Biaxially oriented film
A biaxially stretched film with aliphatic polyketone as the main component achieves enhanced tensile modulus and impact strength, addressing the limitations of conventional films.
Patent Information
- Application Number
- JP2021081916
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-05-13
AI Technical Summary
Conventional aliphatic polyketone films lack sufficient tensile modulus and impact strength, limiting their application in strength-requiring uses.
A biaxially stretched film composed primarily of aliphatic polyketone with specific tensile modulus and impact strength characteristics, achieved through controlled stretching and composition.
The film exhibits excellent tensile modulus and impact strength, making it suitable for diverse applications.
Smart Images

Figure 0007585958000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a biaxially oriented film. [Background technology]
[0002] Conventionally, biaxially stretched films have been used in various applications, and are widely used, for example, in packaging materials, electronic materials, etc. Specific examples of biaxially stretched films include polyolefin films such as polypropylene films, which have excellent mechanical strength, flexibility, water resistance, etc., and therefore have extremely high utility value. In addition, polyester films such as polyethylene terephthalate are also known, which have excellent mechanical properties, surface properties, and water resistance, and therefore are used in various fields, including magnetic materials and industrial materials.
[0003] Aliphatic polyketones are known as materials that can replace polypropylene films and polyester films. Aliphatic polyketones are resins produced from carbon monoxide and olefins as raw materials, and have a variety of excellent properties, so they are expected to be used in a variety of applications. For example, Patent Document 1 discloses that a film with excellent abrasion resistance, durability, etc. can be obtained by using aliphatic polyketones. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-60754 Summary of the Invention [Problem to be solved by the invention]
[0005] However, conventional aliphatic polyketone films have insufficient tensile modulus and impact strength, making them difficult to apply to applications requiring strength. From this perspective, there has been a strong demand for the development of a biaxially oriented film having excellent tensile modulus and impact strength.
[0006] The present invention has been made in view of the above, and has an object to provide a biaxially oriented film that is composed mainly of an aliphatic polyketone film and has excellent tensile modulus and impact strength. [Means for solving the problem]
[0007] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that the above-mentioned object can be achieved by using an aliphatic polyketone as a main component and setting the tensile modulus in a specific direction to a predetermined value or more, thereby completing the present invention.
[0008] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 A biaxially stretched film, Contains aliphatic polyketone as the main component, A biaxially oriented film having a tensile modulus of elasticity of 0.5 GPa or more in one direction on the film surface, and a tensile modulus of elasticity of 0.3 GPa or more in a direction perpendicular to said one direction on the film surface. Section 2 Item 2. The biaxially stretched film according to item 1, wherein the one direction is the TD direction, and the direction perpendicular to the one direction on the film surface is the MD direction. Section 3 Item 3. The biaxially stretched film according to item 1 or 2, having a haze of 10% or less. Section 4 4. The biaxially stretched film according to any one of items 1 to 3, wherein at least one surface has a surface roughness of 0.01 μm or more and 0.1 μm or less. Effect of the Invention
[0009] The biaxially oriented film of the present invention is excellent in tensile modulus and impact strength even though it is mainly composed of an aliphatic polyketone film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".
[0011] 1. Biaxially oriented film The biaxially stretched film of the present invention contains an aliphatic polyketone as a main component, has a tensile modulus of 0.5 GPa or more in one direction on the film surface, and has a tensile modulus of 0.3 GPa or more in a direction perpendicular to the one direction on the film surface. The biaxially stretched film has excellent tensile modulus and impact strength, even though it contains an aliphatic polyketone film as a main component.
[0012] The biaxially stretched film contains aliphatic polyketone as a main component. Here, "containing aliphatic polyketone as a main component" means that the content of aliphatic polyketone contained in the resin component forming the biaxially stretched film is 50% by mass or more. The content of aliphatic polyketone in the resin component is preferably 70% by mass or more, more preferably 80% by mass or more, and particularly preferably 90% by mass or more. The content of aliphatic polyketone in the resin component may be 100% by mass.
[0013] The biaxially stretched film is formed from the resin component (i.e., a resin component containing an aliphatic polyketone). The resin component contained in the biaxially stretched film is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The biaxially stretched film can also be formed from only the resin component.
[0014] The type of aliphatic polyketone contained in the biaxially stretched film is not particularly limited, and for example, any known aliphatic polyketone can be widely applied to the biaxially stretched film.
[0015] The aliphatic polyketone may be, for example, a polyketone represented by the following formula (1): -(CR 1 R 2 -CR3 R 4 -C(=O))- (1) The structural unit represented by the following formula (1) may be included as a repeating unit.
[0016] Here, in formula (1), R 1 , R 2 , R 3 and R 4 are the same or different and represent a hydrogen atom or a methyl group; R 4 R represents hydrogen or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an n-butyl group. When the alkyl group having 1 to 4 carbon atoms has 3 or 4 carbon atoms, it may be either a straight chain or a branched chain. 4 is preferably hydrogen or a methyl group.
[0017] When the aliphatic polyketone has the structural unit represented by the formula (1) as a repeating unit, the content ratio is not particularly limited. For example, the content ratio of the structural unit represented by the formula (1) is preferably 80 mol% or more, more preferably 85 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more, based on the total structural units of the aliphatic polyketone. The content ratio of the structural unit represented by the formula (1) can also be 100 mol% based on the total structural units of the aliphatic polyketone. When the aliphatic polyketone contains a unit other than the structural unit represented by the formula (1), the type of the unit is not particularly limited as long as the effect of the present invention is not impaired.
[0018] The melt flow rate (MFR) of the aliphatic polyketone is preferably 1.0 to 8.0 g / 10 min, more preferably 1.5 to 7.0 g / 10 min, and further preferably 2.0 to 6.0 g / 10 min. The melt flow rate of the aliphatic polyketone is measured by the method described in the Examples.
[0019] The method for producing the aliphatic polyketone is not particularly limited, and for example, the aliphatic polyketone can be obtained by a method similar to a known method for producing an aliphatic polyketone. In addition, the aliphatic polyketone can be obtained from a commercial product, etc.
[0020] The biaxially stretched film may contain one kind of aliphatic polyketone alone, or may contain two or more kinds of aliphatic polyketones.
[0021] The resin components forming the biaxially stretched film may contain additives as necessary. The additives may be, for example, previously contained in the aliphatic polyketone.
[0022] The type of additive is not particularly limited, and examples thereof include known additives added to biaxially stretched films, as well as known additives added to aliphatic polyketones, such as antioxidants, stabilizers such as chlorine absorbers and ultraviolet absorbers, lubricants, crystal nucleating agents, plasticizers, flame retardants, antistatic agents, and colorants.
[0023] The biaxially stretched film of the present invention preferably has a thickness of, for example, 1 μm or more and 100 μm or less. The thickness of the biaxially stretched film is more preferably 2 μm or more, even more preferably 3 μm or more, and particularly preferably 5 μm or more. The thickness of the biaxially stretched film is more preferably 80 μm or less, even more preferably 60 μm or less, and particularly preferably 50 μm or less. The thickness of the biaxially stretched film is a value measured using an outside micrometer (high-precision digital micrometer MDH-25MB manufactured by Mitutoyo Corporation) in accordance with JIS K 7130:1999 A method.
[0024] The biaxially stretched film of the present invention has a tensile modulus of 0.5 GPa or more in one direction on the film surface (hereinafter sometimes referred to as direction A) and a tensile modulus of 0.3 GPa or more in a direction perpendicular to the one direction on the film surface (hereinafter sometimes referred to as direction B). This makes the biaxially stretched film of the present invention a material that is excellent not only in tensile modulus but also in impact strength.
[0025] The tensile modulus in the direction A is preferably 0.6 GPa or more, more preferably 0.7 GPa or more, even more preferably 0.8 GPa or more, and particularly preferably 0.9 GPa or more. The upper limit of the tensile modulus in the direction A is not particularly limited, but may be, for example, 1.5 GPa or less.
[0026] The tensile modulus in the direction B is preferably 0.35 GPa or more, more preferably 0.4 GPa or more, even more preferably 0.45 GPa or more, and particularly preferably 0.5 GPa or more. The upper limit of the tensile modulus in the direction B is not particularly limited, but may be, for example, 0.8 GPa or less.
[0027] It is preferable that the direction A is the TD direction of the biaxially stretched film, and the direction B (i.e., the direction perpendicular to the direction A on the film surface) is the TD direction. In this case, the biaxially stretched film is easily produced, and the material has particularly excellent tensile modulus and impact strength.
[0028] The haze of the biaxially stretched film can be 10% or less, preferably 5% or less, more preferably 3% or less, even more preferably 2% or less, and particularly preferably 1% or less, in order to have high transparency. The haze of the biaxially stretched film may be 0%. The haze of the biaxially stretched film can be measured by a commonly available haze meter, and examples of such a haze meter include the NDH-5000 haze meter manufactured by Nippon Denshoku Industries Co., Ltd.
[0029] The surface roughness of at least one side of the biaxially stretched film is preferably 0.01 μm or more, more preferably 0.02 μm or more. The surface roughness of at least one side of the biaxially stretched film is preferably 0.1 μm or less, more preferably 0.09 μm or less. The surface roughness here means the value of Rpk, which is a linear parameter. The surface roughness can be measured by a non-contact optical interference method, and the optical interference method surface / layer cross-sectional shape measuring instrument "VertScan (registered trademark) 2.0" manufactured by Hitachi High-Tech Corporation can be used as a measuring device. The measurement can be performed in accordance with the provisions of JIS B-0671-2:2002, and among the level difference (Rk) of the core part, the height of the protruding peak (Rpk), and the depth of the protruding valley (Rvk) in the provisions, the level difference (Rk) of the core part and the height of the protruding peak (Rpk) can be used as an index of the surface roughness of the biaxially stretched film.
[0030] The method for producing the biaxially stretched film of the present invention is not particularly limited, and for example, the same method as the known method for producing a biaxially stretched film can be adopted. For example, it is preferable to produce the biaxially stretched film using an unstretched raw sheet. Therefore, the method for producing the biaxially stretched film can include a step of stretching the unstretched raw sheet.
[0031] The method for producing the unstretched raw sheet is not particularly limited, and for example, a known method can be widely applied. For example, the unstretched raw sheet is obtained by supplying the raw material containing the aliphatic polyketone to an extruder, heating and melting it, melt-extruding it from a T-die, and cooling and solidifying it in a metal drum.
[0032] The aliphatic polyketone for obtaining the unstretched raw sheet is not particularly limited in shape, for example, in the form of pellets, powder, etc. The raw material containing the aliphatic polyketone may contain additives as necessary.
[0033] When the raw material containing the aliphatic polyketone is melted by the extruder, the cylinder temperature can be, for example, 220° C. or more and less than 300° C., and the T-die temperature can be, for example, 220° C. or more and less than 300° C. By setting the cylinder temperature and T-die temperature to 220° C. or more, the generation of unmelted resin can be suppressed, and by setting the temperatures to less than 300° C., decomposition of the resin can be suppressed.
[0034] The raw material containing the aliphatic polyketone is preferably passed through a polymer filter before being melt-extruded by a T-die after being heated and melt-melted by an extruder. That is, when producing an unstretched raw sheet, it is preferable to install a polymer filter between the extruder and the T-die. The filtering accuracy of the polymer filter, that is, the opening size of the polymer filter, is not particularly limited, and the type of filter material used in the polymer filter is also not particularly limited.
[0035] The heated and melted raw material is melt-extruded from a T-die, and then cooled and solidified by a metal drum. This forms an unstretched cast raw sheet. During this cooling and solidification, air can be blown onto the resin by an air knife. When cooling by a metal drum, the cooling temperature (metal drum temperature) is not particularly limited. For example, by cooling and solidifying by at least one metal drum maintained at 80 to 140°C, an unstretched raw sheet (cast raw sheet) can be formed.
[0036] The thickness of the resulting unstretched raw sheet is, for example, preferably 0.05 mm or more and 2 mm or less, and more preferably 0.1 mm or more and 1 mm or less.
[0037] The unstretched raw sheet is stretched to produce the desired biaxially stretched film. The method of stretching the unstretched raw sheet is not particularly limited, and for example, any known stretching method can be widely adopted. As the stretching method, biaxial stretching that orients the sheet biaxially in the longitudinal and transverse directions can be adopted, and among them, a sequential biaxial stretching method is preferred.
[0038] An example of the sequential biaxial stretching method is as follows: First, an unstretched raw sheet is kept at a predetermined temperature, passed between rolls with a speed difference, and stretched at a predetermined magnification in the machine direction (MD), and subsequently stretched at a predetermined magnification in the width direction (TD) at a predetermined temperature.
[0039] Thereafter, a biaxially stretched film can be obtained by carrying out an appropriate annealing treatment. It is preferable not to carry out an annealing treatment, since the tensile modulus and impact strength of the biaxially stretched film are likely to be improved.
[0040] The temperature for stretching in the machine direction (MD direction) is, for example, 180° C. or more and less than 220° C., and the temperature for stretching in the width direction (TD direction) is, for example, 180° C. or more and less than 220° C. When the stretching temperature in both directions is 180° C. or more, better moldability can be obtained, and when the temperature is less than 20° C., the melt tension is less likely to decrease, and deterioration of moldability can be suppressed.
[0041] The stretching ratio in the machine direction (MD) is, for example, 3 times or more, preferably 3.5 times or more, more preferably 4 times or more. The stretching ratio in the width direction (TD) is, for example, 3 times or more, preferably 3.5 times or more, more preferably 4 times or more. This makes it easy to adjust the above-mentioned surface roughness (Rpk) to the above-mentioned range.
[0042] The stretching ratio (stretching ratio in MD direction × stretching ratio in TD direction) is 10 times or more. This allows the obtained biaxially stretched film to satisfy the above-mentioned tensile elastic modulus and also has excellent impact strength. If the stretching ratio is less than 10 times, the obtained biaxially stretched film cannot satisfy the above-mentioned tensile elastic modulus, and as a result, the impact strength is poor. The stretching ratio (stretching ratio in MD direction × stretching ratio in TD direction) is preferably 12 times or more, more preferably 14 times or more, even more preferably 18 times or more, and particularly preferably 20 times or more.
[0043] In general, it is not known that there is a relationship between the stretch ratio and the tensile modulus and impact strength in biaxially stretched films. However, the present inventors have surprisingly found that the stretch ratio has a large effect on both the tensile modulus and impact strength in biaxially stretched films containing aliphatic polyketone as the main component. As a result, the present inventors have completed the biaxially stretched film of the present invention, which has a high tensile modulus and excellent impact strength, which was previously difficult to achieve.
[0044] The biaxially stretched film of the present invention is a film containing an aliphatic polyketone as a main component, and usually has a single-layer structure. The biaxially stretched film of the present invention can also be laminated with other films to form a laminate. As the other films, for example, known resin films can be widely adopted. The lamination method is not particularly limited, and known lamination means can be widely adopted.
[0045] The biaxially stretched film of the present invention can be used for various purposes. For example, it can be suitably used as a film for packaging materials. In addition, the biaxially stretched film of the present invention can be used for various purposes such as boiled retort, optical purposes, and backsheets for solar cells. EXAMPLES
[0046] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.
[0047] Example 1 Aliphatic polyketone (abbreviated as POK) was used. Hyosung's POK resin "M701F" (MFR: 4.0 g / 10 min, 230 ° C, 2.16 kg) was fed into an extruder (Toyo Seiki's Lab Plastomill μ single screw extruder D1220B (screw diameter 15 mm, L / D = 20)) and extruded at a cylinder temperature of 230 ° C, a T-die temperature of 260 ° C, and a screw rotation speed of 60 rpm. A continuous unstretched raw sheet was produced using a table cast take-up machine (Toyo Seiki) at a cast roll temperature of 90 ° C and a line speed of 0.2 m / min. The thickness of the obtained unstretched raw sheet was 500 μm and the width was 90 mm. Next, using a table tenter (KARO IV manufactured by Bruckner), the unstretched raw sheet was heated to 200°C and stretched 4 times in the MD direction, then stretched 6 times in the TD direction at a set temperature of 200°C, and then annealed at a set temperature of 200°C for 30 seconds to obtain a biaxially stretched film with a stretch ratio of 24 times. The thickness of the obtained biaxially stretched film was 15 μm.
[0048] Example 2 Except for not carrying out the annealing treatment, a biaxially stretched film was obtained in the same manner as in Example 1. The stretch ratio of the obtained biaxially stretched film was 24 times, and the thickness was 15 μm.
[0049] Example 3 A biaxially stretched film was obtained in the same manner as in Example 2, except that the stretching ratio in the TD direction was changed to 5. The stretching ratio of the obtained biaxially stretched film was 20 times, and the thickness was 18 μm.
[0050] Example 4 A biaxially stretched film was obtained in the same manner as in Example 2, except that the stretching ratio in the TD direction was changed to 4. The stretching ratio of the obtained biaxially stretched film was 16 times, and the thickness was 22 μm.
[0051] Example 5 A biaxially stretched film was obtained in the same manner as in Example 2, except that the stretching ratio in the MD direction was changed to 3 times and the stretching ratio in the TD direction was changed to 6 times. The stretching ratio of the obtained biaxially stretched film was 18 times and the thickness was 19 μm.
[0052] Example 6 A biaxially stretched film was obtained in the same manner as in Example 2, except that the stretching ratio in the MD direction was changed to 3 times and the stretching ratio in the TD direction was changed to 5 times. The stretching ratio of the obtained biaxially stretched film was 15 times and the thickness was 23 μm.
[0053] Example 7 A biaxially stretched film was obtained in the same manner as in Example 2, except that the POK resin was changed to Hyosung's POK resin "M630F" (MFR: 2.0 g / 10 min, 230°C, 2.16 kg). The stretch ratio of the obtained biaxially stretched film was 24 times, and the thickness was 26 μm.
[0054] Example 8 A biaxially stretched film was obtained in the same manner as in Example 2, except that the POK resin was changed to a mixture of Hyosung POK resin "M630F" (MFR: 2.0 g / 10 min, 230°C, 2.16 kg) and Hyosung POK resin "M701F" (MFR: 4.0 g / 10 min, 230°C, 2.16 kg) in a mass ratio of 1:1. The stretch ratio of the obtained biaxially stretched film was 24 times, and the thickness was 23 μm.
[0055] Comparative Example 1 A biaxially stretched film was obtained in the same manner as in Example 2, except that the stretching ratio in the MD direction was changed to 2.5 times and the stretching ratio in the TD direction was changed to 2.5 times. The stretching ratio of the obtained biaxially stretched film was 6.3 times and the thickness was 15 μm.
[0056] Comparative Example 2 A biaxially stretched film was obtained in the same manner as in Example 2, except that the stretching ratio in the MD direction was changed to 3 times and the stretching ratio in the TD direction was changed to 3 times. The stretching ratio of the obtained biaxially stretched film was 9 times and the thickness was 15 μm.
[0057] [Tensile modulus] The biaxially stretched films obtained in each Example and Comparative Example were cut in the MD and TD directions to a length of 150 mm and a width of 15 mm to prepare a tensile test sample. In Comparative Example 3, an unstretched raw sheet was cut into a length of 150 mm and a width of 15 mm to prepare a tensile test sample. The sample was set in a Tensilon universal testing machine (manufactured by Orientec Co., Ltd.) and pulled at a speed of 300 mm / min until the sample broke. At this time, the stress at break (tensile strength) and the elongation at break (tensile elongation) were measured, and the tensile modulus in the MD and TD directions was calculated from the rising slope of the SS curve and the cross-sectional area (width x thickness) of the sample.
[0058] [Impact strength (1 / 4 metal ball)] The impact strength was measured using a Yasuda Seiki film impact tester in accordance with ASTM-D3420. A 15 kgf cm weight and a 1 / 4 inch metal ball were used as the tip ball. The impact strength was measured three times per sample, and the average value was used as the impact strength.
[0059] [Surface roughness] The surface roughness (protruding peak height Rpk) of the biaxially stretched films of the examples and comparative examples was measured by an optical interference non-contact surface profiler. Hitachi High-Tech's "VertScan2.0 (model: R5500GML)" was used as the optical interference non-contact surface profiler. As a measurement sample, the film was cut into an arbitrary size of about 20 cm square, and set on the measurement stage using an electrostatic contact plate or the like in a state where wrinkles were sufficiently stretched out. Using WAVE mode, a 530 white filter and a 1× BODY lens barrel were applied, and measurements were performed per field of view (470.92 μm × 353.16 μm) using a 10x objective lens. This operation was performed at five points at 1 cm intervals in the flow direction from the center in both the flow direction and width direction of the surface of the chill roll side of the measurement sample. The obtained data was subjected to noise removal processing using a median filter (3 x 3), and then Gaussian filter processing with a cutoff value of 30 μm was performed to remove waviness components. This made it possible to properly measure the surface condition. Next, analysis was performed using the "VertScan2.0" analysis software to determine Rpk (μm) and calculate the average value of each value obtained at the above 10 points.
[0060] [Haze] Haze was measured using a haze meter NDH-5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0061] Table 1 shows the production conditions and evaluation results of the physical properties of the biaxially stretched films obtained in each of the Examples and Comparative Examples.
[0062] As shown in Table 1, all of the biaxially stretched films obtained in the examples had a tensile modulus of elasticity in the TD direction of 0.5 GPa or more and a tensile modulus of elasticity in the MD direction of 0.3 GPa or more, and thus had excellent tensile modulus and impact strength. In Comparative Examples 1 and 2, the stretch ratio was insufficient, so the tensile modulus was low and the impact strength was also poor.
[0063] [Table 1]
Claims
1. A biaxially stretched film, Contains aliphatic polyketone as the main component, The melt flow rate of the aliphatic polyketone is 2.0 to 6.0 g / 10 min; The stretching ratio is 20 times or more, The tensile modulus in one direction on the film surface is 0.5 GPa or more, and the tensile modulus in a direction perpendicular to the one direction on the film surface is 0.3 GPa or more, A biaxially stretched film having a ratio of a tensile modulus in one direction on the film plane to a tensile modulus in a direction perpendicular to the one direction on the film plane is less than 0.
97.
2. A biaxially stretched film, Contains aliphatic polyketone as the main component, The melt flow rate of the aliphatic polyketone is 2.0 to 6.0 g / 10 min; The stretching ratio is 20 times or more, A biaxially stretched film having a tensile modulus of 0.9 GPa or more in one direction on the film surface, and a tensile modulus of 0.3 GPa or more and 0.8 GPa or less in a direction perpendicular to the one direction on the film surface.
3. 3. The biaxially stretched film according to claim 1, wherein the one direction is a TD direction, and a direction perpendicular to the one direction on the film surface is a MD direction.
4. The biaxially stretched film according to any one of claims 1 to 3, having a haze of 10% or less.
5. The biaxially stretched film according to any one of claims 1 to 4, wherein the surface roughness of at least one surface is 0.01 µm or more and 0.1 µm or less.
6. The biaxially stretched film according to any one of claims 1 to 5, having a thickness of 15 µm or more.
Citation Information
Patent Citations
Monoaxial or biaxial orientation film
JP1991120028A
Biaxially oriented film and laminated film