Method for producing crystallized glass article and crystallized glass article
A controlled heat treatment process with specific glass composition and slow cooling rates addresses the issue of dimensional changes in crystallized glass, achieving minimal shrinkage and stability for precision applications.
Patent Information
- Application Number
- JP2022515229
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-17
- Filing Date
- 2021-02-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-02-22
AI Technical Summary
Conventional crystallized glass exhibits significant dimensional changes over time, making it unsuitable for precision applications where minimal shrinkage is required.
A method involving a controlled heat treatment process is applied, including a temperature raising step above -80°C and below the nucleation temperature, followed by a slow cooling to 300°C at an average rate of 0.03°C/min, using a specific glass composition comprising SiO2, Al2O3, Li2O, MgO, ZnO, TiO2, ZrO2, P2O5, BaO, Na2O, and K2O, to minimize long-term shrinkage.
The method results in a crystallized glass article with minimal shrinkage over time, achieving a dimensional stability within -0.1 ppm to 0.1 ppm over 8000 hours, suitable for precision applications.
Smart Images

Figure 0007586171000003 
Figure 0007586171000004 
Figure 0007586171000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a crystallized glass article, a method for heat-treating a crystallized glass used in the method for producing a crystallized glass article, and a crystallized glass article. [Background technology]
[0002] 2. Description of the Related Art Crystallized glass has been used conventionally as a component for precision scales, a structural component for precision instruments, or a base material for precision mirrors.
[0003] In the following Patent Document 1, a heat treatment is performed for 24 hours at a temperature between 300°C and the glass transition point, and the difference in the thermal expansion coefficient (Δα) before and after the heat treatment is ±0.20×10 -7 / ℃, and the thermal expansion coefficient at -40℃ to 80℃ after heat treatment is 0±0.3×10 -7 / ° C. Patent Document 1 describes that such crystallized glass can suppress dimensional changes due to temperature changes even when exposed to an environment in which the temperature changes. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 017435 Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, when using crystallized glass for precision scale components, etc., it is required to reduce the amount of secular shrinkage. However, even the crystallized glass of Patent Document 1 has a problem that after a long period of time has passed after heat treatment, dimensional changes occur, and the amount of secular shrinkage cannot be sufficiently reduced.
[0006] The object of the present invention is to provide a method for producing a crystallized glass article, which makes it possible to obtain a crystallized glass article having a small amount of shrinkage over time, a method for heat-treating a crystallized glass used in the method for producing the crystallized glass article, and a crystallized glass article. [Means for solving the problem]
[0007] The manufacturing method of the crystallized glass article according to the present invention is characterized by comprising a crystallization step of crystallizing a crystallizable glass to obtain a crystallized glass, a temperature-raising step of raising the temperature of the crystallized glass from a temperature of 50°C or less to a temperature that is at least 80°C lower than the nucleation temperature of the crystallized glass and less than the nucleation temperature, and a temperature-lowering step of lowering the temperature to a temperature of 300°C or less at an average temperature-lowering rate of 0.03°C / min or less after the temperature-raising step.
[0008] In the present invention, the crystallizable glass preferably comprises glass containing, in mass %, 55.0% to 70.0% SiO2, 15.0% to 30.0% Al2O3, 2.0% to 6.0% Li2O, 0% to 2.0% MgO, 0% to 2.0% ZnO, 20% to 4.0% TiO, 20% to 4.0% ZrO, 50% to 4.0% P2O, 0% to 2.0% BaO, 0% to 4.0% Na2O, and 0% to 4.0% K2O.
[0009] The heat treatment method for crystallized glass according to the present invention is characterized by comprising a heating step of heating the crystallized glass from a temperature of 50°C or less to a temperature that is 80°C or more lower than the nucleation temperature of the crystallized glass and less than the nucleation temperature of the crystallized glass, and a cooling step of cooling the temperature to 300°C or less at an average cooling rate of 0.03°C / min or less after the heating step.
[0010] In a broad aspect, the crystallized glass article according to the present invention is characterized in that the dimensional shrinkage rate with time before and after 8000 hours at an atmospheric temperature of 20° C. is −0.1 ppm or more and 0.1 ppm or less.
[0011] In another broad aspect of the crystallized glass article according to the present invention, the crystallized glass article is characterized in that the dimensional shrinkage rate over time before and after 4800 hours at an atmospheric temperature of 20° C. is −0.13 ppm or more and 0.1 ppm or less.
[0012] In the present invention, the crystallized glass article is preferably made of glass containing, in mass %, 55.0% to 70.0% SiO2, 15.0% to 30.0% Al2O3, 2.0% to 6.0% Li2O, 0% to 2.0% MgO, 0% to 2.0% ZnO, 0% to 4.0% TiO2, 20% to 4.0% ZrO, 50% to 4.0% P2O, 0% to 2.0% BaO, 0% to 4.0% Na2O, and 0% to 4.0% K2O.
[0013] The crystallized glass article according to the present invention is preferably used as a component for a precision scale. Effect of the Invention
[0014] According to the present invention, it is possible to provide a method for producing a crystallized glass article, which makes it possible to obtain a crystallized glass article having a small amount of shrinkage over time, a method for heat-treating a crystallized glass used in the method for producing the crystallized glass article, and a crystallized glass article. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic perspective view showing a crystallized glass article according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing the relationship between the number of days elapsed from the date of initial measurement and the dimensional shrinkage rate of the samples prepared in Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments will be described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments.
[0017] [Method of manufacturing crystallized glass article and method of heat-treating crystallized glass] The method for producing a crystallized glass article of the present invention includes a crystallization step of crystallizing a crystallizable glass to obtain a crystallized glass, a temperature-raising step of raising the temperature of the crystallized glass from a temperature of 50°C or less to a temperature that is at least 80°C lower than the nucleation temperature of the crystallized glass and is lower than the nucleation temperature, and a temperature-lowering step of lowering the temperature to 300°C or less at an average temperature-lowering rate of 0.03°C / min or less after the temperature-raising step.
[0018] The heat treatment method of the crystallized glass of the present invention comprises a temperature increasing step of increasing the temperature of the crystallized glass from 50°C or less to a temperature that is 80°C or more lower than the nucleation temperature of the crystallized glass and less than the nucleation temperature of the crystallized glass, and a temperature decreasing step of decreasing the temperature to 300°C or less at an average temperature decreasing rate of 0.03°C / min or less after the temperature increasing step. Hereinafter, the temperature increasing step and the temperature decreasing step may be collectively referred to as a heat treatment step.
[0019] Therefore, in the manufacturing method of the crystallized glass article of the present invention, the crystallized glass prepared by crystallizing a crystallizable glass is heat-treated using the heat treatment method of the crystallized glass of the present invention, thereby obtaining the crystallized glass article of the present invention.
[0020] In addition, in the manufacturing method of the crystallized glass article of the present invention, the crystallized glass prepared by crystallizing the crystallized glass is heat-treated by the heat-treatment method of the crystallized glass of the present invention, so that the crystallized glass article that has little dimensional change and little secular shrinkage even after a long time can be obtained. This point can be explained as follows.
[0021] It is difficult for the remaining glass phase of the crystallized glass to have a completely compact structure by simply firing it through heat treatment without considering the cooling speed. This is thought to be because the fictive temperature of the remaining glass phase is high, so the structure is still in a state where it can change.
[0022] In contrast, as in the present invention, when the temperature is raised to a temperature lower than the nucleation temperature of crystallized glass-80°C or more and lower than the nucleation temperature, and then slowly cooled to a temperature lower than 300°C at an average cooling rate of 0.03°C / min or less, the fictive temperature can be sufficiently reduced. In the above-mentioned heat treatment, it is preferable to raise the temperature to a temperature lower than the nucleation temperature-70°C or more, more preferably to a temperature lower than the nucleation temperature-60°C or more, and even more preferably to a temperature lower than the nucleation temperature-50°C or more and lower than the nucleation temperature. Since the fictive temperature can be sufficiently reduced, it is considered that by performing heat treatment using the heat treatment method of the present invention, the proportion of the remaining glass phase that causes structural changes over a long period of time can be reduced, and the amount of secular shrinkage of the obtained crystallized glass article can be reduced.
[0023] It has been confirmed that the thermal expansion coefficient is slightly reduced when heat-treated by the heat treatment method of the present invention.Therefore, in order to make the thermal expansion coefficient approach 0 after heat-treated by the heat treatment method of the present invention, it is desirable to adjust the thermal expansion coefficient of the crystallized glass before heat treatment according to the present invention so that it is larger by the difference.The thermal expansion coefficient of the crystallized glass before heat treatment can be adjusted by the crystallization conditions of the crystallizable glass shown below.
[0024] Each step will be described in detail below.
[0025] (crystallization process) In the crystallization step, first, a crystallizable glass is prepared.
[0026] The crystallizable glass is preferably a glass containing, in mass %, SiO2 55.0%-70.0%, Al2O3 15.0%-30.0%, Li2O 2.0%-6.0%, MgO 0%-2.0%, ZnO 0%-2.0%, TiO2 0%-4.0%, ZrO2 0%-4.0%, P2O 50%-4.0%, BaO 0%-2.0%, Na2O 0%-4.0%, and K2O 0%-4.0%. When the crystallizable glass has such a composition, the thermal expansion coefficient of the obtained crystallized glass article can be made even closer to 0 even after the above-mentioned heat treatment. The reason why the above-mentioned glass composition is preferable will be explained below.
[0027] SiO2 is a component that forms the skeleton of glass and also constitutes crystals. The content of SiO2 is preferably 55.0% to 70.0%, more preferably 60.0% to 70.0%, in mass %. When the content of SiO2 is equal to or more than the lower limit, the thermal expansion coefficient of the obtained crystallized glass can be further reduced. On the other hand, when the content of SiO2 is equal to or less than the upper limit, the meltability of glass can be further improved, and more uniform glass can be obtained.
[0028] Al2O3 is a component that forms the skeleton of glass, similar to SiO2, and is also a component that constitutes crystals. The content of Al2O3 is, in mass%, preferably 15.0% to 30.0%, more preferably 17.0% to 28.0%. When the content of Al2O3 is equal to or more than the lower limit, the thermal expansion coefficient of the obtained crystallized glass can be further reduced. On the other hand, when the content of Al2O3 is equal to or less than the upper limit, the meltability of the glass can be further improved, and a more uniform glass can be obtained.
[0029] Li2O is a component that constitutes crystals and also a glass modifying component. The content of Li2O is preferably 2.0% to 6.0%, more preferably 2.0% to 5.5%, by mass %. When the content of Li2O is equal to or more than the lower limit, the desired crystals can be more easily precipitated. On the other hand, when the content of Li2O is equal to or less than the upper limit, the thermal expansion coefficient of the obtained crystallized glass can be further reduced.
[0030] MgO and ZnO are components that form a solid solution in the crystal. The contents of MgO and ZnO are, in mass%, preferably 0% to 2.0%, and more preferably 0% to 1.5%. When the contents of MgO and ZnO are equal to or less than the upper limit, the precipitation of heterogeneous crystals such as spinel and gahnite in addition to the β-quartz solid solution or β-eucryptite solid solution can be further suppressed, and damage due to temperature changes during use can be further suppressed.
[0031] TiO2 and ZrO2 are nucleation components for precipitating crystals. The contents of TiO2 and ZrO2 are, in mass%, preferably 0% to 4.0%, and more preferably 0% to 3.5%. When the contents of TiO2 and ZrO2 are not more than the upper limit values, the glass is more unlikely to devitrify when melted and formed, and more homogeneous glass can be obtained.
[0032] The total amount of TiO2 and ZrO2 is preferably 1.5% to 6.0% by mass. When the total amount of TiO2 and ZrO2 is equal to or more than the lower limit, the desired crystallinity can be obtained more easily, and the nucleation action can be made more sufficient. On the other hand, when the total amount of TiO2 and ZrO2 is equal to or less than the upper limit, the glass is less likely to devitrify when melted and formed, and a more homogeneous glass can be obtained.
[0033] P2O5 is a component that facilitates the nucleation of glass. The content of P2O5 is, in mass %, preferably 0% to 4.0%, more preferably 0% to 3.0%. When the content of P2O5 is equal to or less than the upper limit, the glass is less likely to undergo phase separation, and more homogeneous glass can be obtained.
[0034] BaO is a component that reduces the viscosity of glass and improves glass meltability and formability. The content of BaO is, in mass %, preferably 0% to 2.0%, more preferably 0% to 1.8%. When the content of BaO is equal to or less than the upper limit, the glass is more unlikely to devitrify when melted and formed, and more homogeneous glass can be obtained.
[0035] Na2O and K2O are components that reduce the viscosity of glass and improve the glass melting property and moldability. The content of Na2O and K2O is, in mass %, preferably 0% to 4.0%, more preferably 0% to 2.0%. When the content of Na2O and K2O is equal to or less than the upper limit, the thermal expansion coefficient of the obtained crystallized glass can be further reduced.
[0036] In addition, the glass may contain SrO, CaO, B2O3, etc., which are components that reduce the viscosity of the glass and improve the glass melting property and moldability, and SnO2, Cl, Sb2O3, As2O3, etc., which are fining agents, within a range that does not impair the specified properties. The total amount of these is preferably 10% or less by mass. When the total amount is equal to or less than the above upper limit, the thermal expansion coefficient can be further reduced, and the desired crystals can be more easily precipitated.
[0037] The crystallizable glass can be obtained, for example, by mixing glass raw materials so as to have the above-mentioned glass composition, melting the mixture at a temperature of 1550° C. to 1750° C., and then molding the mixture. The molding method is not particularly limited, but for example, a float method, a press method, a roll-out method, etc. can be used.
[0038] Next, the molded crystallizable glass is heat-treated, for example, at 600°C to 800°C for 0.1 to 10 hours to form crystal nuclei, and then further heat-treated at 800°C to 1000°C for 0.1 to 5 hours to crystallize, thereby obtaining crystallized glass. When the crystallizable glass has the above glass composition, Li2O·Al2O3·nSiO2-based crystals can be precipitated as the main crystals.
[0039] When the nucleation temperature is within the above range or the nucleation time is equal to or greater than the lower limit, the nucleation action can be made more sufficient, and crystals of the desired particle size can be more easily precipitated. On the other hand, when the nucleation time is equal to or less than the upper limit, the production cost can be reduced.
[0040] In addition, when the crystallization temperature and the crystallization time are each equal to or higher than the lower limit, the degree of crystallization can be further increased, and the thermal expansion coefficient of the obtained crystallized glass can be further increased. In addition, when the crystallization temperature is equal to or lower than the upper limit, the precipitated β-quartz solid solution or β-eucryptite solid solution can be made difficult to transition to β-spodumene solid solution. In addition, when the crystallization time is equal to or lower than the upper limit, the manufacturing cost can be reduced.
[0041] (Heat treatment process) In the heat treatment step, the temperature of the crystallized glass is first raised from a temperature of 50° C. or lower to a temperature that is 80° C. lower than the nucleation temperature of the crystallized glass and lower than the nucleation temperature.
[0042] When the temperature at which the temperature of the crystallized glass starts to rise is 50° C. or lower, or when the temperature after the temperature rise is equal to or higher than the nucleation temperature of the crystallized glass minus 80° C., the amount of secular shrinkage of the obtained crystallized glass article can be further reduced. Also, when the temperature after the temperature rise is lower than the nucleation temperature of the crystallized glass, the change in the structure of the crystalline phase can be suppressed.
[0043] From this viewpoint, the temperature at which the temperature of the crystallized glass starts to rise is preferably 10° C. or more and 30° C. or less. The temperature after the temperature rise is preferably the nucleation temperature of the crystallized glass minus 70° C. or more and the nucleation temperature of the crystallized glass minus 10° C. or less, more preferably the nucleation temperature of the crystallized glass minus 60° C. or more and the nucleation temperature of the crystallized glass minus 30° C. or less, and even more preferably the nucleation temperature of the crystallized glass minus 40° C. or less.
[0044] The temperature increase rate in the temperature increase step is not particularly limited, and can be, for example, 0.01° C. / min or more and 400° C. / min or less.
[0045] After the temperature is increased in the temperature increasing step, it is desirable to hold the temperature for a certain period of time until the temperature becomes uniform. The holding time at the temperature after the temperature increase varies depending on the size of the crystallized glass. For example, if the volume of the crystallized glass is 10 cm 3 ~100cm 3 In this case, the time can be from 10 to 120 minutes.
[0046] Next, after the temperature is increased in the temperature increasing step, the crystallized glass is cooled to a temperature of 300° C. or less at an average cooling rate of 0.03° C. / min or less.
[0047] When the average cooling rate is too fast or the temperature after cooling is too high, the crystallized glass cannot be cooled sufficiently, and the fictive temperature of the crystallized glass cannot be lowered sufficiently.When the average cooling rate is too slow or the temperature after cooling is too low, the productivity may decrease.
[0048] From this viewpoint, the average cooling rate of the crystallized glass after the heating step is preferably 0.001° C. / min or more, preferably 0.03° C. / min or less, more preferably 0.025° C. / min or less, even more preferably 0.02° C. / min or less, and particularly preferably 0.015° C. / min or less. The temperature after cooling is preferably 10° C. or more, and preferably 30° C. or less.
[0049] By subjecting the crystallized glass to heat treatment in this manner, the crystallized glass article of the present invention can be obtained.
[0050] [Crystalline glass article] FIG. 1 is a schematic perspective view showing a crystallized glass article according to one embodiment of the present invention.
[0051] 1, in this embodiment, the crystallized glass article 1 is in the form of a rectangular plate. The dimensions of the crystallized glass article 1 are not particularly limited, but may be, for example, a length of 1500 mm to 2000 mm, a width of 1000 mm to 1500 mm, and a height of 1 mm to 10 mm.
[0052] In addition, such a plate-shaped crystallized glass article 1 can be obtained, for example, by subjecting crystallizable glass formed by molding molten glass into a plate shape to the crystallization process and heat treatment process of the present invention. Alternatively, it may be obtained by subjecting crystallizable glass formed by molding molten glass into a lump shape to the crystallization process and heat treatment process of the present invention, and then cutting and polishing the crystallized glass into a plate shape. However, in the present invention, the shape of the crystallized glass article does not have to be plate-shaped and is not particularly limited.
[0053] In a broad aspect of the crystallized glass article according to the present invention, the dimensional shrinkage rate over time before and after 8000 hours at an atmospheric temperature of 20° C. is −0.1 ppm or more and 0.1 ppm or less. By setting the dimensional shrinkage rate over time before and after 8000 hours at an atmospheric temperature of 20° C. within the above range, the amount of secular shrinkage of the crystallized glass article can be reduced.
[0054] The dimensional shrinkage rate of the crystallized glass article with time before and after 8000 hours at an atmospheric temperature of 20° C. is preferably −0.05 ppm or more, and preferably 0.05 ppm or less.
[0055] In another broad aspect of the crystallized glass article according to the present invention, the dimensional shrinkage rate over time before and after 4800 hours at an atmospheric temperature of 20° C. is −0.13 ppm or more and 0.10 ppm or less. By setting the dimensional shrinkage rate over time before and after 4800 hours at an atmospheric temperature of 20° C. within the above range, the amount of secular shrinkage of the crystallized glass article can be reduced.
[0056] The dimensional shrinkage rate may be measured, for example, by measuring the dimension of any one side of the crystallized glass article. In the case of a crystallized glass article having a rectangular plate shape like the crystallized glass article 1, for example, the dimension of the long side may be measured.
[0057] In the present invention, the crystallized glass article preferably has at least one of a β-quartz solid solution and a β-eucryptite solid solution precipitated as the main crystal.
[0058] More specifically, the crystallized glass article is preferably glass containing, in mass %, 55.0% to 70.0% SiO2, 15.0% to 30.0% Al2O3, 2.0% to 6.0% Li2O, 0% to 2.0% MgO, 0% to 2.0% ZnO, 20% to 4.0% TiO, 20% to 4.0% ZrO, 50% to 4.0% PO, 0% to 2.0% BaO, 0% to 4.0% Na2O, and 0% to 4.0% K2O.
[0059] In this case, the thermal expansion coefficient of the crystallized glass article can be brought even closer to 0. The glass composition of the crystallized glass article can adopt the same preferable range as that of the above-mentioned crystallizable glass.
[0060] In the present invention, the average thermal expansion coefficient of the crystallized glass article at temperatures of -40°C or higher and 80°C or lower is preferably 1.0 x 10 -7 / ℃ or less, more preferably 0.5×10 -7 / °C or less, more preferably 0.2×10 -7 / °C or less, and particularly preferably 0.1 × 10 -7 / ° C. or less. In this case, the lens can be more suitably used for lenses of smart glasses or head mounted displays that are used in environments with large temperature changes.
[0061] Since the crystallized glass article of the present invention has a small amount of shrinkage over time, it can be suitably used as a component for precision scales, a structural component for precision instruments, a substrate for precision mirrors, a calibration substrate for imaging devices such as cameras, a mask for semiconductors, or a mask for devices that perform processing in a high-temperature environment.
[0062] The present invention will be described in more detail below with reference to specific examples. The present invention is not limited to the following examples, and can be modified as appropriate within the scope of the present invention.
[0063] Example 1 The raw materials were prepared and mixed to obtain a raw material batch with a composition of SiO2 65.6%, Al2O3 22.2%, Li2O 3.7%, MgO 0.7%, ZnO 0%, TiO2 2.0%, ZrO2 2.2%, P2O5 1.4%, BaO 1.2%, Na2O 0.4%, and K2O 0.3% SnO2 0.3% by mass. The raw material batch was melted at 1650°C for 16 hours and then rolled into a plate to obtain a crystallizable glass.
[0064] Next, the obtained crystallizable glass was subjected to a nucleation treatment at 790°C for 10 hours, and then to a crystallization treatment at a crystallization temperature of 900°C for 6 hours, and then cooled to 20°C to obtain a crystallized glass (nucleation temperature: 750°C). The nucleation temperature is the temperature at which crystal nuclei are generated in the crystallizable glass, and is determined according to the composition of the crystallizable glass.
[0065] The average thermal expansion coefficient of the obtained crystallized glass at temperatures between -40°C and 80°C is 0.4×10 -7 / ° C. The dimensions of the obtained crystallized glass were 100 mm in length, 500 mm in width, and 10 mm in height.
[0066] Next, the crystallized glass obtained by cooling to 20°C was heated to 700°C at a heating rate of 10°C / min and held at 700°C for 30 minutes. Next, the temperature was lowered from 700°C to 20°C at an average cooling rate of 0.01°C / min to obtain a crystallized glass article. The average thermal expansion coefficient of the obtained crystallized glass article at temperatures between -40°C and 80°C was 0.1×10 -7 / ℃.
[0067] Comparative Example 1 Crystallized glass prepared in the same manner as in Example 1 was used as it was without being subjected to heat treatment.
[0068] (evaluation) A block gauge was prepared from the crystallized glass article of Example 1 and the crystallized glass of Comparative Example 1, and was attached to a flat substrate, and its dimensions were measured using an optical interferometer for measuring block gauges owned by the National Institute of Advanced Industrial Science and Technology. A sample was prepared so that the initial measurement value of the dimension was 400 mm, and stored at 20°C for a predetermined period of time. The stored sample was measured for the amount of change with respect to the number of days elapsed since the initial measurement date at 20°C, and the dimensional shrinkage rate with respect to the number of days elapsed since the initial measurement date was obtained. The dimensional change was positive for expansion change and negative for shrinkage change. The results are shown in Table 1 and FIG. 2 below. The dimensional shrinkage rate before and after 357 days (8000 hours) at an atmospheric temperature of 20°C in Example 1 was -0.0995 ppm. The dimensional shrinkage rate before and after 206 days (4800 hours) at an atmospheric temperature of 20°C in Example 1 was -0.1023 ppm.
[0069] [Table 1]
[0070] From Table 1 and Figure 2, it can be seen that the crystallized glass article of Example 1, which was heat-treated by the heat treatment method of the present invention, has a smaller amount of shrinkage over time than the crystallized glass of Comparative Example 1, which was not heat-treated.
[0071] (Reference example 1) The raw materials were prepared and mixed to obtain a raw material batch with a composition of SiO2 65.6%, Al2O3 22.2%, Li2O 3.7%, MgO 0.7%, ZnO 0%, TiO2 2.0%, ZrO2 2.2%, P2O5 1.4%, BaO 1.2%, Na2O 0.4%, and K2O 0.3% SnO2 0.3% by mass. The raw material batch was melted at 1650°C for 16 hours and then rolled into a plate to obtain a crystallizable glass.
[0072] Next, the obtained crystallizable glass was subjected to a nucleation treatment at 790°C for 10 hours, followed by a crystallization treatment at a crystallization temperature of 900°C for 6 hours and then cooled to 20°C to obtain a crystallized glass (nucleation temperature: 750°C). The average thermal expansion coefficient of the obtained unheat-treated crystallized glass at temperatures between -40°C and 80°C was 0.4×10 -7 / ℃.
[0073] Except for using the crystallized glass thus produced, a heat treatment was carried out in the same manner as in Example 1 to produce a crystallized glass article.
[0074] (Reference examples 2~7) In Reference Examples 2 to 7, crystallized glass articles were produced in the same manner as in Reference Example 1, except that the average temperature decreasing rate during the heat treatment was changed from 0.01° C. / min to values as shown in Table 2 below.
[0075] The thermal expansion coefficients of Reference Examples 1 to 7 were measured at temperatures of -40° C. or higher and 80° C. or lower, and the differences in thermal expansion coefficients from those of crystallized glass that was not subjected to heat treatment were determined. The results are shown in Table 2 below.
[0076] [Table 2]
[0077] From Table 2, it can be seen that the thermal expansion coefficient of the crystallized glass article in Reference Example 1, in which the average cooling rate is 0.03°C / min or less, is smaller than that of the crystallized glass that has not been heat-treated (the difference from the thermal expansion coefficient of the unheat-treated product is large), whereas the thermal expansion coefficient of the crystallized glass articles in Reference Examples 2 to 4, in which the average cooling rate is greater than 0.03°C / min, is almost the same as that of the crystallized glass that has not been heat-treated. From this, it is considered that when the average cooling rate is greater than 0.03°C / min, the fictive temperature of the crystallized glass article cannot be sufficiently lowered, and the proportion of the remaining glass phase that causes structural changes over a long period of time cannot be sufficiently reduced. Therefore, it is considered that when the average cooling rate is greater than 0.03°C / min, the amount of aging shrinkage of the obtained crystallized glass article cannot be sufficiently reduced. Also, from Reference Examples 5 to 7, it can be seen that the same difference in thermal expansion coefficient as Reference Example 1 is obtained if the average cooling rate is 0.03°C / min or less and the temperature is lowered to 300°C or less. This confirms that if, after the heating step, the temperature is lowered to 300°C or lower at an average cooling rate of 0.03°C / min or less, the amount of secular shrinkage of the resulting crystallized glass article can be sufficiently reduced. [Explanation of symbols]
[0078] 1...Crystallized glass article
Claims
1. a crystallization step of crystallizing the crystallizable glass to obtain crystallized glass; A temperature raising step of raising the temperature of the crystallized glass from a temperature of 50° C. or less to a temperature of the nucleation temperature of the crystallized glass minus 80° C. or more and less than the nucleation temperature of the crystallized glass; a temperature decreasing step of decreasing the temperature to a temperature of 300° C. or less at an average temperature decreasing rate of 0.03° C. / min or less after the temperature increasing step; Equipped with The method for producing a crystallized glass article comprises the crystallizable glass having a glass composition, in mass %, of 55.0% to 70.0% SiO 2 , 15.0% to 30.0% Al 2 O 3 , 2.0% to 6.0% Li 2 O , 0% to 2.0% MgO , 0% to 2.0% ZnO , 0% to 4.0% TiO 2 , 0% to 4.0% ZrO 2 , 0% to 4.0% P 2 O 5 , 0% to 2.0% BaO , 0% to 4.0% Na 2 O , and 0% to 4.0% K 2 O .
2. A glass composition containing, by mass%, 55.0%-70.0% SiO2, 15.0%-30.0% Al2O3, 2.0%-6.0% Li2O, 0%-2.0% MgO, 0%-2.0% ZnO, 0%-2.0% TiO2, 0%-4.0% ZrO2, 0%-4.0% P2O5, 0%-2.0% BaO, 0%-4.0% Na2O, and 0%-4.0% K2O; A crystallized glass article having a dimensional shrinkage rate over time of -0.1 ppm or more and 0.1 ppm or less before and after 8000 hours at an atmospheric temperature of 20°C.
3. A glass composition containing, by mass%, 55.0% to 70.0% SiO2, 15.0% to 30.0% Al2O3, 2.0% to 6.0% Li2O, 0% to 2.0% MgO, 0% to 2.0% ZnO, 0% to 2.0% TiO2, 0% to 4.0% ZrO2, 0% to 4.0% P2O5, 0% to 2.0% BaO, 0% to 4.0% Na2O, and 0% to 4.0% K2O; A crystallized glass article having a dimensional shrinkage rate over time of -0.13 ppm or more and 0.1 ppm or less before and after 4800 hours at an atmospheric temperature of 20°C.
4. The crystallized glass article according to claim 2 or 3, which is used as a component for a precision scale.
Citation Information
Patent Citations
Opaque variable glass ceramic product and manufacture thereof
JP1993213629A
Glass ceramics and temperature compensating parts
JP2002104841A
Lithium oxide-alumina-silica-based crystalline glass and crystallized glass, and method of manufacturing the crystalline glass and the crystallized glass
JP2004075441A
Crystallized glass and its production method
JP2006056745A
Crystallized glass
WO2016017435A1