Resin composition and molded article

A resin composition with specific polyimide and aromatic resin ratios forms a microphase-separated structure, addressing moldability and dielectric property challenges, achieving low dielectric constants and thermal stability for high-frequency applications.

JP7586379B2Active Publication Date: 2024-11-19MITSUBISHI GAS CHEM CO INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024521110
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-12-05
Filing Date
2023-11-22
Publication Date
2024-11-19
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

Existing thermoplastic resin compositions, particularly those containing thermoplastic polyimide and other low dielectric resins, face challenges in moldability and film appearance during extrusion, limiting their application in high-frequency circuit boards and other components requiring low dielectric properties and good formability.

Method used

A resin composition is formulated with specific polyimide structural units in a predetermined ratio combined with an aromatic resin, achieving a microphase-separated structure and excellent low dielectric properties through a controlled mass ratio of components, enhancing film formability and thermal stability.

Benefits of technology

The resin composition achieves a dielectric constant of 3.0 or less and a dielectric loss tangent of 0.005 or less at 10 GHz, with a linear thermal expansion coefficient of 100 ppm/°C or less, suitable for high-frequency applications and improved film formability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586379000024
    Figure 0007586379000024
  • Figure 0007586379000025
    Figure 0007586379000025
  • Figure 0007586379000001
    Figure 0007586379000001
Patent Text Reader

Abstract

Provided are: a resin composition comprising (A) a polyimide resin and (B) a resin represented by specific formula (5) or an acid-modified product of the resin, in which the polyimide resin (A) contains a repeating constituent unit represented by formula (1) and a repeating constituent unit represented by formula (2), the ratio of the content of the repeating constituent unit represented by formula (1) relative to the total content of the repeating constituent unit represented by formula (1) and the repeating constituent unit represented by formula (2) is 20 to 70 mol%, and the ratio of the content mass of the component (B) relative to the total content mass of the components (A) and (B), i.e., [(B) / ((A)+(B))], is 0.50 or less; and a molded body comprising the resin composition. (R1 represents a bivalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure; R2 represents a bivalent linear aliphatic group having 5 to 16 carbon atoms; and X1 and X2 each independently represent a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a molded article. [Background technology]

[0002] Polyimide resins are useful engineering plastics that have high thermal stability, high strength, and high solvent resistance due to the rigidity of their molecular chains, resonance stabilization, and strong chemical bonds, and are used in a wide range of fields. Although polyimide resins have high heat resistance, they do not exhibit thermoplasticity and have the problem of low moldability. However, in recent years, polyimide resins with thermoplasticity have been reported. Thermoplastic polyimide resins have excellent moldability in addition to the heat resistance that polyimide resins inherently have. Therefore, thermoplastic polyimide resins can be used for molded products used in harsh environments where general-purpose thermoplastic resins such as nylon and polyester could not be used.

[0003] Polyimide resins are also known to exhibit low dielectric constants and low dielectric loss tangents (hereinafter, these are also collectively referred to as "low dielectric properties"). For example, Patent Document 1 discloses a film having low dielectric properties made of a thermoplastic polyimide resin, and describes that the film can be applied to high-frequency circuit boards, copper-clad laminates, etc. Patent Document 2 also discloses that a resin composition containing a predetermined liquid crystal polymer and a specific crystalline thermoplastic polyimide resin has excellent handleability when molten, is easy to melt-knead and extrude, and can achieve both a low dielectric constant and a low dielectric loss tangent. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 202150 [Patent Document 2] International Publication No. 2022 / 004471 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been an increasing demand for low dielectric materials as components related to the fifth generation mobile communication system (5G) and the sixth generation mobile communication system (6G), and from the viewpoint of obtaining high electrical properties, further reductions in the dielectric constant and dielectric loss tangent are also desired for organic materials. However, for example, in a thermoplastic resin composition using a thermoplastic polyimide in combination with another low dielectric resin as in the technology disclosed in Patent Document 2, although it is possible to produce a molded body by injection molding, the moldability is low in film molding by extrusion, and it may be difficult to produce a film with good appearance. An object of the present invention is to provide a resin composition having excellent low dielectric properties and good film formability, and a molded article containing the resin composition. [Means for solving the problem]

[0006] The present inventors have found that the above-mentioned problems can be solved by a resin composition containing a polyimide resin in which specific different polyimide structural units are combined in a specific ratio, and an aromatic resin having a specific structure, in a predetermined ratio. That is, the present invention relates to the following. [1] A resin composition comprising: a polyimide resin (A) containing a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content ratio of the repeating structural unit of the formula (1) to the total content of the repeating structural units of the formulas (1) and (2) is 20 to 70 mol %, and a resin represented by the following formula (5) or an acid-modified product thereof (B), wherein the ratio of the mass content of the component (B) to the total content of the components (A) and (B) [(B) / {(A)+(B)}] is 0.50 or less. [ka] (R1 is a divalent group having 6 to 22 carbon atoms containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms containing at least one aromatic ring.) [ka] (R 51 ~R 55 , and R 61 ~R 64 are each independently a hydrogen atom, a hydroxyl group, or an alkyl group having 1 to 4 carbon atoms; R 65 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. n is the number of repeating structural units and is a number of 10 or more. [2] The resin composition according to the above [1], wherein the total content of the component (A) and the component (B) in the resin composition is 50 mass% or more. [3] The resin composition according to the above [1] or [2], wherein the intrinsic viscosity of the component (B) measured in chloroform at 30° C. is 0.20 to 0.60 dL / g. [4] The resin composition according to any one of the above [1] to [3], wherein the resin composition is obtained by melt-kneading at a temperature exceeding the melting point of the component (A). [5] The resin composition according to any one of the above [1] to [4], wherein a pellet made of the resin composition has a microphase separation structure. [6] The resin composition according to any one of the above [1] to [5], which has a dielectric constant of 3.0 or less and a dielectric loss tangent of 0.005 or less at a measurement frequency of 10 GHz. [7] The resin composition according to any one of the above [1] to [6], wherein a molded article obtained by molding the resin composition has an absolute value of a coefficient of linear thermal expansion in the temperature range of 23 to 210°C, as measured in accordance with JIS K7197:2012, of 100 ppm / °C or less. [8] A molded article comprising the resin composition according to any one of the above [1] to [7]. [9] The molded article according to [8] above, wherein the molded article is a film. Effect of the Invention

[0007] According to the present invention, it is possible to provide a resin composition having excellent low dielectric properties and good film moldability, and a molded article containing the resin composition. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram showing a method for preparing a sample (ultrathin section) used for observation with a field emission scanning transmission electron microscope (FE-STEM). [Diagram 2] 1 is a micrograph of a cross section of the resin composition (pellet) of Example 5 cut in a direction perpendicular to the machine direction (MD), observed by FE-STEM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Resin composition] The resin composition of the present invention contains a polyimide resin (A) containing a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content ratio of the repeating structural unit of the formula (1) to the total content of the repeating structural units of the formula (1) and the repeating structural units of the formula (2) is 20 to 70 mol %, and a resin represented by the following formula (5) or an acid-modified product thereof (B), wherein the ratio of the content of the component (B) to the total content of the components (A) and (B) [(B) / {(A)+(B)}] is 0.50 or less. [ka] (R1 is a divalent group having 6 to 22 carbon atoms containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms containing at least one aromatic ring.) [ka] (R 51 ~R 55 , and R61 ~R 64 are each independently a hydrogen atom, a hydroxyl group, or an alkyl group having 1 to 4 carbon atoms; R 65 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. n is the number of repeating structural units and is a number of 10 or more.

[0010] The resin composition of the present invention contains the polyimide resin (A) obtained by combining specific different polyimide structural units in the above-mentioned specific ratio, and the resin represented by the formula (5) or an acid-modified product thereof (B) in a predetermined ratio, and thus has excellent low dielectric properties and good film formability. The reason why the above-mentioned effects are obtained in the present invention is not clear, but is thought to be as follows. Both components (A) and (B) are thermoplastic resins having low dielectric properties, with component (A) being a crystalline thermoplastic resin and component (B) being an amorphous thermoplastic resin. By using components (A) and (B), a resin composition having excellent low dielectric properties can be obtained. However, crystalline thermoplastic resins and amorphous thermoplastic resins are usually difficult to make compatible with each other, and although it is possible to produce molded articles by injection molding from resin compositions obtained by compounding these, there are cases in which the moldability is poor when molded into films by extrusion, making it difficult to produce films with good appearance. In the present invention, by using component (A) having excellent moldability as a crystalline thermoplastic resin and by using components (A) and (B) in a specific ratio, it becomes possible for components (A) and (B) to have a micro- to nano-level finely dispersed structure (microphase separation structure). In particular, by setting the mass ratio [(B) / {(A)+(B)}] to 0.50 or less, when components (A) and (B) form a sea-island structure as a microphase separation structure, component (A) is more likely to be present on the sea side. This suppresses discoloration and other problems resulting from oxidative deterioration of component (B), which is believed to have improved film moldability by extrusion while maintaining low dielectric properties.

[0011] In addition, the resin composition of the present invention can be a resin composition having high crystallinity derived from component (A) by having the mass ratio [(B) / {(A)+(B)}] be 0.50 or less. As a result, the obtained resin composition and molded article are also excellent in, for example, solder reflow resistance. In this specification, the crystallinity of the resin composition can be determined using the heat of fusion as an index. Furthermore, the resin composition of the present invention allows the production of molded articles that have a low coefficient of linear thermal expansion and excellent dimensional stability.

[0012] <Polyimide resin (A)> The polyimide resin (A) used in the present invention contains a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), and the content of the repeating structural unit of the formula (1) relative to the total of the repeating structural units of the formula (1) and the repeating structural units of the formula (2) is 20 to 70 mol %. [ka] (R1 is a divalent group having 6 to 22 carbon atoms containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms containing at least one aromatic ring.)

[0013] The polyimide resin (A) used in the present invention is a thermoplastic resin, and is preferably in the form of powder or pellets. Thermoplastic polyimide resins are distinguished from polyimide resins that have no glass transition temperature (Tg), and are formed by molding a polyimide precursor such as polyamic acid and then closing the imide ring, or polyimide resins that decompose at a temperature lower than the glass transition temperature.

[0014] The repeating unit of formula (1) is described in detail below. R1 is a divalent group containing at least one alicyclic hydrocarbon structure and having 6 to 22 carbon atoms. Here, the alicyclic hydrocarbon structure means a ring derived from an alicyclic hydrocarbon compound, and the alicyclic hydrocarbon compound may be saturated or unsaturated, and may be monocyclic or polycyclic. Examples of the alicyclic hydrocarbon structure include, but are not limited to, a cycloalkane ring such as a cyclohexane ring, a cycloalkene ring such as a cyclohexene ring, a bicycloalkane ring such as a norbornane ring, and a bicycloalkene ring such as norbornene. Among these, a cycloalkane ring is preferred, a cycloalkane ring having 4 to 7 carbon atoms is more preferred, and a cyclohexane ring is even more preferred. R1 has 6 to 22 carbon atoms, and preferably 8 to 17 carbon atoms. R1 contains at least one alicyclic hydrocarbon structure, and preferably contains 1 to 3 alicyclic hydrocarbon structures.

[0015] R1 is preferably a divalent group represented by the following formula (R1-1) or (R1-2). [ka] (m 11 and m 12 are each independently an integer of 0 to 2, preferably 0 or 1. 13 ~m 15 are each independently an integer of 0 to 2, preferably 0 or 1.

[0016] R1 is particularly preferably a divalent group represented by the following formula (R1-3). [ka] In the divalent group represented by the above formula (R1-3), the positional relationship of the two methylene groups to the cyclohexane ring may be either cis or trans, and the ratio of cis to trans may be any value.

[0017] X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a single ring or a condensed ring, and examples thereof include, but are not limited to, a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred. X1 has 6 to 22 carbon atoms, and preferably 6 to 18 carbon atoms. X1 contains at least one aromatic ring, and preferably contains 1 to 3 aromatic rings.

[0018] X1 is preferably a tetravalent group represented by any one of the following formulas (X-1) to (X-4). [ka] (R 11 ~R 18 are each independently an alkyl group having 1 to 4 carbon atoms. 11 ~p 13 are each independently an integer of 0 to 2, and preferably 0. 14 , p 15 , p 16 and p 18 are each independently an integer of 0 to 3, and preferably 0. 17 is an integer of 0 to 4, preferably 0. 11 ~L 13 are each independently a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms. Since X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, R 12 , R 13 , p 12 and p 13 is selected so that the tetravalent group represented by formula (X-2) has 10 to 22 carbon atoms. Similarly, L in formula (X-3) 11 , R 14 , R 15 , p 14 and p 15is selected so that the number of carbon atoms of the tetravalent group represented by formula (X-3) is in the range of 12 to 22, and L in formula (X-4) 12 , L 13 , R 16 , R 17 , R 18 , p 16 , p 17 and p 18 is selected so that the tetravalent group represented by formula (X-4) has 18 to 22 carbon atoms.

[0019] X1 is particularly preferably a tetravalent group represented by the following formula (X-5) or (X-6). [ka]

[0020] Next, the repeating unit of formula (2) will be described in detail below. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms, preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms. Here, the chain aliphatic group means a group derived from a chain aliphatic compound, and the chain aliphatic compound may be saturated or unsaturated, may be linear or branched, and may contain a heteroatom such as an oxygen atom. R2 is preferably an alkylene group having 5 to 16 carbon atoms, more preferably an alkylene group having 6 to 14 carbon atoms, still more preferably an alkylene group having 7 to 12 carbon atoms, and particularly preferably an alkylene group having 8 to 10 carbon atoms. The alkylene group may be a linear alkylene group or a branched alkylene group, but is preferably a linear alkylene group. R2 is preferably at least one selected from the group consisting of an octamethylene group and a decamethylene group, and particularly preferably an octamethylene group.

[0021] Another preferred embodiment of R2 is a divalent chain aliphatic group containing an ether group and having 5 to 16 carbon atoms. The number of carbon atoms is preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10. Among these, a divalent group represented by the following formula (R2-1) or (R2-2) is preferred. [ka] (m 21 and m 22 are each independently an integer of 1 to 15, preferably an integer of 1 to 13, more preferably an integer of 1 to 11, and even more preferably an integer of 1 to 9. 23 ~m 25 are each independently an integer of 1 to 14, preferably 1 to 12, more preferably 1 to 10, and even more preferably 1 to 8. In addition, since R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms (preferably having 6 to 14 carbon atoms, more preferably having 7 to 12 carbon atoms, and further preferably having 8 to 10 carbon atoms), m in formula (R2-1) 21 and m 22 is selected so that the carbon number of the divalent group represented by formula (R2-1) is in the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). That is, m 21 +m 22 is 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and further preferably 8 to 10). Similarly, m in formula (R2-2) 23 ~m 25 is selected so that the carbon number of the divalent group represented by formula (R2-2) is in the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). That is, m 23 +m 24 +m 25 has 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and further preferably 8 to 10 carbon atoms).

[0022] X2 is defined the same as X1 in formula (1), and the preferred embodiments are also the same.

[0023] The content ratio of the repeating structural unit of formula (1) to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2) is 20 to 70 mol%. When the content ratio of the repeating structural unit of formula (1) is within the above range, it becomes possible to sufficiently crystallize the polyimide resin even in a general injection molding cycle. If the content ratio is less than 20 mol%, the moldability decreases, and if it exceeds 70 mol%, the crystallinity decreases, and therefore the heat resistance decreases. The content ratio of the repeating structural unit of formula (1) relative to the total of the repeating structural units of formula (1) and formula (2) is preferably 65 mol % or less, more preferably 60 mol % or less, and even more preferably 50 mol % or less, from the viewpoint of achieving high crystallinity. In particular, the content ratio of the repeating structural unit of formula (1) to the total of the repeating structural units of formula (1) and formula (2) is preferably 20 mol % or more and less than 40 mol %. Within this range, the crystallinity of the polyimide resin (A) becomes high, and a resin composition having better heat resistance can be obtained. From the viewpoint of molding processability, the above content is preferably 25 mol% or more, more preferably 30 mol% or more, and even more preferably 32 mol% or more, and from the viewpoint of expressing high crystallinity, it is even more preferably 35 mol% or less.

[0024] The total content of the repeating units of formula (1) and formula (2) relative to all repeating units constituting the polyimide resin (A) is preferably 50 to 100 mol %, more preferably 75 to 100 mol %, even more preferably 80 to 100 mol %, and still more preferably 85 to 100 mol %.

[0025] The polyimide resin (A) may further contain a repeating unit of the following formula (3). In this case, the content ratio of the repeating unit of the formula (3) to the total of the repeating unit of the formula (1) and the repeating unit of the formula (2) is preferably 25 mol% or less. On the other hand, the lower limit is not particularly limited, and it is sufficient that it is more than 0 mol%. From the viewpoint of improving heat resistance, the content ratio is preferably 5 mol % or more, more preferably 10 mol % or more, while from the viewpoint of maintaining crystallinity, the content ratio is preferably 20 mol % or less, more preferably 15 mol % or less. [ka] (R3 is a divalent group having 6 to 22 carbon atoms containing at least one aromatic ring. X3 is a tetravalent group having 6 to 22 carbon atoms containing at least one aromatic ring.)

[0026] R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a single ring or a condensed ring, and examples thereof include, but are not limited to, a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred. R3 has 6 to 22 carbon atoms, and preferably 6 to 18 carbon atoms. R3 contains at least one aromatic ring, and preferably contains 1 to 3 aromatic rings. The aromatic ring may have a monovalent or divalent electron-withdrawing group bonded thereto. Examples of the monovalent electron-withdrawing group include a nitro group, a cyano group, a p-toluenesulfonyl group, halogens, halogenated alkyl groups, a phenyl group, and an acyl group. Examples of the divalent electron-withdrawing group include a fluorinated alkylene group (e.g., -C(CF3)2-, -(CF2) p In addition to halogenated alkylene groups such as - (where p is an integer from 1 to 10), examples include -CO-, -SO2-, -SO-, -CONH-, -COO-, and the like.

[0027] R3 is preferably a divalent group represented by the following formula (R3-1) or (R3-2). [ka] (m 31 and m 32 are each independently an integer of 0 to 2, preferably 0 or 1. 33 and m 34 are each independently an integer of 0 to 2, preferably 0 or 1. 21 , R 22 , and R 23 are each independently an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or an alkynyl group having 2 to 4 carbon atoms. 21 , p 22 and p 23 is an integer of 0 to 4, preferably 0. 21 is a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms. Since R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, m in formula (R3-1) 31 , m 32 , R 21 and p 21 is selected so that the divalent group represented by formula (R3-1) has 6 to 22 carbon atoms. Similarly, L in formula (R3-2) 21 , m 33 , m 34 , R 22 , R 23 , p 22 and p 23 is selected so that the divalent group represented by formula (R3-2) has 12 to 22 carbon atoms.

[0028] X3 is defined the same as X1 in formula (1), and the preferred embodiments are also the same.

[0029] The polyimide resin (A) may further contain a repeating unit represented by the following formula (4). [ka] (R4 is -SO2- or -Si(R x )(R y ) O-containing divalent group, R x and R y each independently represents a chain aliphatic group having 1 to 3 carbon atoms or a phenyl group. X4 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. X4 is defined the same as X1 in formula (1), and the preferred embodiments are also the same.

[0030] The terminal structure of the polyimide resin (A) is not particularly limited, but it is preferable that the polyimide resin (A) has a chain aliphatic group having 5 to 14 carbon atoms at the terminal. The chain aliphatic group may be saturated or unsaturated, and may be linear or branched. When the polyimide resin (A) has the specific group at its terminal, a resin composition having excellent heat aging resistance can be obtained. Examples of the saturated chain aliphatic group having 5 to 14 carbon atoms include an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, a lauryl group, an n-tridecyl group, an n-tetradecyl group, an isopentyl group, a neopentyl group, a 2-methylpentyl group, a 2-methylhexyl group, a 2-ethylpentyl group, a 3-ethylpentyl group, an isooctyl group, a 2-ethylhexyl group, a 3-ethylhexyl group, an isononyl group, a 2-ethyloctyl group, an isodecyl group, an isododecyl group, an isotridecyl group, and an isotetradecyl group. Examples of the unsaturated chain aliphatic group having 5 to 14 carbon atoms include a 1-pentenyl group, a 2-pentenyl group, a 1-hexenyl group, a 2-hexenyl group, a 1-heptenyl group, a 2-heptenyl group, a 1-octenyl group, a 2-octenyl group, a nonenyl group, a decenyl group, a dodecenyl group, a tridecenyl group, and a tetradecenyl group. Among them, the chain aliphatic group is preferably a saturated chain aliphatic group, and more preferably a saturated linear chain aliphatic group. From the viewpoint of obtaining heat aging resistance, the chain aliphatic group preferably has 6 or more carbon atoms, more preferably 7 or more carbon atoms, even more preferably 8 or more carbon atoms, and preferably has 12 or less carbon atoms, more preferably 10 or less carbon atoms, and even more preferably has 9 or less carbon atoms. The chain aliphatic group may be of only one type, or of two or more types. The chain aliphatic group is particularly preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, a 2-ethylhexyl group, an n-nonyl group, an isononyl group, an n-decyl group, and an isodecyl group, further preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, a 2-ethylhexyl group, an n-nonyl group, and an isononyl group, and most preferably at least one selected from the group consisting of an n-octyl group, an isooctyl group, and a 2-ethylhexyl group. From the viewpoint of heat aging resistance, the polyimide resin (A) preferably has only chain aliphatic groups having 5 to 14 carbon atoms at its terminals in addition to terminal amino groups and terminal carboxy groups. When the polyimide resin (A) has groups other than the above at its terminals, the content thereof is preferably 10 mol % or less, more preferably 5 mol % or less, based on the chain aliphatic groups having 5 to 14 carbon atoms.

[0031] From the viewpoint of exhibiting excellent heat aging resistance, the content of the chain aliphatic group having 5 to 14 carbon atoms in the polyimide resin (A) is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, and even more preferably 0.2 mol% or more, based on 100 mol% of the total of all repeating units constituting the polyimide resin (A). In order to ensure a sufficient molecular weight and obtain good mechanical properties, the content of the chain aliphatic group having 5 to 14 carbon atoms in the polyimide resin (A) is preferably 10 mol% or less, more preferably 6 mol% or less, and even more preferably 3.5 mol% or less, based on 100 mol% of the total of all repeating units constituting the polyimide resin (A). The content of the chain aliphatic group having 5 to 14 carbon atoms in the polyimide resin (A) can be determined by depolymerizing the polyimide resin (A).

[0032] The polyimide resin (A) preferably has a melting point of 360° C. or less and a glass transition temperature of 150° C. or more. From the viewpoint of heat resistance, the melting point of the polyimide resin (A) is more preferably 280° C. or more, and even more preferably 290° C. or more, and from the viewpoint of high moldability, it is preferably 345° C. or less, more preferably 340° C. or less, and even more preferably 335° C. or less. From the viewpoint of heat resistance, the glass transition temperature of the polyimide resin (A) is more preferably 160° C. or more, and even more preferably 170° C. or more, and from the viewpoint of high moldability, it is preferably 250° C. or less, more preferably 230° C. or less, and even more preferably 200° C. or less. The melting point and glass transition temperature of the polyimide resin (A) can both be measured by a differential scanning calorimeter. From the viewpoint of improving crystallinity, heat resistance, mechanical strength, and chemical resistance, the polyimide resin (A) preferably has a heat value of a crystallization exothermic peak (hereinafter, simply referred to as "crystallization heat value") of 5.0 mJ / mg or more, more preferably 10.0 mJ / mg or more, and even more preferably 17.0 mJ / mg or more, as measured by a differential scanning calorimeter, when the polyimide resin (A) is melted and then cooled at a temperature drop rate of 20°C / min. The upper limit of the crystallization heat value is not particularly limited, but is usually 45.0 mJ / mg or less. The melting point, glass transition temperature and heat of crystallization of the polyimide resin (A) can be specifically measured by the method described in the Examples.

[0033] The logarithmic viscosity of a 0.5% by mass solution of polyimide resin (A) in concentrated sulfuric acid at 30°C is preferably in the range of 0.2 to 2.0 dL / g, more preferably 0.3 to 1.8 dL / g. If the logarithmic viscosity is 0.2 dL / g or more, sufficient mechanical strength is obtained when the resulting resin composition is molded into a molded article, and if it is 2.0 dL / g or less, moldability and handleability are good. The logarithmic viscosity μ is calculated from the following formula by measuring the flow time of concentrated sulfuric acid and the above polyimide resin solution at 30°C using a Cannon-Fenske viscometer. μ=ln(ts / t0) / C t0: Time for concentrated sulfuric acid to flow ts: Flow time of polyimide resin solution C: 0.5 (g / dL)

[0034] The weight average molecular weight Mw of the polyimide resin (A) is preferably in the range of 10,000 to 150,000, more preferably 15,000 to 100,000, even more preferably 20,000 to 80,000, still more preferably 30,000 to 70,000, and even more preferably 35,000 to 65,000. If the weight average molecular weight Mw of the polyimide resin (A) is 10,000 or more, the mechanical strength of the obtained molded article becomes good, if it is 40,000 or more, the stability of the mechanical strength becomes good, and if it is 150,000 or less, the moldability becomes good. The weight average molecular weight Mw of the polyimide resin (A) can be measured by gel permeation chromatography (GPC) using polymethyl methacrylate (PMMA) as a standard sample.

[0035] (Production method of polyimide resin (A)) The polyimide resin (A) can be produced by reacting a tetracarboxylic acid component with a diamine component, the tetracarboxylic acid component containing at least one aromatic ring-containing tetracarboxylic acid and / or its derivative, and the diamine component containing at least one alicyclic hydrocarbon structure-containing diamine and a chain aliphatic diamine.

[0036] The tetracarboxylic acid containing at least one aromatic ring is preferably a compound in which four carboxy groups are directly bonded to the aromatic ring, and may contain an alkyl group in the structure. The tetracarboxylic acid preferably has 6 to 26 carbon atoms. As the tetracarboxylic acid, pyromellitic acid, 2,3,5,6-toluenetetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, etc. are preferable. Among these, pyromellitic acid is more preferable.

[0037] The derivative of tetracarboxylic acid containing at least one aromatic ring may be an anhydride or an alkyl ester of tetracarboxylic acid containing at least one aromatic ring. The tetracarboxylic acid derivative preferably has 6 to 38 carbon atoms. The anhydride of tetracarboxylic acid may be pyromellitic monoanhydride, pyromellitic dianhydride, 2,3,5,6-toluenetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, etc. Examples of the alkyl ester of tetracarboxylic acid include dimethyl pyromellitic acid, diethyl pyromellitic acid, dipropyl pyromellitic acid, diisopropyl pyromellitic acid, dimethyl 2,3,5,6-toluenetetracarboxylate, dimethyl 3,3',4,4'-diphenylsulfonetetracarboxylate, dimethyl 3,3',4,4'-benzophenonetetracarboxylate, dimethyl 3,3',4,4'-biphenyltetracarboxylate, dimethyl 1,4,5,8-naphthalenetetracarboxylate, etc. In the alkyl ester of tetracarboxylic acid, the number of carbon atoms of the alkyl group is preferably 1 to 3.

[0038] As the tetracarboxylic acid and / or derivative thereof containing at least one aromatic ring, at least one compound selected from the above may be used alone, or two or more compounds may be used in combination.

[0039] The number of carbon atoms of the diamine containing at least one alicyclic hydrocarbon structure is preferably 6 to 22, and examples thereof include 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, 4,4'-methylenebis(2-methylcyclohexylamine), carvonediamine, limonenediamine, isophoronediamine, norbornanediamine, bis(aminomethyl)tricyclo[5.2.1.0]diamine, and the like.2,6 ]decane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylpropane, etc. are preferred. These compounds may be used alone, or two or more compounds selected from these may be used in combination. Of these, 1,3-bis(aminomethyl)cyclohexane is preferably used. Diamines containing an alicyclic hydrocarbon structure generally have structural isomers, but the ratio of cis isomers / trans isomers is not limited.

[0040] The chain aliphatic diamine may be linear or branched, and has preferably 5 to 16 carbon atoms, more preferably 6 to 14, and further preferably 7 to 12. In addition, when the number of carbon atoms in the chain portion is 5 to 16, an ether bond may be contained therein. Preferred examples of the chain aliphatic diamine include 1,5-pentamethylenediamine, 2-methylpentane-1,5-diamine, 3-methylpentane-1,5-diamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine, and 2,2'-(ethylenedioxy)bis(ethyleneamine). The chain aliphatic diamine may be used alone or in combination. Among these, a chain aliphatic diamine having 8 to 10 carbon atoms is preferably used, and in particular, at least one selected from the group consisting of 1,8-octamethylenediamine and 1,10-decamethylenediamine is preferably used.

[0041] When producing the polyimide resin (A), the molar ratio of the amount of the diamine containing at least one alicyclic hydrocarbon structure to the total amount of the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine is preferably 20 to 70 mol %. The molar amount is preferably 25 mol % or more, more preferably 30 mol % or more, and even more preferably 32 mol % or more, and from the viewpoint of expressing high crystallinity, is preferably 60 mol % or less, more preferably 50 mol % or less, even more preferably less than 40 mol %, and even more preferably 35 mol % or less.

[0042] The diamine component may contain a diamine containing at least one aromatic ring. The carbon number of the diamine containing at least one aromatic ring is preferably 6 to 22, and examples thereof include orthoxylylenediamine, metaxylylenediamine, paraxylylenediamine, 1,2-diethynylbenzenediamine, 1,3-diethynylbenzenediamine, 1,4-diethynylbenzenediamine, 1,2-diaminobenzene, 1,3-diaminobenzene, 1,4-diaminobenzene, 4,4'-diaminodiphenylether, 3,4'-diaminodiphenylether, 4,4'-diaminodiphenylmethane, α,α'-bis(4-aminophenyl)1,4-diisopropylbenzene, α,α'-bis(3-aminophenyl)-1,4-diisopropylbenzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,6-diaminonaphthalene, and 1,5-diaminonaphthalene.

[0043] In the above, the molar ratio of the amount of the diamine containing at least one aromatic ring to the total amount of the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine is preferably 25 mol% or less. On the other hand, the lower limit is not particularly limited, and it is sufficient if it is more than 0 mol%. From the viewpoint of improving heat resistance, the molar ratio is preferably 5 mol % or more, more preferably 10 mol % or more, while from the viewpoint of maintaining crystallinity, the molar ratio is preferably 20 mol % or less, more preferably 15 mol % or less. Moreover, from the viewpoint of reducing coloration of the polyimide resin (A), the molar ratio is preferably 12 mol % or less, more preferably 10 mol % or less, even more preferably 5 mol % or less, and still more preferably 0 mol %.

[0044] When producing the polyimide resin (A), the ratio of the amount of the tetracarboxylic acid component to the amount of the diamine component is preferably 0.9 to 1.1 moles of the diamine component per mole of the tetracarboxylic acid component.

[0045] When producing the polyimide resin (A), a terminal blocking agent may be mixed in addition to the tetracarboxylic acid component and the diamine component. The terminal blocking agent is preferably at least one selected from the group consisting of monoamines and dicarboxylic acids. The amount of the terminal blocking agent used may be any amount that allows a desired amount of terminal groups to be introduced into the polyimide resin (A), and is preferably 0.0001 to 0.1 mol, more preferably 0.001 to 0.06 mol, and even more preferably 0.002 to 0.035 mol, per mol of the tetracarboxylic acid and / or its derivative. Among them, as the end-capping agent, a monoamine end-capping agent is preferable, and from the viewpoint of improving heat aging resistance by introducing the above-mentioned chain aliphatic group having 5 to 14 carbon atoms to the end of the polyimide resin (A), a monoamine having a chain aliphatic group having 5 to 14 carbon atoms is more preferable, and a monoamine having a saturated linear aliphatic group having 5 to 14 carbon atoms is even more preferable. The end-capping agent is particularly preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, isononylamine, n-decylamine, and isodecylamine, more preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, and isononylamine, and most preferably at least one selected from the group consisting of n-octylamine, isooctylamine, and 2-ethylhexylamine.

[0046] As the polymerization method for producing the polyimide resin (A), a known polymerization method can be applied, and the method described in WO 2016 / 147996 can be used.

[0047] <Resin represented by formula (5) or acid-modified product thereof (B)> The resin composition of the present invention contains a polyimide resin (A) and a resin represented by the following formula (5) or an acid-modified product thereof (B). [ka] (R 51 ~R 55 , and R 61 ~R 64 are each independently a hydrogen atom, a hydroxyl group, or an alkyl group having 1 to 4 carbon atoms; R 65 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. n is the number of repeating structural units and is a number of 10 or more.

[0048] In formula (5), R 51 ~R 55 , and R 61 ~R 65 The alkyl group having 1 to 4 carbon atoms in may be either linear or branched, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. Among these, a methyl group, an ethyl group, an n-propyl group, or an isopropyl group is preferred, and a methyl group is more preferred.

[0049] In formula (5), R 51 , R 53 , R 61 , and R 63 is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or a methyl group, and even more preferably a hydrogen atom. R 52 , R 54 , R 62 , and R 64is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group. R 65 is preferably a hydrogen atom.

[0050] In formula (5), n is a number of 10 or more, and more preferably 20 or more.

[0051] The resin represented by the formula (5) is preferably poly(2,6-dimethyl-1,4-phenylene ether), which is a resin represented by the following formula (5-1). [ka] (In the formula, n is the same as above.)

[0052] The acid-modified product of the resin represented by the formula (5) includes a resin obtained by modifying the resin represented by the formula (5) with a carboxylic acid or a carboxylic acid derivative. As the carboxylic acid or the carboxylic acid derivative, an unsaturated carboxylic acid or its derivative is preferable from the viewpoint of reactivity with the resin represented by the formula (5). Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, citraconic acid, sorbic acid, mesaconic acid, angelic acid, etc. Examples of the derivatives of the unsaturated carboxylic acid include acid anhydrides, esters, amides, imides, and metal salts, and among these, acid anhydrides are preferred. Among the above, from the viewpoints of obtaining low dielectric properties, improving film formability, and availability, the acid-modified product of the resin represented by the formula (5) is preferably a resin obtained by modifying the resin represented by the formula (5) with maleic acid or a maleic acid derivative (a maleic acid-modified product of the resin represented by the formula (5)), and more preferably a resin obtained by modifying the resin represented by the formula (5) with maleic anhydride.

[0053] Examples of the maleic acid modified resin represented by the formula (5) include resins having structures represented by the following formula (5-2) and / or formula (5-3). [ka] [ka] (In the formula, R 51 ~R 55 , R 61 , R 63 , R 64 , R 65 , and n are the same as above.)

[0054] The acid modification rate of the acid modified product of the resin represented by the formula (5) is preferably 0.01 to 5.0 mass%, more preferably 0.05 to 3.0 mass%, even more preferably 0.1 to 2.0 mass%, and even more preferably 0.2 to 1.0 mass%, from the viewpoints of obtaining low dielectric properties, improving film moldability, and availability. The acid modification rate here refers to the content (mass%) of structures derived from an acid in the acid modified product. For example, when the acid modified product of the resin represented by the formula (5) is a resin obtained by modifying the resin represented by the formula (5) with maleic anhydride, the acid modification rate refers to the content (mass%) of structures derived from maleic anhydride in the acid modified product.

[0055] From the viewpoints of obtaining low dielectric properties, improving film formability, and availability, component (B) is preferably a resin represented by the formula (5) or a maleic acid modified product thereof, more preferably a resin represented by the formula (5), and even more preferably a resin represented by the formula (5-1), that is, poly(2,6-dimethyl-1,4-phenylene ether).

[0056] The intrinsic viscosity of component (B) measured in chloroform at 30°C is preferably 0.20 to 0.60 dL / g, more preferably 0.30 to 0.50 dL / g, and even more preferably 0.30 to 0.45 dL / g, from the viewpoints of obtaining low dielectric properties and improving film formability.

[0057] As the resin represented by the formula (5), commercially available products such as "PX100F" (poly(2,6-dimethyl-1,4-phenylene ether), Tg = 207°C, intrinsic viscosity at 30°C measured in chloroform = 0.37 dL / g) and "PX100L" (poly(2,6-dimethyl-1,4-phenylene ether), Tg = 210°C, intrinsic viscosity at 30°C measured in chloroform = 0.47 dL / g) manufactured by Polyxylenol Singapore Pte. Ltd. can also be used. Commercially available products of the resin represented by the formula (5) modified with maleic anhydride (maleic acid modified product) include "Iupiace PME-80" (maleic anhydride modification rate: 0.38% by mass) manufactured by Mitsubishi Engineering Plastics Corporation.

[0058] <Content> The ratio of the mass content of component (B) to the total mass content of components (A) and (B) in the resin composition [(B) / {(A)+(B)}] is 0.50 or less, preferably 0.40 or less, more preferably 0.30 or less, even more preferably 0.20 or less, and even more preferably 0.15 or less, from the viewpoint of improving film moldability. The lower limit is more than 0, and from the viewpoint of obtaining low dielectric properties, it is preferably 0.005 or more, more preferably 0.01 or more, even more preferably 0.05 or more, and even more preferably 0.10 or more.

[0059] The content of component (A) in the resin composition is not particularly limited as long as it is within a range in which the ratio [(B) / {(A)+(B)}] is 0.50 or less. From the viewpoint of obtaining low dielectric properties and improving film formability, the content of component (A) is preferably 50 to 99.9 mass%, more preferably 60 to 99.5 mass%, even more preferably 70 to 99.5 mass%, still more preferably 80 to 99 mass%, even more preferably 80 to 98 mass%, and even more preferably 80 to 95 mass%.

[0060] The content of component (B) in the resin composition is not particularly limited as long as it is in the range in which the above-mentioned [(B) / {(A)+(B)}] is 0.50 or less. From the viewpoint of obtaining low dielectric properties and improving film moldability, the content is preferably 0.1 to 50 mass%, more preferably 0.5 to 40 mass%, even more preferably 0.5 to 30 mass%, still more preferably 1 to 20 mass%, even more preferably 2 to 20 mass%, and even more preferably 5 to 20 mass%.

[0061] <Additives> The resin composition of the present invention may contain additives such as fillers, reinforcing fibers, matting agents, plasticizers, antistatic agents, coloring inhibitors, antigelling agents, colorants, sliding property improvers, antioxidants, conductive agents, resin modifiers, and compatibilizers, as necessary. When the above-mentioned additives are used, there are no particular limitations on the amount of the additives used. From the viewpoint of exerting the effects of the additives while maintaining low dielectric properties and film formability, the amount of the additives used in the resin composition is usually 50% by mass or less, preferably 0.0001 to 30% by mass, more preferably 0.001 to 15% by mass, and even more preferably 0.01 to 10% by mass.

[0062] In addition, the resin composition of the present invention may contain resins other than component (A) and component (B) to the extent that the properties of the composition are not impaired. As the resin, a highly heat-resistant thermoplastic resin is preferable, and examples thereof include polyamide resins, polyester resins, polyimide resins other than polyimide resin (A), polycarbonate resins, polyetherimide resins, polyamideimide resins, polyphenylene etherimide resins, polyphenylene sulfide resins, polysulfone resins, polyethersulfone resins, polyarylate resins, liquid crystal polymers, polyetheretherketone resins, polyetherketone resins, polyetherketoneketone resins, polyetheretherketoneketone resins, polybenzimidazole resins, and fluorine-based resins. Examples of fluorine-based resins include polytetrafluoroethylene, perfluoroalkylvinylether copolymers, tetrafluoroethylene-ethylene copolymers, polyvinylidene fluoride, and polychlorotrifluoroethylene. Among these, from the viewpoints of heat resistance, moldability, strength, and solvent resistance, one or more types selected from the group consisting of polyetherimide resins, polyphenylene sulfide resins, and polyether ether ketone resins are preferred, from the viewpoint of low water absorption, liquid crystal polymers are preferred, and from the viewpoint of obtaining high flame retardancy, one or more types selected from the group consisting of polyphenylene sulfide resins, polytetrafluoroethylene, and perfluoroalkyl vinyl ether copolymers are preferred. When resins other than the components (A) and (B) are used in combination, there are no particular limitations on the amount of such resins added, so long as the properties of the resin composition are not impaired.

[0063] However, from the viewpoint of obtaining the effects of the present invention, the total content of component (A) and component (B) in the resin composition of the present invention is preferably 30 mass% or more, more preferably 40 mass% or more, even more preferably 50 mass% or more, still more preferably 70 mass% or more, still more preferably 80 mass% or more, still more preferably 90 mass% or more, still more preferably 95 mass% or more, and is 100 mass% or less.

[0064] From the viewpoint of forming a pellet, the resin composition of the present invention preferably does not contain a solvent. Specifically, the content of the solvent in the resin composition is preferably 5% by mass or less, more preferably 1% by mass or less, and further preferably 0.1% by mass or less.

[0065] <Form of Resin Composition> The resin composition of the present invention may take any form, but from the viewpoint of obtaining excellent low dielectric properties by forming a microphase separation structure described later, it is preferably one obtained by melt kneading at a temperature exceeding the melting point of component (A), and more preferably a pellet obtained by melt kneading at a temperature exceeding the melting point of component (A). That is, it is preferable that component (A) in the resin composition of the present invention has been subjected to a heat history, and the resin composition is distinguished from a resin composition containing component (A) in a powder state. Since the resin composition of the present invention has thermoplasticity, for example, after component (A), component (B), and various optional components as required are added and dry blended, or after component (B) and optional components are separately fed from a location other than the feeding of component (A) to the extruder, the mixture is melt-kneaded in the extruder to extrude strands, and the strands are cut to form pellets. Moreover, the pellets can be introduced into various molding machines and thermoformed by the method described below to easily produce molded articles having the desired shapes.

[0066] From the viewpoint of obtaining low dielectric properties, it is preferable that the pellets made of the resin composition of the present invention and the molded article obtained by molding the resin composition have a microphase-separated structure. The microphase-separated structure is a phase-separated structure at the micro to nano level formed by phase separation between component (A) and component (B), and may be a sea-island structure or a co-continuous structure, but a sea-island structure is preferable. In the sea-island structure, either component may form the "sea" depending on the mass ratio of component (A) and component (B) in the pellet, but from the viewpoint of obtaining excellent film formability, it is preferable that component (A) forms the "sea". Whether or not the pellet or molded article has a microphase-separated structure can be determined by observing the surface or cross section of the pellet or molded article with a scanning transmission electron microscope (STEM).

[0067] The heat of fusion (Hm) of the resin composition of the present invention is preferably 10 mJ / mg or more, more preferably 12 mJ / mg or more, even more preferably 15 mJ / mg or more, and even more preferably 18 mJ / mg or more, from the viewpoint of improving crystallinity, film moldability, and the solder reflow resistance of the obtained molded article. The upper limit is not particularly limited, but is usually 45.0 mJ / mg or less. The heat of fusion (Hm) can be specifically measured by the method described in the Examples.

[0068] [Molded body] The present invention provides a molded article comprising the resin composition. The shape of the molded article is not particularly limited, and examples thereof include sheets, films, strands, filaments, etc. These may be intermediate parts of industrial products or final products. From the viewpoint of effectively exerting the effect of the present invention, the molded article of the present invention is preferably a film. The thickness of the film is not particularly limited, but the thickness of the film produced by extrusion molding is usually 500 μm or less, preferably 200 μm or less, more preferably less than 100 μm, even more preferably 80 μm or less, and even more preferably 60 μm or less. The lower limit of the thickness of the film is usually 5 μm or more, preferably 10 μm or more. In this specification, the term "film thickness" refers to the average thickness of the film. The film-shaped molded product includes not only a resin film, but also a resin layer constituting a multilayer laminate, a coating layer, and the like.

[0069] Since the resin composition of the present invention has thermoplasticity, the molded article of the present invention can be easily produced by thermoforming. Thermoforming methods include injection molding, extrusion molding, inflation molding, blow molding, hot press molding, vacuum molding, compressed air molding, laser molding, welding, and adhesion, and any molding method that involves a thermal melting step can be used for molding. When a film-shaped molded product is produced, extrusion molding is preferred, and molding can be performed, for example, in a temperature range of 290°C or higher and 400°C or lower, preferably 290°C or higher and 360°C or lower.

[0070] As a method for producing a molded article, for example, the pellets produced by the above-mentioned method are dried, and then the pellets are introduced into various molding machines and thermoformed to produce a molded article having a desired shape.

[0071] <Low dielectric properties> The resin composition and molded article of the present invention have low dielectric properties, and can achieve, for example, a dielectric constant of 3.0 or less and a dielectric loss tangent of 0.005 or less at a measurement frequency of 10 GHz. The dielectric constant is preferably 2.90 or less, more preferably 2.85 or less, even more preferably 2.70 or less, even more preferably 2.50 or less, and even more preferably 2.40 or less, and the dielectric loss tangent is preferably 0.004 or less, more preferably 0.003 or less. The dielectric constant and dielectric loss tangent can be specifically measured by the method described in the Examples.

[0072] <Coefficient of thermal expansion (CTE)> The resin composition and molded article of the present invention exhibit a low CTE. For example, the absolute value of the coefficient of linear thermal expansion of the molded article obtained by molding the resin composition in the temperature range of 23 to 210°C, measured in accordance with JIS K7197:2012, can be preferably 100 ppm / °C or less, more preferably 90 ppm / °C or less, even more preferably 85 ppm / °C or less, still more preferably 80 ppm / °C or less, still more preferably 75 ppm / °C or less, and still more preferably 70 ppm / °C or less. In addition, since the CTE value varies when the molded article is stretched, the molded article used for the CTE measurement is preferably a non-stretched molded article, and more preferably an injection molded article. In the case of an injection molded article, there is a flow direction (MD) and a direction perpendicular thereto (TD), and the CTE may differ between MD and TD. In this case, it is preferable that the average of the absolute values ​​of the linear thermal expansion coefficients in MD and TD is within the above range. Here, the average of the absolute values ​​of the linear thermal expansion coefficients in MD and TD means {(absolute value of linear thermal expansion coefficient in MD) + (absolute value of linear thermal expansion coefficient in TD)} / 2. Furthermore, from the viewpoint of dimensional stability, the absolute value of the coefficient of linear thermal expansion in at least one of MD and TD, preferably in MD, is preferably 55 ppm / °C or less, more preferably 50 ppm / °C or less. The coefficient of linear thermal expansion of the molded body is a value measured in compression mode by thermomechanical analysis (TMA method), and specifically, can be measured by the method described in the examples.

[0073] <Application> The resin composition and molded article of the present invention are useful in a wide range of applications requiring a low dielectric constant and a low dielectric dissipation factor, for example, 5G or sixth-generation mobile communication system (6G) related members using a frequency band of 70G to 300GHz (smartphones, flexible printed circuit boards, metal foil laminates such as copper-clad laminates, antennas, antenna substrates, etc.), various antennas other than those mentioned above (microwave antennas, millimeter wave antennas, waveguide slot antennas, horn antennas, lens antennas, printed antennas, triplate antennas, microstrip antennas, patch antennas, etc.), various antenna substrates (antenna substrates for 77GHz vehicle-mounted millimeter wave radar, antenna substrates for terahertz wave radar, antenna substrates for aircraft radar, antenna substrates for caterpillar-type special vehicles, antenna substrates for WiGig, etc.), wire coating materials (low dielectric wire coating materials, etc.), bonding sheets, insulating films, raw materials for carbon fiber reinforced plastics (CFRP), high frequency circuit boards, printed wiring boards, chip-on-film (COF) flexible Substrates, multilayer laminates, LED-mounted substrates, industrial robot substrates, communication substrates for household robots, semiconductor element materials, wafers for high-frequency devices, Wi-fi chips, wireless communication devices, transmission lines (coaxial lines, strip lines, microstrip lines, coplanar lines, parallel lines, etc.), bearing coatings, heat-insulating shafts, trays, various belts (seamless belts, etc.), heat-resistant low-dielectric tapes, heat-resistant low-dielectric tubes, various sensors (touch sensors, etc.), various radars (automotive radars, aerospace radars, etc.), radomes (radar domes), optical communication modules (TOSA / ROSA), 8k-TV cables, mobile terminals or digital home appliances (tablet terminals, notebook PCs, thin TVs, retractable TVs, digital cameras, smart glasses, smart watches, etc.), base stations (macrocell base stations, small cell base stations, C-RAN base stations, etc.), drones (commercial drones, long-distance drones, etc.), surveillance cameras, indoor or outdoor servers, artificial satellites, communication equipment for space stations, etc. EXAMPLES

[0074] The present invention will now be described in more detail with reference to examples, but the present invention is not limited thereto. In addition, various measurements and evaluations in each Production Example and Example were carried out as follows.

[0075] <Infrared spectroscopy (IR measurement)> IR measurements of polyimide resins were carried out using a JIR-WINSPEC50 manufactured by JEOL Ltd.

[0076] <Logarithmic viscosity μ> The polyimide resin was dried at 190 to 200°C for 2 hours, and then 0.100 g of the polyimide resin was dissolved in 20 mL of concentrated sulfuric acid (96%, Kanto Chemical Co., Ltd.) to prepare a polyimide resin solution for measurement, and measurement was performed at 30°C using a Cannon-Fenske viscometer. The logarithmic viscosity μ was calculated by the following formula. μ=ln[(ts / t0) / C] t0: Time for concentrated sulfuric acid to flow ts: Flow time of polyimide resin solution C: 0.5 g / dL

[0077] <Melting point, glass transition temperature, crystallization temperature, heat of fusion, heat of crystallization> The melting point Tm, glass transition temperature Tg, crystallization temperature Tc, heat of fusion Hm, and heat of crystallization Hc of the resin used alone or the resin composition obtained in each example were measured using a differential scanning calorimeter ("DSC-25" manufactured by TA Instruments). In measuring the crystallization temperature Tc, a resin powder was used as a measurement sample for the polyimide resin, and a pellet was used as a measurement sample for the crystalline thermoplastic resin composition. The measurement sample was subjected to the following thermal history under a nitrogen atmosphere: first heating (heating rate 10°C / min), then cooling (cooling rate 20°C / min), then second heating (heating rate 10°C / min). The melting point Tm was determined by reading the peak top value of the endothermic peak observed during the second heating. The glass transition temperature Tg was determined by reading the value observed during the second heating. The crystallization temperature Tc was determined by reading the peak top value of the exothermic peak observed during cooling. For Tm, Tg, and Tc, when multiple peaks were observed, the peak top value of each peak was read. The heat of fusion Hm (mJ / mg) was calculated from the area of ​​the heat of fusion peak (endothermic peak) observed near the melting point when the measurement sample was heated to a temperature above the melting point at a heating rate of 10°C / min to melt, cooled at a heating rate of 20°C / min, and melted again at a heating rate of 10°C / min. The heat of crystallization Hc (mJ / mg) was calculated from the area of ​​the heat of crystallization peak observed when the measurement sample was heated to a temperature above the melting point at a heating rate of 10°C / min to melt, and then cooled at a heating rate of 20°C / min.

[0078] <Crystallization half time> The half-crystallization time of the polyimide resin was measured using a differential scanning calorimeter (DSC-6220, manufactured by SII NanoTechnology, Inc.). The polyimide resin was kept at 420°C for 10 minutes in a nitrogen atmosphere until it was completely melted, and then rapidly cooled at a rate of 70°C / min. The time taken from the appearance of the observed crystallization peak until it reached its peak top was calculated. In Table 1, when the half crystallization time was 20 seconds or less, it is indicated as "<20."

[0079] <Weight average molecular weight> The weight average molecular weight (Mw) of the polyimide resin was measured under the following conditions using a gel permeation chromatography (GPC) measuring device "Shodex GPC-101" manufactured by Showa Denko K.K. Column: Shodex HFIP-806M Mobile phase solvent: hexafluoroisopropanol (HFIP) containing 2 mM sodium trifluoroacetate Column temperature: 40℃ Mobile phase flow rate: 1.0mL / min Sample concentration: Approximately 0.1% by mass Detector: IR detector Injection amount: 100μm Calibration curve: Standard PMMA

[0080] <Heat distortion temperature (HDT)> The resin used in each example alone or the resin composition obtained in each example was used to manufacture a molded body of 80 mm x 10 mm x 4 mm thick by the injection molding method described below, and used for the measurement. The measurements were performed flatwise in accordance with JIS K7191-1,2:2015. Specifically, the heat distortion temperature was measured using the HDT tester "Auto-HDT3D-2" (manufactured by Toyo Seiki Seisakusho Co., Ltd.) under the conditions of a support distance of 64 mm, a load of 1.80 MPa, and a heating rate of 120°C / hour.

[0081] <Film formability> The resin alone used in each example, or pellets of the resin composition obtained in each example, were fed into a Labo Plastomill T-die extrusion molding device (manufactured by Toyo Seiki Seisakusho Co., Ltd., extruder Φ20 mm, L / D=25, T-die die width 150 mm, lip width 0.4 mm), and extrusion molding was performed for about 15 minutes under conditions of an extrusion temperature of 310 to 350°C and a target thickness of 50 μm to produce a film. The film during extrusion molding was visually observed, and the film moldability was evaluated according to the following criteria. A: There are no bumps or gunk on the film surface. B: There are some bumps and eye gunk on the film surface, but it is within the acceptable range. C: Numerous bumps and gunk have appeared on the film surface.

[0082] <Dielectric constant, dielectric loss tangent> Using the resin alone or the resin composition obtained in each example, a film having a thickness of 50 to 60 μm was produced by the method described in the "film moldability" evaluation and used for the measurement. Using a "PNA network analyzer N5222B" manufactured by Keyside Technology Co., Ltd. and a cavity resonator "CP531" manufactured by Kanto Electronics Application Development Co., Ltd., the dielectric constant and dielectric loss tangent were measured at a temperature of 23 ° C, humidity of 50%, and a measurement frequency of 10 GHz by the cavity resonator perturbation method in accordance with IEC 62810. The measured values ​​were the average values ​​of n = 2. The film was conditioned at a temperature of 23 ° C and humidity of 50% for 24 hours or more, and then immediately used for the measurement.

[0083] <Coefficient of thermal expansion (CTE)> CTE was measured in accordance with JIS K7197:2012. Using the resin alone or pellets of the resin composition obtained in each example, an injection molded article of JIS K 7139:2009 multipurpose test piece type A1 was produced by the method described below. A test piece measuring 5 mm x 4 mm x 10 mm was cut from the parallel part of this injection molded article and used for the measurement. Using the above test piece as a measurement sample, thermomechanical analysis (TMA) was performed using a thermomechanical analyzer "TMA7100C" manufactured by Hitachi High-Tech Science Corporation, in a nitrogen gas flow (150 mL / min), compression mode, a load of 49 mN, and a temperature increase rate of 5°C / min, with the temperature increased from 23 to 300°C. The TMA measurement was performed in the flow direction (MD) of the injection molded body and in the direction perpendicular thereto (TD), and the CTE was calculated from the measured values ​​at 23 to 210°C. In addition, (CTE in MD + CTE in TD) / 2 was taken as the average value of the CTE in MD and TD.

[0084] Production Example 1 (Production of Polyimide Resin 1) 500g of 2-(2-methoxyethoxy)ethanol (manufactured by Nippon Nyukazai Co., Ltd.) and 218.12g (1.00mol) of pyromellitic dianhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were introduced into a 2L separable flask equipped with a Dean-Stark apparatus, a Liebig condenser, a thermocouple, and four paddle blades, and after nitrogen flow, the mixture was stirred at 150 rpm to obtain a uniform suspension solution. Meanwhile, using a 500mL beaker, 49.79g (0.35mol) of 1,3-bis(aminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd., cis / trans ratio = 7 / 3) and 93.77g (0.65mol) of 1,8-octamethylenediamine (manufactured by Kanto Chemical Co., Ltd.) were dissolved in 250g of 2-(2-methoxyethoxy)ethanol to prepare a mixed diamine solution. This mixed diamine solution was gradually added using a plunger pump. Although the drop generates heat, the internal temperature was adjusted to be within 40 to 80°C. The mixed diamine solution was dropped under nitrogen flow conditions, and the stirring blade rotation speed was 250 rpm. After the drop was completed, 130 g of 2-(2-methoxyethoxy)ethanol and 1.284 g (0.010 mol) of n-octylamine (Kanto Chemical Co., Ltd.), which is a terminal blocking agent, were added and further stirred. At this stage, a pale yellow polyamic acid solution was obtained. Next, the stirring speed was set to 200 rpm, and the polyamic acid solution in the 2L separable flask was heated to 190°C. During the temperature increase, precipitation of polyimide resin powder and dehydration due to imidization were confirmed when the liquid temperature was between 120 and 140°C. After holding at 190°C for 30 minutes, the solution was allowed to cool to room temperature and filtered. The obtained polyimide resin powder was washed with 300 g of 2-(2-methoxyethoxy)ethanol and 300 g of methanol, filtered, and then dried in a dryer at 180°C for 10 hours to obtain 317 g of crystalline thermoplastic polyimide resin 1 (hereinafter simply referred to as "polyimide resin 1") powder. The IR spectrum of polyimide resin 1 was measured, and ν(C=O) 1768, 1697 (cm -1The inherent viscosity was 1.30 dL / g, Tm was 323°C, Tg was 184°C, Tc was 266°C, heat of fusion was 21.0 mJ / mg, heat of crystallization was 20.3 mJ / mg, half-crystallization time was less than 20 seconds, and Mw was 55,000.

[0085] Production Example 2 (Production of Polyimide Resin 2) 769g of 2-(2-methoxyethoxy)ethanol (manufactured by Nippon Nyukazai Co., Ltd.) and 174.50g (0.80mol) of pyromellitic dianhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were introduced into a 2L separable flask equipped with a Dean-Stark apparatus, a Liebig condenser, a thermocouple, and a four-paddle blade, and after nitrogen flow, the mixture was stirred at 150 rpm to obtain a uniform suspension solution. Meanwhile, using a 500mL beaker, 22.76g (0.16mol) of 1,3-bis(aminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd., cis / trans ratio = 7 / 3) and 92.33g (0.64mol) of 1,8-octamethylenediamine (manufactured by Kanto Chemical Co., Ltd.) were dissolved in 250g of 2-(2-methoxyethoxy)ethanol to prepare a mixed diamine solution. This mixed diamine solution was gradually added using a plunger pump. Although the drop generates heat, the internal temperature was adjusted to be within 40 to 80°C. The mixed diamine solution was dropped under nitrogen flow conditions, and the stirring blade rotation speed was 250 rpm. After the drop was completed, 10 g of 2-(2-methoxyethoxy)ethanol and 1.027 g (0.008 mol) of n-octylamine (Kanto Chemical Co., Ltd.), which is a terminal blocking agent, were added and further stirred. At this stage, a pale yellow polyamic acid solution was obtained. Next, the stirring speed was set to 200 rpm, and the polyamic acid solution in the 2L separable flask was heated to 185°C. During the temperature increase, precipitation of polyimide resin powder and dehydration due to imidization were confirmed when the liquid temperature was between 120 and 140°C. After holding at 185°C for 30 minutes, the solution was allowed to cool to room temperature and filtered. The obtained polyimide resin powder was washed with 600 g of methanol, filtered, and then dried in a dryer at 185°C for 10 hours to obtain 256 g of crystalline thermoplastic polyimide resin 2 (hereinafter simply referred to as "polyimide resin 2") powder. Polyimide resin 2 had a Tm of 344° C., a Tg of 166° C., a Tc of 299° C., a heat of fusion of 40 mJ / mg, a heat of crystallization of 35 mJ / mg, and a Mw of 36,000.

[0086] The compositions and evaluation results of the polyimide resins obtained in Production Examples 1 and 2 are shown in Table 1. The mole percentages of the tetracarboxylic acid component and the diamine component in Table 1 are values ​​calculated from the amounts of each component charged when the polyimide resin is produced.

[0087] [Table 1]

[0088] The abbreviations in Table 1 are as follows. PMDA; Pyromellitic dianhydride 1,3-BAC; 1,3-bis(aminomethyl)cyclohexane OMDA; 1,8-octamethylenediamine n-OcA; n-Octylamine

[0089] Example 1 (Preparation and Evaluation of Resin Composition) The powder of polyimide resin 1 obtained in Production Example 1 and the powder of poly(2,6-dimethyl-1,4-phenylene ether) (Polyxylenol Singapore Pte. Ltd. "PX100F", Tg = 207 ° C, intrinsic viscosity at 30 ° C measured in chloroform = 0.37 dL / g) as component (B) were dry blended in the ratio shown in Table 2, and then melt-kneaded and extruded using a co-rotating twin-screw kneading extruder (Parker Corporation "HK-25D", screw diameter 25 mm Φ, L / D = 41) under conditions of barrel temperature 330 to 340 ° C and screw rotation speed 120 rpm. The strand extruded from the extruder was air-cooled and then pelletized with a pelletizer (Hoshi Plastics Co., Ltd. "Fan Cutter FC-Mini-4 / N"). The obtained pellets were dried at 80 ° C for 12 hours and then used for injection molding. Using an injection molding machine (FANUC Corporation's "ROBOSHOT α-S30iA"), injection molding was performed at a barrel temperature of 360°C, a mold temperature of 180°C, and a molding cycle of 67 seconds to produce injection molded bodies of the specified shape to be used in the above evaluation. Further, a film was produced by the method described in the above-mentioned evaluation of "film formability". The pellets, injection molded articles, and films obtained were subjected to various evaluations by the methods described above. The results are shown in Table 2.

[0090] Examples 2 to 4, Comparative Examples 2 to 4 The powder of polyimide resin 1 obtained in Production Example 1 and the powder of poly(2,6-dimethyl-1,4-phenylene ether) "PX100F" were used in the ratio shown in Table 2, and injection molding was performed in the range of a molding cycle of 52 to 77 seconds (Example 2: 52 seconds, Example 3: 65 seconds, Example 4: 67 seconds, Comparative Example 2: 67 seconds, Comparative Example 3: 72 seconds, Comparative Example 4: 77 seconds). Except for this, pellets, injection molded articles, and films were produced in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 2.

[0091] Comparative Example 1 The powder of polyimide resin 1 obtained in Production Example 1 was melt-kneaded and extruded using a Labo Plastomill (manufactured by Toyo Seiki Seisakusho Co., Ltd.) at a barrel temperature of 360°C and a screw rotation speed of 150 rpm. The strand extruded from the extruder was air-cooled and then pelletized using a pelletizer (Hoshi Plastics Co., Ltd.'s "Fan Cutter FC-Mini-4 / N"). The obtained pellets were dried at 150°C for 12 hours and then used for injection molding. Using an injection molding machine ("ROBOSHOT α-S30iA" manufactured by Fanuc Corporation), injection molding was performed at a barrel temperature of 350°C, a mold temperature of 200°C, and a molding cycle of 50 seconds to produce injection molded bodies of a specified shape to be used in the above evaluation (HDT measurement). Further, a film was produced by the method described in the above-mentioned evaluation of "film formability". The pellets, injection molded articles, and films obtained were subjected to various evaluations by the methods described above. The results are shown in Table 2.

[0092] [Table 2]

[0093] Example 5, Comparative Examples 5 to 7 Pellets, injection molded articles, and films were prepared and various evaluations were carried out in the same manner as described above, except that in Example 1, "PX100L" manufactured by Polyxylenol Singapore Pte. Ltd. was used in place of "PX100F" as poly(2,6-dimethyl-1,4-phenylene ether) in the proportions shown in Table 3. The results are shown in Table 3.

[0094] Comparative Example 8 In Comparative Example 1, polyimide resin 2 obtained in Production Example 2 was used instead of polyimide resin 1, and the barrel temperature during injection molding was changed to 360° C., and the mold temperature was changed to 180° C., and pellets, injection molded products, and films were produced and evaluated in the same manner as described above. The results are shown in Table 3.

[0095] Example 6 Pellets, injection molded articles, and films were prepared in the same manner as in Example 1, except that the polyimide resin 2 obtained in Production Example 2 and "PX100L" manufactured by Polyxylenol Singapore Pte. Ltd. as poly(2,6-dimethyl-1,4-phenylene ether) were used in the ratios shown in Table 3. The results are shown in Table 3.

[0096] Example 7 In Example 5, instead of "PX100L", maleic anhydride modified polyphenylene ether ("Iupiace PME-80" manufactured by Mitsubishi Engineering Plastics Corporation, maleic anhydride modification rate: 0.38% by mass) was used, and the barrel temperature during injection molding was changed to 360°C, and the mold temperature was changed to 160°C. In the same manner as above, pellets, injection molded products, and films were produced and various evaluations were performed. The results are shown in Table 3.

[0097] [Table 3]

[0098] Details of each component shown in Tables 2 and 3 are as follows. <Component (A)> Polyimide resin 1: crystalline thermoplastic polyimide resin 1 obtained in Production Example 1 Polyimide resin 2: crystalline thermoplastic polyimide resin 2 obtained in Production Example 2 <Ingredient (B)> PX100F: Poly(2,6-dimethyl-1,4-phenylene ether), "PX100F" manufactured by Polyxylenol Singapore Pte. Ltd., Tg = 207°C, intrinsic viscosity measured in chloroform at 30°C = 0.37 dL / g PX100L: Poly(2,6-dimethyl-1,4-phenylene ether), "PX100L" manufactured by Polyxylenol Singapore Pte. Ltd., Tg = 210°C, intrinsic viscosity measured in chloroform at 30°C = 0.47 dL / g PME80: Maleic anhydride modified polyphenylene ether, "Iupiace PME-80" manufactured by Mitsubishi Engineering Plastics Corporation, maleic anhydride modification rate 0.38 mass%

[0099] As shown in Tables 2 to 3, the resin compositions of the present examples have good film formability. Furthermore, the molded articles made of the resin compositions of Examples 1 to 5 and 7 exhibited lower dielectric properties and lower CTE than the molded article of Comparative Example 1 made of component (A), and in particular, exhibited a lower CTE in MD. The molded article made of the resin composition of Example 6 also exhibited lower dielectric properties than the molded article of Comparative Example 8 made of component (A). Moreover, it is understood that the resin compositions of Examples 1 to 5 and 7 have higher heats of fusion Hm than those of Comparative Examples 2 to 7, that is, have higher crystallinity.

[0100] Furthermore, the morphology of the pellets obtained in Example 5 was confirmed by the following method. The pellet obtained in Example 5 was cut using an ultramicrotome (Leica Microsystems' "EM UC7") in a direction perpendicular to the flow direction (MD) of the pellet as shown in Figure 1 (i.e., so that the TD cross section appears) to prepare an ultrathin section. In Figure 1, 1 is the pellet and 2 is the ultrathin section. The sections were stained in the gas phase of ruthenium tetroxide for 30 minutes, and then observed by transmission using a field emission scanning transmission electron microscope (FE-STEM, Carl Zeiss Gemini SEM500) with an acceleration voltage of 30 kV, column mode: Normal, aperture size: 20 μm, working distance: 3.6 mm, detection signal: aSTEM A, and observation magnification: 10,000 times, using a STEM detector (Figure 2). In the observation image in Figure 2, the dark areas correspond to the stained areas, and the light areas correspond to the non-stained areas. In the observation image, it was determined that the dark colored areas were composed of resin (B) that is easily stained by ruthenium tetroxide. 2, it can be seen that the polyimide resin (A) and the resin (B) form a sea-island structure in the pellet obtained in Example 5. It is also presumed that the polyimide resin (A) forms the sea portion, and the resin (B) forms the island portion.

[0101] Examples 8 to 11 The powder of polyimide resin 1 obtained in Production Example 1 and the powder of poly(2,6-dimethyl-1,4-phenylene ether) "PX100F" were used in the ratio shown in Table 4, and additives were further added in the amounts shown in Table 4, and injection molding was performed with a molding cycle of 61 to 88 seconds. Except for this, pellets, injection molded articles, and films were produced in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 4. The oxygen index shown in Table 4 was evaluated by the following method.

[0102] <Oxygen Index> Using the resin alone used in each example and the resin composition produced in each example, an injection molded body of 80 mm x 10 mm x 4 mm thick was produced by the above method. The oxygen index of this molded body was measured as a test piece using a candle combustion tester type D (manufactured by Toyo Seiki Seisakusho) according to the method of JIS K 7201:1995. The higher the oxygen index, the better the flame retardancy.

[0103] [Table 4]

[0104] Details of each component shown in Table 4 are as follows. <Component (A)> Polyimide resin 1: crystalline thermoplastic polyimide resin 1 obtained in Production Example 1 <Ingredient (B)> PX100F: Poly(2,6-dimethyl-1,4-phenylene ether), "PX100F" manufactured by Polyxylenol Singapore Pte. Ltd., Tg = 207°C, intrinsic viscosity measured in chloroform at 30°C = 0.37 dL / g <Additives> 201 FF: "201FF Stabilizer" manufactured by PolyAd Services GmbH, antioxidant, KI / CuI / Zn Stearate = 80 / 10 / 10 (mass ratio) Irganox 1010: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], manufactured by BASF Japan Ltd., phenolic antioxidant SR-3000: Daihachi Chemical Industry Co., Ltd., condensed phosphate ester flame retardant

[0105] As shown in Table 4, even in resin compositions containing additives such as antioxidants and flame retardants, low dielectric properties and film moldability can be maintained. In particular, the resin compositions of Examples 10 and 11, which contained flame retardants, showed excellent low dielectric properties and flame retardancy. [Industrial Applicability]

[0106] According to the present invention, it is possible to provide a resin composition having excellent low dielectric properties and good film moldability, and a molded article containing the resin composition.

Claims

1. A thermoplastic resin composition comprising: a crystalline thermoplastic polyimide resin (A) containing a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), in which the content ratio of the repeating structural unit of the formula (1) to the total content of the repeating structural units of the formula (1) and the repeating structural units of the formula (2) is 20 to 70 mol %, and a resin represented by the following formula (5) or an acid-modified product thereof (B), in which the ratio of the content of the mass of the component (B) to the total content of the components (A) and (B), [(B) / {(A)+(B)}], is 0.50 or less. 【Chemistry 1】 (R 1 R is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. 2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. 1 and X 2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. 【Chemistry 2】 (R 51 ~R 55 , and R 61 ~R 64 are each independently a hydrogen atom, a hydroxyl group, or an alkyl group having 1 to 4 carbon atoms; R 65 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. n is the number of repeating structural units and is a number of 10 or more.

2. The thermoplastic resin composition according to claim 1, wherein the total content of the component (A) and the component (B) in the thermoplastic resin composition is 50 mass% or more.

3. 2. The thermoplastic resin composition according to claim 1, wherein the intrinsic viscosity of the component (B) measured in chloroform at 30° C. is 0.20 to 0.60 dL / g.

4. The thermoplastic resin composition according to claim 1 , wherein the thermoplastic resin composition is obtained by melt kneading at a temperature exceeding the melting point of the component (A).

5. The thermoplastic resin composition according to claim 1 , wherein the pellets made of the thermoplastic resin composition have a microphase-separated structure.

6. 2. The thermoplastic resin composition according to claim 1, having a dielectric constant of 3.0 or less and a dielectric loss tangent of 0.005 or less at a measurement frequency of 10 GHz.

7. The thermoplastic resin composition according to claim 1, wherein the absolute value of the coefficient of linear thermal expansion of a molded body obtained by molding the thermoplastic resin composition in a temperature range of 23 to 210 ° C., as measured in accordance with JIS K7197:2012, is 100 ppm / ° C. or less.

8. The thermoplastic resin composition described in claim 1, wherein the ratio of the mass content of component (B) to the total mass content of component (A) and component (B) [(B) / {(A)+(B)}] is 0.01 or more and 0.30 or less.

9. The thermoplastic resin composition described in claim 1, wherein the solvent content in the thermoplastic resin composition is 5 mass% or less.

10. A molded article comprising the thermoplastic resin composition according to any one of claims 1 to 9.

11. The molded article according to claim 10, wherein the molded article is a film.

Citation Information

Patent Citations

  • Resin composition, resin sheet, laminate, and multilayer circuit board

    JP2022063409A

  • Conductive resin composition and molded object

    WO2005026260A1

  • Flame retardant polyamide resin composition and molding

    WO2007108202A1

  • Conductive resin composition and molded article obtained by molding the same

    WO2008018349A1

  • Polyimide resin composition

    WO2020184355A1