Powdered fine cellulose fibers, resin composition, molded body and method for producing same

Chemically modified powdery fine cellulose fibers with controlled bulk density are produced via freeze-drying and pulverization, addressing dispersibility issues in hydrophobic resins, enhancing resin moldability and adhesion without dispersants.

JP7586623B2Active Publication Date: 2024-11-19TOKUSHU TOKAI PAPER
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020074345
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-17
Publication Date
2024-11-19
Estimated Expiration
2040-04-17

AI Technical Summary

Technical Problem

Existing methods for dispersing fine cellulose fibers in hydrophobic resins like polypropylene and polyethylene face issues such as poor dispersibility, potential bleeding of dispersants, and degradation of resin properties, particularly affecting adhesion and heat resistance.

Method used

Production of chemically modified powdery fine cellulose fibers with a bulk density of 10 to 85 g/L, achieved through freeze-drying and pulverization of cellulose fiber pastes with controlled solid content concentration, followed by chemical modification to enhance dispersibility without using dispersants.

Benefits of technology

The method ensures uniform dispersion of cellulose fibers in resins, improving resin moldability and production efficiency while maintaining excellent adhesion and avoiding issues associated with dispersants, such as resin degradation and yellowing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586623000001
    Figure 0007586623000001
Patent Text Reader

Abstract

To provide a cellulose nanofiber which has high dispersibility in a resin, is powdery and is chemically modified, and a method for producing the same.SOLUTION: A powdery fine cellulose fiber has a bulk density of 10-85 g / L and is chemically modified, and can achieve both dispersibility into a resin and productivity in resin molding without using a dispersant by using the fiber.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to powdered fine cellulose fibers having good dispersibility in resin, and a method for producing the same. [Background technology]

[0002] Fine cellulose fibers, known as microfibrillated cellulose and cellulose nanofibers, are lightweight yet have high elastic modulus and strength, and in recent years have been developed to be composited with fine cellulose fibers in order to improve the strength and functionality of resins. In addition, because they are carbon neutral and there is a growing movement to move away from plastic due to the social issue of marine pollution caused by microplastics, they are also attracting attention as a plant-based material. When composited with this resin, there is a problem in that fine cellulose fibers are extremely hydrophilic and have particularly poor dispersibility in general-purpose resin materials such as hydrophobic polypropylene and polyethylene.

[0003] Therefore, Patent Document 1 proposes a method of obtaining a resin in which acetylated fine cellulose fibers are uniformly dispersed by acetylating wood pulp and then kneading the pulp with a resin and then proceeding with defibration at the same time. Although acetylation contributes to improving the heat resistance of cellulose, and since the defibration process and kneading are performed simultaneously, it has the effect of being able to be produced at low cost, the obtained material is always in the form of a resin composition complexed with a resin. Therefore, when considering applications to various resins and uses, it is clear that the degree of freedom in application is higher when the material is in the form of only fine cellulose fibers rather than in the form of a resin composition. In addition, since acetylation is performed in a state where defibration has not progressed, the fine cellulose fibers that are not acetylated are also included after defibration, so there is a risk that the effect of complexing with fine cellulose fibers is not fully exerted.

[0004] On the other hand, Patent Document 2 proposes a method of adding a dispersant to a cellulose nanofiber slurry in advance, and then pulverizing the nanofibers through freeze-drying, and a composition in which the powdered nanofibers are kneaded with a resin. However, although this method improves the dispersibility of the cellulose nanofibers in the resin, the dispersant does not bond with the cellulose nanofibers, so the dispersant bleeds out, and there is a risk of problems with the adhesion and adhesion to other members when using the resin composition after kneading, for example. In addition, if the dispersant is an acid type, the heat resistance of the cellulose nanofibers contained in the resin composition is deteriorated. Furthermore, if the counter ion of the dispersant is a metal ion, the cellulose nanofibers may yellow, the resin composition may deteriorate, and when the resin composition is used in electronic and electrical components such as printed circuit boards, the wiring may corrode. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-25338 A [Patent Document 2] JP 2017-210596 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above-mentioned circumstances, and aims to obtain fine cellulose fibers in a single form that have good dispersibility in a resin when composited with the resin. Another aim of the present invention is to provide powdery fine cellulose fibers that are excellent in production efficiency when molding a composition consisting of chemically modified fine cellulose fibers and a resin, and in adhesiveness and adhesion to other members, and to provide a production method that enables the fine cellulose fibers to be easily chemically modified. [Means for solving the problem]

[0007] As a result of intensive research into solving the above problems, the inventors have discovered that by using chemically modified powdered fine cellulose fibers having a bulk density of 10 to 85 g / L, it is possible to achieve both dispersibility in resin without the use of a dispersant and productivity during resin molding, and have thus completed the present invention.

[0008] That is, the present invention relates to powdery fine cellulose fibers which have a bulk density of 10 to 85 g / L and are chemically modified.

[0009] The powdered fine cellulose fibers preferably have an average fiber diameter of 3 to 1000 nm.

[0010] The powdered fine cellulose fibers preferably do not contain a dispersant, and more preferably the dispersant does not contain an anionic dispersant.

[0011] It is particularly preferable that the powdered fine cellulose fibers do not contain a dispersant whose counter ion is a metal ion.

[0012] The present invention also relates to a resin composition comprising the powdery fine cellulose fibers and a resin.

[0013] Furthermore, the present invention relates to a molded article comprising the resin composition.

[0014] Furthermore, the present invention also relates to a method for producing powdery fine cellulose fibers, which comprises a step of freeze-drying a paste of fine cellulose fibers and a step of pulverizing the paste, and the solid content of the paste is from 5.1 to less than 9.0 mass %.

[0015] The dispersion medium of the paste is preferably a mixture of water and an organic solvent.

[0016] The organic solvent preferably contains at least one of alcohols and carbonates.

[0017] The paste preferably contains a chemically modified component for cellulose.

[0018] It is preferable to have a step of chemically modifying cellulose after the freeze-drying step.

[0019] The powdered fine cellulose fibers obtained by the above production method preferably have a bulk density of 10 to 85 g / L. Effect of the Invention

[0020] In the present invention, powdered fine cellulose fibers that are sufficiently chemically modified can be obtained, so that they can be uniformly dispersed in resin. In addition, since the viscosity during kneading is low, the resin has excellent moldability and production efficiency. Furthermore, since the fine cellulose fibers are obtained alone, resin compositions in which the fine cellulose fibers are combined with various types of resins can be used for various purposes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] [Powdered fine cellulose fiber] A first aspect of the present invention is powdery fine cellulose fibers which have a bulk density of 10 to 85 g / L and are chemically modified.

[0022] The bulk density of the powdered fine cellulose fiber must be 10 to 85 g / L. The bulk density value is measured according to JIS K7365. If the bulk density is less than 10 g / L, the specific surface area of ​​the powdered fine cellulose fiber is too large, so that the viscosity increases significantly when the powdered fine cellulose fiber is kneaded with a resin, and the torque applied to the rotor during kneading increases. If the kneading torque increases, excessive energy and time are required to obtain a good dispersion state, resulting in poor production efficiency and high costs. If the bulk density exceeds 85 g / L, the increase in kneading torque can be kept low, but the powdered fine cellulose fiber may be poorly dispersed in the resin and may exist as large particles. In addition, the effects of improving strength properties such as tensile strength, elastic modulus, and toughness, and improving thermal stability such as heat resistance and low linear thermal expansion coefficient, which are expected from the powdered fine cellulose when composited with a resin, may be poor.

[0023] The powdered fine cellulose fiber is chemically modified. Here, "chemical modification" means any treatment in which all or part of the hydroxyl groups of the fine cellulose fiber are replaced with functional groups different from the hydroxyl groups. Since the powdered fine cellulose fiber has appropriate functional groups depending on the resin used for compounding with the resin, such as kneading, the functional groups to be replaced can be designed arbitrarily. For example, it is preferable to chemically modify polypropylene and polyethylene, which are typical general-purpose resins, with functional groups that impart hydrophobicity, such as alkyl groups, silyl groups, and phenyl groups, by acylation or esterification of the hydroxyl groups. The acylation and esterification of the hydroxyl groups of cellulose are well known and commonly used in the technical field, and the chemical modification method that can be applied varies depending on the state of the fine cellulose fiber, such as powder, aqueous dispersion, and organic solvent dispersion, so the chemical modification material used is not particularly limited. In particular, as a chemical modification, it is preferable to replace the hydroxyl groups of cellulose with hydrophobic groups using a hydrophobizing agent. Examples of such hydrophobization treatment include any hydrophobization such as acylation, esterification, alkylation, etherification, tosylation, and epoxidation.

[0024] The term "powdered" in the powdered fine cellulose fibers refers to a state in which fine cellulose having a solid form is finely crushed. A part of the fine cellulose fibers does not have to be in a powdered state.

[0025] The fine cellulose fibers of the present invention are obtained by subjecting cellulose fibers to a micronization treatment. The apparatus for micronizing cellulose fibers is not particularly limited, but examples thereof include high-pressure homogenizer treatment (high-pressure dispersion treatment using a Manton-Gaulin type disperser), a Lanier type pressure homogenizer, ultra-high-pressure homogenizer treatment (Alteimiser TM (manufactured by Sugino Machine Co., Ltd.)), dispersion devices such as beads mills and Ryusei mills, and homogenizers such as Masscolloider (manufactured by Masuko Sangyo Co., Ltd.). The degree of beating is not particularly limited, but it is also possible to use a beater used in papermaking, such as a double disk refiner or beater, for pretreatment before the micronization treatment. In particular, in the case of a type of micronization treatment device that passes through an orifice, such as a high-pressure homogenizer, if the raw material is not beaten in the pretreatment, there is a risk that the raw material will be clogged or stable micronization will not be possible. In addition, since the above-mentioned micronization treatment device generally has low production efficiency, it is preferable to perform pretreatment with a beater in advance, as this increases production efficiency. Furthermore, it is possible to use cellulose nanofibers (TOCN) that have been nanofiberized by chemical treatment using a TEMPO oxidation catalyst, but mechanical processing in which pretreatment is performed with a beater and then pulverization is performed with a homogenizer is preferred.

[0026] The cellulose fibers that can be used in the pulverization treatment are not particularly limited, and known cellulose fibers can be used. For example, bleached wood chemical pulps such as softwood bleached kraft pulp (NBKP), hardwood bleached kraft pulp (LBKP), and softwood bleached sulfite pulp (NBSP), groundwood pulp (GP), thermomechanical pulp (TMP), and chemical thermomechanical pulp (BCTMP), and non-wood pulps such as hemp, bamboo, straw, kenaf, mitsumata, kozo, and cotton, and waste paper pulp can be used. One of these cellulose fibers can be used alone or two or more can be used in combination. In the present invention, the type of cellulose, such as cellulose type I and cellulose type II, is not particularly limited, but natural fibers of cellulose type I, such as cotton, cotton linters, and wood pulp, are preferred. More preferred is NBKP, a bleached wood pulp derived from softwood, which is more likely to undergo fibrillation than cutting during fiber defibration. Cellulose type II fibers, represented by regenerated cellulose, have a lower degree of crystallinity than cellulose type I fibers and are more likely to become short fibers when subjected to fibrillation treatment, which is undesirable because it may reduce the effect of improving strength when composited with resin.

[0027] The cellulose fibers are the main component, but if necessary, modified pulps such as cationic pulp and mercerized pulp, synthetic fibers such as rayon, vinylon, nylon, acrylic, polyester, polyolefin, carbon, aramid, and other chemical fibers, or microfibrillated pulp can be used alone or in combination.

[0028] Cellulose fibers can be uniformly dispersed in water due to the hydroxyl groups of the cellulose molecules, but the viscosity of the slurry depends on the fiber length and surface area of ​​the cellulose fibers. As the cellulose fibers become thinner, the surface area of ​​the cellulose increases, and the viscosity of the slurry inevitably increases. Fine cellulose fibers obtained by chemical treatment such as TOCN have a fiber diameter of the single nano order, but due to the above-mentioned reasons, the viscosity is extremely high and the concentration cannot be increased. In the present invention, which obtains powdered chemically modified fine cellulose fibers, the concentration is not preferred because it is greatly affected by the cost.

[0029] In the present invention, the average fiber diameter of the chemically modified fine cellulose fiber is preferably 3 nm to 1000 nm, more preferably 3 nm to 500 nm, even more preferably 3 nm to 300 nm, even more preferably 3 nm to 200 nm, and most preferably 30 nm to 200 nm. When the fiber diameter is in this range, the dispersibility when kneaded with a resin is good, and various effects expected from the fine cellulose fiber as described later are exhibited. The average fiber diameter is measured by the following procedure. First, the powder of the chemically modified cellulose fiber is placed on a sample stage and observed with a high-resolution electron microscope (FE-SEM), and lines are drawn in the horizontal and vertical directions on the obtained SEM image. Next, the fiber diameters of all fibers intersecting with the two lines are actually measured from the enlarged image, and the number average fiber diameter is calculated from the measurement results. Furthermore, the number average fiber diameter is calculated in the same manner for at least two points on the surface of the powder placed on the sample stage, and the average value of all the number average fiber diameters is taken as the average fiber diameter.

[0030] Cellulose fibers have the property of forming hydrogen bonds between fibers during the dehydration process due to their hydroxyl groups. In the process of forming these hydrogen bonds, for example in the case of a sheet such as paper, while strength is developed, the interaction between the fibers causes shrinkage during the drying process. This shrinkage is particularly noticeable as the fiber diameter becomes thinner, as the stiffness of the fiber decreases and the cohesive force acting between the fibers increases. It is also known that sheets made from extremely fibrillated fibers are transparent because the fibers are completely in contact with each other. In other words, it is difficult to isolate fine cellulose fibers using normal dehydration and drying methods. For this reason, in order to isolate fine cellulose fibers, it is necessary to suppress shrinkage during drying or inhibit hydrogen bonds between the fibers. Specific methods that have been proposed so far include replacing fine cellulose fibers with a hydrophilic solvent such as acetone, and then replacing it with a more hydrophobic solvent such as a mixed solvent of toluene and acetone and drying it. However, this method has two problems. The first is the process of replacing the dispersion solvent water with acetone. Since the water retention of cellulose fibers increases as the fiber diameter becomes thinner, the replacement of water with a solvent is a very time-consuming task, which is a factor in reducing productivity in terms of actual production. In addition, since the water is replaced with a highly hydrophobic solvent, hydrogen bonds are inhibited, and the surface tension of the solvent is also low, so the cohesive force is smaller than that of water, but shrinkage occurs, and the large specific surface area that fine cellulose fibers originally possess is inevitably reduced.

[0031] Therefore, it is preferable to freeze-dry the fine cellulose fibers after the micronization treatment in order to remove water without shrinking and agglomerating. Freeze-drying is a technique in which a mixture of cellulose fibers and a dispersion medium is depressurized while in a frozen state to sublimate the dispersion medium, thereby drying the material without shrinking. In the present invention, it is preferable to freeze-dry the paste consisting of the fine cellulose fibers and the dispersion medium after the micronization treatment. The freezing method of the paste in freeze-drying is not particularly limited, but there are, for example, a method in which the paste is placed in a refrigerant such as liquid nitrogen and frozen, a method in which the paste is placed in a low-temperature atmosphere at atmospheric pressure and frozen, and a method in which the paste is placed in a low-temperature atmosphere under reduced pressure and frozen. A method in which the paste is placed in a low-temperature atmosphere under atmospheric pressure and frozen is preferable. The freezing temperature of the paste needs to be below the freezing point of the dispersion medium, preferably -20°C or less, and more preferably -30°C or less. Freeze-drying involves sublimation after freezing, but drying will be slow unless the pressure is reduced. The pressure during decompression is preferably 0.10 kPa or less, and more preferably 0.05 kPa or less.

[0032] In the present invention, the dispersion medium used in the paste of the fine cellulose fibers is preferably a mixture of water and an organic solvent, and more preferably a mixed paste containing at least one of alcohols and carbonates as the organic solvent. By mixing such an organic solvent, it is possible to suppress the aggregation of the fine cellulose fibers during drying. The alcohols and carbonates are not particularly limited as long as they are uniformly miscible with water, but t-butyl alcohol and ethylene carbonate, which can be recovered by freezing the sublimated organic solvent, are particularly preferred. The content of the organic solvent in the dispersion solvent is preferably 10% or more, more preferably 20% or more.

[0033] In the present invention, the concentration of the fine cellulose fibers in the mixed paste is preferably 5.1% or more and less than 9.0%. When the fine cellulose fibers in the mixed paste are less than 5.1%, the dispersibility of the fine cellulose fibers in the dispersion medium of the mixed paste is good, but the specific surface area is high after freeze-drying, so the viscosity increases when kneading with the resin, and the work efficiency and production efficiency when molding the resin composition are poor, which is not preferable because it lacks practicality. Furthermore, due to the high specific surface area, there is a risk that the fibers that are not partially modified during chemical modification will increase, resulting in the generation of aggregates that are not dispersed in the resin. In addition, when the fine cellulose fibers in the mixed paste are 9.0% or more, there are many aggregates of fine cellulose fibers that cannot be pulverized and dispersed even in the subsequent pulverization process and kneading process with the resin, and the dispersibility of the fine cellulose fibers when composited with the resin will be poor, which is not preferable because it is difficult to obtain the transparency of the resin and the strength improvement effect.

[0034] To make the dried product after freeze-drying of the fine cellulose fibers into a powder, a pulverization process is required. Examples of pulverizers used in the pulverization process include cutter mills, ball mills, disk mills, and airflow pulverizers. Of these, there are no particular limitations as long as the conditions can be set so that the fine cellulose fibers after freeze-drying are not aggregated into lumps, but it is preferable to use an airflow pulverizer after pre-pulverization with a cutter mill. The airflow pulverizer is preferable because it pulverizes the raw materials by the impact of colliding with each other, so that the raw materials are not subjected to excessive compression force and the bulk density of the powder can be reduced. Examples of the airflow pulverizer include Super Jet Mill (manufactured by Nisshin Engineering Co., Ltd.) and Dryburn (manufactured by Sugino Machine Co., Ltd.).

[0035] In the present invention, the density of the porous body, which is the dry product after freeze-drying, is 0.051 g / cm 3 More than 0.090g / cm 3 It is preferable that the density of the porous body is less than 0.051 g / cm 3If the specific surface area is less than 0.090 g / cm, the bulk density after pulverization will be too low due to the large specific surface area of ​​the fine cellulose fibers, and this is undesirable because it may increase the resin torque, which affects the production efficiency of the resin composition, and it may be difficult to sufficiently replace the hydroxyl groups of the cellulose in the chemical modification step with other functional groups. 3 In the above cases, since the bulk density after pulverization is low, the increase in resin torque can be suppressed, but it is not preferable because the fine cellulose fibers cannot be uniformly dispersed in the resin. Since the density of the porous body depends on the concentration of the paste, the density of the porous body can be adjusted by the solid content concentration of the paste.

[0036] The powdered fine cellulose fiber is chemically modified. The chemical modification step may be performed simultaneously with the freeze-drying step, or after the freeze-drying step. The method for chemically modifying the fine cellulose fiber performed simultaneously with the freeze-drying step is not particularly limited as long as the fine cellulose fiber can be treated in the presence of water in the mixed paste, and the dispersibility is good when kneaded with the resin and the viscosity during kneading is not significantly improved. For example, a silane coupling agent is preferably used. Silane coupling agents are industrially produced compounds having various functional groups such as vinyl groups, epoxy groups, methacryl groups, phenyl groups, amino groups, fluoro groups, and isocyanate groups, and the design of chemical modification is wide. Therefore, it is preferable because the chemically modified fine cellulose fiber can be designed to match the resin to be compounded. Examples of the silane coupling agent include trimethoxyphenylsilane, phenyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-(2-aminoethyl)3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)3-aminopropylmethyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, vinyltrimethoxysilane, N-(2-(vinylbenzylamino)ethyl)3-aminopropyltrimethoxysilane hydrochloride, 3-methacryloxypropyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, and 3-chloropropyltrimethoxysilane. In addition, isocyanate compounds, like silane coupling agents, are industrially produced with a variety of functional groups, and have a wide range of chemical modifications. They are inexpensive materials, and therefore are cost-effective. However, since isocyanate groups are highly reactive with hydroxyl groups, when chemically modifying during the freeze-drying process, tolylene diisocyanate (TDI) or diphenylmethane diisocyanate (MDI), which have blocked isocyanate groups, are preferred.Performing the chemical modification process simultaneously with the freeze-drying process has the advantage of reducing the number of steps and therefore the cost. However, since the mixed paste contains water, it is not possible to employ techniques such as modification using reagents that are highly reactive with water or reaction in a low-polarity solvent.

[0037] In the present invention, if chemical modification is not performed during the freeze-drying process, the chemical modification process is performed after the pulverization process. If the fine cellulose fiber powder has been subjected to the freeze-drying process and the powdering process, it can be chemically modified in a low polarity solvent such as toluene or hexane, but this is not limited as long as the dispersion is good when kneaded with a resin and the viscosity during kneading is significantly improved. However, reactions involving water are not preferred because they will cause the fine cellulose fiber powder to re-aggregate unless the water is removed after treatment. For example, when using a silane coupling agent, it is preferable to use a silane stock solution or a diluted solution of an organic solvent, or to perform chemical modification by a gas phase method such as vapor deposition, rather than a hydrolysis solution. In addition, since the moisture is removed by the freeze-drying process, it is possible to use octadecyl isocyanate, phenyl isocyanate, etc., in which the isocyanate group is not blocked. Since unblocked isocyanate has extremely high reactivity with hydroxyl groups, it is preferable because the reaction proceeds at a lower temperature than blocked isocyanate. Furthermore, acetylation, which is a simple method with low production costs and maintains high heat resistance even after chemical modification, can also be preferably used.

[0038] It is preferable that the powdered fine cellulose fiber does not contain a dispersant. When the dispersant is contained, in the process of mixing the powdered fine cellulose fiber with the resin to form a resin composition, the dispersibility of the powdered fine cellulose fiber in the resin is improved, and the mechanical performance of the resin composition is improved. However, when the obtained resin composition is actually used, it may be used in combination with other members, or by bonding or compounding. In such a case, it is not preferable because there is a risk of problems with the adhesion and adhesion to other members. The dispersant here is not particularly limited as long as it improves the dispersibility when dispersing the powdered fine cellulose fiber in water, and refers to a known dispersant. In particular, when the dispersant is an anionic dispersant, it is affected by the counter ion and has a negative effect on the fine cellulose fiber contained in the resin composition. For example, in the case of a dispersant having a structure such as a phosphate group, a carboxylate group, or a sulfonic acid group in which the counter ion becomes a proton, the pH becomes acidic, and the heat resistance and strength of the fine cellulose fiber are deteriorated. Furthermore, when the counter ions of these dispersants are metal ions, especially alkali metals such as Na, they promote the yellowing of cellulose when heated or over time, making them unsuitable for use in components and housings for personal computers, smartphones, home appliances, toys, etc., due to problems with appearance and design. In addition, when the counter ions are ammonium salts, they may be released as ammonia gas when heated. Specifically, it is known that ammonium salt-type carboxymethylcellulose becomes an acid type when heated to about 150°C, with ammonia being released. When kneading with thermoplastic resins, heat is applied to at least about 200°C, so the conditions for generating ammonia are easily reached. The generated ammonia gas promotes the deterioration of the resin. For example, polycarbonate, which is widely used in transportation equipment such as aircraft and automobiles, electrical, electronic, optical, and medical equipment, and bulletproof glass materials, is known to be hydrolyzed and deteriorated by ammonia. In addition, dispersants may contain halogen elements such as chlorine that remain as impurities during the manufacturing process and these halogen elements may corrode the wiring of electronic and electrical components such as printed circuit boards.

[0039] The resin composition of the present invention can use thermoplastic resins, thermosetting resins, and rubbers. There is no particular restriction on the type of resin that can be used, but examples of thermoplastic resins include polyethylene resins, polypropylene resins, polylactic acid resins, polyvinyl alcohol resins, polyamide resins, acrylonitrile-butadiene-styrene (ABS) resins, acrylonitrile-styrene (AS) resins, polymethyl methacrylate resins, polyvinylidene chloride resins, ethylene vinyl alcohol resins, polyacrylonitrile resins, polyacetal resins, polyketone resins, and cyclic polyolefin resins. Examples of thermosetting resins include epoxy resins, phenolic resins, melamine resins, urea resins, and unsaturated polyester resins. Examples of rubber include natural rubber (NR), polyisoprene rubber (IR), styrene-butadiene copolymer rubber (SBR), polybutadiene rubber (BR), butyl rubber (IIR), nitrile rubber (NBR), chloroprene rubber (CR), acrylic rubber (ACM), fluororubber (FKM), ethylene propylene rubber (EPDM), chlorosulfonated polyethylene (CSM), urethane rubber (U), silicone rubber (Q), etc. In addition, within the scope of not impairing the performance of the present invention, the resin composition can be appropriately mixed with assistants such as defoamers, preservatives, fillers, colorants, plasticizers, leveling agents, conductive agents, antistatic agents, ultraviolet absorbers, deodorants, and heat-resistant materials, as well as fiber materials such as reinforcing fibers, conductive fibers, and heat-resistant fibers.

[0040] The resin composition of the present invention can be obtained as a molded product by various molding methods. It is necessary to use an appropriate molding method depending on the type of resin and the shape of the desired molded product, and examples of the molding method include extrusion molding, injection molding, heat press molding, melt extrusion molding, blow molding, vacuum molding, and heat molding.

[0041] [Resin composition] A second aspect of the present invention is a resin composition comprising the above powdery fine cellulose fibers and a resin.

[0042] Regarding the powdered fine cellulose fibers, the resin and the resin composition, the above explanations in the first aspect of the present invention also apply to the second aspect.

[0043] The method for compounding the powdered fine cellulose fiber and the resin is not particularly limited, and includes known methods such as melt kneading and dry mixing, but melt kneading is preferable. In kneading, the powdered fine cellulose fiber can be uniformly dispersed with the resin because it is in powder form. In addition, chemical modification according to the type of resin can be imparted. For kneading, known kneading machines such as an extruder, a mixing roller, a kneader, and a mixer can be used.

[0044] [Molded body] A third aspect of the present invention is a molded article containing the resin composition.

[0045] Regarding the resin composition, the above description regarding the second aspect of the present invention also applies to the third aspect.

[0046] The molded article refers to any shape such as a film, a sheet, a structure, etc., and is produced using a resin composition. The method for producing the molded article is not particularly limited, and a known method is used, for example, injection molding, extrusion molding, blow molding, press molding, etc. can be applied.

[0047] The shape and manufacturing method of the molded article can be selected according to the purpose of use. It can be used in place of parts used in electronic devices, home appliances, various containers, building materials, furniture, stationery, automobiles, and household goods. For example, it can be used in housings and exterior parts of electronic devices and home appliances, various storage cases, tableware, interior parts of building materials, interior materials of automobiles, and other daily necessities.

[0048] [Method of manufacturing fine powdered cellulose fiber] A fourth aspect of the present invention is a method for producing powdery fine cellulose fibers, comprising a step of freeze-drying a paste of fine cellulose fibers and a step of pulverizing the paste, and characterized in that the solid content of the paste is less than 5.1 to 9.0 mass %.

[0049] For the fine cellulose fibers, paste, freeze-dried, pulverized, and powdered fine cellulose fibers, the above explanations in the first to third aspects of the present invention also apply to the fourth aspect.

[0050] By setting the solid content concentration of the paste to 5.1% by mass or more, the bulk density is increased, but the amount of unmodified fine cellulose fibers can be reduced, making it difficult for poor dispersion to occur when kneading with a resin. Also, by setting the solid content concentration to less than 9.0% by mass, the bulk density can be satisfied.

[0051] According to the method for producing powdery fine cellulose fibers of the present invention, a resin composition can be produced with good dispersibility when compounded with a resin, such as by kneading, and the resin composition can exhibit good moldability. EXAMPLES

[0052] The present invention will be described in more detail below using examples and comparative examples, but the scope of the present invention is not limited to the examples.

[0053] [Measurement items and test methods in the examples] (Mixing test) A kneader (product name: Labo Plastomill, model: 4C-150, manufactured by Toyo Seiki Co., Ltd.) and a mixer (model number: R60, manufactured by Toyo Seiki Co., Ltd.) were used for the kneading test. 41 g of polypropylene resin (model number: J105G, manufactured by Prime Polymer Co., Ltd.) was weighed out and charged into a mixer heated to 220°C, and pre-kneaded at 10 rpm. The rotation speed was then changed to 30 rpm, 1 g of fine cellulose fiber powder was weighed out and charged, and after the charging was completed, the rotation speed was changed to 50 rpm and kneaded for 10 minutes. The torque value at the end of kneading was read, and a score of 0 or higher was determined to be acceptable according to the following criteria. ◎: Less than 1.2 times the torque value for resin only ○: Less than 1.5 times the torque value of resin only △: Less than 2.0 times the torque value of resin only ×: Less than 3.0 times the torque value of resin alone (Dispersibility evaluation) Weigh out 30 mg of the composite resin, place it on a glass slide, and heat it with a hot stirrer (product name: REXIM, model number: RSH-6DN, manufactured by AS ONE Co., Ltd.) at 240°C. When the resin is melted, cover it with another glass slide, press it, and cool it to obtain a sample for dispersion evaluation. A biological microscope (product name: Eclipse, model number: Ni-U, manufactured by Nikon Corporation) equipped with a differential interference device and a phase contrast device was used to evaluate dispersibility. Ten fields of view were randomly observed at 200x magnification, and coarse objects of 10μm or more were counted. Based on the total number of the 10 fields of view, a score of 0 or higher was determined as passing according to the following criteria. ◎: No bulky items. ○: Less than 10 bulky items. △: 10-100 large items ×: 100 or more bulky items (density measurement of porous materials) The porous body was cut into 10 cm squares, and the weight was measured using an electronic balance (model number: FZ-3000iWp, manufactured by Mettler Toledo K.K.), and the thickness was measured at 10 points using a thickness gauge (model number: 547-401, manufactured by Mitutoyo Corporation), and the average value was calculated. The density was calculated from the weight and thickness. (Measurement of bulk density of powder) Measurements were performed in accordance with JIS K7365.

[0054] Example 1 [Microfiber cellulose fiber preparation process] Bleached coniferous kraft pulp was dispersed in ion-exchanged water to a concentration of 2% by weight, beaten using a double disc refiner, and further treated 10 times using a high-pressure homogenizer (LAB1000, manufactured by SMT Corporation) at a pressure adjusted to 750 bar to obtain fine cellulose fibers.

[0055] [Fine cellulose fiber concentration process] The fine cellulose fibers obtained in the above preparation process were sandwiched between a 420 mesh polyester mesh (model number: T-No. 420T, manufactured by NBC Meshtec Co., Ltd.) and absorbent paper, and then pressed and dehydrated to prepare a fine cellulose fiber paste with a solid content of 15%.

[0056] [Mixed paste preparation process] To the fine cellulose fiber paste obtained in the above concentration process, t-butyl alcohol and ion-exchanged water were added so that the solid concentration of the fine cellulose fiber was 5.5% and the concentration of t-butyl alcohol was 20%, and the mixture was kneaded until homogenous using a planetary mixer (model number: PVM-5, manufactured by Asada Iron Works Co., Ltd.) to obtain a mixed paste.

[0057] [Lyophilization process] The freeze-drying was performed using a vacuum freeze-drying device (model number: SF-4KB, manufactured by Sansho Industry Co., Ltd.) The resulting mixed paste was spread on a stainless steel tray and pre-frozen at -35°C for 6 hours, and then the temperature was gradually increased while adjusting the vacuum to 0.1 kPa or less, to obtain a porous body of fine cellulose fibers.

[0058] [Crushing process] The above porous body was pre-pulverized using a homomixer (model number: CM-100, manufactured by As One Corporation), and then pulverized using an airflow mill (product name: Drystorm, model number: DB-100S, manufactured by Sugino Machine Corporation) at a rotation speed of 18,000 rev / min to obtain powdered fine cellulose fibers.

[0059] [Chemical modification step 1] 100 ml of acetone and 0.75 g of trimethoxyphenylsilane (Tokyo Chemical Industry Co., Ltd.) were added to a 200 ml beaker and stirred with a magnetic stirrer, after which 1.5 g of the fine cellulose fiber powder was added and stirred for 2 hours. The mixture was then filtered with a filter equipped with a PTFE-type membrane filter (product name: Omnipore, diameter: 1.0 μm, Merck Millipore), and the residue was dried at 120° C. for 2 hours to obtain chemically modified powdered fine cellulose fiber E1.

[0060] Example 2 [Chemical modification step 2] A 50 ml beaker containing 2.5 g of phenyltrimethoxysilane was placed in a 2.5 L stainless steel airtight container, and the fine cellulose fiber powder was spread in the gap. The container was placed in a 120°C oven and reacted for 2 hours to obtain chemically modified powdered fine cellulose fiber E2.

[0061] Example 3 [Chemical modification step 3] 100 ml of acetone and 0.75 g of phenyl isocyanate (Tokyo Chemical Industry Co., Ltd.) were added to a 200 ml beaker and stirred with a magnetic stirrer, after which 1.5 g of the fine cellulose fiber powder was added and stirred for 2 hours. The mixture was then filtered through a filter equipped with a PTFE membrane filter (product name: Omnipore, diameter: 1.0 μm, Merck Millipore), and the mixture was further filtered and washed once with cyclohexane and once with acetone. The residue was then dried at 105°C for 4 hours to obtain chemically modified fine cellulose fiber powder E3.

[0062] Example 4 [Chemical modification step 4] In the mixed paste preparation step, 50 parts by weight of phenyltrimethoxysilane was mixed with 100 parts by weight of fine cellulose fibers, and freeze-dried in the same manner as in Example 1. The obtained porous body was treated in an oven at 120°C for 2 hours, and a pulverization step was carried out in the same manner as in Example 1. The obtained powder was filtered and washed once with cyclohexane and once with acetone using a filter equipped with a PTFE membrane filter (product name: Omnipore, diameter: 1.0 μm, manufactured by Merck Millipore), and the residue was dried at 105°C for 4 hours to obtain chemically modified powdered fine cellulose fibers E4.

[0063] Example 5 Chemically modified fine cellulose fibers E5 were obtained in the same manner as in Example 1, except that in the mixed paste preparation step, the solid content concentration of the fine cellulose fibers was 8.5%.

[0064] Comparative Example 1 Chemically modified powdery fine cellulose fibers CE1 were obtained in the same manner as in Example 1, except that in the mixed paste preparation step, the solid content concentration of the fine cellulose fibers was 4.5%.

[0065] Comparative Example 2 Chemically modified powdered fine cellulose fibers CE2 were obtained in the same manner as in Example 1, except that in the mixed paste preparation step, the solid content concentration of the fine cellulose fibers was 9.5%.

[0066] Comparative Example 3 Chemically modified powdered fine cellulose fibers CE3 were obtained in the same manner as in Example 1, except that in the mixed paste preparation step, the solid content concentration of the fine cellulose fibers was 1.0%.

[0067] Comparative Example 4 Chemically modified fine cellulose fiber CE4 was obtained in the same manner as in Example 1, except that in the grinding process, a grinder equipped with a 50 ml stainless steel grinding jar and 25 mm diameter stainless steel balls (product name: Mixer Mill, model number: MM400, manufactured by Recche Co., Ltd.) was used and the processing was performed for 3 minutes at 25 Hz.

[0068] Comparative Example 5 Powdered fine cellulose fiber CE5 was obtained in the same manner as in Example 1, except that in the mixed paste preparation process, 10 parts by weight of a dispersant (product name: Aron A-6114, manufactured by Toa Gosei Co., Ltd.) was added to 100 parts by weight of fine cellulose fiber, and the subsequent chemical modification process was not performed.

[0069] [Table 1] TIFF0007586623000001.tif93170

[0070] The results of Examples 1 to 5 show that the powdery fine cellulose fiber of the present invention can be efficiently molded while having good dispersibility when composited with a resin. On the other hand, the results of Comparative Examples show that when the bulk density is outside the range of the present invention, there is a problem with dispersibility or moldability.

Claims

1. Powdered fine cellulose fibers which are pulverized freeze-dried porous material having a density of 0.051 g / cm 3 or more and less than 0.090 g / cm 3 , characterized in that the powdered fine cellulose fibers have a bulk density of 10 to 85 g / L and are chemically modified.

2. The powdered fine cellulose fibers according to claim 1, characterized in that the powdered fine cellulose fibers have an average fiber diameter of 3 to 1000 nm.

3. 3. The powdered fine cellulose fibers according to claim 1 or 2, which does not contain a dispersing agent.

4. 4. The powdered fine cellulose fibers according to claim 3, wherein the dispersant is an anionic dispersant.

5. 5. The powdered fine cellulose fibers according to claim 4, wherein the counter ion of the anionic dispersant is a metal ion.

6. A resin composition comprising the powdered fine cellulose fiber according to any one of claims 1 to 5 and a resin.

7. A molded article comprising the resin composition according to claim 6.

Citation Information

Patent Citations

  • Chemical modified cellulose nanofiber and fiber reinforced resin composition containing thermoplastic resin

    JP2017025338A

  • Powdery cellulose nanofibers for the production of compositions, method for producing the same, and compositions

    JP2017210596A

  • Manufacturing method of dry powder of cellulose fiber

    JP2022001631A