Polyamide resin composition and molded article containing same

A balanced polyamide resin composition with polypropylene, acid-modified homopolypropylene, glass fiber, and a heat-resistant agent addresses hydrolysis resistance and weld durability issues, ensuring mechanical strength in high-temperature conditions.

JP7585905B2Active Publication Date: 2024-11-19TORAY INDUSTRIES INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021044518
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-18
Publication Date
2024-11-19
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

Polyamide resins used in applications like automobile parts suffer from high water absorption leading to mechanical property deterioration and dimensional changes, particularly when exposed to long-term high-temperature conditions, with existing compositions lacking sufficient hydrolysis resistance and weld durability.

Method used

A polyamide resin composition comprising specific amounts of polypropylene resin, acid-modified homopolypropylene resin, glass fiber, and a heat-resistant agent, balanced to enhance mechanical properties both dry and after water absorption, with improved hydrolysis resistance and weld durability.

Benefits of technology

The composition exhibits excellent mechanical properties and hydrolysis resistance in high-temperature environments, maintaining strength and durability both when dry and after water absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585905000001
    Figure 0007585905000001
  • Figure 0007585905000002
    Figure 0007585905000002
Patent Text Reader

Abstract

To provide a polyamide resin composition which is characterized as exhibiting excellent mechanical characteristics in both of a bone-dry state and after water absorption, and being excellent in hydrolysis resistance under a high temperature environment and in durability of a weld part.SOLUTION: A polyamide resin composition is formed by compounding 10-75 pts.wt. polypropylene resin (B), 0.5-30 pts.wt. acid-modified homopolypropylene resin (C) with MFR of 200-300 measured at temperature of 190°C and loading of 2.16 kg according to ISO1133(2011), 10-125 pts.wt. glass fiber (D) and 0.01-5 pts.wt. thermostable material (E), based on 100 pts.wt. polyamide resin (A) with amino terminal group concentration of 10×10-5 mol / g or more (provided that, no cupper compound is contained).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide resin composition and a molded article containing the same. [Background technology]

[0002] Polyamide resins are used in various applications such as automobile parts, electrical parts, and general machine parts because of their excellent mechanical properties, heat resistance, and chemical resistance. However, polyamide resins have high water absorption and tend to have reduced mechanical properties and dimensional changes. In particular, when applied to automobile parts, polyamide resins have the disadvantage of hydrolysis and reduced mechanical properties when exposed to long-life coolants (hereinafter referred to as LLC) used in cooling water under high-temperature conditions for a long period of time.

[0003] In response to the above problems, Patent Document 1 proposes a polyamide resin composition in which a polyamide resin contains a polypropylene resin or a modified polyolefin resin. Patent Document 2 proposes a polyamide resin composition in which a polyamide resin contains an acid-modified homopolypropylene resin, glass fiber, and a phenolic heat stabilizer. Patent Document 3 further proposes a polyamide resin composition for automobile cooling and air conditioning parts in which a polyamide resin contains an acid-modified homopolypropylene resin modified with maleic anhydride, glass fiber, and a heat stabilizer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-111841 A [Patent Document 2] Patent No. 6095799 [Patent Document 3] JP 2006-291118 A Summary of the Invention [Problem to be solved by the invention]

[0005] In designing a molded product, a high tensile strength in an absolute dry state of a polyamide resin composition is an important index. In particular, when a molded product comes into contact with water or the like and is exposed to high temperatures for a long time in that state, hydrolysis resistance is necessary. Furthermore, molded products of polyamide resin generally have welds, which are the joining points of molten resin during molding. In particular, the mechanical properties of the welds of molded products made of a polyamide resin composition containing glass fibers are significantly reduced compared to other parts, and the durability of the molded product is likely to be insufficient.

[0006] In the above-mentioned Patent Document 1, although the mechanical property retention rate when absorbing water is high, the mechanical properties when completely dry are insufficient. Also, there is a problem of poor hydrolysis resistance.

[0007] In addition, although the heat resistance is excellent in Patent Document 2, the mechanical properties in an absolutely dry state are insufficient. In addition, there is no description on the melt flow rate (hereinafter, sometimes referred to as MFR) of the acid-modified homopolypropylene resin, and there is no mention at all of the effect on the physical properties and mechanical properties of the polyamide resin composition.

[0008] In addition, Patent Document 3 has excellent hydrolysis resistance (durability) and calcium chloride resistance against LLC at high temperatures, but there is no description about the MFR as an acid-modified homopolypropylene resin, and there is no mention at all of the effect on the physical properties and mechanical properties of the polyamide resin composition.

[0009] Until now, it was thought that an acid-modified homopolypropylene resin with a large MFR, i.e., a small molecular weight, would have poor mechanical properties in itself, and therefore would be inferior in mechanical properties and hydrolysis resistance of a polyamide resin composition. Therefore, it was common to use an acid-modified homopolypropylene resin with a small MFR, i.e., a large molecular weight, which has high mechanical properties in itself.

[0010] In view of the problems with the conventional techniques, the present invention aims to provide a polyamide resin composition that exhibits excellent mechanical properties both in the bone-dry state and after absorbing water, and that also exhibits excellent hydrolysis resistance and weld durability in high-temperature environments. [Means for solving the problem]

[0011] That is, the present invention has the following configuration.

[0012] Amino end group concentration is 10 x 10 -5 A polyamide resin composition (not including a copper compound) comprising 100 parts by weight of polyamide resin (A) having a molecular weight of at least mol / g, 10 to 75 parts by weight of polypropylene resin (B), 0.5 to 30 parts by weight of acid-modified homopolypropylene resin (C) having an MFR of 200 to 300 measured in accordance with ISO1133 (2011) at a temperature of 190°C under a load of 2.16 kg, 10 to 125 parts by weight of glass fiber (D), and 0.01 to 5 parts by weight of a heat stabilizer (E).

[0013] A molded article comprising the polyamide resin composition described above. Effect of the Invention

[0014] According to the present invention, it is possible to provide a polyamide resin composition which exhibits excellent mechanical properties both in the bone dry state and after absorbing water, and which is characterized by excellent hydrolysis resistance in a high-temperature environment and durability of welds. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below with reference to embodiments.

[0016] The polyamide resin composition of the present invention has an amino terminal group concentration of 10×10 -5A polyamide resin composition (not including a copper compound) comprising 100 parts by weight of polyamide resin (A) having a molecular weight of at least mol / g, 10 to 75 parts by weight of polypropylene resin (B), 0.5 to 30 parts by weight of acid-modified homopolypropylene resin (C) having an MFR of 200 to 300 measured in accordance with ISO1133 (2011) at a temperature of 190°C under a load of 2.16 kg, 10 to 125 parts by weight of glass fiber (D), and 0.01 to 5 parts by weight of a heat stabilizer (E).

[0017] Generally, as a means for improving the mechanical properties of polyamide resin compositions, a method of balancing the mechanical properties using the above-mentioned acid-modified homopolypropylene resin is known. In contrast, by focusing on the interface state of the resin and the fiber, it was conceived that resin diffusion and reaction progress can be promoted by using a low molecular weight acid-modified homopolypropylene resin, which leads to adhesion at the interface and excellent mechanical strength can be obtained. However, until now, it was thought that an acid-modified homopolypropylene resin with a large MFR, i.e., a small molecular weight, has poor mechanical properties in itself, and therefore the mechanical properties and hydrolysis resistance of the polyamide resin composition are poor. Therefore, it was common to use an acid-modified homopolypropylene resin with a small MFR, i.e., a large molecular weight, which has high mechanical properties in itself.

[0018] Therefore, the inventors of the present application have determined that (A) the amino terminal group concentration is 10×10 -5 The inventors discovered that by incorporating specific amounts of (A) a polyamide resin having a viscosity of 100 mol / g or more, (B) a polypropylene resin, (C) an acid-modified homopolypropylene resin having a specific viscosity range, (D) glass fiber, and (E) a heat resistance agent, it is possible to eliminate the above-mentioned trade-off, and to exhibit excellent mechanical properties both in the bone dry state and after absorbing water, as well as excellent hydrolysis resistance and durability of welds in high-temperature environments, thereby completing the present invention.

[0019] According to the present invention, (A) the amino terminal group concentration is 10×10 -5The composition must contain specific amounts of (A) a polyamide resin having a viscosity of 1.0 mol / g or more, (B) a polypropylene resin, (C) an acid-modified homopolypropylene resin having a specific viscosity range, (D) glass fiber, and (E) a heat-resistant agent.

[0020] The polyamide resin (A) used in the present invention is a polyamide whose main components are amino acids, lactams, or diamines and dicarboxylic acids. Specific examples include lactams such as ε-caprolactam, enantholactam, and ω-laurolactam, amino acids such as ε-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, tetramethylenediamine, hexamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 1.2.2.4- / 2.4.4-1-trimethylhexamethylenediamine, 5=methylnonamethylenediamine, m-xylylenediamine, p-xylylenediamine, These include diamines such as 1.3-bisaminomethylcyclohexane, 1.4-bisaminomethylcyclohexane, bis-p-aminocyclohexylmethane, bis-p-aminocyclohexylpropane, isophoronediamine, etc., and dicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sepacic acid, dodecanedioic acid, 1.4-cyclohexanedicarboxylic acid, 1.3-cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, dimer acid, etc. These constituent components are subjected to polymerization alone or in the form of a mixture of two or more kinds, and either the polyamide homopolymer or copolymer thus obtained can be used in the present invention. Particularly useful polyamides in the present invention are polycaproamide (polyamide 6), polyhexamethylene adipamide (polyamide 66), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), polyhexamethylene terephthalamide (polyamide 6T), polyhexamethylene isophthalamide (polyamide 6I), polyundecane amide (polyamide 11), polydodecanamide (polyamide 12), and copolymers and mixtures of these polyamides. In terms of appearance, strength, rigidity, and toughness, polyamide 6, polyamide 66, and polyamide 610 are preferred. Polyamide 66 is even more preferred.

[0021] The amino terminal group concentration of the polyamide resin (A) used in the present invention is 10×10 -5 mol / g or more. The amino end group concentration of the polyamide resin is 10×10 -5 When the amount of the polyamide resin composition is less than 11 to 14×10 mol / g, the adhesion to the acid-modified homopolypropylene resin and the glass fiber is reduced, leading to a decrease in hydrolysis resistance. From the viewpoint of the processability and moldability of the polyamide resin composition, the amino terminal group concentration of the polyamide resin is 11 to 14×10 -5 The mol / g range is preferred.

[0022] (A) The carboxyl end group concentration of polyamide resin is 6×10 -5 mol / g or less. By using a polyamide resin having a carboxy end group concentration in this range, hydrolysis of the polyamide resin composition by the acid of the carboxy end group is suppressed, and hydrolysis resistance is improved. From the viewpoint of the balance between mechanical properties and hydrolysis resistance in an absolutely dry state, the carboxy end group concentration of the polyamide resin is preferably 2 to 5×10 -5 The mol / g range is more preferred.

[0023] The ratio of the amino end group concentration to the carboxy end group concentration of the (A) polyamide resin is preferably in the range of 2:1 to 7:1, more preferably 3:1 to 5:1. By using a polyamide resin having the ratio of the amino end group concentration to the carboxy end group concentration in this range, the mechanical properties and hydrolysis resistance in an absolutely dry state are improved.

[0024] The degree of polymerization of the (A) polyamide resin is preferably in the range of 110 to 210 ml / g, more preferably 120 to 200 ml / g, as a viscosity number measured in accordance with ISO 307. If the degree of polymerization of the polyamide resin is 120 ml / g or more, the mechanical properties of the polyamide resin itself are high, and the mechanical properties of the polyamide resin composition when completely dried are high, which is preferable. On the other hand, if the degree of polymerization of the polyamide resin is 200 ml / g or less, the dispersibility during melt kneading is good, the adhesion with the acid-modified homopolypropylene resin is high, and the mechanical properties, hydrolysis resistance, and durability of the welds when completely dried are high, which is preferable.

[0025] The polypropylene resin (B) used in the present invention preferably has an MFR of 0.1 to 50, more preferably 0.3 to 30, and even more preferably 0.5 to 10, as measured in accordance with ISO1133 (2011) at a temperature of 230°C and a load of 2.16 kg. If the MFR of the polypropylene resin is 0.5 or more, the flowability is good and the durability of the welds is high, which is preferable. On the other hand, if the MFR of the polypropylene resin is 10 or less, the mechanical properties of the polypropylene resin itself are high, and the mechanical properties of the polyamide resin composition when completely dried are high, which is preferable.

[0026] Examples of the polypropylene resin (B) include homopolypropylene, ethylene-propylene random copolymer, ethylene-propylene block copolymer, propylene-1-butene copolymer, etc., and if necessary, a copolymer of a propylene monomer and another copolymerizable monomer can be used. In particular, from the viewpoints of heat resistance and rigidity at high temperatures, homopolypropylene, ethylene-propylene random copolymer, and ethylene-propylene block copolymer are preferred, and homopolypropylene is more preferred.

[0027] The polymerization method for the polypropylene resin (B) is not limited, and may be any of a high-pressure method, a slurry method, a solution method, and a gas phase method. The polymerization catalyst is not particularly limited, and may be a Ziegler catalyst, a metallocene catalyst, or the like.

[0028] The acid-modified homopolypropylene resin (C) used in the present invention has an MFR in the range of 200 to 300 g / 10 min, measured at a temperature of 190 ° C. and a load of 2.16 kg according to ISO 1133 (2011). When an acid-modified homopolypropylene resin with an MFR of less than 200 g / 10 min is blended, the dispersibility during melt kneading is poor, and the adhesion with polyamide resin and polypropylene resin is reduced, leading to a decrease in mechanical properties when completely dried. In addition, since a large amount of the acid component in the acid-modified homopolypropylene resin remains in an unreacted state, this leads to a decrease in hydrolysis resistance and durability of the welded portion. On the other hand, when an acid-modified homopolypropylene resin with an MFR of more than 300 g / 10 min is blended, the mechanical properties of the acid-modified homopolypropylene resin itself are low, leading to a decrease in mechanical properties of the polyamide resin composition when completely dried.

[0029] The acid-modified homopolypropylene resin (C) is a homopolypropylene resin having a reactive functional group derived from an organic acid. The acid-modified homopolypropylene resin (C) used in the present invention may have a polymer main chain of a homopropylene resin and a side chain containing a reactive functional group derived from an organic acid. More specifically, the acid-modified homopolypropylene resin may have a polymer main chain and a side chain containing a carboxyl group formed by an unsaturated carboxylic acid or its acid anhydride, or a metal salt or ammonium salt thereof.

[0030] The acid value of the (C) acid-modified homopolypropylene resin is preferably in the range of 1 to 50 mgKOH / g, more preferably in the range of 3 to 25 mgKOH / g, and even more preferably in the range of 5 to 15 mgKOH / g. If the acid value of the acid-modified homopolypropylene resin is 5 mgKOH / g or more, the adhesion to the polyamide resin is high, and the mechanical properties in an absolutely dry state, the hydrolysis resistance, and the durability of the welds are high, which is preferable. On the other hand, if the acid value of the acid-modified homopolypropylene resin is 15 mgKOH / g or less, the amount of the acid component in the unreacted acid-modified homopolypropylene resin remaining in the polyamide resin composition is small, which is preferable because the hydrolysis resistance and the durability of the welds are high.

[0031] The polymerization method for the acid-modified homopolypropylene resin (C) is not limited, and may be any of a high-pressure method, a slurry method, a solution method, and a gas phase method. The polymerization catalyst is not particularly limited, and may be a Ziegler catalyst, a metallocene catalyst, or the like.

[0032] Examples of unsaturated carboxylic acids and their anhydrides include acrylic acid, (meth)acrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, itaconic anhydride, crotonic acid, isocrotonic acid, citraconic acid, allylsuccinic acid, mesaconic acid, glutaconic acid, nadic acid, methylnadic acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, etc. In particular, maleic anhydride, itaconic anhydride, acrylic acid, and (meth)acrylic acid are preferred because they are easily copolymerized. Only one type of unsaturated carboxylic acid may be used for copolymerization with propylene or graft copolymerization to propylene, or two or more types of unsaturated carboxylic acids may be used.

[0033] (C) Acid-modified homopolypropylene resin is flexible despite having many functional groups in one molecule, and therefore has high reactivity with polyamide resins. The type of acid-modified component of the (C) acid-modified homopolypropylene resin used in the present invention is not particularly limited as long as it is a functional group that reacts with the polyamide resin, and for example, reactive functional groups of acid components consisting of unsaturated carboxylic acids, carboxyl metal salts, and oxazoline groups are used.

[0034] As the acid anhydride constituting the unsaturated carboxylic acid described above, maleic anhydride and itaconic anhydride are preferably used. The functional group of these acid anhydride components may be one type or multiple types.

[0035] When an unsaturated carboxylic acid or an acid anhydride thereof is introduced into a polypropylene resin, the method can be generally known and is not particularly limited. For example, the method can be carried out by copolymerizing the unsaturated carboxylic acid or anhydride with a monomer that is a raw material of the polypropylene resin, or by grafting the unsaturated carboxylic acid or anhydride onto the polypropylene resin, using a thermal reaction device such as a polymerization tank or an extruder.

[0036] The glass fiber (D) used in the present invention is preferably treated with an epoxy-, urethane- or acrylic-based coating or sizing agent, more preferably with a urethane-based coupling agent, and is preferably treated with a silane- or titanate-based coupling agent or other surface treatment agent, more preferably with an aminosilane-based coupling agent.

[0037] The (D) glass fiber is preferably a chopped type glass fiber having a fiber length of 1 to 10 mm and a fiber diameter of 5 to 20 μm, more preferably a fiber length of 2 to 6 mm and a fiber diameter of 7 to 14 μm. By using glass fibers in this range, a composition excellent in processability during melt kneading and mechanical properties when bone-dried as a polyamide resin composition can be obtained.

[0038] Examples of the heat stabilizer (E) used in the present invention include hindered phenol-based, sulfur-based, phosphorus-based and organic compounds based on substitution products thereof.

[0039] It does not contain copper salts such as copper iodide, copper bromide, copper bromide, copper acetate, copper sulfide, copper terephthalate, copper isophthalate, copper salicylate, and copper nicotinate, which are commonly used in the heat aging resistance of polyamide resins, or copper complex salts in which chelating agents such as ethylenediamine and ethylenediaminetetraacetic acid are coordinated to copper. By using a copper compound-based heat resistance agent, the copper ions (B) cause a catalytic effect (redox reaction) that promotes the autoxidation reaction of polypropylene, inducing copper damage that deteriorates polypropylene. Copper damage causes a decrease in mechanical properties and hydrolysis resistance when completely dry.

[0040] Among the organic heat-resistant agents described above, preferred are hindered phenol compounds. Specific examples of the hindered phenol compounds include triethylene glycol-bis[3-t-butyl-(5-methyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene bis(3,5-di-t-butyl-4-hydroxy-hydrocinamide), N,N'-(hexane-1,6-diyl)[4-hydroxy-3,5-bis(t-butyl)benzenepropanamide], tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, pentaerythrityl tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 4,4'-butylidenebis(3-methyl-6-t-butylphenol), n-octadecyl-3-(3,5-di-t-butyl-4-hydroxy-phenyl)propionate, 3,9-bis[2-(3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, 1,3,5-trimethyl-2,4,6-tris-(3,5-di-t-butyl-4-hydroxybenzyl)benzene, and the like. Among the above hindered phenol compounds, N,N'-(hexane-1,6-diyl)[4-hydroxy-3,5-bis(t-butyl)benzenepropanamide], 3,9-bis[2-(3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, etc. are particularly preferably used. These can be used alone or in combination of two or more.

[0041] To the polyamide resin composition of the present invention, one or more types of conventional additives, such as an ultraviolet absorber, a crystal nucleating agent, a color inhibitor, a weathering agent, a release agent, a plasticizer, a lubricant, an antistatic agent, a flame retardant, and a colorant including a dye or pigment, may be added, provided that the object of the present invention is not impaired.

[0042] Examples of such various additives include ultraviolet absorbers such as benzotriazole-based, phenol-based, and phosphorus-based ones, organic nucleating agents such as metal salts of aromatic carboxylic acids, sorbitol-based derivatives, organic phosphates, and aromatic amide compounds, and other organic nucleating agents, crystal nucleating agents including inorganic nucleating agents such as talc and boron nitride, weather resistance agents such as resorcinol-based, salicylate-based, benzotriazole-based, benzophenone-based, and hindered amine-based ones, release agents such as aliphatic alcohols, aliphatic amides, aliphatic bisamides, ethylene bisstearylamide, and higher fatty acid esters, plasticizers such as octyl p-oxybenzoate and N-butylbenzenesulfonamide, lubricants such as wax, and alkyl sulfate-type anion. Examples of suitable flame retardants include flame retardants such as brominated flame retardants based on quaternary ammonium salt type cationic agents, nonionic agents such as polyoxyethylene sorbitan monostearate, betaine-based amphoteric antistatic agents, hydroxides such as melamine cyanurate, magnesium hydroxide, and aluminum hydroxide, ammonium polyphosphate, brominated polystyrene, brominated polyphenylene oxide, brominated polycarbonate, brominated epoxy resin, and combinations of these brominated flame retardants with antimony trioxide, and dyes such as azo, anthraquinone, and perylene, and colorants containing pigments such as azo, anthraquinone, phthalocyanine, quinacridone, perylene, carbon black, titanium dioxide, and ultramarine.

[0043] It is also possible to use two or more of the various additives such as ultraviolet absorbers, crystal nucleating agents, coloring inhibitors, weathering agents, release agents, plasticizers, lubricants, antistatic agents, flame retardants, and colorants including dyes and pigments. The content is not particularly limited, but is generally 0.01 parts by weight or more and less than 3 parts by weight per 100 parts by weight of the total of (A) polyamide resin, (B) polypropylene resin, (C) acid-modified homopolypropylene resin, (D) glass fiber, and (E) heat resistance agent.

[0044] The polyamide resin composition of the present invention contains 100 parts by weight of (A) polyamide resin, 10 to 75 parts by weight of (B) polypropylene resin, 0.5 to 30 parts by weight of (C) acid-modified homopolypropylene resin, 10 to 125 parts by weight of (D) glass fiber, and 0.01 to 5 parts by weight of (E) heat stabilizer.

[0045] If the amount of the polypropylene resin (B) used in the present invention is less than 10 parts by weight, the amount of the polyamide resin, which is a water-absorbing component, increases, and the hydrolysis resistance decreases. If the amount of the polypropylene resin (B) exceeds 75 parts by weight, the mechanical properties of the polyamide resin composition in an absolutely dry state decrease. From the perspective of the balance between the mechanical properties in an absolutely dry state and the hydrolysis resistance, the amount of the polypropylene resin (B) is preferably 30 to 75 parts by weight, more preferably 40 to 70 parts by weight, per 100 parts by weight of the polyamide resin (A).

[0046] If the amount of the acid-modified homopolypropylene resin (C) used in the present invention is less than 0.5 parts by weight, the adhesion between the polyamide resin, the polypropylene resin, and the acid-modified homopolypropylene resin decreases, and the mechanical properties in the bone-dry state decrease. If the amount of the acid-modified homopolypropylene resin (C) exceeds 30 parts by weight, a large amount of the acid component in the acid-modified homopolypropylene resin remains unreacted, leading to a decrease in hydrolysis resistance. From the perspective of the balance between the mechanical properties in the bone-dry state and the hydrolysis resistance, the amount of the acid-modified homopolypropylene resin (C) is preferably 1 to 27 parts by weight, more preferably 3 to 25 parts by weight, per 100 parts by weight of the polyamide resin (A).

[0047] The weight ratio of the (B) polypropylene resin to the (C) acid-modified homopolypropylene resin is preferably in the range of 2: 1 to 10: 1. By setting the weight ratio in this range, it is possible to obtain a polyamide resin composition having excellent mechanical properties and hydrolysis resistance in an absolutely dry state.

[0048] If the amount of the (D) glass fiber used in the present invention is less than 10 parts by weight, the resin reinforcing effect of the glass fiber is poor, and the mechanical properties in the bone-dry state are insufficient. If the amount of the (D) glass fiber exceeds 125 parts by weight, the durability of the welds of the polyamide resin composition decreases. From the viewpoint of the balance between the mechanical properties in the bone-dry state and the durability of the welds, the amount of the (D) glass fiber is preferably 25 to 115 parts by weight, more preferably 50 to 100 parts by weight, per 100 parts by weight of the (A) polyamide resin.

[0049] If the amount of the heat resistant agent (E) used in the present invention is less than 0.01 parts by weight, the hydrolysis resistance at high temperatures is poor. If the amount of the heat resistant agent (E) is more than 5 parts by weight, the mechanical properties of the polyamide resin composition at bone dry temperature and the durability of the welds are reduced. From the viewpoint of the balance of the hydrolysis resistance at high temperatures, the mechanical properties at bone dry temperature, and the durability of the welds, the amount of the heat resistant agent (E) is preferably 0.1 to 4 parts by weight, more preferably 0.3 to 3 parts by weight, per 100 parts by weight of the polyamide resin (A).

[0050] The method for producing the polyamide resin composition of the present invention is not particularly limited, and examples thereof include a method in which (A) polyamide resin, (B) polypropylene resin, (C) acid-modified homopolypropylene resin, (D) glass fiber, and (E) heat resistance agent are blended together and melt-kneaded to produce the composition, and a method in which (D) glass fiber is added by a side feed or the like while (A) polyamide resin, (B) polypropylene resin, (C) acid-modified homopolypropylene resin, and (E) heat resistance agent are melt-kneaded.

[0051] The polyamide resin composition of the present invention can be molded by any method, and the molding method is not limited, and examples of the molding method include extrusion molding, injection molding, blow molding, calendar molding, compression molding, vacuum molding, foam molding, blow molding, rotational molding, etc. Among them, it is preferable to adopt a method selected from injection molding, injection compression molding, and compression molding, because it has excellent productivity and is therefore preferable for carrying out the present invention industrially.

[0052] Molded articles made from the polyamide resin composition of the present invention can be used for a variety of purposes, including electric and electronic parts, automobile parts, vehicle-related parts, building material-related parts, general and industrial machinery parts, sporting goods, daily necessities, home and office supplies, and furniture parts. EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. Measurement methods used in the examples and comparative examples are described below.

[0054] (1) Amino end group concentration of polyamide resin (A) 1.000g of polyamide resin pellets and 50ml of a solution of 83.5vol% phenol and 16.5vol% ethanol were weighed into a 200ml Erlenmeyer flask and shaken for about 4.5 hours to completely dissolve. 3-4 drops of thymol blue indicator were added to this solution, mixed, and titrated with 0.02N hydrochloric acid to determine the titration volume (A) ml when the color of the solution changed from yellow to faint red. In addition, titration was performed in the same manner as above using only a solution that did not dissolve the pellets, and the titration volume (B) ml was determined, and the amino end group concentration was calculated using the following formula. Amino end group concentration (×10 -5 mol / g) = (AB) × f × 0.02 × 10 -3 / Bone dry sample weight where f is the titer of 0.02N hydrochloric acid

[0055] (2) Carbo terminal group concentration of polyamide resin (A) 0.500g of polyamide resin pellets and 20ml of benzyl alcohol were weighed into a test tube, heated to 195℃, and stirred for about 1 hour to completely dissolve. 5-10 drops of phenolphthalein indicator were added to this solution, mixed, and titrated with 0.02N potassium hydroxide aqueous solution to determine the titration volume (A) ml when the color of the solution turned pink. In addition, titration was performed in the same manner as above using only benzyl alcohol, which does not dissolve the pellets, to determine the titration volume (B) ml, and the carbo terminal group concentration was calculated using the following formula. Carbo end group concentration (×10 -5mol / g) = (AB) × f × 0.02 × 10 -3 / Bone dry sample weight Here, f is the titer of a 0.02N potassium hydroxide solution.

[0056] (3) Melt flow rate (MFR) Measurements were performed according to ISO 1133 (2011). Measurement temperatures: 190°C, 230°C, load: 2.16 kg.

[0057] (4) Viscosity number Measurements were performed according to ISO 307. Solvent used: 96% sulfuric acid.

[0058] (5) Acid value 0.500g of sample and 70ml of xylene were weighed into a 200ml Erlenmeyer flask, an air-cooled tube was attached, and the solution was dissolved by heating at 135℃ for 15 minutes. Three drops of phenolphthalein indicator were added to this solution, mixed, and titrated with 0.025mol / L NaOH benzyl alcohol solution on a hot stirrer at about 100℃. The titration volume (A) ml was calculated when the solution remained a light red color for 30 seconds. In addition, titration was performed in the same manner as above using only xylene, which does not dissolve the sample, to determine the titration volume (B) ml, and the acid value was calculated using the following formula. Acid value (mgKOH / g) = (AB) x f x 0.025 x 56.11 / bone dry sample weight (g) where f is the titer of a 0.025 mol / L NaOH benzyl alcohol solution

[0059] (6) Tensile strength of molded product (absolute dry, saturated water absorption) The pellets obtained in the examples and comparative examples were injection molded using an injection molding machine NEX1000 manufactured by Nissei Plastic Industrial Co., Ltd. under conditions of a cylinder temperature of 280°C and a mold surface temperature of 80°C to prepare ISO Type-A standard test pieces, and tensile tests were carried out in accordance with ISO527-1 and -2. The tensile strength in an absolutely dry state is the tensile strength of an injection-molded ISO Type-A standard dumbbell-shaped test piece. The tensile strength at water saturation is the tensile strength of an ISO Type-A standard dumbbell-shaped test piece when it reaches water absorption equilibrium in warm water at 80°C.

[0060] (7) Hydrolysis resistance of molded products (normal parts) The pellets obtained in the examples and comparative examples were injection molded using an injection molding machine NEX1000 manufactured by Nissei Plastic Industrial Co., Ltd. under the conditions of a cylinder temperature of 280°C and a mold surface temperature of 80°C to prepare ISO Type-A standard test pieces. The injection molded ISO Type-A standard dumbbell-shaped test pieces were immersed for 2000 hours in a 50 vol% aqueous solution of LLC (Toyota genuine Long Life Coolant) heated to 130°C, and tensile tests were carried out in accordance with ISO527-1 and -2. The tensile strength retention rate (%) after the immersion treatment was calculated, assuming that the tensile strength at saturated water absorption was 100%. The higher this value, the better the hydrolysis resistance.

[0061] (8) Hydrolysis resistance of molded products (welds) The shape of the molded product is the same as that of the ISO Type-A standard test piece, but the dumbbell-shaped test piece has gates at both ends and a weld at the center of the test piece. The pellets obtained in the examples and comparative examples were injection molded using an injection molding machine NEX1000 manufactured by Nissei Plastic Industrial Co., Ltd. under the conditions of a cylinder temperature of 280°C and a mold surface temperature of 80°C to prepare dumbbell-shaped test pieces. The injection-molded dumbbell-shaped test pieces were immersed for 1000 hours in a 50 vol% aqueous solution of LLC (Toyota genuine Long Life Coolant) heated to 130°C. In accordance with ISO527-1 and -2, tensile tests were performed on the dumbbell-shaped test pieces at the time of saturated water absorption when the water absorption equilibrium was reached in warm water at 80°C and after immersion in a 50 vol% aqueous solution of LLC, and the tensile strength retention rate (%) after immersion in a 50 vol% aqueous solution of LLC was calculated, with the tensile strength at saturated water absorption being taken as 100%. The higher this value, the more excellent the hydrolysis resistance (durability of the weld portion).

[0062] The raw materials used in each of the examples and comparative examples are shown below. (A) Polyamide resin: A-1: Amino end group concentration 12.4×10 -5 mol / g, Carbo end group concentration 3.5×10 -5mol / g, and a viscosity number of 129 ml / g. Polyamide 66 resin. A-2: Amino end group concentration 3.3×10 -5 mol / g, Carbo end group concentration 11.3×10 -5 mol / g, and a viscosity number of 137 ml / g. Polyamide 66 resin. A-3: Amino end group concentration 3.0×10 -5 mol / g, Carbo end group concentration 8.0×10 -5 mol / g, and a viscosity number of 150 ml / g.

[0063] (B) Polypropylene resin B-1: Homopolypropylene resin "Prime Polypro" E111G" (Prime Polymer Co., Ltd.). MFR: 0.5g / 10min (temperature 230℃, load 2.16kg). B-2: Homopolypropylene resin "Prime Polypro" J105G (Prime Polymer Co., Ltd.). MFR: 9.0g / 10min (temperature 230℃, load 2.16kg). B-3: Homopolypropylene resin "Prime Polypro" J106MG (Prime Polymer Co., Ltd.). MFR: 16g / 10min (temperature 230℃, load 2.16kg). B-4: Homopolypropylene resin "Prime Polypro J108M" (Prime Polymer Co., Ltd.). MFR: 45g / 10min (temperature 230℃, load 2.16kg).

[0064] (C) Acid-modified homopolypropylene resin C-1: Maleic anhydride modified homopolypropylene resin with MFR of 250g / 10min (temperature 190℃, load 2.16kg) and acid value of 8.8.

[0065] (D) Glass fiber D-1:ECS 03 T-211H (manufactured by Nippon Electric Glass Co., Ltd.).

[0066] (E) Heat resistance agent E-1: Hindered phenol compound "Irganox1098" (registered trademark) (manufactured by Chiba Specialty Chemicals Co., Ltd.). E-2: Hindered phenol compound "AO-80" (registered trademark) (manufactured by ADEKA Corporation). E-3: Phosphite compound "PEP-36" (registered trademark) (manufactured by ADEKA Corporation). E-4: Thioether compound "AO-412S" (registered trademark) (manufactured by ADEKA Corporation). E-5: Copper-based heat resistance agent Cuprous iodide (manufactured by Nippon Chemical Industry Co., Ltd.).

[0067] (F) Acid-modified polyolefin resin F-1: Maleic anhydride modified homopolypropylene resin with MFR of 50g / 10min (temperature 190°C, load 2.16kg) and acid value of 3.3. F-2: Maleic anhydride modified homopolypropylene resin with MFR: 480g / 10min (temperature 190℃, load 2.16kg) and acid value: 16. F-3: Maleic anhydride modified block polypropylene resin with MFR of 130g / 10min (temperature 190℃, load 2.16kg) and acid value of 26.

[0068] [Examples 1 to 10] (A) Polyamide resin, (B) Polypropylene resin, (C) Acid-modified homopolypropylene resin, (D) Glass fiber, and (E) Heat-resistant agent were mixed according to the formulation shown in Table 1, and melt-extruded at a barrel temperature of 300°C using a twin-screw extruder (Toshiba Machine Co., Ltd., TEM37) with a screw diameter of 37 mm while removing volatile matter with a vacuum pump. The discharge rate was 60 kg / hr, and the screw rotation speed was 250 rpm. The extruded resin was pulled into a strand shape, cooled by passing it through a cooling bath, and cut while being taken up by a pelletizer to obtain pellets of a polyamide resin composition.

[0069] [Comparative Examples 1 to 10] (A) Polyamide resin, (B) Polypropylene resin, (D) Glass fiber, (E) Heat-resistant agent, and (F) Acid-modified polyolefin resin were mixed according to the formulation shown in Table 2, and melt-extruded at a barrel temperature of 300°C using a twin-screw extruder (Toshiba Machine Co., Ltd., TEM37) with a screw diameter of 37 mm while removing volatile matter with a vacuum pump. The discharge rate was 60 kg / hr, and the screw rotation speed was 250 rpm. The extruded resin was drawn into a strand shape, cooled by passing it through a cooling bath, and cut while being taken up by a pelletizer, to obtain pellets of a polyamide resin composition.

[0070] From Examples 1 to 10 and Comparative Examples 1 to 10, it was found that molded articles obtained by molding polyamide resin compositions containing specific amounts of (A) to (E) had excellent mechanical properties in an absolutely dry state, and also had excellent hydrolysis resistance and durability of welds in a high-temperature environment.

[0071] [Table 1]

[0072] [Table 2]

Claims

1. Amino end group concentration is 10×10 -5 A polyamide resin composition (not including a copper compound) comprising 100 parts by weight of a polyamide resin (A) having a molecular weight of at least mol / g, 10 to 75 parts by weight of a polypropylene resin (B), 0.5 to 30 parts by weight of an acid-modified homopolypropylene resin (C) having an MFR of 200 to 300 measured in accordance with ISO1133 (2011) at a temperature of 190°C under a load of 2.16 kg, 10 to 125 parts by weight of a glass fiber (D), and 0.01 to 5 parts by weight of a heat-resistant agent (E).

2. The polyamide resin (A) has a terminal carboxyl group concentration of 6×10 -5 mol / g or less.

3. The polyamide resin composition according to any one of claims 1 to 2, wherein the (B) polypropylene resin has an MFR of 0.1 to 50 g / 10 min measured at a temperature of 230 ° C. and a load of 2.16 kg in accordance with ISO 1133 (2011).

4. The polyamide resin composition according to any one of claims 1 to 3, wherein the (E) heat stabilizer comprises at least one selected from the group consisting of hindered phenol-based, sulfur-based, and phosphorus-based heat stabilizers.

5. A molded article comprising the polyamide resin composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Programmable read-only memory

    JP1985095799A

  • Reinforced polyamide-polyolefin resin composition

    JP1993043797A

  • Polypropylene composition

    JP1994179784A