Method for producing powdered dry solids

A simplified method for producing cellulose nanofiber dry solids using inorganic particles inhibits aggregation, enhancing handleability and redispersibility, addressing the limitations of existing methods.

JP7586665B2Active Publication Date: 2024-11-19TOA PAINT CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020133227
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-05
Publication Date
2024-11-19
Estimated Expiration
2040-08-05

AI Technical Summary

Technical Problem

Existing methods for producing cellulose nanofibers as dry solids are complicated, limit fiber length, result in lower strength, and require large amounts of water-soluble polymers, leading to limited cellulose nanofiber addition and poor water resistance.

Method used

A method involving a liquid mixture preparation step followed by evaporation and pulverization to form a thin film-like dry solid, then grinding into powder, without shortening the fibers, using inorganic particles like calcium carbonate and titanium oxide to inhibit aggregation.

Benefits of technology

The method produces a powdery dry solid that is easy to handle and less likely to aggregate, allowing for higher cellulose nanofiber content and improved redispersibility in aqueous dispersions, with applications in coatings exhibiting deodorizing effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586665000002
    Figure 0007586665000002
  • Figure 0007586665000003
    Figure 0007586665000003
  • Figure 0007586665000001
    Figure 0007586665000001
Patent Text Reader

Abstract

To provide a method for producing a powdery dry solid that can produce, in a simple process, a dry solid having good handleability while preventing the aggregation in preparing an aqueous dispersion.SOLUTION: The present invention pertains to a method for producing powdery dry solid comprising a composite of cellulose nanofibers and particles, the method including a liquid mixture preparation step for preparing a liquid mixture having particles dispersed in an aqueous dispersion of cellulose nanofibers, and a drying-pulverizing step in which the liquid mixture is evaporated and dried with a heat medium to make a thin film-like dry solid and the thin film-like dry solid is then pulverized into powder.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a powdery dry solid. More specifically, the present invention relates to a method for producing a powdery dry solid that contains cellulose nanofibers, is less likely to cause aggregation during preparation of an aqueous dispersion, and is easy to handle. [Background technology]

[0002] Conventionally, cellulose nanofibers are prone to aggregation between fine fibers due to interactions such as hydrogen bonds. For this reason, cellulose nanofibers are sometimes prepared and handled as aqueous dispersions. However, to ensure stability, aqueous dispersions require water several times to several hundred times the weight of the cellulose nanofibers. Thus, Patent Document 1 proposes a method for producing a dry solid of cellulose nanofibers. Furthermore, Patent Document 2 discloses a method for producing a dry solid of cellulose nanofibers and a water-soluble polymer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-95664 A [Patent Document 2] JP 2017-8176 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the method described in Patent Document 1 requires a step of shortening the cellulose nanofibers. As a result, the manufacturing method is complicated, and the fiber length of the obtained cellulose nanofibers is limited. The strength of the shortened cellulose nanofibers is likely to decrease. Furthermore, the method described in Patent Document 2 results in poor water resistance when the obtained cellulose nanofiber dry solid is blended with paint or the like. Furthermore, the method described in Patent Document 2 requires blending a large amount of water-soluble polymer with the cellulose nanofibers. Therefore, the amount of cellulose nanofiber that can be added is likely to be limited.

[0005] The present invention has been made in consideration of such conventional problems, and has an object to provide a method for producing a powdery dry solid material which is a simple production method, is less likely to cause aggregation when preparing an aqueous dispersion, and can give a dry solid material that is easy to handle. [Means for solving the problem]

[0006] The method for producing a powdery dry solid material of the present invention that solves the above problems mainly includes the following configurations.

[0007] (1) A method for producing a powdery dry solid in which cellulose nanofibers and particles are composited, comprising the steps of: preparing a mixed liquid in which particles are dispersed in an aqueous dispersion of cellulose nanofibers; evaporating and drying the mixed liquid using a heat medium to obtain a thin-film dry solid; and then pulverizing the thin-film dry solid into powder.

[0008] According to this configuration, the production method of the present invention is simple and does not require a step of shortening the cellulose nanofibers. Furthermore, the powdery dry solid obtained by the production method of the present invention is less likely to cause aggregation between the cellulose nanofibers. Therefore, the powdery dry solid is less likely to cause aggregation when preparing an aqueous dispersion, and is easy to handle.

[0009] (2) The method for producing a powdery dry solid according to (1), wherein the particles are inorganic particles.

[0010] According to this configuration, the resulting powdery dry solid is less susceptible to aggregation between the cellulose nanofibers, and therefore the powdery dry solid is less susceptible to aggregation during preparation of an aqueous dispersion, making it easier to handle.

[0011] (3) The method for producing a powdery dry solid according to (1) or (2), wherein the drying and grinding step is a step of supplying the mixed liquid to the surface of a rotating drum containing a heat transfer medium therein, evaporating and drying the mixed liquid to obtain the thin-film dry solid, and then grinding the thin-film dry solid into powder by continuously scraping it off from the drum surface with a knife.

[0012] According to this configuration, the manufacturing method of the present invention can be easily carried out by the drum drying device employing the above-mentioned steps.

[0013] (4) The method for producing a powdery dry solid material according to any one of (1) to (3), wherein the particles have a volume average particle size of 0.001 to 100 μm as measured by a laser diffraction / scattering method.

[0014] According to this configuration, in the production method of the present invention, by using particles having the above volume average particle diameter, aggregation between fibers of the cellulose nanofibers is more unlikely to occur.

[0015] (5) The method for producing a powdery dry solid material according to any one of (1) to (4), wherein the particles contain at least one of calcium carbonate and titanium oxide.

[0016] According to this configuration, the production method of the present invention makes it more difficult for aggregation to occur between the cellulose nanofibers.

[0017] (6) The method for producing a powdery dry solid material according to any one of (1) to (5), wherein the cellulose molecules constituting the cellulose nanofibers have at least one of a carboxyl group, a hydrazide group, a hydrazine group, and a primary amino group.

[0018] According to this configuration, the obtained powdery dry solid has excellent redispersibility and is easy to prepare a coating composition. The obtained coating composition uses the cellulose nanofibers composed of the above-mentioned cellulose molecules, and therefore exhibits an excellent deodorizing effect against daily odors in indoor spaces such as residences. Effect of the Invention

[0019] According to the present invention, there can be provided a method for producing a powdery dry solid material, which is a simple production method, is less likely to cause aggregation when preparing an aqueous dispersion, and can produce a dry solid material that is easy to handle. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a scanning electron micrograph of the powdery dry solid produced in an embodiment of the present invention (Example 2). [Diagram 2] FIG. 2 is a scanning electron microscope photograph of the powdery dry solid produced in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] <Method of manufacturing powdered dry solid> A method for producing a powdery dry solid according to one embodiment of the present invention (hereinafter simply referred to as the production method of this embodiment) is a method for producing a powdery dry solid in which cellulose nanofibers and particles are composited. The production method of this embodiment includes a mixed solution preparation step of preparing a mixed solution in which particles are dispersed in an aqueous dispersion of cellulose nanofibers, and a drying and grinding step of evaporating and drying the mixed solution using a heat medium to obtain a thin-film dry solid, and then grinding the thin-film dry solid into a powder. Each step will be described below.

[0022] (mixture preparation process) The mixed liquid preparation step is a step of preparing a mixed liquid in which particles are dispersed in an aqueous dispersion of cellulose nanofibers.

[0023] Cellulose nanofiber Cellulose nanofibers are fine fibers obtained by fibrillating cellulose fibers. The cellulose nanofibers are provided as an aqueous dispersion of cellulose nanofibers. The raw material of the cellulose nanofibers is not particularly limited. For example, the raw material of the cellulose nanofibers may be derived from a plant material such as wood, an animal material such as a sea squirt, or a microorganism such as bacteria. Examples of the plant material include wood, straw, bamboo, bagasse, bamboo grass, reeds, and rice husks. In addition, the method of producing cellulose nanofibers using a plant material may include, for example, a chemical fiberization method in which the raw material is chemically treated to make it easy to fiberize, and then a physical treatment using mechanical shear force is performed to fiberize the raw material, or a mechanical fiberization method using known high shear force such as a high-pressure homogenizer method, a grinder grinding method, a freeze crushing method, a high shear force kneading method, and a ball mill grinding method.

[0024] The average fiber diameter of the cellulose nanofibers is not particularly limited. For example, the average fiber diameter of the cellulose nanofibers is preferably about 2 to 1000 nm, and more preferably about 5 to 300 nm. Cellulose nanofibers with such an average fiber diameter are easy to produce industrially. The average fiber diameter can be calculated by observing the cellulose fibers using a scanning electron microscope.

[0025] The average fiber length of the cellulose nanofibers is not particularly limited. For example, the average fiber length of the cellulose nanofibers is preferably about 0.5 to 10,000 μm, and more preferably about 10 to 3,000 μm. Cellulose nanofibers with such an average fiber length are easy to produce industrially. The average fiber length can be calculated by observing the cellulose fibers using a scanning electron microscope.

[0026] The aspect ratio (average fiber length / average fiber diameter) of the cellulose nanofiber is not particularly limited. For example, the aspect ratio of the cellulose nanofiber is preferably about 3 to 10,000, and more preferably about 5 to 1,000. Cellulose nanofibers with such an aspect ratio are easy to produce industrially.

[0027] The cellulose molecules constituting the cellulose nanofibers preferably have at least one of a carboxyl group, a hydrazide group, a hydrazine group, and a primary amino group. By using such cellulose nanofibers (modified cellulose nanofibers), the resulting coating composition exhibits an excellent deodorizing effect against odors from daily life in indoor spaces such as dwellings.

[0028] The carboxyl group is preferably a primary hydroxyl group at the C6 position of a glucose unit, which is a constituent unit of a cellulose molecule, oxidized. Cellulose fibers in which the primary hydroxyl group at the C6 position of a glucose unit is oxidized can be easily synthesized by using 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO). By reacting a cellulose molecule with TEMPO, the primary hydroxyl group at the C6 position of the glucose unit can be selectively oxidized to introduce a carboxyl group.

[0029] In this case, the content of carboxyl groups in the cellulose molecules is preferably 0.1 mmol or more, more preferably 0.5 mmol or more, per 1 g of cellulose nanofiber. When the content of carboxyl groups is within the above range, the resulting cellulose nanofiber can exhibit excellent adsorption performance for ammonia or amine. On the other hand, the content of carboxyl groups is preferably 5 mmol or less per 1 g of cellulose nanofiber. The above content can be calculated by titration.

[0030] In addition, the carboxyl group easily bonds with ammonia or amines, so the resulting coating composition containing cellulose nanofibers is suitable as an adsorbent for ammonia or amines.

[0031] Cellulose nanofibers containing cellulose molecules having hydrazide groups or hydrazine groups can be obtained by mixing and reacting cellulose fibers with a nitrogen-containing compound to bond the cellulose molecules with the nitrogen-containing compound. A suitable production method is to mix and react cellulose nanofibers having an average fiber diameter of about 2 to 1000 nm with a nitrogen-containing compound having a hydrazide group or hydrazine group.

[0032] The nitrogen-containing compound is not particularly limited as long as it has a hydrazide group or a hydrazine group. The nitrogen-containing compound having a hydrazide group is a monohydrazide compound having one hydrazide group in the molecule, a polyhydrazide compound having two or more hydrazide groups in the molecule, etc. Among these, a polyhydrazide compound having two or more hydrazide groups in the molecule is preferred, and a dihydrazide compound having two hydrazide groups in the molecule is more preferred.

[0033] The dihydrazide compound is not particularly limited. Examples of the dihydrazide compound include adipic acid dihydrazide, succinic acid dihydrazide, sebacic acid dihydrazide, isophthalic acid dihydrazide, and terephthalic acid dihydrazide. Among these, the dihydrazide compound is preferably adipic acid dihydrazide.

[0034] The nitrogen-containing compound having a hydrazine group is not particularly limited. For example, the nitrogen-containing compound having a hydrazine group is a monohydrazine compound having one hydrazine group in the molecule, a polyhydrazine compound having two or more hydrazine groups in the molecule, etc. Among these, the nitrogen-containing compound having a hydrazine group is preferably a monohydrazine compound having one hydrazine group in the molecule.

[0035] The hydrazide or hydrazine group easily bonds with aldehyde, so the resulting coating composition containing cellulose nanofibers is suitable as an aldehyde adsorbent.

[0036] Cellulose nanofibers containing cellulose molecules having primary amino groups can be prepared by a method of mixing and reacting cellulose fibers with a nitrogen-containing compound having multiple primary amino groups.

[0037] The nitrogen-containing compound is not particularly limited. For example, the nitrogen-containing compound may be a compound having a plurality of primary amino groups, and is preferably an aliphatic polyamine compound having a plurality of primary amino groups, and more preferably an aliphatic polyamine compound having two or more primary amino groups (-NH2) in the molecule.

[0038] Aliphatic polyamine compounds have a secondary amino group (-NHR 1 ) and tertiary amino groups (-NR 1 R 2 ) may be present. 1 and R 2 is any monovalent substituent. 1 and R 2 may be the same or different. The aliphatic polyamine compound may have a functional group other than an amino group, as long as the effect of the cellulose nanofiber of this embodiment is not impaired. Such functional groups include hydroxyl groups, halogen groups, ester groups, amide groups, nitro groups, and nitrile groups.

[0039] The carbon chain of the aliphatic polyamine compound may be linear or branched. Here, the aliphatic polyamine compound is preferably a compound (-CH2NH2) in which a primary amino group is bonded to a methylene group. In this case, the obtained cellulose nanofiber contains -CH2NH2. The aliphatic polyamine compound is preferably a diamine such as ethylenediamine, diaminopropane, diaminobutane, diaminopentane, diaminohexane, N,N'-bis(3-aminopropyl)ethylenediamine, and derivatives thereof; or a polyamine having three or more amino groups such as tris(2-aminoethyl)amine (TAEA), diethylenetriamine, triethylenetriamine, tetraethylenepentamine, polyethyleneimine (PEI), and derivatives thereof. Among these, the aliphatic polyamine compound is preferably a polyamine having three or more amino groups, and more preferably TAEA or PEI.

[0040] The molecular weight of the polyamine is preferably 100000 or less. From the viewpoint of excellent adsorption performance of fatty acids, the molecular weight of the polyamine is preferably 50000 or less, more preferably 10000 or less, and even more preferably 5000 or less. The molecular weight of the polyamine is usually 50 or more.

[0041] Primary amino groups react easily with carboxyl groups, so the resulting coating composition containing cellulose nanofibers can exhibit excellent adsorption performance for fatty acids that cause bad odors.

[0042] The fatty acids to be adsorbed are, for example, short-chain fatty acids having 8 or less carbon atoms, more specifically, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, hexenoic acid (e.g., (E)-3-methyl-2-hexenoic acid), and structural isomers thereof. These fatty acids are known to be the causative substances of malodors. Therefore, a paint composition containing cellulose nanofibers containing primary amino acids is likely to adsorb these substances that cause malodors, and shows excellent adsorption performance, especially for isovaleric acid.

[0043] The content of cellulose nanofibers in the aqueous dispersion (converted into solid content) is not particularly limited. For example, the content of cellulose nanofibers in the aqueous dispersion is preferably 0.1% by mass or more, more preferably 0.5% by mass or more. The content of cellulose nanofibers in the aqueous dispersion is preferably 20% by mass or less, more preferably 10% by mass or less. Since the content of cellulose nanofibers in the aqueous dispersion is within the above range, the production method of this embodiment is easy to evaporate and dry the mixed liquid in which particles are dispersed in the aqueous dispersion of cellulose nanofibers in the drying and grinding step, and has excellent production efficiency. Furthermore, the powdery dry solid of this embodiment can have a high content of cellulose nanofibers in this way. This is because, as described later, when producing the powdery dry solid of this embodiment, particles are used in combination, so that the particles adhere to the fibers of the cellulose nanofibers in the obtained powdery dry solid, making it difficult for the individual fibers of the cellulose nanofibers to come into contact with each other. As a result, the cellulose nanofibers can be highly blended because the aggregation between fibers is suppressed.

[0044] The organic solvent is preferably water or a mixed solvent of water and an organic solvent, which constitutes an aqueous dispersion. The organic solvent is not particularly limited as long as it is miscible with water. For example, the organic solvent is preferably an alcohol, more preferably ethanol.

[0045] ·particle The particles of this embodiment are blended together with the cellulose nanofibers to form a composite. By blending the particles, aggregation between the cellulose nanofiber fibers is less likely to occur in the resulting powdery dry solid. Specifically, by adhering the particles to the cellulose nanofiber fibers, the individual fibers of the cellulose nanofiber are less likely to come into contact with each other. This inhibits aggregation between the fibers when the dry solid is obtained. In this embodiment, "composite" refers to a state in which the particles are adsorbed and integrated with the cellulose nanofiber fibers. The particles may be primary particles, or may be secondary particles that are an aggregate of two or more particles.

[0046] The particles are not particularly limited. For example, the particles may be inorganic particles or organic particles that can withstand the heat treatment and the like in the mixed solution preparation step of this embodiment.

[0047] The inorganic particles are not particularly limited. Examples of the inorganic particles include metal particles such as barium ferrite, metal oxide particles such as titanium oxide, copper oxide, silicon oxide (silica), and iron oxide, and inorganic pigments such as silica (silicon oxide), calcium carbonate, talc, zeolite, alumina, barium sulfate, kaolinite, and carbon black.

[0048] The organic particles are not particularly limited. For example, the organic particles are synthetic resin particles, natural polymer particles, organic pigments, etc., which are useful as organic fillers. The organic particles are particles of resins such as acrylic resin, polyethylene, polypropylene, polyethylene oxide, polypropylene oxide, polyethyleneimine, polystyrene, polyurethane, polyurea, polyester, polyamide, polyimide, carboxymethyl cellulose, gelatin, starch, chitin, chitosan, etc. The organic pigments are phthalocyanine pigments, pyrrolopyrrole pigments, quinacridone pigments, etc.

[0049] In the manufacturing method of this embodiment, among the above particles, it is preferable that inorganic particles are contained, and it is more preferable that at least one of calcium carbonate and titanium oxide is contained. These are generally used as pigments in various types of paints, so that the obtained powdery dry solid can be applied to various types of paints and has high versatility in paints.

[0050] The volume average particle diameter of the particles is preferably 0.001 μm or more, more preferably 0.01 μm or more. The volume average particle diameter of the particles is preferably 100 μm or less, more preferably 50 μm or less. When the volume average particle diameter of the particles is within the above range, the resulting powdery dry solid is less likely to cause aggregation between the fibers of the cellulose nanofibers. Therefore, the powdery dry solid is less likely to cause aggregation when preparing an aqueous dispersion, and is more easily handled. The volume average particle diameter can be calculated by a laser diffraction / scattering method. The volume average particle diameter can be measured using a laser diffraction / scattering type particle size distribution measuring device (LA-910, manufactured by Horiba, Ltd.).

[0051] Returning to the explanation of the mixed solution preparation step, the method for preparing the mixed solution in which the above-mentioned aqueous dispersion and particles are dispersed is not particularly limited. As an example, the mixed solution can be prepared by mixing particles with an aqueous dispersion containing cellulose nanofibers and stirring with a disperser. The obtained mixed solution is then subjected to a drying and grinding step.

[0052] (Drying and grinding process) The drying and pulverizing step is a step of evaporating and drying the mixture using a heat medium to obtain a thin-film dry solid, and then pulverizing the thin-film dry solid into a powder. The moisture content of the dry solid after drying and pulverizing is, for example, 5% by mass or less.

[0053] The drying and pulverizing step may be carried out by a commercially available dryer. As an example, the drying and pulverizing step may be carried out by using an electrically conductive heating drum dryer (D-0405, manufactured by Katsuragi Kogyo Co., Ltd.). This allows the manufacturing method of this embodiment to be carried out easily. The mixed liquid is supplied to the surface of a rotating drum with a heat medium inside, and is evaporated and dried in a short time. This allows a thin-film dry solid from which the solvent of the aqueous dispersion has been removed to be obtained. The thin-film dry solid is then pulverized by a knife attached to the drum dryer. Specifically, the thin-film dry solid formed during one rotation of the drum is continuously scraped off from the drum surface by the knife. In the case of this drum dryer, a powder-like dry solid such as a sawdust-like, spherical, or pellet-like one can be obtained by adjusting the shape of the knife. In addition, the drying and pulverizing step does not necessarily require a step of shortening the cellulose nanofibers. Therefore, the manufacturing method of this embodiment is simpler than the conventional method because the step of shortening the fibers can be omitted. As other manufacturing methods using the drum dryer in the drying and pulverizing step, a manufacturing method using a horizontal thin film dryer or a vertical thin film dryer, a manufacturing method in which a mixed liquid is supplied to the top of a metal plate heated from the bottom, and the dried solid obtained on the metal plate is scraped off the surface of the metal plate with a knife, and a manufacturing method in which a mixed liquid is supplied to the inside of a rotating drum whose outside is covered with a heat medium, and the dried solid obtained on the inner surface of the drum is scraped off with a knife to obtain a dried solid can also be easily carried out. As in the case of a drum dryer, a powder-like dried solid such as a sawdust-like, spherical, or pellet-like shape can be obtained by adjusting the shape of the knife. In addition, the drying and pulverizing step does not require a step of shortening the cellulose nanofibers. Therefore, the manufacturing method of this embodiment is simpler than the conventional method because the step of shortening the fibers can be omitted.

[0054] The heat medium is not particularly limited. For example, the heat medium is steam, water, oil, etc. When the heat medium is steam, the steam is water vapor. As a result, the drum surface is heated to about 100 to 200°C, and the supplied mixed liquid can be evaporated and dried in a short time.

[0055] The specifications of the drum dryer are not particularly limited. For example, the drum dryer may be of a normal pressure type or a vacuum type. In addition, the drum dryer may be of a double drum type, a twin drum type, or a single drum type.

[0056] The rotation speed of the drum in the drum dryer is not particularly limited. For example, the rotation speed of the drum is 1 to 6 rpm. This allows the mixed liquid supplied to the drum surface to evaporate and dry during one rotation of the drum, making it easy to produce a thin-film dry solid.

[0057] The method of supplying the mixed liquid is not particularly limited. For example, the mixed liquid may be supplied by a dip method, a spray method, a splash method, an upper roll method (single stage, multistage), a side roll method, a lower roll method, etc. By adopting these methods, the mixed liquid is easily supplied uniformly and in an appropriate amount to the drum surface.

[0058] In this embodiment, a drum dryer that continuously dries the mixed liquid and pulverizes the obtained thin-film dried product is exemplified as an apparatus for performing the drying and pulverization process. The apparatus for performing the drying and pulverization process of this embodiment is not limited to the drum dryer described above. That is, in the drying and pulverization process of this embodiment, a drying device that dries the mixed liquid and a pulverization device that pulverizes the obtained thin-film dried product may be provided separately.

[0059] As described above, the manufacturing method of this embodiment does not require a step of shortening the cellulose nanofibers, and is therefore simple. Furthermore, the resulting powdery dry solid highly suppresses aggregation between the cellulose nanofibers due to the incorporation of particles. Therefore, the powdery dry solid is less likely to aggregate when preparing an aqueous dispersion, and is easy to handle.

[0060] The size of the powdery dry solid is not particularly limited. For example, the size is 10 mesh (1.70 mm mesh size) or less. A powdery dry solid having such a size is lightweight and easily mixed with other powdery chemicals. For example, the powdery dry solid can be suitably formulated as a paint composition or the like.

[0061] Furthermore, as described above, when the cellulose molecules constituting the cellulose nanofibers have at least one of a carboxyl group, a hydrazide group, a hydrazine group, and a primary amino group, a powdery dry solid containing such cellulose nanofibers can be suitably used as a coating composition exhibiting a deodorizing effect. That is, since the powdery dry solid has excellent adsorption performance for substances that can cause malodors, it is suitable as a coating composition used as a coating material for the walls and ceilings of indoor spaces such as residences (especially toilets, etc.), chemical plants, wastewater treatment plants, sewage treatment plants, hospitals, nursing homes, agricultural product processing plants, and livestock processing plants. As a result, the coating composition can exhibit an excellent deodorizing effect, for example, in the various application locations described above. EXAMPLES

[0062] The present invention will be described in more detail below with reference to the following examples. The present invention is not limited to these examples. Unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass".

[0063] The raw materials used are shown below. <Cellulose nanofiber> Cellulose nanofiber 1: AAn-CAT, manufactured by Maniwa Biochemical Co., Ltd., cellulose nanofiber bound with adipic acid dihydrazide, average fiber diameter 20-200 nm, average fiber length 500 μm Cellulose nanofiber 2: i-CAT, manufactured by Maniwa Biochemical Co., Ltd., cellulose nanofiber with primary amino groups bonded, average fiber diameter 5-300 nm, average fiber length 500 μm, Cellulose nanofiber 3: CNF mixture, manufactured by Maniwa Biochemical Co., Ltd., an equal mixture of cellulose nanofibers 1, 2 and 4, average fiber diameter 20-200 nm, average fiber length 500 μm Cellulose nanofiber 4: Cellfim (CNF) C-100, manufactured by Mori Machinery Co., Ltd., average fiber diameter 20-200 nm, average fiber length 500 μm, mechanically defibrated Cellulose nanofiber 5: Rheocrysta, Daiichi Kogyo Seiyaku Co., Ltd., average fiber diameter 3 nm, average fiber length 150 to 3000 nm, chemically defibrated The contents in Table 1 are all for aqueous dispersions (solvent: water) in which these cellulose nanofibers are dispersed so that the solid content is 1% by mass. <particle> Calcium carbonate: Sunlight SL-300, Takehara Chemical Industry Co., Ltd., calcium bicarbonate, volume average particle size 5 μm Titanium oxide: Ti-Pure R-706, manufactured by Chemours, Inc., volume average particle size 0.36 μm Carbon black: MA100, manufactured by Mitsubishi Chemical Corporation, volume average particle size 13 to 76 μm

[0064] Example 1 100 parts by mass of calcium carbonate and 100 parts by mass of an aqueous dispersion of cellulose nanofiber 1 (solid content 1% by mass) were mixed and stirred with a disperser to prepare a mixture (mixture preparation process). The mixture obtained was evaporated and dried using a drum dryer (D-0405 model, Katsuragi Kogyo Co., Ltd., heat medium: water vapor) at a vapor pressure of 0.3 MPa·G and a drum rotation speed of 2 rpm to produce a thin-film dry solid, which was then scraped off from the drum surface with a scraper knife attached to the drum dryer to obtain a sawdust-like dry solid (grain size 10 mesh or less).

[0065] (Examples 2 to 15) A thin-film-like dry solid was obtained in the same manner as in Example 1, except that the composition was changed to the composition (parts by mass) shown in Table 1 below.

[0066] Comparative Example 1 100 parts by mass of an aqueous dispersion of cellulose nanofiber 4 (solid content 1% by mass) was evaporated and dried using a drum dryer (D-0405 model, Katsuragi Kogyo Co., Ltd., heat medium: water vapor) at a steam pressure of 0.3 MPa·G and a drum rotation speed of 2 rpm to produce a thin-film dry solid. The thin-film dry solid was then scraped off from the drum surface with a scraper knife attached to the drum dryer to obtain a sawdust-like dry solid (particle size 10 mesh or less).

[0067] Comparative Example 2 A sawdust-like dry solid (particle size 10 mesh or less) was obtained using a tumbling fluidized bed granulator (SPIR-A-FLOW SFC-MINI, manufactured by Freund Corporation) to spray 100 parts by mass of an aqueous dispersion of cellulose nanofiber 1 (solid content 1% by mass) onto 100 parts by mass of calcium carbonate at a liquid feed rate of 8 g / min.

[0068] [Table 1]

[0069] The obtained powdery dry solid was observed using a scanning electron microscope (manufactured by JEOL Ltd., secondary electron image, 5000x magnification). FIG. 1 is a scanning electron microscope photograph of the powdery dry solid produced in Example 2. In FIG. 1, reference symbol 1 indicates cellulose nanofiber fibers. Reference symbol 2 indicates particles (calcium carbonate). As shown in FIG. 1, in the powdery dry solid of Example 2, cellulose nanofiber fiber 1 was less likely to cause aggregation between fibers, and many fibers without aggregation were observed. In addition, when the powdery dry solids produced in Examples 1 and 3 to 15 were also observed under a microscope, they had the same appearance, and many sites where the aggregation between the cellulose nanofiber fibers was relaxed were observed. Thus, according to the production method of the present invention, since the aggregation between the cellulose nanofiber fibers is suppressed, it was considered that the obtained powdery dry solid is less likely to cause aggregation when preparing an aqueous dispersion and has excellent handleability. In addition, as seen in Examples 3 and 4, the powdery dry solid contains a large proportion (solid content) of cellulose nanofibers. Even in such a case, the powdery dry solid is unlikely to aggregate when preparing an aqueous dispersion. Therefore, for example, when a coating composition is prepared using such a powdery dry solid, the coating composition may contain a large amount of cellulose nanofibers.

[0070] Meanwhile, Fig. 2 is a scanning electron microscope photograph of the powdery dry solid produced in Comparative Example 1. In Fig. 2, reference symbol 3 indicates aggregated cellulose nanofiber fibers. As shown in Fig. 2, in the powdery dry solid of Comparative Example 1, the cellulose nanofiber fibers were tightly aggregated. It was considered that such a dry solid of cellulose nanofibers in which fibers were aggregated was prone to aggregation when preparing an aqueous dispersion, and had poor handleability.

[0071] The processing time required to produce the dry solids in Examples 1 to 15 was 1 to 2 minutes / kg. On the other hand, the processing time required to produce the powdery dry solids in Comparative Example 2 was 90 minutes / kg. Therefore, the production method of the present invention was efficient with a short processing time.

Claims

1. A method for producing a powdery dry solid material in which cellulose nanofibers and particles are composited, The particles include at least one of calcium carbonate, titanium oxide, and carbon black, The blending ratio (mass ratio) of the cellulose nanofiber (solid content) to the particles is cellulose nanofiber (solid content):particles=1:100 to 90:10, A mixed liquid preparation step of preparing a mixed liquid in which particles are dispersed in an aqueous dispersion of cellulose nanofibers; a drying and grinding step of evaporating and drying the mixed liquid using a heat medium to obtain a thin-film dry solid, and then grinding the thin-film dry solid into a powder.

2. 2. The method for producing a powdery dry solid according to claim 1, wherein the drying and grinding step is a step of supplying the mixed liquid to a surface of a rotating drum containing a heat transfer medium therein, evaporating and drying the mixed liquid to obtain the thin-film dry solid, and then grinding the thin-film dry solid into powder by continuously scraping it off from the drum surface with a knife.

3. The method for producing a powdery dry solid material according to claim 1 or 2, wherein the particles have a volume average particle size of 0.001 to 100 μm as measured by a laser diffraction / scattering method.

4. The method for producing a powdery dry solid material according to any one of claims 1 to 3, wherein the particles contain at least one of calcium carbonate or titanium oxide.

5. The method for producing a powdery dry solid material according to any one of claims 1 to 4, wherein the cellulose molecules constituting the cellulose nanofibers have at least one of a carboxyl group, a hydrazide group, a hydrazine group, and a primary amino group.

Citation Information

Patent Citations

  • A method for producing a dispersion containing nanoparticles and the dispersion produced by the said method.

    JP2014530946A

  • Dry solid article of cellulose nanofiber and manufacturing method thereof

    JP2017008176A

  • Fine fibrous cellulose-containing material

    JP2017057391A

  • Manufacturing method of dry solid article of cellulose nanofiber

    JP2017095664A

  • Polyanion type positive electrode active material granulated body and method for producing the same

    JP2018026253A