Method for producing copolyamide

By controlling the mixing and reaction temperatures of ε-caprolactam and adipic acid with hexamethylene diamine, the method addresses the inefficiencies and coloration issues in existing copolyamide production, achieving high-quality copolyamide production with reduced water usage and continuous processing.

JP7586084B2Active Publication Date: 2024-11-19UBE CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021545186
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-30
Filing Date
2020-08-19
Publication Date
2024-11-19
Estimated Expiration
2040-08-19

AI Technical Summary

Technical Problem

Existing methods for producing copolyamide require large amounts of water removal, leading to energy-intensive processes and risk significant coloration of the polyamide resin, particularly when high temperatures are used.

Method used

A method involving mixing ε-caprolactam and adipic acid at controlled temperatures between 69°C and 115°C, followed by reaction with hexamethylene diamine at specific conditions to produce a copolyamide, minimizing water generation and preventing coloration.

Benefits of technology

This method efficiently produces high-quality copolyamide with reduced coloration, allowing for continuous production with minimal water removal and improved operational efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586084000002
    Figure 0007586084000002
  • Figure 0007586084000001
    Figure 0007586084000001
Patent Text Reader

Abstract

The present invention relates to a method for producing a copolymerized polyamide, said method enabling the efficient production of a copolymerized polyamide of good quality, while comprising the first step and the second step described below. First step: a step for preparing a mixed liquid by mixing (A) ε-caprolactam and (B) adipic acid at a temperature of not less than 69°C but less than 115°C, wherein adipic acid (B) in a solid state is added to ε-caprolactam (A) in a liquid state so as to mix the ε-caprolactam (A) and the adipic acid (B) with each other, and from 1 mole to 20 moles of the ε-caprolactam (A) is used relative to 1 mole of the adipic acid (B) Second step: a step for obtaining a copolymerized polyamide by mixing and subsequently reacting the mixed liquid obtained in the first step with (C) hexamethylenediamine
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polyamide copolymer. [Background technology]

[0002] Conventionally, as methods for producing a copolymerized polyamide, there have been disclosed, for example, a method in which a dicarboxylic acid and a diamine are mixed in water to form a salt (amide salt), and then the mixture is heated and polymerized (see, for example, Non-Patent Document 1), and a method in which molten adipic acid and molten hexamethylenediamine are mixed, heated, and polymerized (see, for example, Patent Document 1).

[0003] Furthermore, as a method for producing a copolymerized polyamide, there has been disclosed a method in which terephthalic acid, an aqueous solution of hexamethylenediamine, caprolactam and water are mixed to form an aminocarboxylate, which is then heated and polymerized (see, for example, Patent Document 2 (Example 8)); and a method in which ω-lactam and dicarboxylic acid are polymerized by heating and melting at a temperature exceeding the melting point of the dicarboxylic acid to obtain an oligomer having carboxylic acids at both ends, and then a diamine is added to carry out a condensation reaction (see, for example, Patent Document 3 (Example 1) and Patent Document 4 (Comparative Example 301)).

[0004] Furthermore, Patent Document 5 discloses a method for producing a copolymerized polyamide by mixing a solid dicarboxylic acid into a liquid lactam and reacting the mixture with a diamine. Patent Document 5 also describes an example in which adipic acid and ε-caprolactam are mixed at 115° C., and an example in which dodecanedioic acid and laurinlactam are mixed at 115° C. and the mixture is reacted with decanediamine to produce a colorless copolymerized polyamide. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-53359 A [Patent Document 2] JP 2010-116575 A [Patent Document 3] Japanese Patent Application Publication No. 3-111424 [Patent Document 4] International Publication No. 2011 / 081099 [Patent Document 5] Japanese Patent Application Publication No. 9-124542 [Non-patent literature]

[0006] [Non-Patent Document 1] "New Polymer Manufacturing Process" edited by Koji Saeki and Shinji Omi, Industrial Research Institute Summary of the Invention [Problem to be solved by the invention]

[0007] In the methods described in Patent Documents 1 and 2, since it is necessary to mix a dicarboxylic acid and a diamine in water to form a salt (amide salt), a large amount of water must be removed during or after the reaction, which poses the problem of requiring an apparatus and a large amount of energy for this purpose. In addition, in the methods described in Patent Documents 3 and 4, since the temperature for obtaining the melt is high, there is a risk that the obtained polyamide resin will be significantly discolored (e.g., yellow).

[0008] When adipic acid and caprolactam are mixed at 115° C. as in Patent Document 5, there is a risk that the resulting polyamide resin will become significantly discolored (for example, yellow).

[0009] An object of the present invention is to provide a method for producing a copolyamide, which can efficiently produce a high-quality copolyamide. [Means for solving the problem]

[0010] The object of the present invention is achieved by the method for producing a copolyamide according to any one of [1] to

[10] . [1] A method for producing a copolyamide, comprising the following first and second steps: First step: a step of preparing a mixed liquid by mixing ε-caprolactam (A) and adipic acid (B) at 69°C or higher and lower than 115°C, in which solid adipic acid (B) is added to liquid ε-caprolactam (A) to mix ε-caprolactam (A) and adipic acid (B), and the amount of ε-caprolactam (A) used per mole of adipic acid (B) is 1 to 20 moles. The second step is a step of mixing the mixture obtained in the first step with hexamethylenediamine (C) and then reacting them to obtain a copolymer polyamide. [2] The method for producing a copolyamide according to [1], wherein in the first step, the ε-caprolactam (A) and the adipic acid (B) are mixed at 69° C. to 110° C. [3] The method for producing a copolyamide according to [1] or [2], wherein in the first step, the amount of ε-caprolactam (A) used is 2 to 15 moles per mole of adipic acid (B). [4] The method for producing a copolyamide according to any one of [1] to [3], wherein in the first step, the resulting mixed liquid has a color value of less than 0.5. [5] The method for producing a copolyamide according to any one of [1] to [4], wherein in the second step, hexamethylenediamine (C) is added at 20 to 100° C. [6] The method for producing a copolyamide according to any one of [1] to [5], wherein in the second step, the reaction temperature between the mixed liquid obtained in the first step and hexamethylenediamine (C) is 180 to 300°C. [7] The method for producing a copolyamide according to any one of [1] to [6], wherein in the second step, the reaction pressure between the mixed liquid obtained in the first step and hexamethylenediamine (C) is 0.05 to 0.5 MPa. [8] The method for producing a copolymerized polyamide according to any one of [1] to [7], wherein in the second step, the amount of hexamethylenediamine (C) used is 0.01 to 100 mol per 1 mol of adipic acid (B) used in the first step. [9] A method for producing a copolymer polyamide according to any of [1] to [8], wherein, in all constitutional units of the copolymer polyamide obtained in the second step, the proportion of constitutional units derived from ε-caprolactam (A) is 10 to 98 mol %, the proportion of constitutional units derived from adipic acid (B) is 1 to 45 mol %, and the proportion of constitutional units derived from hexamethylenediamine (C) is 1 to 45 mol %.

[10] A method for producing a copolyamide according to any one of [1] to [9], further comprising the following third step: The third step is to periodically extract the copolymer polyamide obtained in the second step from the container. Effect of the Invention

[0011] INDUSTRIAL APPLICABILITY The present invention provides a method for producing a copolyamide, which can efficiently produce a high-quality copolyamide. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing an example of a production apparatus used in the method for producing a copolyamide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Method of producing copolymerized polyamide] The method for producing a copolyamide includes the following first and second steps. First step: a step of preparing a mixed liquid by mixing ε-caprolactam (A) and adipic acid (B) at 69°C or higher and lower than 115°C, in which solid adipic acid (B) is added to liquid ε-caprolactam (A) to mix ε-caprolactam (A) and adipic acid (B), and the amount of ε-caprolactam (A) used per mole of adipic acid (B) is 1 to 20 moles. The second step is a step of mixing the mixture obtained in the first step with hexamethylenediamine (C) and then reacting them to obtain a copolymer polyamide.

[0014] In the following, ε-caprolactam (A), adipic acid (B), and hexamethylenediamine (C) may be collectively referred to as "raw materials", or may be referred to as each raw material individually. Additionally, "or less" means "same as or less than," and "or more" means "same as or greater than."

[0015] The method for producing a copolymerized polyamide allows efficient production of the copolymerized polyamide. That is, the main component of water produced in the step of producing the copolymerized polyamide is water generated during copolymerization. Therefore, there is no need for a complicated operation such as removing a large amount of water that is generated when using an aqueous solution. Furthermore, the method for producing a copolymerized polyamide allows production of a high-quality copolymerized polyamide. That is, coloration (e.g., yellowing) of the obtained copolymerized polyamide is reduced or almost nonexistent. The method for producing the copolyamide may be carried out in a continuous manner, or in a semi-batch or batch manner.

[0016] (copolyamide) The copolymerized polyamide, which is the product of the method for producing a copolymerized polyamide, is an ε-caprolactam / hexamethylenediaminoadipic acid copolymer (polyamide 6 / 66), and has constitutional units derived from ε-caprolactam (A), constitutional units derived from adipic acid (B), and constitutional units derived from hexamethylenediamine (C).

[0017] The preferred proportions of each of the constituent units in the total constituent units of the copolymerized polyamide (the total number of moles of the constituent units derived from ε-caprolactam (A), the constituent units derived from adipic acid (B), and the constituent units derived from hexamethylenediamine (C)) are 10 to 98 mol % for the constituent units derived from ε-caprolactam (A), 1 to 45 mol % for the constituent units derived from adipic acid (B), and 1 to 45 mol % for the constituent units derived from hexamethylenediamine (C). Here, the content ratio of the constituent units of the copolymerized polyamide can be determined from the amount of each raw material charged.

[0018] (1st step) The first step is a step of preparing a mixed liquid by mixing ε-caprolactam (A) and adipic acid (B) at 69 to 115°C, in which solid adipic acid (B) is added to liquid ε-caprolactam (A) to mix ε-caprolactam (A) and adipic acid (B), and the amount of ε-caprolactam (A) used per mole of adipic acid (B) is 1 to 20 moles.

[0019] It is desirable to remove oxygen from the ε-caprolactam (A) and adipic acid (B) in advance in order to prevent discoloration and deterioration during the process of producing the copolyamide.

[0020] In the first step, the ε-caprolactam (A) and the adipic acid (B) are mixed at a temperature of 69° C. or higher and lower than 115° C. Specifically, in the first step, the ε-caprolactam (A) is heated to its melting point of 69° C. or higher to melt it into a liquid (molten liquid), and the adipic acid (B) is added in a solid state to the liquid (molten liquid) at a temperature of 69° C. or higher and lower than 115° C. to perform the mixing.

[0021] By mixing ε-caprolactam (A) and adipic acid (B) at 69°C or higher and lower than 115°C, solid adipic acid (B) is added to molten (liquid) ε-caprolactam (A) to mix monomer (A) and adipic acid (B), resulting in excellent operability and uniformity. In addition, by setting the mixing temperature of ε-caprolactam (A) and adipic acid (B) within the above range, thermal deterioration of ε-caprolactam (A) and adipic acid (B) and reaction between ε-caprolactam (A) and adipic acid (B) can be suppressed. If ε-caprolactam (A) and adipic acid (B) are mixed at 115°C or higher, coloring (e.g., yellow coloring) of the resulting copolymerized polyamide may become noticeable. From the viewpoint of obtaining a copolymerized polyamide of better quality, the mixing of the ε-caprolactam (A) and the adipic acid (B) is more preferably carried out at a temperature of 69°C to 110°C, further preferably 69°C to 100°C, and particularly preferably 69°C to 85°C.

[0022] In the first step, the amount of ε-caprolactam (A) used (mixed amount) is 1 to 20 moles per mole of adipic acid (B). From the viewpoint of obtaining a copolymerized polyamide of better quality, the amount of ε-caprolactam (A) used in the first step is preferably 2 to 15 moles, particularly preferably 3 to 10 moles, per mole of adipic acid (B).

[0023] In order to prevent discoloration of the target copolymerized polyamide, it is preferable to carry out the first step in the absence of oxygen or in an inert gas atmosphere. Examples of the inert gas include rare gases (helium, neon, argon, etc.) and nitrogen. The inert gas may be one type or a combination of two or more types.

[0024] The first step produces a mixed solution containing ε-caprolactam (A) and adipic acid (B). From the viewpoint of preventing the final product, ie, the copolymerized polyamide, from being colored, the chromaticity of the mixed solution produced in the first step is preferably 2 or less, more preferably 1.5 or less, even more preferably 0.7 or less, and particularly preferably less than 0.5. The chromaticity of the mixed solution can be measured by the method described in the examples below.

[0025] The mixture obtained in the first step may be stored as a mixture (liquid mixture) prior to the second step, or may be cooled to room temperature (e.g., 25°C) and stored as a solid mixture (solid mixture) or a slurry (e.g., a slurry-like mixture in which a part of solid adipic acid (B) is dispersed in a melt of ε-caprolactam (A). Here, depending on the melting point of the mixture and the components contained in the mixture, and the saturated dissolution amount of adipic acid (B) in the melt of ε-caprolactam (A), the mixture obtained in the first step may be a solid mixture, a slurry, or a mixed liquid at room temperature. When the solid mixture or slurry is used as a raw material in the second step, the solid mixture or slurry can be heated to form a mixed liquid. As a result, it can be used as the "mixture obtained in the first step" in the second step. The cooling method can be performed using a known cooling device or by leaving the mixed liquid at room temperature. The heating temperature for obtaining the mixed liquid is, for example, a heating temperature for obtaining a homogeneous mixed liquid.

[0026] From the viewpoint of transferring the mixture obtained in the first step to a vessel in which the second step is performed, it is particularly preferable to heat the mixture to make it homogeneous. Here, "homogeneous" means that adipic acid (B) is substantially completely dissolved in ε-caprolactam (A) to form a solution 1. In addition, adipic acid (B) may be dispersed without dissolving in the melt of ε-caprolactam (A) as long as it does not affect the subsequent steps. That is, the method for producing a copolyamide preferably includes a step of heating the mixture obtained in the first step to obtain a homogeneous mixture before the second step. The heating temperature is preferably 69°C or more and less than 115°C, more preferably 69°C to 110°C, even more preferably 69°C to 100°C, and particularly preferably 69°C to 85°C.

[0027] (2nd process) The second step is a step of mixing the mixture obtained in the first step (i.e., a mixture containing ε-caprolactam (A) and adipic acid (B)) with hexamethylenediamine (C) and then reacting them to obtain a copolymerized polyamide. In the second step, the raw materials (ε-caprolactam (A), adipic acid (B) and hexamethylenediamine (C)) react with each other to obtain a copolymerized polyamide.

[0028] The hexamethylenediamine (C) is as described above. Hexamethylenediamine (C) may be used as a high-concentration aqueous solution of hexamethylenediamine (C) (for example, an aqueous solution of 80% by mass of hexamethylenediamine (C)). It is preferable to remove oxygen from hexamethylenediamine (C) in advance to prevent coloration and deterioration during the process of producing a copolymerized polyamide.

[0029] When the mixture obtained in the first step is heated to become a homogeneous mixture, it is preferable to heat the hexamethylenediamine (C) in advance in order to maintain the homogeneous state. In this case, the hexamethylenediamine (C) is added in the second step at a temperature of preferably 20 to 100°C, more preferably 30 to 90°C, and particularly preferably 40 to 80°C.

[0030] The method of mixing and supplying the mixed solution and hexamethylenediamine (C) is not particularly limited, but it is preferable to quantitatively supply and mix them using a feed pump capable of delivering liquid, or a supply system in which a known flow meter, concentration meter, valve, etc. are attached to a supply line.

[0031] In the second step, the reaction temperature between the mixed liquid obtained in the first step and hexamethylenediamine (C) is not particularly limited as long as the raw materials undergo a polymerization reaction to obtain a desired copolymer polyamide, but is preferably 180 to 300° C., more preferably 190 to 280° C., and particularly preferably 200 to 260° C. By setting the temperature within this range, the polymerization time can be shortened and side reactions such as decomposition and gelation can be suppressed.

[0032] In the second step, the reaction pressure between the mixed liquid obtained in the first step and hexamethylenediamine (C) is not particularly limited, but is preferably 0.05 to 0.5 MPa, and more preferably 0.1 MPa (absolute pressure basis). To adjust the pressure, for example, known vacuum equipment such as a Nash pump, a mechanical booster, or a steam ejector can be used.

[0033] In the second step, the proportion (mixing proportion) of hexamethylenediamine (C) used can be appropriately adjusted depending on the type of the desired copolymerized polyamide. In the second step, the amount of hexamethylenediamine (C) used is preferably 0.01 to 100 mol, more preferably 0.1 to 10 mol, and particularly preferably 0.5 to 5 mol, per mol of adipic acid (B) used in the first step.

[0034] In order to prevent discoloration of the desired copolymerized polyamide, the second step is preferably carried out in the absence of oxygen or in an inert gas atmosphere, as described above in the first step. The second step produces an ε-caprolactam / hexamethylenediaminoadipic acid copolymer (polyamide 6 / 66). The content ratio of the structural units in polyamide 6 / 66 can be appropriately set depending on the amount of the raw material components charged.

[0035] <Polymerization catalyst> In order to improve productivity, the second step can be carried out in the presence of a known polymerization catalyst. Specific examples of such a polymerization catalyst include: phosphoric acid; Phosphates such as sodium phosphate, magnesium phosphate, potassium phosphate, calcium phosphate, vanadium phosphate, manganese phosphate, nickel phosphate, and cobalt phosphate; Hypophosphites, such as sodium hypophosphite, magnesium hypophosphite, potassium hypophosphite, calcium hypophosphite, vanadium hypophosphite, manganese hypophosphite, nickel hypophosphite, and cobalt hypophosphite; acidic phosphate esters such as monomethyl phosphate ester, dimethyl phosphate ester, monoethyl phosphate ester, diethyl phosphate ester, propyl phosphate ester, isopropyl phosphate ester, dipropyl phosphate ester, diisopropyl phosphate ester, butyl phosphate ester, isobutyl phosphate ester, dibutyl phosphate ester, diisobutyl phosphate ester, monophenyl phosphate ester, and diphenyl phosphate ester; Phosphate esters such as trimethyl phosphate, triethyl phosphate, tri-n-propyl phosphate, tri-i-propyl phosphate, tri-n-butyl phosphate, tri-i-butyl phosphate, triphenyl phosphate, tri-n-hexyl phosphate, tri-n-octyl phosphate, tri(2-ethylhexyl) phosphate, and tridecyl phosphate; Phosphite esters such as dimethyl phosphite, diethyl phosphite, di-n-propyl phosphite, di-i-propyl phosphite, di-n-butyl phosphite, di-i-butyl phosphite, diphenyl phosphite, di-n-hexyl phosphite, di-n-octyl phosphite, di(2-ethylhexyl) phosphite, didecyl phosphite, etc.; However, preferred is hypophosphite, and more preferred is sodium hypophosphite. The polymerization catalyst may be one type or a combination of two or more types.

[0036] The method of supplying or adding the polymerization catalyst is not particularly limited, and the polymerization catalyst may be supplied to the reactor alone in the form of an aqueous solution or water slurry, or may be present in each of the raw materials ((A), (B) or (C)) in advance. The amount of the polymerization catalyst used is not particularly limited, but when a catalyst containing phosphorus atoms is used, the amount is preferably 0.1 to 1000 ppm by mass in terms of phosphorus atoms relative to the total mass of the raw materials.

[0037] (3rd step) The method for producing a copolymerized polyamide can further include a third step. The third step is a step of extracting the copolymerized polyamide produced in the second step from the vessel at any time. By including the third step in the method for producing a copolymerized polyamide, the copolymerized polyamide can be produced continuously.

[0038] In the third step, the occasional withdrawal from the vessel can be, for example, continuous, semi-batch, or batch. In addition, in the third step, a specific method for withdrawing the copolymerized polyamide produced in the second step can be, for example, withdrawing the polymer that has reached the bottom of the vessel (for example, reactor) from a withdrawal port. This withdrawal operation is not particularly limited, but in order to continuously and stably and quantitatively withdraw the polymer, it is desirable to use a discharge device such as a perforated plate, a gear pump, or a ball valve at the bottom of the reactor.

[0039] <Preferred embodiment> Both the first and second steps are preferably carried out in the absence of oxygen or in an inert gas atmosphere as described above.

[0040] (Reaction Apparatus) A production apparatus used in the production method for a copolyamide is composed of, for example, a vessel 1 for carrying out the first step, a vessel 2 containing hexamethylenediamine (C), and a reactor for carrying out the second step, as shown in Fig. 1. There are no particular limitations on the materials for these vessels and reactors, so long as they are not corroded or deteriorated by contact with the raw materials and are not softened or melted by heating.

[0041] As the reactor, a known reactor such as a tank-type continuous reactor or a tubular continuous reactor is used. The number of reactors can be changed depending on the production amount, etc. When a plurality of reactors are used, they can be arranged in series or in parallel.

[0042] The reactor is desirably equipped with a fractionator for distilling off water (water contained in the raw materials or water generated) and each raw material, and may be equipped with known pressure reducing equipment such as a Nash pump, a mechanical booster, or a steam ejector for controlling the reaction pressure. It is desirable to install a heat exchanger at the top of the distillation column and perform a reflux operation to condense the distillate gas to increase the separation efficiency. In addition, necessary devices and equipment other than those described above may be installed within the scope that does not impair the effects of the present invention.

[0043] The rectification column is preferably a column having trays (plates) and / or packings as internals, where the internals refer to the part inside the column where gas and liquid actually come into contact with each other. Suitable examples of the trays that can be used include bubble trays, perforated plate trays, ripple trays, ballast trays, valve trays, countercurrent trays, Unifrax trays, Superfrac trays, Maxfrac trays, dual flow trays, grid plate trays, turbogrid plate trays, Kittel trays, and Oldershaw type perforated plates. As the packing, for example, random packing such as Raschig rings, Lessing rings, Pall rings, Berl saddles, Intalox saddles, Dixon packing, McMahon packing, and Helipack, and ordered packing such as Melapack, Gempack, Technopack, Flexipak, Sulzer packing, Goodroll packing, and Glitch grid are preferably used. EXAMPLES

[0044] The present invention will now be described in detail with reference to examples, but the scope of the present invention is not limited to these examples.

[0045] (Method of measuring chromaticity) Standard solutions of each chromaticity are prepared, with the color produced when 1 mg of platinum in potassium chloroplatinate and 0.5 mg of cobalt in cobalt chloride are contained in 1 L of purified water being taken as chromaticity 1, and the absorbance of each standard chromaticity solution at a wavelength of 370 nm is measured. Then, a calibration curve of chromaticity and absorbance is prepared. Next, the absorbance of a 50 wt% aqueous solution of the mixed solution obtained in the first step at a wavelength of 370 nm is measured. The chromaticity with which the absorbances match is taken as the chromaticity of the mixed solution obtained in the first step.

[0046] (How to check for yellow color) The yellowness of the obtained copolymerized polyamide was measured in accordance with JIS K 7373 using a color meter (ZE6000, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0047] Example 1 (Production of Copolyamide (Polyamide 6 / 66)) (1st step) In a nitrogen atmosphere, ε-caprolactam was added to a container 1 (volume: 1 L) and heated to 80°C to melt it, and then adipic acid was added while stirring and the mixture was kept at the same temperature for 24 hours to obtain a mixed liquid (adipic acid content: 12 mass%, ε-caprolactam / adipic acid=778 / 82 (molar ratio)). The color of the resulting mixture was less than 0.5. (2nd process) In a nitrogen atmosphere, an 80% by mass aqueous solution of hexamethylenediamine was added to vessel 2 (volume: 1 L) and heated with stirring until the liquid temperature reached 60° C. Next, the mixed solution obtained in the first step from vessel 1 was supplied at 56.5 g / h (ε-caprolactam: 439.4 mmol / h, adipic acid: 46.5 mmol / h) and the aqueous solution of hexamethylenediamine was supplied at 6.9 g / h (hexamethylenediamine: 47.8 mmol / h) to a tank-type reactor having an internal volume of 1 L and a stirrer, and then the mixture was heated to 230° C. and polymerized for 4 hours while distilling off water to obtain a copolymerized polyamide. The amount of water distilled off during the polymerization reaction was 3.0 g / h. No yellow coloring was observed in the obtained copolymerized polyamide.

[0048] Example 2 (Production of Copolyamide (Polyamide 6 / 66)) (1st step) In a nitrogen atmosphere, ε-caprolactam was added to a container 1 (volume: 1 L) and heated to 80°C to melt it, and then adipic acid was added while stirring and the mixture was kept at the same temperature for 12 hours to obtain a mixed liquid (adipic acid content: 12 mass%, ε-caprolactam / adipic acid=778 / 82 (molar ratio)). The color of the resulting mixture was less than 0.5.

[0049] (2nd process) In a nitrogen atmosphere, an 80% by mass aqueous solution of hexamethylenediamine was added to vessel 2 (volume: 1 L) and heated with stirring until the liquid temperature reached 60° C. Next, the mixed liquid obtained in the first step from vessel 1 was supplied at 56.5 g / h (ε-caprolactam: 439.4 mmol / h, adipic acid: 46.5 mmol / h) and the aqueous hexamethylenediamine solution was supplied at 6.9 g / h (hexamethylenediamine: 47.8 mmol / h) to a tubular reactor (length: 620 mm, inner diameter: 20 mm), and then the mixture was heated to 230° C. to carry out a polymerization reaction while distilling off water. The amount of water distilled off during the polymerization reaction was 3.0 g / h.

[0050] (3rd step) 2.7 hours after the start of the supply in the second step, the copolymerized polyamide produced was obtained from the outlet at the bottom of the reactor. No yellow coloring was observed in the copolymerized polyamide obtained. During the third step, the first and second steps were carried out, and the amount of water distilled off was small, allowing efficient and continuous production of the copolymerized polyamide.

[0051] Example 3 (Production of Copolyamide (Polyamide 6 / 66)) (1st step) In a nitrogen atmosphere, ε-caprolactam was added to a container 1 (volume: 1 L) and heated to 110°C to melt it, and then adipic acid was added while stirring and the mixture was kept at the same temperature for 24 hours to obtain a mixed liquid (adipic acid content: 12 mass%, ε-caprolactam / adipic acid=778 / 82 (molar ratio)). The color of the resulting mixture was 0.7. (2nd process) In a nitrogen atmosphere, an 80% by mass aqueous solution of hexamethylenediamine was added to vessel 2 (volume: 1 L) and heated with stirring until the liquid temperature reached 60° C. Next, the mixed solution obtained in the first step from vessel 1 was supplied at 56.5 g / h (ε-caprolactam: 439.4 mmol / h, adipic acid: 46.5 mmol / h) and the aqueous solution of hexamethylenediamine was supplied at 6.9 g / h (hexamethylenediamine: 47.8 mmol / h) to a tank-type reactor having an internal volume of 1 L and a stirrer, and then the mixture was heated to 230° C. and polymerized for 4 hours while distilling off water to obtain a copolymerized polyamide. The amount of water distilled off during the polymerization reaction was 3.0 g / h. No yellow coloring was observed in the obtained copolymerized polyamide.

[0052] Example 4 (Production of Copolyamide (Polyamide 6 / 66)) (1st step) In a nitrogen atmosphere, ε-caprolactam was added to a container 1 (volume: 1 L) and heated to 80°C to melt it, and then adipic acid was added while stirring and the mixture was kept at the same temperature for 24 hours to obtain a mixed liquid (adipic acid content: 20 mass%, ε-caprolactam / adipic acid=399.4 / 77.3 (molar ratio)). The color of the resulting mixture was less than 0.5. (2nd process) In a nitrogen atmosphere, an 80% by mass aqueous solution of hexamethylenediamine was added to vessel 2 (volume: 1 L) and heated with stirring until the liquid temperature reached 60° C. Next, the mixed solution obtained in the first step from vessel 1 was supplied at 56.5 g / h (ε-caprolactam: 399.4 mmol / h, adipic acid: 77.3 mmol / h) and the aqueous solution of hexamethylenediamine was supplied at 11.6 g / h (hexamethylenediamine: 79.8 mmol / h) to a tank-type reactor having an internal volume of 1 L and a stirrer, and then the mixture was heated to 230° C. and polymerized for 4 hours while distilling off water to obtain a copolymerized polyamide. The amount of water distilled off during the polymerization reaction was 3.5 g / h. No yellow coloring was observed in the obtained copolymerized polyamide.

[0053] Comparative Example 1 (Production of Copolyamide (Polyamide 6 / 66)) In a nitrogen atmosphere, ε-caprolactam was added to container 1 (volume: 1 L) and melted by heating to 80° C., and then the mixture was kept for 24 hours while being stirred. In a nitrogen atmosphere, adipic acid, water, and an 80% by mass aqueous solution of hexamethylenediamine were added in this order to container 2 (volume: 1 L) to obtain a 50% by mass aqueous solution of an amide salt consisting of adipic acid and hexamethylenediamine. The temperature of the aqueous solution was then maintained at 60°C. ε-caprolactam was supplied from the vessel 1 at a rate of 49.7 g / h (ε-caprolactam: 439.4 mmol / h) and the aqueous amide salt solution was supplied from the vessel 2 at a rate of 24.4 g / h (adipic acid: 46.5 mmol / h, hexamethylenediamine: 46.5 mmol / h) to a tubular reactor (length: 600 mm, inner diameter: 20 mm), and then the mixture was heated to 230° C. to carry out a polymerization reaction while distilling off water. The amount of water distilled off during the polymerization reaction was 13 g / h. 2.7 hours after the start of the supply of ε-caprolactam, the copolymerized polyamide produced was obtained from the outlet at the bottom of the reactor. No yellow coloring was observed in the obtained copolymerized polyamide. During the time the copolymerized polyamide was being withdrawn, the reaction between adipic acid, hexamethylenediamine, and ε-caprolactam was occurring, and it was possible to produce the copolymerized polyamide continuously. However, the amount of water distilled off was large, and it could not be said to be efficient.

[0054] Comparative Example 2 (Production of Copolyamide (Polyamide 6 / 66)) (1st step) In a nitrogen atmosphere, ε-caprolactam was added to a container 1 (volume: 1 L) and heated to 120°C to melt it, and then adipic acid was added with stirring and maintained at the same temperature for 12 hours to obtain a mixed liquid (adipic acid content: 12 mass%, ε-caprolactam / adipic acid=778 / 82 (molar ratio)). The color of the resulting mixture was 6.4. (2nd process) In a nitrogen atmosphere, an 80% by mass aqueous solution of hexamethylenediamine was added to vessel 2 (volume: 1 L) and heated with stirring until the liquid temperature reached 60° C. Next, the mixed liquid obtained in the first step from vessel 1 was supplied at 56.5 g / h (ε-caprolactam: 439.4 mmol / h, adipic acid: 46.5 mmol / h) and the aqueous hexamethylenediamine solution was supplied at 6.9 g / h (hexamethylenediamine: 47.8 mmol / h) to a tubular reactor (length: 620 mm, inner diameter: 20 mm), and then the mixture was heated to 230° C. to carry out a polymerization reaction while distilling off water. The amount of water distilled off during the polymerization reaction was 3.0 g / h. (3rd step) 2.7 hours after the start of the supply in the second step, collection of the produced copolymerized polyamide was started from the outlet at the bottom of the reactor. During the third step, the first and second steps were carried out, and the amount of water distilled off was small, allowing efficient and continuous production of the copolymerized polyamide. However, yellow coloration was observed in the obtained copolymerized polyamide.

[0055] Comparative Example 3 (Production of Copolyamide (Polyamide 6 / 66)) (1st step) In a nitrogen atmosphere, ε-caprolactam was added to container 1 (volume: 1 L) and melted by heating to 160°C (above the melting point of adipic acid (152°C)). Adipic acid was then added with stirring and the mixture was maintained at the same temperature for 24 hours to obtain a mixed solution (adipic acid content: 12% by mass, ε-caprolactam / adipic acid=778 / 82 (molar ratio)). The color of the resulting mixture was 5.5. (2nd process) In a nitrogen atmosphere, an 80% by mass aqueous solution of hexamethylenediamine was added to vessel 2 (volume: 1 L) and heated with stirring until the liquid temperature reached 60° C. Next, the mixed liquid obtained in the first step was supplied from vessel 1 at 56.5 g / h (ε-caprolactam: 439.4 mmol / h, adipic acid: 46.5 g / h) and the aqueous hexamethylenediamine solution was supplied from vessel 2 at 6.9 g / h (hexamethylenediamine: 47.8 mmol / h) to a tubular reactor (length: 600 mm, inner diameter: 20 mm), and then the mixture was heated to 230° C. to carry out a polymerization reaction while distilling off water. The amount of water distilled off during the polymerization reaction was 3.0 g / h. (3rd step) 2.7 hours after the start of the supply in the second step, the produced copolymerized polyamide was collected from the outlet at the bottom of the reactor. During the third step, the first and second steps were carried out, and the amount of water distilled off was small, allowing efficient and continuous production of the copolymerized polyamide. However, yellow coloration was observed in the obtained copolymerized polyamide.

[0056] The results are summarized in Table 1.

[0057] [Table 1]

[0058] From the above results, it is seen that the amount of water distilled off is less in the Examples than in the Comparative Examples, and that the copolymerized polyamide can be produced efficiently. It is also seen that the copolymerized polyamide production method of the present invention can be suitably applied not only to the batch system (Example 1) but also to the continuous system (Example 2). Furthermore, in the case of Example 2 including the third step, a high-quality copolymerized polyamide could be continuously produced. A comparison with Examples 3 and 4 shows that the chromaticity of the mixed liquid obtained in the first step decreased as the mixing temperature decreased.

[0059] On the other hand, in Comparative Example 1, adipic acid (B) and hexamethylenediamine (C) were mixed in water to form a salt (amide salt), and then the mixture was heated and polymerized, so that a large amount of water was distilled off. Therefore, in Comparative Example 1, it was not possible to efficiently produce a copolymer polyamide.

[0060] In Comparative Examples 2 and 3, ε-caprolactam (A) and adipic acid (B) were mixed at a temperature of 115° C. or higher, and thus coloring of the mixed liquid obtained in the first step was observed. In Comparative Examples 2 and 3, in which the chromaticity of the mixed liquid obtained in the first step was greater, yellow coloring of the obtained copolymerized polyamide was observed. Thus, in Comparative Examples 2 and 3, a good quality copolymerized polyamide could not be produced. From the above, it can be said that a good quality copolymerized polyamide cannot be produced in Patent Document 5 (JP Patent Publication 9-124542 A), which describes only an example in which the mixing temperature of ε-caprolactam and adipic acid is 115° C.

Claims

1. A method for producing a copolyamide, comprising the following first and second steps: First step: a step of preparing a mixed liquid by heating ε-caprolactam (A) to a melting point of 69° C. or higher to melt it into a molten liquid, and adding solid adipic acid (B) to the molten liquid at 69° C. to 110° C. to mix ε-caprolactam (A) and adipic acid (B), in which the amount of ε-caprolactam (A) used per mole of adipic acid (B) is 1 to 20 moles. Second step: A step of mixing the mixture obtained in the first step with hexamethylenediamine (C) and then reacting them to obtain a copolymerized polyamide.

2. 2. The method for producing a copolyamide according to claim 1, wherein in the first step, the amount of ε-caprolactam (A) used is 2 to 15 moles per mole of adipic acid (B).

3. 3. The method for producing a copolyamide according to claim 1 or 2, wherein in the first step, the mixed liquid obtained has a color value of less than 0.

5.

4. The method for producing a copolyamide according to any one of claims 1 to 3, wherein in the second step, hexamethylenediamine (C) is added at 20 to 100°C.

5. The method for producing a copolyamide according to any one of claims 1 to 4, wherein in the second step, the reaction temperature between the mixed liquid obtained in the first step and hexamethylenediamine (C) is 180 to 300°C.

6. The method for producing a copolyamide according to any one of claims 1 to 5, wherein in the second step, the reaction pressure between the mixed liquid obtained in the first step and hexamethylenediamine (C) is 0.05 to 0.5 MPa.

7. The method for producing a copolyamide according to any one of claims 1 to 6, wherein in the second step, the amount of hexamethylenediamine (C) used is 0.01 to 100 moles per mole of adipic acid (B) used in the first step.

8. The method for producing a copolymerized polyamide according to any one of claims 1 to 7, wherein, in all the constitutional units of the copolymerized polyamide obtained in the second step, the proportion of constitutional units derived from ε-caprolactam (A) is 10 to 98 mol%, the proportion of constitutional units derived from adipic acid (B) is 1 to 45 mol%, and the proportion of constitutional units derived from hexamethylenediamine (C) is 1 to 45 mol%.

9. The method for producing the copolyamide according to any one of claims 1 to 8, further comprising the following third step: Third step: A step of withdrawing the copolymerized polyamide obtained in the second step from the vessel at regular intervals.

Citation Information

Patent Citations

  • Method for producing copolyamide

    JP1991111424A

  • Preparation of solution of dicarboxylic acid and copolyamide

    JP1997124542A

  • Continuous polymerization method for polyamide

    JP1998509760A

  • Method and apparatus for consecutively producing polyamide prepolymer and polyamide

    JP2010053359A

  • Method for continuously producing polyamide

    JP2010116575A