerization method (phosgene method), melt transesterification method, solution polymerization method (pyridine method), ring-opening polymerization method of a cyclic carbonate compound, and solid-phase transesterification method of a prepolymer.
[0019] (2) Vinyl copolymer (B) The vinyl copolymer (B) used in the present invention is a copolymer of a monomer mixture containing an aromatic vinyl monomer and a vinyl cyanide monomer, and examples of the aromatic vinyl monomer include styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene, o-methylstyrene, vinyltoluene, and t-butylstyrene. The aromatic vinyl monomer may contain two or more of these. Among the aromatic vinyl monomers, styrene is preferred from the viewpoint of the flowability of the thermoplastic resin composition and the molded product.
[0020] The content of the aromatic vinyl monomer in the monomer mixture is preferably 50% by mass or more, more preferably 60% by mass or more, based on 100% by mass of the total monomer mixture, from the viewpoints of flowability and moldability of the thermoplastic resin composition, while the content of the aromatic vinyl monomer in the monomer mixture is preferably 90% by mass or less, more preferably 80% by mass or less, from the viewpoints of impact resistance of the molded product.
[0021] Examples of the vinyl cyanide monomer include acrylonitrile, methacrylonitrile, and ethacrylonitrile. The vinyl cyanide monomer may contain two or more of these. Among the vinyl cyanide monomers, acrylonitrile is preferred from the viewpoint of further improving the impact resistance of the molded product.
[0022] From the viewpoint of impact resistance of the molded article, the content of the vinyl cyanide monomer in the monomer mixture is preferably 5% by mass or more and 40% by mass or less, and more preferably 15% by mass or more and 35% by mass or less, relative to 100% by mass of the total monomer mixture.
[0023] The monomer mixture constituting the vinyl copolymer (B) may contain, in addition to an aromatic vinyl monomer and a vinyl cyanide monomer, a (meth)acrylic acid ester monomer, a maleimide monomer, an acid anhydride monomer, an unsaturated fatty acid, an acrylamide monomer, and the like.
[0024] In the present invention, the method for producing the vinyl copolymer (B) may be, for example, a polymerization method such as bulk polymerization, suspension polymerization, bulk suspension polymerization, solution polymerization, emulsion polymerization, or precipitation polymerization. Two or more of these may be combined. The method for feeding the monomers constituting each copolymer is not particularly limited, and the monomers may be fed all at once at the beginning, or the monomers may be fed in several batches in order to adjust the composition distribution of the copolymer to a desired range.
[0025] In the present invention, it is important that the vinyl copolymer (B) contains at least two vinyl copolymers (B-1) and (B-2) below, which have a specific structure using the above monomers. The vinyl copolymer (B-1) and the vinyl copolymer (B-2) are both copolymers consisting of at least an aromatic vinyl monomer and a cyanide vinyl monomer, and have different weight-average molecular weights. That is, the vinyl copolymer (B-1) has a weight-average molecular weight of 250,000 or more and 400,000 or less. The vinyl copolymer (B-2) has a weight-average molecular weight of 80,000 or more and 135,000 or less. By using two types of vinyl copolymers (B-1) and (B-2) with different weight-average molecular weights in this way, a resin composition that has excellent vibration welding strength, flow resistance, and impact resistance when molded into a molded product can be obtained.
[0026] Vinyl copolymer (B-1) and vinyl copolymer (B-2) If the weight average molecular weight of the vinyl copolymer (B-1) is less than 250,000, the vibration welding strength is poor, and if it exceeds 400,000, flow marks are likely to occur. If the weight average molecular weight of the vinyl copolymer (B-2) is less than 80,000, the vibration welding strength is poor, and if it exceeds 100,000, flow marks are likely to occur.
[0027] Here, the weight average molecular weight of the vinyl copolymer (B) is a weight average molecular weight measured using a gel permeation chromatography (GPC) device and converted into polystyrene (PS) equivalent.
[0028] (3) Acrylic graft copolymer (C) The acrylic graft copolymer (C) used in the present invention is a graft copolymer obtained by graft polymerization of a monomer mixture containing an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of an acrylic rubber polymer obtained by copolymerizing a monomer mixture containing an acrylic acid ester monomer and a polyfunctional monomer.
[0029] The acrylic ester monomer constituting the acrylic rubber polymer is preferably one having an alkyl group having 1 to 10 carbon atoms, such as methyl acrylate, ethyl acrylate, n-butyl acrylate, t-butyl acrylate, and octyl acrylate. Two or more of these may be used. Among these, n-butyl acrylate is preferred.
[0030] The polyfunctional monomer constituting the acrylic rubber polymer is not particularly limited as long as it has two or more functional groups, and examples of the functional group include groups having a carbon-carbon double bond such as an allyl group and a (meth)acryloyl group. Examples of the polyfunctional monomer include allyl compounds such as allyl acrylate, allyl methacrylate, diallyl maleate, triallyl cyanurate, and triallyl isocyanurate, and di(meth)acrylic acid ester compounds such as divinylbenzene, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, and propylene glycol dimethacrylate. Two or more of these may be used. Among these, allyl methacrylate is preferred.
[0031] The polymerization method for the acrylic rubber polymer can be any method such as emulsion polymerization, suspension polymerization, continuous bulk polymerization, or solution continuous polymerization, and two or more of these methods may be combined. Among these, emulsion polymerization or bulk polymerization is preferred. The emulsion polymerization is the most preferred because it is easy to adjust the volume average particle size to a desired range by removing heat during polymerization.
[0032] The emulsifier used in the emulsion polymerization method is not particularly limited, and various surfactants can be used. As the surfactant, anionic surfactants such as carboxylate type, sulfate ester salt type, and sulfonate salt type are preferably used. Two or more of these may be used.
[0033] Specific examples of anionic surfactants include caprylates, caprates, laurates, myristic acid salts, palmitates, stearates, oleates, linoleates, linolenates, rosinates, behenates, castor oil sulfates, lauryl alcohol sulfates, dodecylbenzenesulfonates, alkylnaphthalenesulfonates, alkyldiphenyletherdisulfonates, naphthalenesulfonate condensates, dialkylsulfosuccinates, polyoxyethylene lauryl sulfates, polyoxyethylene alkylether sulfates, polyoxyethylene alkylphenylether sulfates, etc. Examples of the salts mentioned here include alkali metal salts such as ammonium salts, sodium salts, lithium salts, and potassium salts.
[0034] The initiator used in the polymerization is not particularly limited, and peroxides, azo compounds, persulfates, etc. may be used.
[0035] Specific examples of peroxides include benzoyl peroxide, cumene hydroperoxide, dicumyl peroxide, diisopropylbenzene hydroperoxide, t-butyl hydroperoxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, t-butyl isopropyl carbonate, di-t-butyl peroxide, t-butyl peroctate, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and t-butylperoxy-2-ethylhexanoate.
[0036] Specific examples of azo compounds include azobisisobutyronitrile, azobis(2,4-dimethylvaleronitrile), 2-phenylazo-2,4-dimethyl-4-methoxyvaleronitrile, 2-cyano-2-propylazoformamide, 1,1'-azobiscyclohexane-1-carbonitrile, azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl 2,2'-azobisisobutyrate, 1-t-butylazo-2-cyanobutane, and 2-t-butylazo-2-cyano-4-methoxy-4-methylpentane.
[0037] Specific examples of persulfates include potassium persulfate, sodium persulfate, and ammonium persulfate.
[0038] Two or more of these initiators may be used. In the emulsion polymerization method, potassium persulfate, cumene hydroperoxide, etc. are preferably used. Redox initiators can also be used.
[0039] The glass transition temperature of the acrylic rubber polymer is preferably -60°C or higher from the viewpoint of suppressing flow marks, and more preferably -50°C or higher. Also, from the viewpoint of impact resistance, it is preferably -30°C or lower. The glass transition temperature is the midpoint glass transition temperature when a DSC curve is obtained under the following conditions. The glass transition temperature of the acrylic rubber polymer may be measured by subjecting the acrylic rubber polymer to DSC, or may be measured by subjecting the acrylic graft copolymer (C) or a thermoplastic resin composition containing the acrylic graft copolymer (C) to DSC, as long as there is no baseline change due to the glass transition due to other components in the vicinity or the baseline change is negligible. Atmosphere gas: Nitrogen Gas flow rate: 30ml / min Starting temperature: -140℃ Heating rate: 20℃ / min Hold temperature: 30℃.
[0040] The monomer mixture constituting the graft portion of the acrylic graft copolymer (C) contains an aromatic vinyl monomer and a vinyl cyanide monomer, and may further contain a monomer copolymerizable therewith, if necessary.
[0041] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene, o-methylstyrene, and t-butylstyrene. Two or more of these may be used. Among these, styrene is preferred.
[0042] Examples of vinyl cyanide monomers include acrylonitrile, methacrylonitrile, and ethacrylonitrile. Two or more of these may be used. Among these, acrylonitrile is preferred.
[0043] The copolymerizable other monomer is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include unsaturated carboxylic acid alkyl ester monomers, unsaturated fatty acids, acrylamide monomers, maleimide monomers, etc. Two or more of these may be used.
[0044] Examples of the unsaturated carboxylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, chloromethyl (meth)acrylate, etc. Two or more of these may be used.
[0045] Examples of unsaturated fatty acids include itaconic acid, maleic acid, fumaric acid, butenoic acid, acrylic acid, methacrylic acid, etc. Two or more of these may be used.
[0046] Examples of the acrylamide monomer include acrylamide, methacrylamide, N-methylacrylamide, etc. Two or more of these may be used. Examples of the maleimide monomer include N-methylmaleimide, N-isopropylmaleimide, N-butylmaleimide, N-hexylmaleimide, N-octylmaleimide, N-dodecylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, etc. Two or more of these may be used.
[0047] The mixing ratio of the monomer mixture is preferably in the range of 60 to 80 weight % of aromatic vinyl monomers, 20 to 40 weight % of vinyl cyanide monomers, and 0 to 20 weight % of other copolymerizable monomers, based on 100 weight % of the total amount of the monomer mixture.
[0048] The graft ratio of the acrylic graft copolymer (C) is preferably from 5 to 40%, more preferably from 5 to 35%, and even more preferably from 5 to 30%, from the viewpoint of the impact strength of the molded article.
[0049] The graft ratio of the acrylic graft copolymer (C) can be determined by the following method. First, 100 ml of acetonitrile is added to a predetermined amount (m; about 1.5 g) of the graft copolymer (I) that has been vacuum dried at 80°C for 3 hours, and the mixture is refluxed in a water bath at 70°C for 3 hours. After centrifuging the solution at 9000 rpm for 40 minutes, the insoluble matter is filtered, and the insoluble matter is vacuum dried at 80°C for 5 hours, and the weight (n) is measured. The graft ratio is calculated by the following formula. Here, L is the rubber content (wt%) of the graft copolymer (i.e., the content (wt%) of the acrylic rubber polymer (A) in the graft copolymer). Graft rate (%) = {[(n)-((m)×L / 100)] / [(m)×L / 100]} x100.
[0050] The graft ratio of the acrylic graft copolymer (C) can be adjusted to a desired range by using, for example, the above-mentioned acrylic rubber polymer and by adjusting the amounts of the chain transfer agent, emulsifier, initiator, etc. used in the polymerization.
[0051] The polymerization method of the acrylic graft copolymer (C) can be any method such as emulsion polymerization, suspension polymerization, continuous bulk polymerization, and solution continuous polymerization, and two or more of these may be combined. Among these, emulsion polymerization or bulk polymerization is preferred. Emulsion polymerization is most preferred because it is easy to control the temperature during polymerization.
[0052] The emulsifier used in the emulsion polymerization of the acrylic graft copolymer (C) may be any of those exemplified as the emulsifier used in the emulsion polymerization of the acrylic rubber polymer. The polymerization initiator used in the polymerization of the graft portion may be any of those exemplified as the initiator used in the polymerization of the acrylic rubber polymer.
[0053] A chain transfer agent can be used for the purpose of adjusting the degree of polymerization and the graft rate of the grafted portion. Specific examples of the chain transfer agent include mercaptans such as n-octyl mercaptan, t-dodecyl mercaptan, n-dodecyl mercaptan, n-tetradecyl mercaptan, and n-octadecyl mercaptan, and terpenes such as terpinolene. Two or more of these may be used. Among these, n-octyl mercaptan and t-dodecyl mercaptan are preferably used.
[0054] From the viewpoint of adjusting the graft ratio within the above-mentioned preferred range, it is preferable to use 0.05 to 0.5 parts by weight of a chain transfer agent, 0.5 to 5 parts by weight of an emulsifier, and 0.1 to 0.5 parts by weight of an initiator in the polymerization of the graft portion relative to 100 parts by weight in total of the acrylic rubber polymer and the monomer mixture.
[0055] The acrylic graft copolymer (C) can be recovered by adding a coagulant to the acrylic graft copolymer (C) latex produced by emulsion polymerization. An acid or a water-soluble salt is used as the coagulant. Specific examples of the coagulant include acids such as sulfuric acid, hydrochloric acid, phosphoric acid, and acetic acid, and water-soluble salts such as calcium chloride, magnesium chloride, barium chloride, aluminum chloride, magnesium sulfate, aluminum sulfate, ammonium aluminum sulfate, potassium aluminum sulfate, and sodium aluminum sulfate. Two or more of these may be used. In addition, when coagulation is performed with an acid, a method of recovering the acrylic graft copolymer (C) after neutralizing the acid with an alkali can also be used.
[0056] In the above-mentioned method, the monomer mixture containing the aromatic vinyl monomer and the vinyl cyanide monomer is graft-copolymerized onto the acrylic rubber polymer, but the monomer mixture containing the vinyl cyanide monomer may not be entirely graft-copolymerized onto the acrylic rubber polymer. Therefore, the acrylic graft copolymer (C) in the present invention may contain a copolymer consisting of a monomer mixture containing the aromatic vinyl monomer and the vinyl cyanide monomer that is not graft-copolymerized onto the acrylic rubber polymer.
[0057] Examples of the acrylic graft copolymer (C) include acrylonitrile-acrylic rubber polymer-styrene graft copolymer (ASA resin), methyl methacrylate-acrylic rubber polymer-styrene graft copolymer (MSA resin), methyl methacrylate-acrylonitrile-acrylic rubber polymer-styrene graft copolymer (MASA resin), etc. Among them, acrylonitrile-acrylic rubber polymer-styrene graft copolymer (ASA resin) is preferred.
[0058] (4) Acrylic block copolymer (D) In the present invention, an acrylic block copolymer (D) can be further blended with the thermoplastic resin composition. The acrylic block copolymer (D) used is a copolymer having one or more polymer blocks obtained by polymerizing a monomer component containing acrylic acid or methacrylic acid and their derivatives as a main component. By using the acrylic block copolymer (D), it is possible to improve the vibration welding strength and impact resistance without deteriorating the flow mark resistance of the resin composition.
[0059] The type of the acrylic block copolymer (D) contained in the resin composition of the present invention is not particularly limited, but it is preferable that the acrylic block copolymer (D) is composed of a polymer block containing a structural unit derived from an acrylic acid ester and a polymer block containing a structural unit derived from a methacrylic acid ester.
[0060] In the polymer block containing a structural unit derived from an acrylic acid ester, examples of the structural unit derived from an acrylic acid ester include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, and isobutyl acrylate. In addition, examples include n-octyl acrylate, dodecyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, phenyl acrylate, and dimethylaminoethyl acrylate. These are structural units derived from monomers, and one or more of these are used.
[0061] In the polymer block containing a methacrylic acid ester-derived structural unit, examples of the methacrylic acid ester-derived structural unit include methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, and hexyl methacrylate. In addition, examples include cyclohexyl methacrylate, octyl methacrylate, nonyl methacrylate, octadecyl methacrylate, dodecyl methacrylate, and 2-ethylhexyl methacrylate. These are structural units derived from monomers, and one or more of these are used.
[0062] The state of the molecular chain of the acrylic block copolymer (D) is not particularly limited, and may be, for example, linear, branched, radial, or any other suitable state.
[0063] The acrylic block copolymer (D) may be a commercially available product or a mixture thereof. Commercially available products include, for example, "CLARITY (registered trademark)" manufactured by Kuraray Co., Ltd.
[0064] (5) Other ingredients In addition, other resins can be added within a range that does not impair the characteristics of the present invention.Specifically, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polypropylene terephthalate, polycyclohexylene dimethylene ethylene terephthalate, polyarylate, liquid crystal polymer, polylactic acid, and polycaprolactone, polyamide resins such as nylon 6, nylon 6,6, nylon 6,10, nylon 4,6, nylon 6T, nylon 9T, and nylon 11, and other resins such as polyphenylene sulfide (PPS), polyacetal, crystalline styrene, and polyphenylene ether (PPE) can be used according to the purpose.
[0065] Furthermore, within the scope of the present invention, it is also possible to add, as necessary, hindered phenol-based antioxidants, sulfur-containing compound-based antioxidants, phosphorus-containing organic compound-based antioxidants, phenol-based, acrylate-based and other thermal antioxidants, benzotriazole-based, benzophenone-based, succinate-based and other ultraviolet absorbers, decabromobiphenyl ether, tetrabromobisphenol A, chlorinated polyethylene, brominated epoxy oligomer, brominated polycarbonate, antimony trioxide, condensed phosphate ester and other flame retardants / flame retardant assistants, antibacterial agents typified by silver-based antibacterial agents, antifungal agents, carbon black, titanium oxide, mold release agents, lubricants, pigments, dyes and the like.
[0066] Various fillers can also be added.
[0067] Examples of fillers include those in the form of fibers, plates, powders, and particles, and any of these may be used in the present invention. Specifically, examples include polyacrylonitrile (PAN)-based or pitch-based carbon fibers, metal fibers such as stainless steel fibers, aluminum fibers, and brass fibers, organic fibers such as aromatic polyamide fibers, gypsum fibers, ceramic fibers, asbestos fibers, zirconia fibers, alumina fibers, silica fibers, titanium oxide fibers, silicon carbide fibers, glass fibers, rock wool, potassium titanate whiskers, barium titanate whiskers, aluminum borate whiskers, and silicon nitride whiskers, as well as powdery, granular, or plate-like fillers such as mica, talc, kaolin, silica, calcium carbonate, glass flakes, glass beads, glass microballoons, clay, molybdenum disulfide, wollastonite, montmorillonite, titanium oxide, zinc oxide, barium sulfate, calcium polyphosphate, and graphite. These may be used alone or in combination of two or more.
[0068] (6) Thermoplastic resin composition The thermoplastic resin composition of the present invention contains 35 to 60 parts by mass, preferably 45 to 55 parts by mass, of (A) relative to 100 parts by mass of the total of polycarbonate resin (A), vinyl copolymer (B), and acrylic graft copolymer (C). If (A) is less than 35 parts by mass, the impact resistance is poor, and if it exceeds 60 parts by mass, the flow mark resistance is poor. Furthermore, the thermoplastic resin composition of the present invention contains 15 to 25 parts by mass, preferably 18 to 22 parts by mass, of vinyl copolymer (B-1) having a weight average molecular weight of 250,000 to 400,000 relative to 100 parts by mass of the total of vinyl copolymer (B) and acrylic graft copolymer (C). If (B-1) is less than 15 parts by mass, the vibration welding strength is poor, and if it exceeds 25 parts by mass, the flow mark resistance is poor.
[0069] In the thermoplastic resin composition of the present invention, the impact resistance and flow mark resistance of the molded article can be improved without adversely affecting the flow mark resistance. For this reason, the acrylic block copolymer (D) is contained in an amount of preferably 0.5 to 5 parts by mass, and more preferably 1.5 to 3 parts by mass, per 100 parts by mass of the total of (A), (B), and (C).
[0070] (7) Method for producing thermoplastic resin composition The thermoplastic resin composition of the present invention can be obtained by melt mixing each of the resin components. There is no particular limitation on the melt mixing method, but a method of melt mixing using a single or twin screw in a cylinder having a heating device and a vent can be adopted. The heating temperature during melt mixing is preferably selected from a temperature range of 230 to 300°C, but it is also possible to freely set the temperature gradient during melt mixing within a range that does not impair the object of the present invention. In addition, when twin screws are used, they may rotate in the same direction or in different directions.
[0071] (8) Molding The molding method of the thermoplastic resin composition of the present invention is not particularly limited, but can be any known method currently used for molding thermoplastic resins, such as injection molding, extrusion molding, blow molding, vacuum molding, compression molding, gas-assisted molding, etc., and the molding method is not particularly limited.
[0072] The uses of the molded article of the present invention are not particularly limited, and include, for example, materials for automobiles, electrical appliances, electronics, aviation, space, machinery, miscellaneous goods, housing facilities and building materials, chemical plant parts, etc., but due to the characteristics of the molded article of the present invention and its effects, it is effective as a long member that is used without painting. In particular, it is suitable as a spoiler and garnish material for automobiles, but is not limited thereto. EXAMPLES
[0073] In order to more specifically explain the present invention, examples are given below. However, the present invention should not be construed as being limited to these examples. The measurement or evaluation methods for each example, comparative example, and raw material are as follows.
[0074] (1) Vibration welding strength: From the pellets obtained in each Example and Comparative Example, a plate-shaped test piece (240 mm x 70 mm x 2 mm thick) was molded using an injection molding machine with a cylinder temperature set to 250°C and a mold temperature set to 60°C. From this plate-shaped test piece, a strip-shaped test piece of 65 mm x 20 mm x 2 mm thick was cut out. As shown in FIG. 1(i), two of these strip-shaped test pieces were prepared and fixed above and below a vibration welding machine, and the 20 mm x 2 mm surface of one was welded to the 65 mm x 20 mm surface of the other. The welding conditions are shown below. Vibration welding machine: Branson MICRO PPL Frequency: 240Hz Pressure: 2.5MPa Amplitude: 1.0mm Push stroke: 0.8mm The bottom surface of the welded test piece shown in Figure 1 (ii) was fixed to the tensile tester, and the part 55 mm from the bottom surface was fixed with a grip. It was pulled at a speed of 50 mm / min, and the maximum stress until the top part peeled off from the bottom surface or the bottom surface broke was recorded as a function of the welded area (0.4 cm2). 2 ) was divided by the above to evaluate the weld strength.
[0075] (2) Flow mark resistance: From the pellets obtained in each of the Examples and Comparative Examples, a plate-shaped test piece (240 mm × 70 mm × 2 mm thick) was molded using an injection molding machine (electric, screw diameter 32 mm) with a cylinder temperature set to 250° C. and a mold temperature set to 40° C. During molding, the set injection speed was increased by 1 mm / s from 35 mm / s, and the maximum set injection speed at which no flow marks were generated was evaluated as the limit speed.
[0076] (3) Weight average molecular weight of vinyl copolymer (B): The weight average molecular weight of vinyl copolymer (B) was measured in terms of polystyrene (PS) using a gel permeation chromatography (GPC) apparatus manufactured by Water Corporation, a differential refractometer (Water2414) as a detector, MIXED-B (2 columns) manufactured by Polymer Laboratories, Inc. as a column, and acetone as a distillate under the conditions of a flow rate of 1 ml / min and a column temperature of 40°C.
[0077] (4) Charpy impact strength: From the pellets obtained in each of the Examples and Comparative Examples, a multipurpose test piece A-type defined in ISO3167:2014 was molded using an injection molding machine with a cylinder temperature set to 250°C and a mold temperature set to 60°C, and a rectangular test piece (80 mm x 10 mm x 4 mm thick) cut out from the pellets was used to measure the notched Charpy impact strength in accordance with ISO179:2010.
[0078] (5) Glass transition temperature The glass transition temperatures of the acrylic graft copolymers (C-1), (C-2) and the diene graft copolymer (E) were measured using a differential scanning calorimeter under the following conditions: Equipment: Shimadzu Corporation DSC-60 differential scanning calorimeter Atmosphere gas: Nitrogen Gas flow rate: 30ml / min Starting temperature: -140℃ Heating rate: 20℃ / min Hold temperature: 30℃.
[0079] The materials and manufacturing methods used in each of the examples and comparative examples are shown below.
[0080] <Polycarbonate resin (A-1)> The polycarbonate resin (A-1) used was "Iupilon (registered trademark)" S-3000 manufactured by Mitsubishi Engineering Plastics Corporation. The melt volume rate of this polycarbonate resin (A-1) measured under the conditions of temperature: 300°C and load: 1.2 kg was 14 cm 3 / 10 minutes.
[0081] <Polycarbonate resin (A-2)> Mitsubishi Engineering Plastics Corporation's "Iupilon (registered trademark)" H-3000 was used. The melt volume rate of this polycarbonate resin (A-2) measured under the conditions of temperature: 300°C and load: 1.2 kg was 28 cm 3 / 10 minutes.
[0082] <Polycarbonate resin (a-1)> The polycarbonate resin (a-1) used was "Iupilon (registered trademark)" H-4000 manufactured by Mitsubishi Engineering Plastics Corporation. The melt volume rate of this polycarbonate resin (a-1) measured under the conditions of temperature: 300°C and load: 1.2 kg was 60 cm 3 / 10 minutes.
[0083] <Polycarbonate resin (a-2)> The polycarbonate resin (a-2) used was "Novarex (registered trademark)" 7022R manufactured by Mitsubishi Engineering Plastics Corporation. The melt volume rate of this polycarbonate resin (a-2) measured under the conditions of temperature: 300°C and load: 1.2 kg was 13 cm 3 / 10 minutes.
[0084] <Vinyl copolymer (B-1-1)> A solution of 0.05% by weight of methyl methacrylate / acrylamide copolymer (described in JP-B-45-24151) dissolved in 165% by weight of ion-exchanged water was added to a stainless steel autoclave with a capacity of 20 L and equipped with a baffle and a Faudler-type stirring blade, and the inside of the system was replaced with nitrogen gas while stirring at 400 rpm. Next, a mixed solution of 29% by weight of acrylonitrile, 71% by weight of styrene, 0.04% by weight of t-dodecyl mercaptan, and 0.30% by weight of 2,2'-azobisisobutyronitrile was added to the reaction system while stirring, and the copolymerization reaction was started at 70°C. The temperature was raised to 100°C over 3 hours from the start of copolymerization and held for 30 minutes, and then the slurry obtained by cooling was washed, dehydrated, and dried to prepare a vinyl copolymer (B-1-1). The weight average molecular weight of the vinyl copolymer (B-1-1) measured in an acetone solvent (temperature: 40° C.) was 350,000.
[0085] <Vinyl copolymer (B-1-2)> Vinyl copolymer (B-1-2) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.11% by weight. The weight average molecular weight of vinyl copolymer (B-1-2) measured in acetone solvent (temperature 40°C) was 250,000.
[0086] <Vinyl copolymer (B-1-3)> Vinyl copolymer (B-1-3) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.01% by weight. The weight average molecular weight of vinyl copolymer (B-1-3) measured in acetone solvent (temperature 40°C) was 400,000.
[0087] <Vinyl copolymer (B-2-1)> Vinyl copolymer (B-2-1) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.40% by weight. The weight average molecular weight of vinyl copolymer (B-2-1) measured in acetone solvent (temperature 40°C) was 98,000.
[0088] <Vinyl copolymer (B-2-2)> Vinyl copolymer (B-2-2) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.43% by weight. The weight average molecular weight of vinyl copolymer (B-2-2) measured in acetone solvent (temperature 40°C) was 82,000.
[0089] <Vinyl copolymer (B-2-3)> Vinyl copolymer (B-2-3) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.30% by weight. The weight average molecular weight of vinyl copolymer (B-2-3) measured in acetone solvent (temperature 40°C) was 133,000.
[0090] <Vinyl copolymer (b-1)> Vinyl copolymer (b-1) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.45% by weight. The weight average molecular weight of vinyl copolymer (b-1) measured in acetone solvent (temperature 40°C) was 75,000.
[0091] <Vinyl copolymer (b-2)> Vinyl copolymer (b-2) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.25% by weight. The weight average molecular weight of vinyl copolymer (b-2) measured in acetone solvent (temperature 40°C) was 155,000.
[0092] <Vinyl copolymer (b-3)> Vinyl copolymer (b-3) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.15% by weight. The weight average molecular weight of vinyl copolymer (b-3) measured in acetone solvent (temperature 40°C) was 220,000.
[0093] <Vinyl copolymer (b-4)> Vinyl copolymer (b-4) was prepared in the same manner as vinyl copolymer (B-1-1) except that t-dodecyl mercaptan was 0.005% by weight. The weight average molecular weight of vinyl copolymer (b-4) measured in acetone solvent (temperature 40°C) was 470,000.
[0094] <Acrylic graft copolymer (C-1)> 130 parts by mass of pure water and 1 part by mass (solid content equivalent) of a disproportionated potassium rosinate aqueous solution, which is an emulsifier, were charged into a reaction vessel, and the temperature was raised to 75°C. Under stirring, a mixture of 19.8 parts by mass of n-butyl acrylate and 0.2 parts by mass of allyl methacrylate was continuously added over 1 hour. Next, 10 parts by mass of a 2% by mass potassium persulfate aqueous solution and 1.5 parts by mass of a disproportionated potassium rosinate aqueous solution (solid content equivalent) were continuously added over 6 hours, respectively. In addition, 2 hours after the start of the addition of the potassium persulfate aqueous solution and the disproportionated potassium rosinate aqueous solution, a mixture of 79.2 parts by mass of n-butyl acrylate and 0.8 parts by mass of allyl methacrylate was added over 4 hours, and the mixture was held for another 1 hour after the completion of the addition to obtain an acrylic rubber polymer latex. In the presence of 50 parts by mass (solid content equivalent) of this acrylic rubber polymer latex (weight average particle diameter 190 nm), a monomer mixture consisting of 36.5 parts by mass of styrene and 13.5 parts by mass of acrylonitrile and 0.2 parts by mass of t-dodecyl mercaptan were added, and emulsion polymerization was carried out using potassium oleate to obtain a rubber-reinforced styrene resin latex. This was added to a 0.3% aqueous magnesium sulfate solution at a temperature of 90°C to cause coagulation, and then the mixture was washed, dehydrated, and dried to prepare an acrylic graft copolymer (C-1). The graft ratio was 30%. The glass transition temperature of this acrylic graft copolymer (C-1) was -41°C.
[0095] <Acrylic graft copolymer (C-2)> As the ASA resin, "Kane Ace (registered trademark)" M-190 manufactured by Kaneka Corp. The glass transition temperature of this acrylic graft copolymer (C-2) was -36°C.
[0096] <Acrylic graft copolymer (C-3)> Acrylic graft copolymer (C-3) was prepared in the same manner as acrylic graft copolymer (C-1), except that the reaction vessel temperature was 20°C and 2-ethylhexyl acrylate was used instead of n-butyl acrylate. The graft ratio was 30%. The glass transition temperature of this acrylic graft copolymer (C-1) was -62°C.
[0097] <Acrylic block copolymer (D)> The material used was "Clarity (registered trademark)" LA2270 (a triblock copolymer of PMMA (polymer methyl methacrylate) block-PnBA (polymer n-butyl acrylate) block-PMMA block) manufactured by Kuraray Co., Ltd.
[0098] <Acrylic random copolymer (d)> A 5-liter stainless steel autoclave equipped with a baffle and a Faudler-type agitator was charged with 300% ion-exchanged water, and the system was replaced with nitrogen gas while stirring at 400 rpm. Next, a mixed solution of 40% methyl methacrylate, 60% n-butyl acrylate, 0.5% n-octyl mercaptan, and 1.1% sodium dodecylbenzenesulfonate was added to the reaction system while stirring, and the internal temperature was raised to 60°C. 0.15% potassium persulfate and 5% ion-exchanged water were added to start the copolymerization reaction. The system was kept at 60°C for 2 hours from the start of copolymerization, and then cooled. The resulting slurry was washed, dehydrated, and dried to prepare a methyl methacrylate-n-butyl acrylate random copolymer (d).
[0099] <Diene-based graft copolymer (E)> In the presence of 60 parts by mass (solid content equivalent) of polybutadiene latex (weight average particle diameter 350 nm), a monomer mixture consisting of 29 parts by mass of styrene and 11 parts by mass of acrylonitrile and 0.2 parts by mass of t-dodecyl mercaptan were added, and emulsion polymerization was performed using potassium stearate to obtain a rubber-reinforced styrene resin latex. This was added to a 0.3% dilute sulfuric acid aqueous solution at a temperature of 90°C to cause coagulation, and then neutralized with an aqueous sodium hydroxide solution, followed by washing, dehydration, and drying processes to prepare a diene-based graft copolymer (E). The graft ratio was 37%. The glass transition temperature of this diene-based graft copolymer (E) was -81°C.
[0100] <Production of Resin Composition> The above ingredients were mixed in the ratios shown in Tables 1 to 3, and then mixed in a blender for 1 minute. The mixture was melt-kneaded in a co-rotating twin-screw extruder with a screw diameter of 30 mm (PCM-30 manufactured by Ikegai Corporation, temperature range: 250 to 260°C), and the molten resin discharged from the die nozzle was taken up by a cutter through a water tank and cut into resin pellets.
[0101] [Table 1]
[0102] [Table 2]
[0103] [Table 3]
[0104] From Tables 1 to 3, the following is clear. All of the flame-retardant thermoplastic resin compositions of the present invention (Examples 1 to 23) were excellent in vibration weld strength, flow mark resistance, and Charpy impact strength. Furthermore, Examples 15 to 20, which contain 0.5 parts by mass or more and 5 parts by mass or less of the acrylic block copolymer (D) relative to 100 parts by mass of the total of (A), (B), and (C), were superior in vibration weld strength and impact resistance. Moreover, in Example 23, in which the acrylic random copolymer (d) was used instead of (D), such an effect was not observed. On the other hand, Comparative Example 1, which used (a-1) having a polycarbonate resin melt volume rate of more than 45, had poor Charpy impact strength. Comparative Example 2, which used (a-2) having a polycarbonate resin melt volume rate of less than 14, had poor flow mark resistance. Comparative Example 3, in which (A) was less than 35 parts by mass relative to 100 parts by mass of the total of (A), (B), and (C), had poor Charpy impact hardness. Comparative Example 4, in which (A) was more than 60 parts by mass relative to the total of 100 parts by mass of (A), (B), and (C), had poor flow mark resistance and vibration weld strength. Comparative Example 5, which is a combination of (b-3) and (B-2) having a weight average molecular weight of less than 250,000, had poor vibration weld strength. Comparative Example 6, which is a combination of (b-4) and (B-2) having a weight average molecular weight of more than 450,000, had poor flow mark resistance. Comparative Example 7, which is a combination of (b-1) and (B-1) having a weight average molecular weight of less than 80,000, had poor vibration weld strength. Comparative Example 8, which is a combination of (b-2) and (B-1) having a weight average molecular weight of more than 135,000, had poor flow mark resistance. Comparative Example 9, in which (B-1) was less than 15 parts by mass per 100 parts by mass of the total of (B) and (C), had poor vibration weld strength. Comparative Example 10, in which (B-1) was more than 25 parts by mass per 100 parts by mass of the total of (B) and (C), had poor flow mark resistance. Comparative Example 11, in which a diene graft copolymer (E) was used instead of the acrylic graft copolymer (C), had poor flow mark resistance. [Industrial Applicability]
[0105] The thermoplastic resin composition of the present invention is excellent in vibration welding strength, flow mark resistance, and Charpy impact strength. Due to these characteristics, it is possible to obtain large unpainted molded articles that require adhesion with good appearance and high productivity. It can be particularly suitably used for automobile spoilers and garnishes. In addition to these applications, it can be suitably used in the fields of automobile interior and exterior parts, communication-related equipment, home appliances, office automation equipment, and miscellaneous goods. [Explanation of symbols]
[0106] 1: Strip-shaped test piece (65mm x 20mm x 2mm thick) 2: Welding surface 3: Bottom surface of welded test piece
Claims
1. A thermoplastic resin composition comprising (A) a polycarbonate resin, (B) a vinyl copolymer obtained by copolymerizing a monomer mixture containing an aromatic vinyl monomer and a vinyl cyanide monomer, and (C) an acrylic graft copolymer obtained by graft copolymerizing a monomer mixture containing at least an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of an acrylic rubber polymer, wherein the melt volume rate of the polycarbonate resin (A) is 14 cm 3 / 10 minutes or more 45 cm 3 The vinyl copolymer (B) comprises (B-1) having a weight average molecular weight of 250,000 or more and 400,000 or less and (B-2) having a weight average molecular weight of 80,000 or more and 135,000 or less, and the vinyl copolymer (B) is in an amount of 35 parts by mass or more and 60 parts by mass or less, (B-1) is in an amount of 8 parts by mass or more and 13 parts by mass or less, (B-2) is in an amount of 22 parts by mass or more and 42 parts by mass or less, and (C) is in an amount of 10 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass in total of (A), (B) and (C).
2. The thermoplastic resin composition according to claim 1, further comprising: (D) an acrylic block copolymer in an amount of 0.5 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the total of (A), (B), and (C).
3. The thermoplastic resin composition according to claim 2, wherein the acrylic block copolymer (D) is an acrylic block copolymer (D) having a polymer block containing a methacrylic acid ester unit and a polymer block containing an acrylic acid ester unit.
4. 4. The thermoplastic resin composition according to claim 1, wherein the glass transition temperature of the acrylic rubber polymer contained in the acrylic graft copolymer (C) is −60° C. or higher.
5. A method for producing a thermoplastic resin composition, comprising melt-kneading a graft copolymer obtained by graft copolymerizing a monomer mixture containing at least an aromatic vinyl monomer and a vinyl cyanide monomer in the presence of (A) a polycarbonate resin, (B) a vinyl copolymer obtained by copolymerizing a monomer mixture containing an aromatic vinyl monomer and a vinyl cyanide monomer, and (C) an acrylic graft copolymer, wherein the melt volume rate of the polycarbonate resin (A) is 14 cm 3 / 10 minutes or more 45 cm 3 The vinyl copolymer (B) comprises (B-1) having a weight average molecular weight of 250,000 or more and 400,000 or less and (B-2) having a weight average molecular weight of 80,000 or more and 135,000 or less, and the vinyl copolymer (B) is in an amount of 35 parts by mass or more and 60 parts by mass or less, (B-1) is in an amount of 8 parts by mass or more and 13 parts by mass or less, (B-2) is in an amount of 22 parts by mass or more and 42 parts by mass or less, and (C) is in an amount of 10 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass in total of (A), (B) and (C).
6. A molded article obtained by molding the thermoplastic resin composition according to any one of claims 1 to 4.
Citation Information
Patent Citations
JP164774A
Thermoplastic resin composition
JP2000154329A
Thermoplastic resin composition and molded product thereof
JP2000302824A
Thermoplastic resin composition
JP2000327900A
Thermoplastic resin composition
JP2016190924A