Cyclic olefin copolymer and method for producing the same

A controlled addition polymerization process using a titanocene catalyst and borate compound in cyclic olefin copolymers with specific α-olefins addresses the challenge of achieving both high breaking strain and toughness, resulting in improved mechanical properties for diverse applications.

JP7586666B2Active Publication Date: 2024-11-19POLYPLASTICS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020134008
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-06
Publication Date
2024-11-19
Estimated Expiration
2040-08-06

AI Technical Summary

Technical Problem

Existing cyclic olefin copolymers with specific α-olefins face challenges in achieving both excellent breaking strain and toughness, making them unsuitable for molding materials.

Method used

A cyclic olefin copolymer with a specific α-olefin composition, utilizing a titanocene catalyst and borate compound, is produced through controlled addition polymerization with a mole ratio of α-olefin between 10% to 40% and multiple glass transition temperatures ranging from 0°C to 300°C.

Benefits of technology

The resulting copolymer exhibits enhanced mechanical properties, including tensile strength, strain at break, and toughness, suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586666000001
    Figure 0007586666000001
  • Figure 0007586666000002
    Figure 0007586666000002
  • Figure 0007586666000003
    Figure 0007586666000003
Patent Text Reader

Abstract

To provide: a cyclic olefin copolymer having both excellent fracture strain and excellent toughness, which is a copolymer of a cyclic olefin monomer and a C3-20 α-olefin; and a method for producing a cyclic olefin copolymer, which enables satisfactory production of the cyclic olefin copolymer.SOLUTION: There is provided a copolymer of a cyclic olefin monomer and a C3-20 α-olefin, where a content of a structural unit derived from the α-olefin is set to 10 mole% to 40 mole% relative to whole structural units and the cyclic olefin copolymer is configured to have two or more glass transition temperatures in a range of 0°C to 300°C as obtained by solid viscoelasticity measurement.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cyclic olefin copolymer and a method for producing the cyclic olefin copolymer. [Background technology]

[0002] Cyclic olefin polymers and cyclic olefin copolymers (also called "COP" and "COC", respectively) have low moisture absorption and high transparency. For this reason, COPs and COCs are used in various applications, including the field of optical materials such as optical disk substrates, optical films, and optical fibers. A representative COC is a copolymer of cyclic olefin and ethylene. The glass transition temperature of such a copolymer can be changed by the copolymerization composition of the cyclic olefin and ethylene. For this reason, a copolymer of cyclic olefin and ethylene can be produced as a copolymer with a higher glass transition temperature (Tg) than COP, and it is possible to realize a Tg of over 200°C, which is difficult to achieve with COP. However, such copolymers are hard and brittle. For this reason, such copolymers have problems such as low mechanical strength and poor handling and processability.

[0003] One of the methods to improve the mechanical strength of high TgCOC is to copolymerize cyclic olefins with α-olefins other than ethylene (hereinafter referred to as "specific α-olefins"). Various studies have been conducted on the copolymerization of cyclic olefins with specific α-olefins.

[0004] The copolymerization of cyclic olefins and specific α-olefins is significantly different from the copolymerization of cyclic olefins and ethylene. Under the conditions where a high molecular weight material is obtained by the copolymerization of cyclic olefins and ethylene, a chain transfer reaction caused by the specific α-olefin occurs in the copolymerization of cyclic olefins and specific α-olefins, so that it has been difficult to obtain a high molecular weight material. Therefore, the copolymer of cyclic olefins and specific α-olefins has been considered to be unsuitable for molding materials (for example, see Non-Patent Document 1).

[0005] For this reason, various studies have been conducted on improving the moldability of copolymers of cyclic olefins and specific α-olefins.For example, as a method for producing a copolymer of cyclic olefins and specific α-olefins that has a relatively high molecular weight and can be molded into a film, a method has been proposed in which a cyclic olefin and a specific α-olefin are copolymerized in the presence of a titanocene catalyst having a specific structure and triphenylmethylium tetrakis(pentafluorophenyl)borate (see Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2016-56275 A [Non-patent literature]

[0007] [Non-Patent Document 1] Jung, HY et al., Polyhedron, 2005, Vol. 24, pp. 1269-1273 Summary of the Invention [Problem to be solved by the invention]

[0008] However, even by the method described in Patent Document 1, it is difficult to produce a copolymer of a cyclic olefin and a specific α-olefin, which has both excellent breaking strain and toughness, as a cyclic olefin copolymer.

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a cyclic olefin copolymer, which is a copolymer of a cyclic olefin monomer and an α-olefin having from 3 to 20 carbon atoms, and which combines excellent breaking strain and excellent toughness, and a method and process for producing the cyclic olefin copolymer, which can satisfactorily produce the cyclic olefin copolymer. [Means for solving the problem]

[0010] The present inventors have found that the above-mentioned problems can be solved by controlling the amount of structural units derived from α-olefin to 10 mol % to 40 mol % of the total structural units in a copolymer of a cyclic olefin monomer and an α-olefin having 3 to 20 carbon atoms, and by making the cyclic olefin copolymer have two or more glass transition temperatures determined by solid viscoelasticity measurement within the range of 0°C to 300°C, and have thus completed the present invention. More specifically, the present invention provides the following.

[0011] (I) A cyclic olefin copolymer which is an addition polymer of a cyclic olefin monomer and an α-olefin having 3 to 20 carbon atoms, the ratio of the number of moles of structural units derived from α-olefins to the number of moles of all structural units is 10 mol % or more and 40 mol % or less; A cyclic olefin copolymer having two or more glass transition temperatures within the range of 0°C to 300°C as determined by viscoelasticity measurement.

[0012] (II) The cyclic olefin copolymer according to (I), which has at least one glass transition temperature within the range of 0°C to 100°C and at least one glass transition temperature within the range of 160°C to 300°C.

[0013] (III) The cyclic olefin copolymer according to (I) or (II), which has at least one glass transition temperature in the range of less than 0°C, in the range of 0°C to 100°C, and in the range of 160°C to 300°C.

[0014] (VI) A method for producing the cyclic olefin copolymer according to any one of (I) to (III), comprising the steps of: The method includes addition polymerizing the cyclic olefin monomer and the α-olefin in the presence of a titanocene catalyst represented by the following formula (1) and a co-catalyst, The co-catalyst comprises a borate compound and a hindered phenol; A production method in which a cyclic olefin monomer and an α-olefin are each added in two or more batches to a reaction system in which addition polymerization is carried out. [ka] (In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms; R 4 and R 5 are each independently an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or a halogen atom; R 6 ~R 13 are each independently a hydrogen atom, an alkyl group having from 1 to 12 carbon atoms, an aryl group having from 6 to 12 carbon atoms, or a silyl group which may have a monovalent hydrocarbon group having from 1 to 12 carbon atoms as a substituent.

[0015] (V) A method for producing the cyclic olefin copolymer according to (I) or (II), comprising the steps of: The method includes addition polymerizing a cyclic olefin monomer and an α-olefin in the presence of a titanocene catalyst represented by the following formula (1) and a cocatalyst, The co-catalyst comprises a borate compound and a hindered phenol; The process for producing the product, wherein the addition polymerization is carried out at a temperature in the range of 10°C or more and 60°C or less. [ka] (In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms; R 4 and R 5 are each independently an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or a halogen atom; R 6 ~R 13 are each independently a hydrogen atom, an alkyl group having from 1 to 12 carbon atoms, an aryl group having from 6 to 12 carbon atoms, or a silyl group which may have a monovalent hydrocarbon group having from 1 to 12 carbon atoms as a substituent. Effect of the Invention

[0016] According to the present invention, there can be provided a cyclic olefin copolymer, which is a copolymer of a cyclic olefin monomer and an α-olefin having from 3 to 20 carbon atoms, having both excellent breaking strain and excellent toughness, and a method and process for producing the cyclic olefin copolymer, which can satisfactorily produce the cyclic olefin copolymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments.

[0018] <Cyclic olefin copolymer> The cyclic olefin copolymer is an addition polymer of a cyclic olefin monomer and an α-olefin having 3 to 20 carbon atoms. In the cyclic olefin copolymer, the ratio of the number of moles of structural units derived from α-olefin to the number of moles of all structural units is 10 mol % to 40 mol %. In addition, the cyclic olefin copolymer has two or more glass transition temperatures within the range of 0°C to 300°C as determined by viscoelasticity measurement.

[0019] Although the detailed mechanism is unclear, the above-mentioned cyclic olefin copolymer has both excellent breaking strain and excellent toughness. Specifically, the cyclic olefin copolymer exhibits a tensile strength of preferably 25 MPa or more, more preferably 30 MPa or more, and even more preferably 40 MPa or more, as measured in a tensile test performed at 23°C using a No. 2 dumbbell test piece having a thickness of 50 μm according to a method in accordance with ISO 527-3. Furthermore, the cyclic olefin copolymer preferably exhibits a breaking strain of 3.5% or more, more preferably 5% or more, as measured by the tensile test according to the above method. Furthermore, the cyclic olefin copolymer preferably exhibits a tensile modulus of 1000 MPa or more, more preferably 1100 MPa or more, and even more preferably 1500 MPa or more, as measured by the tensile test according to the above method.

[0020] In the cyclic olefin copolymer, the ratio of the number of moles of structural units derived from α-olefin to the number of moles of all structural units is 10 mol% or more and 40 mol% or less, preferably 20 mol% or more and 30 mol% or less. If the ratio of the number of moles of structural units derived from α-olefin is too high, it is difficult to obtain a cyclic olefin copolymer having high tensile strength and tensile modulus. If the ratio of the number of moles of structural units derived from α-olefin is too high, it is difficult to obtain a cyclic olefin copolymer having a high glass transition temperature and excellent heat resistance. The ratio of the number of moles of structural units derived from α-olefins is 13 It can be calculated by measuring the C-NMR spectrum.

[0021] The cyclic olefin copolymer may contain structural units other than the structural units derived from the cyclic olefin monomer and the structural units derived from an α-olefin having 3 to 20 carbon atoms, provided that the object of the present invention is not impaired. As the other structural units, structural units derived from a compound having a carbon-carbon unsaturated double bond and capable of copolymerizing with the cyclic olefin monomer and the α-olefin having 3 to 20 carbon atoms may be adopted. Typically, structural units derived from ethylene are preferred as the other structural units.

[0022] In the cyclic olefin copolymer, the sum of the ratio of the number of moles of structural units derived from cyclic olefin monomers and the ratio of the number of moles of structural units derived from α-olefins to the number of moles of all structural units is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and most preferably 100 mol%.

[0023] The cyclic olefin copolymer has two or more glass transition temperatures within the range of 0°C to 300°C as determined by viscoelasticity measurement. The glass transition temperature can be measured by observing the viscoelastic behavior of a 50 μm-thick film-like molded product with a solid rheometer at −100° C. to 300° C. Specifically, the glass transition temperature is determined as the peak top temperature of the tan δ chart obtained by the above-mentioned measurement.

[0024] The cyclic olefin copolymer preferably has at least one glass transition temperature within the range of 0°C to 100°C and at least one glass transition temperature within the range of 160°C to 300°C, since the mechanical properties measured by the above tensile test are good. In particular, since the breaking strain measured by the above tensile test is large, it is preferable that the cyclic olefin copolymer has at least one glass transition temperature each in the range of less than 0°C, in the range of 0°C to 100°C, and in the range of 160°C to 300°C. Within the above range of 0°C to 100°C, the range of 30°C to 80°C is preferred, and the range of 40°C to 70°C is more preferred. Within the above range of 160°C to 300°C, 170°C to 280°C is preferred, and 180°C to 270°C is more preferred. Within the above range of less than 0°C, -50°C to 0°C is preferred, and -40°C to -10°C is more preferred.

[0025] Typically, the cyclic olefin copolymer has one glass transition temperature each in the range of 0°C to 100°C and in the range of 160°C to 300°C, or has one glass transition temperature each in the range below 0°C, the range of 0°C to 100°C, and the range of 160°C to 300°C.

[0026] The molecular weight of the cyclic olefin copolymer is not particularly limited. The weight average molecular weight (Mw) of the cyclic olefin copolymer is preferably 5,000 to 200,000, more preferably 10,000 to 100,000, in terms of polystyrene, measured by gel permeation chromatography (GPC). The number average molecular weight (Mn) of the cyclic olefin copolymer is preferably 5,000 or more and 200,000 or less, and more preferably 10,000 or more and 100,000 or less, in terms of polystyrene, measured by gel permeation chromatography (GPC). The dispersion ratio (Mw / Mn) is preferably 1.2 or more, and more preferably 1.3 or more.

[0027] <Cyclic olefin monomer> The cyclic olefin monomer is not particularly limited as long as it does not impair the object of the present invention. Typically, norbornene and substituted norbornene are preferably used as the cyclic olefin monomer. Norbornene is particularly preferred as the cyclic olefin monomer, in terms of the good balance of cost, polymerizability, and physical properties of the resulting cyclic olefin copolymer. The cyclic olefin monomer may be used alone or in combination of two or more.

[0028] The substituted norbornene is not particularly limited. Examples of the substituents of the substituted norbornene include halogen atoms and monovalent or divalent hydrocarbon groups. Specific examples of the substituted norbornene include the compound represented by the following formula (I).

[0029] [ka]

[0030] In formula (I), R a1 ~R a12 may be the same or different and are atoms or groups selected from the group consisting of hydrogen atoms, halogen atoms, and hydrocarbon groups. R a9 and R a10 , R a11 and R 12 may combine together to form a divalent hydrocarbon group. R a9 or R a10 And, R a11 or R a12 may be bonded to each other to form a ring. n is 0 or a positive integer. If n is 2 or more, R a5 ~R a8 may be the same or different in each repeating unit. However, if n is 0, then R a1 ~R a4 and R a9 ~R a12 At least one of is not a hydrogen atom.

[0031] R a1 ~R a8 Specific examples of R include a hydrogen atom; a halogen atom such as fluorine, chlorine, and bromine; and an alkyl group having 1 to 20 carbon atoms. a1 ~R a8 may all consist of different atoms or groups. a1 ~R a8 Some or all of these may be the same atom or group.

[0032] R a9 ~R a12 Specific examples of R include a hydrogen atom; halogen atoms such as fluorine, chlorine, and bromine; alkyl groups having 1 to 20 carbon atoms; cycloalkyl groups such as a cyclohexyl group; substituted or unsubstituted aromatic hydrocarbon groups such as a phenyl group, a tolyl group, an ethylphenyl group, an isopropylphenyl group, a naphthyl group, and an anthryl group; and aralkyl groups such as a benzyl group and a phenethyl group. a9 ~R a12 may all consist of different atoms or groups. a9 ~R a12 Some or all of these may be the same atom or group.

[0033] R a9 and R a10 , or R a11 and R a12 Specific examples of divalent hydrocarbon groups that can be formed by combining the above include alkylidene groups such as an ethylidene group, a propylidene group, and an isopropylidene group.

[0034] R a9 or R a10 And, R a11 or R a12 When they are bonded to each other to form a ring, the ring formed may be a monocyclic ring or a polycyclic ring. The ring formed may be a polycyclic ring having a bridge. The ring formed may have a double bond. The ring formed may have a substituent such as a methyl group.

[0035] Specific examples of the substituted norbornene represented by formula (I) include 5-methyl-bicyclo[2.2.1]hept-2-ene, 5,5-dimethyl-bicyclo[2.2.1]hept-2-ene, 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-butyl-bicyclo[2.2.1]hept-2-ene, 5-ethylidene-bicyclo[2.2.1]hept-2-ene, 5-hexyl-bicyclo[2.2.1]hept-2-ene, 5-methyl-bicyclo[2.2.1]hept-2-ene, 5,5-dimethyl-bicyclo[2.2.1]hept-2-ene, 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-hexyl ... Bicyclic olefins such as cyclo[2.2.1]hept-2-ene, 5-octyl-bicyclo[2.2.1]hept-2-ene, 5-octadecyl-bicyclo[2.2.1]hept-2-ene, 5-methylidene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, and 5-propenyl-bicyclo[2.2.1]hept-2-ene; Tricyclo[4.3.0.1 2,5 ]Deca-3,7-diene (common name: dicyclopentadiene), tricyclo[4.3.0.1 2,5 ]dec-3-ene; tricyclo[4.4.0.1 2,5 ]Undeca-3,7-diene or tricyclo[4.4.0.1 2,5 ]Undeca-3,8-diene or partially hydrogenated products thereof (or an adduct of cyclopentadiene and cyclohexene) 2,5 ]undec-3-ene; three-ring cyclic olefins such as 5-cyclopentyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexenyl-bicyclo[2.2.1]hept-2-ene, and 5-phenyl-bicyclo[2.2.1]hept-2-ene; Tetracyclo[4.4.0.12,5 .1 7,10 ]dodec-3-ene (also called tetracyclododecene), 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethyltetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-methylidenetetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethylidenetetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-vinyltetracyclo[4,4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-propenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] 4-ring cyclic olefins such as dodec-3-ene; 8-Cyclopentyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-cyclohexyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-cyclohexenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-phenyl-cyclopentyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene;tetracyclo[7.4.1 3,6 .0 1,9 .0 2,7 ]tetradeca-4,9,11,13-tetraene (also called 1,4-methano-1,4,4a,9a-tetrahydrofluorene), tetracyclo[8.4.1 4,7 .0 1,10 .0 3,8 ]Pentadeca-5,10,12,14-tetraene (also called 1,4-methano-1,4,4a,5,10,10a-hexahydroanthracene); Pentacyclo[6.6.1.1 3,6 .0 2,7 .0 9,14 ]-4-Hexadecene, Pentacyclo[6.5.1.13,6 .0 2,7 .0 9,13 ]-4-Pentadecene, Pentacyclo[7.4.0.0 2,7 .1 3,6 .1 10,13 ]-4-Pentadecene;Heptacyclo[8.7.0.1 2,9 .1 4,7 .1 11,17 .0 3,8 .0 12,16 ]-5-Eicosene, heptacyclo[8.7.0.1 2,9 .0 3,8 .1 4,7 .0 12,17 .1 13,l6 ]-14-eicosene; and polycyclic olefins such as a tetramer of cyclopentadiene.

[0036] Among these, for example, alkyl-substituted norbornenes such as bicyclo[2.2.1]hept-2-ene substituted with one or more alkyl groups, and alkylidene-substituted norbornenes such as bicyclo[2.2.1]hept-2-ene substituted with one or more alkylidene groups are preferred. 5-Ethylidene-bicyclo[2.2.1]hept-2-ene (common name: 5-ethylidene-2-norbornene, or simply ethylidenenorbornene) is particularly preferred.

[0037] <α-Olefin> The α-olefin is an α-olefin having 3 to 20 carbon atoms. As such an α-olefin, not only unsubstituted α-olefins but also substituted α-olefins having a substituent such as a halogen atom can be used. The number of carbon atoms in the α-olefin is 3 to 20, preferably 4 to 12, and more preferably 6 to 10.

[0038] Specific examples of α-olefins having 3 to 12 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, and 1-dodecene. Among these, 1-hexene, 1-octene, and 1-decene are preferred.

[0039] The above-mentioned cyclic olefin copolymer may be mixed with various additives as necessary, and then molded into, for example, a film, a sheet, etc., and may be used widely in various applications such as packaging applications, optical applications, etc. Examples of additives that may be added to the cyclic olefin copolymer include antioxidants, weather stabilizers, ultraviolet absorbers, antibacterial agents, flame retardants, colorants, etc. These additives are added to the cyclic olefin copolymer in amounts taking into account the general amounts used according to the type of additive.

[0040] <Method for producing cyclic olefin copolymer> The method for producing the cyclic olefin copolymer will now be described. The method for producing a cyclic olefin copolymer includes addition polymerizing a cyclic olefin monomer and an α-olefin in the presence of a titanocene catalyst represented by the following formula (1) and a co-catalyst, the co-catalyst including a borate compound and a hindered phenol. In the above production method, the cyclic olefin monomer and the α-olefin are each added in two or more batches into the reaction system where the addition polymerization is carried out. [ka] (In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms; R 4 and R 5are each independently an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or a halogen atom; R 6 ~R 13 are each independently a hydrogen atom, an alkyl group having from 1 to 12 carbon atoms, an aryl group having from 6 to 12 carbon atoms, or a silyl group which may have a monovalent hydrocarbon group having from 1 to 12 carbon atoms as a substituent.

[0041] According to this method, a cyclic olefin copolymer satisfying any one of the constituent requirements (I) to (III) above can be provided. Hereinafter, this method will also be referred to as the "first production method."

[0042] The following production method is also preferred as a method for producing a cyclic olefin copolymer, which can provide a cyclic olefin copolymer that satisfies the constituent requirement described in (I) or (II) above. Specifically, this method includes addition polymerizing a cyclic olefin monomer and an α-olefin in the presence of a titanocene catalyst represented by formula (1) and a co-catalyst. The co-catalyst includes a borate compound and a hindered phenol. The addition polymerization is carried out at a temperature in the range of 10°C to 60°C. The titanocene catalyst represented by formula (1) is the same as the titanocene catalyst described above for the first production method. Hereinafter, this method will also be referred to as the "second production method."

[0043] <First manufacturing method> In the first production method, a monomer containing the above-mentioned cyclic olefin monomer and α-olefin is used. The type of cyclic olefin monomer, the type of α-olefin, and the copolymerization ratio thereof are the same as those described for the cyclic olefin copolymer.

[0044] In the first production method, the cyclic olefin monomer and the α-olefin are each added in two or more portions to a reaction system in which addition polymerization is carried out. In this way, by adding the cyclic olefin monomer and the α-olefin, it is easy to obtain a cyclic olefin copolymer having good mechanical properties. Also, by adding the cyclic olefin monomer and the α-olefin, it is easy to obtain a cyclic olefin copolymer having a glass transition temperature in the range of less than 0°C.

[0045] When adding in portions, the number of portions is not particularly limited. For example, the number of portions is preferably from 2 to 5, more preferably 2 or 3, and even more preferably 2. When adding in portions, the amount of cyclic olefin monomer or α-olefin added per portion is preferably TA / N×0.5 or more and TA / N×1.5 or less, more preferably TA / N×0.7 or more and TA / N×1.3 or less, and even more preferably TA / N×0.9 or more and TA / N×1.1 or less, where TA is the mass of the total amount added and N is the number of portions added.

[0046] When the number of divisions is two, the amount of cyclic olefin monomer or α-olefin added per division is preferably 25% by mass or more and 75% by mass or less, more preferably 35% by mass or more and 65% by mass or more, and even more preferably 45% by mass or more and 55% by mass or less, based on the total mass of the addition amount.

[0047] When the divided addition is performed, at least one of the cyclic olefin monomer and the α-olefin is added to the reaction vessel at or before the start of the addition polymerization, and then, at any timing after the start of the addition polymerization, the second or subsequent addition of the cyclic olefin monomer or the α-olefin is performed. When the addition is carried out in portions, the time between each addition is preferably from 3 to 20 minutes, more preferably from 5 to 15 minutes. When the divided additions are carried out, the timing of addition of the cyclic olefin monomer and the timing of addition of the α-olefin may be simultaneous or different. The number of portions for adding the cyclic olefin monomer may be different from the number of portions for adding the α-olefin.

[0048] As described above, the titanocene catalyst represented by the above formula (1) is used in producing a cyclic olefin copolymer. In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms. Specific examples thereof include alkyl groups such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, a hexyl group, a cyclopentyl group, and a cyclohexyl group; and aryl groups such as a phenyl group, a biphenyl group, a phenyl group or a biphenyl group having the above alkyl group as a substituent, a naphthyl group, and a naphthyl group having the above alkyl group as a substituent.

[0049] R 4 and R 5 are each independently an alkyl group having from 1 to 12 carbon atoms, an aryl group having from 6 to 12 carbon atoms, or a halogen atom, and specific examples thereof include a halogen atom such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom; a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a cyclopentyl group, a cyclohexyl group, or any of these alkyl groups having the above-mentioned halogen atom as a substituent; a phenyl group, a biphenyl group, a naphthyl group, or any of these aryl groups having the above-mentioned halogen atom or alkyl group as a substituent.

[0050] R 6 ~R 13are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or a silyl group which may have a monovalent hydrocarbon group having 1 to 12 carbon atoms as a substituent. Specific examples of the alkyl group having 1 to 12 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a cyclopentyl group, and a cyclohexyl group. Specific examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a biphenyl group, a naphthyl group, and the above aryl groups having the alkyl group as a substituent. Furthermore, specific examples of silyl groups having a monovalent hydrocarbon group having from 1 to 12 carbon atoms as a substituent include silyl groups having an alkyl group having from 1 to 12 carbon atoms as a substituent, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a cyclopentyl group, or a cyclohexyl group.

[0051] Specific examples of the titanocene catalyst represented by the general formula (1) include (isopropylamido)dimethyl-9-fluorenylsilane titanium dimethyl, (isobutylamido)dimethyl-9-fluorenylsilane titanium dimethyl, (t-butylamido)dimethyl-9-fluorenylsilane titanium dimethyl, (isopropylamido)dimethyl-9-fluorenylsilane titanium dichloride, (isobutylamido)dimethyl-9-(3,6-dimethylfluorenyl)silane titanium dichloride, (t-butylamido)dimethyl-9-fluorenylsilane titanium dichloride, ( Isopropylamido)dimethyl-9-(3,6-dimethylfluorenyl)silanetitanium dichloride, (isobutylamido)dimethyl-9-(3,6-dimethylfluorenyl)silanetitanium dichloride, (t-butylamido)dimethyl-9-(3,6-dimethylfluorenyl)silanetitanium dimethyl, (isopropylamido)dimethyl-9-[3,6-di(i-propyl)fluorenyl]silanetitanium dichloride, (isobutylamido)dimethyl-9-[3,6-di(i-propyl)fluorenyl]silanetitanium dichloride, (t-butylamido)dimethyl dimethyl-9-[3,6-di(i-propyl)fluorenyl]silanetitanium dimethyl, (isopropylamido)dimethyl-9-[3,6-di(t-butyl)fluorenyl]silanetitanium dichloride, (isobutylamido)dimethyl-9-[3,6-di(t-butyl)fluorenyl]silanetitanium dichloride, (t-butylamido)dimethyl-9-[3,6-di(t-butyl)fluorenyl]silanetitanium dimethyl, (isopropylamido)dimethyl-9-[2,7-di(t-butyl)fluorenyl]silanetitanium dichloride, (isobutylamido)dimethyl Examples of the silane titanium dichloride include (t-butylamido)dimethyl-9-[2,7-di(t-butyl)fluorenyl]silanetitanium dichloride, (t-butylamido)dimethyl-9-[2,7-di(t-butyl)fluorenyl]silanetitanium dimethyl, (isopropylamido)dimethyl-9-(2,3,6,7-tetramethylfluorenyl)silanetitanium dichloride, (isobutylamido)dimethyl-9-(2,3,6,7-tetramethylfluorenyl)silanetitanium dichloride, and (t-butylamido)dimethyl-9-(2,3,6,7-tetramethylfluorenyl)silanetitanium dimethyl.Preferably, (t-butylamido)dimethyl-9-fluorenylsilanetitanium dimethyl ((t-BuNSiMe. 2 Flu)TiMe 2 ) is. 2 Flu)TiMe 2 is a titanium complex represented by the following formula (2), and can be easily synthesized, for example, based on the description in "Macromolecules, Vol. 31, p. 3184, 1998."

[0052] [ka] (In the formula, Me represents a methyl group, and t-Bu represents a tert-butyl group.)

[0053] The amount of the titanocene catalyst is not particularly limited as long as the addition polymerization reaction proceeds well. The amount of the titanocene catalyst is preferably 0.001 parts by mass or more and 10 parts by mass or less, more preferably 0.01 parts by mass or more and 5 parts by mass or less, and even more preferably 0.1 parts by mass or more and 1 part by mass or less, based on 100 parts by mass of the total amount of the cyclic olefin monomer and the α-olefin.

[0054] The addition polymerization of a cyclic olefin monomer and a monomer containing an α-olefin is carried out in the presence of the titanocene catalyst and a cocatalyst, which includes a borate compound and a hindered phenol. By carrying out addition polymerization in the presence of the titanocene catalyst and a cocatalyst so as to satisfy the above-mentioned predetermined conditions, a cyclic olefin copolymer having both excellent breaking strain and excellent toughness can be obtained.

[0055] As the borate compound, any borate compound that has been used as a cocatalyst in homopolymerization or copolymerization of cyclic olefin monomers can be used without any particular limitation.Preferred specific examples of the borate compound include triphenylmethylium tetrakis(pentafluorophenyl)borate, dimethylphenylammonium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, and N-methyldinormaldecylammonium tetrakis(pentafluorophenyl)borate.

[0056] As the hindered phenol, any hindered phenol that has been conventionally used as a co-catalyst in the homopolymerization or copolymerization of a cyclic olefin monomer can be used without any particular limitation. Here, the hindered phenol is a phenol having a bulky substituent at least on one of the two adjacent positions of the phenolic hydroxyl group. Examples of the bulky substituent include alkyl groups other than methyl groups such as isopropyl, isobutyl, sec-butyl, and tert-butyl, alkenyl groups, alkynyl groups, aryl groups, heterocyclic groups, alkoxy groups, aryloxy groups, substituted amino groups, alkylthio groups, and arylthio groups.

[0057] Specific examples of the hindered phenol include 2,6-di-tert-butyl-4-hydroxytoluene (BHT), 2,6-di-tert-butylphenol, 2-tert-butylphenol, 2-tert-butyl-p-cresol, 3,3',5,5'-tetra-tert-butyl-4,4'-dihydroxybiphenyl, 3,3',5,5'-tetra-tert-butyl-2,2'-dihydroxybiphenyl, 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), 2,2'-methylenebis(6-tert-butyl-4-methylphenol), 4,4',4"-(1-methylpropanyl-3-ylidene)tris(6-tert-butyl-m-cresol), and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)2,4,6-trimethylbenzene. Among these, 2,6-di-tert-butyl-4-hydroxytoluene (BHT) and 2,6-di-tert-butylphenol are preferred because they have a small molecular weight and the desired effect of using the hindered phenol can be easily obtained by using a small amount of the hindered phenol.

[0058] In addition, the hindered phenol can increase the yield of the cyclic olefin copolymer by reacting with the alkylaluminum compound in the polymerization system, and therefore it is preferable that the co-catalyst further contains an alkylaluminum compound. Specific examples of alkylaluminum compounds include trialkylaluminums such as trimethylaluminum, triethylaluminum, triisopropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-sec-butylaluminum, and tri-n-octylaluminum; dialkylaluminum halides such as dimethylaluminum chloride and diisobutylaluminum chloride; dialkylaluminum hydrides such as diisobutylaluminum hydride; and dialkylaluminum alkoxides such as dimethylaluminum methoxide.

[0059] The amount of the borate compound used is not particularly limited as long as the addition polymerization reaction proceeds well and a cyclic olefin copolymer with desired properties is obtained. The amount of the borate compound used is preferably 0.01 parts by mass or more and 100 parts by mass or less, more preferably 0.1 parts by mass or more and 10 parts by mass or less, and even more preferably 1 part by mass or more and 5 parts by mass or less, based on 100 parts by mass of the total amount of the cyclic olefin monomer and the α-olefin.

[0060] The amount of the hindered phenol used is not particularly limited as long as the addition polymerization reaction proceeds well and a cyclic olefin copolymer with desired properties is obtained.The amount of the hindered phenol used is preferably 0.001 parts by mass or more and 100 parts by mass or less, more preferably 0.01 parts by mass or more and 10 parts by mass or less, and even more preferably 0.1 parts by mass or more and 1 part by mass or less, based on 100 parts by mass of the total amount of the cyclic olefin monomer and the α-olefin.

[0061] The amount of the alkylaluminum compound used is not particularly limited as long as the addition polymerization reaction proceeds well and a cyclic olefin copolymer having desired properties is obtained. The amount of the alkylaluminum compound used is preferably 0.001 parts by mass or more and 10 parts by mass or less, more preferably 0.01 parts by mass or more and 5 parts by mass or less, and even more preferably 0.1 parts by mass or more and 1 part by mass or less, based on 100 parts by mass of the total amount of the cyclic olefin monomer and the α-olefin.

[0062] The addition polymerization may be carried out in the presence of a solvent. The solvent is not particularly limited as long as it does not inhibit the polymerization reaction. Preferred solvents include, for example, hydrocarbon solvents and halogenated hydrocarbon solvents, and hydrocarbon solvents are preferred because of their excellent handling properties, thermal stability, and chemical stability. Specific examples of preferred solvents include hydrocarbon solvents such as pentane, hexane, heptane, octane, isooctane, isododecane, mineral oil, cyclohexane, methylcyclohexane, decahydronaphthalene (decalin), benzene, toluene, and xylene, and halogenated hydrocarbon solvents such as chloroform, methylene chloride, dichloromethane, dichloroethane, and chlorobenzene.

[0063] The solvent may be charged into the polymerization vessel alone, or may be charged into the polymerization vessel in the form of a monomer solution, a catalyst solution, or a cocatalyst solution.

[0064] When a solvent is used, the amount of the solvent is not particularly limited. The amount of the solvent used is preferably 100 parts by mass or more and 100,000 parts by mass or less, more preferably 500 parts by mass or more and 10,000 parts by mass or less, and even more preferably 1,000 parts by mass or more and 5,000 parts by mass or less, relative to 100 parts by mass of the total amount of the cyclic olefin monomer and the α-olefin.

[0065] The temperature of the addition polymerization is not particularly limited. For example, the temperature of the addition polymerization is preferably from -20°C to 200°C, more preferably from -10°C to 10°C, and further preferably from -5°C to 5°C. When producing a cyclic olefin copolymer having a glass transition temperature in the range of less than 0°C, 0°C to 100°C, or 160°C to 300°C, the addition polymerization temperature is preferably -20°C or higher and lower than 10°C. The time for addition polymerization is not particularly limited, and is, for example, preferably from 5 minutes to 30 minutes, more preferably from 8 minutes to 20 minutes, and further preferably from 10 minutes to 15 minutes.

[0066] The atmosphere in which the above-mentioned addition polymerization reaction is carried out is not particularly limited, but an inert gas atmosphere is preferable. As the inert gas, nitrogen gas or helium gas can be used.

[0067] After the addition polymerization is carried out as described above to produce the cyclic olefin copolymer, the cyclic olefin copolymer is recovered from the reaction vessel in a conventional manner.

[0068] <Second manufacturing method> The second production method is similar to the first production method, except that the method of feeding the cyclic olefin monomer and the α-olefin is not particularly limited, and the addition polymerization is carried out at a temperature in the range of 10°C or higher and 60°C or lower.

[0069] In the second production method, the method of feeding the cyclic olefin monomer and the α-olefin may be the same as that in the first production method. Since the feeding operation is simple, the method of feeding the cyclic olefin monomer and the α-olefin in the second production method is preferably a method of feeding the cyclic olefin monomer and the α-olefin all at once into a reaction vessel at or before the start of the addition polymerization reaction. It is particularly preferably used as an optical sheet, a film or sheet material for packaging material, etc. EXAMPLES

[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0071] [Examples 1 to 3 and Comparative Example 1] In Examples 1 to 3 and Comparative Example 1, 2-norbornene (Nb) and 1-octene (Oct) were used in the ratios shown in Table 1, so that the total amount of 2-norbornene and 1-octene was 118.8 mmol. A half amount of 2-norbornene, 0.198 mmol of tri-n-octyl aluminum, and 0.396 mmol of 2,6-di-tert-butyl-4-hydroxytoluene were added to a 500 mL eggplant-shaped flask substituted with a nitrogen atmosphere. Then, the contents of the flask were diluted with toluene to a volume of 258 mL. Next, the contents of the flask were cooled to 0°C. After cooling, a toluene solution of titanocene catalyst with a concentration of 0.04 mmol / L was added to the reaction solution so that the amount of titanocene catalyst was 0.22 mmol. As the titanocene catalyst, a compound represented by the above formula (2) was used. Next, a toluene solution of a borate compound with a concentration of 0.008 mmol / L was added to the reaction solution so that the amount of the borate compound was 0.22 mmol. Triphenylmethylium tetrakis(pentafluorophenyl)borate was used as the borate compound. After adding the titanocene catalyst and the borate compound to start the addition polymerization, the reaction solution was stirred with a magnetic stirrer and reacted at 0°C for 15 minutes. After the 15-minute reaction, the remaining half of the amounts of 2-norbornene and 1-octene, 0.022 mmol of tri-n-octyl aluminum, and 0.044 mmol of 2,6-di-tert-butyl-4-hydroxytoluene were added to the eggplant-shaped flask. The addition polymerization reaction was then continued for 10 minutes. After a total of 25 minutes of reaction, a small amount of 2-propanol was added to the reaction solution to terminate the addition polymerization reaction. Hydrochloric acid was added to the reaction solution and stirred for 10 minutes, and then the organic layer was washed with ion-exchanged water. After repeated washing with ion-exchanged water until the aqueous layer became neutral, the washed organic layer was recovered. The recovered organic layer was dropped into a large amount of acetone to precipitate the produced cyclic olefin copolymer. After recovering the precipitated copolymer by filtration, the copolymer was washed twice or more with metallole and acetone. The washed copolymer was dried under reduced pressure at 110°C for 16 hours or more to obtain a dried cyclic olefin copolymer.

[0072] For the obtained cyclic olefin copolymer, the ratio of the number of moles of structural units derived from an α-olefin (1-octene) (α-olefin ratio) was determined by the following method. Approximately 50 mg of the obtained cyclic olefin copolymer was dissolved in 0.6 mL of chloroform-d, and the resulting solution was subjected to 300 K, 90° pulse, 30 seconds repetition time, and 1000 cumulative pulses using a BRUKER AVANCE III 400+ cryoprobe. 13 C-NMR spectrum was measured. From the obtained spectrum, the ratio of α-olefin was calculated based on the following formula in accordance with the method described in Macromolecules 2010, 43, 4527-4531. The results are shown in Table 1 as the Oct ratio in the resin. Ratio of α-olefins (mol%) = [integral value of carbon derived from α-olefins / (integral value of carbon derived from α-olefins + integral value of carbon derived from cyclic olefin monomers)] × 100

[0073] The molecular weight of the obtained cyclic olefin copolymer was measured by gel permeation chromatography, the glass transition temperature was measured by the above-mentioned method, and a tensile test was performed by the above-mentioned method. The measurement results are shown in Table 1. The tensile test conditions were a temperature of 23°C, a chuck distance of 50 mm, and a tensile speed of 50 mm / min.

[0074] The films used as samples in the measurement of glass transition temperature and the tensile test were prepared by the following method. A Kapton (registered trademark) film measuring 10 cm x 10 cm x 50 μm was used to prepare a mold with a depth of 50 μm. After filling the mold with the obtained cyclic olefin copolymer, the cyclic olefin copolymer filled in the mold was vacuum-pressed using a hot vacuum press under conditions of a pressure of 15 MPa, a temperature of 320 to 340°C, and a time of 15 minutes. After pressing, the pressed cyclic olefin copolymer was sandwiched between metal plates at room temperature to rapidly cool it. After cooling, the metal plates were removed to obtain a cyclic olefin copolymer film with a thickness of about 50 μm.

[0075] [Examples 4 to 6 and Comparative Example 2] A cyclic olefin copolymer was obtained in the same manner as in Example 1, except that the norbornene and 1-octene were charged all at once before the addition polymerization reaction was started, the reaction temperature was changed to 25° C., and the reaction time was changed to 10 minutes. The charging ratio of norbornene and 1-octene is as shown in Table 1. The molecular weight of the obtained cyclic olefin copolymer was measured by gel permeation chromatography, the glass transition temperature was measured by the above-mentioned method, and the tensile test was performed by the above-mentioned method in the same manner as in Example 1. The measurement results are shown in Table 1.

[0076] [Comparative Example 3] A cyclic olefin copolymer was obtained in the same manner as in Comparative Example 2, except that the reaction temperature was changed to 0° C. The charging ratio of norbornene and 1-octene is as shown in Table 1. The molecular weight of the obtained cyclic olefin copolymer was measured by gel permeation chromatography, the glass transition temperature was measured by the above-mentioned method, and the tensile test was performed by the above-mentioned method in the same manner as in Example 1. The measurement results are shown in Table 1.

[0077] [Comparative Example 4] A cyclic olefin copolymer was obtained in the same manner as in Example 1, except that 0.97 mmol of CC1 and 0.68 mmol of CC2 were used as cocatalysts, the reaction temperature was changed to 40° C., and the polymerization time was changed to 4 hours. The charging ratio and charging method of norbornene and 1-octene are as shown in Table 1. The molecular weight of the obtained cyclic olefin copolymer was measured by gel permeation chromatography, the glass transition temperature was measured by the above-mentioned method, and the tensile test was performed by the above-mentioned method in the same manner as in Example 1. The measurement results are shown in Table 1. CC1: 6.5 mass% (as Al atom content) MMAO-3A toluene solution ([ (CH 3 ) 0.7 (iso-C 4 H9 ) 0.3 AlO] n (Tosoh Finechem Co., Ltd., containing 6 mol% trimethylaluminum based on the total aluminum) CC2: 9.0 mass% (as the content of Al atoms) TMAO-211 toluene solution (a solution of methylaluminoxane, manufactured by Tosoh Finechem Co., Ltd., containing 26 mol% trimethylaluminum relative to the total Al)

[0078] [Comparative Example 5] A cyclic olefin copolymer was obtained in the same manner as in Example 1, except that only 0.22 mmol of triphenylmethylium tetrakis(pentafluorophenyl)borate was used as a cocatalyst, the reaction temperature was changed to 25° C., and the reaction time was changed to 2 hours. The charging ratio of norbornene and 1-octene is as shown in Table 1. The molecular weight of the obtained cyclic olefin copolymer was measured by gel permeation chromatography, the glass transition temperature was measured by the above-mentioned method, and the tensile test was performed by the above-mentioned method in the same manner as in Example 1. The measurement results are shown in Table 1.

[0079] [Table 1]

[0080] According to Table 1, the cyclic olefin copolymers of Examples 1 to 6, in which the ratio of the number of moles of structural units derived from α-olefins to the number of moles of all structural units is 10 mol % or more and 40 mol % or less, and which have two or more glass transition temperatures measured by viscoelasticity measurement within the range of 0°C to 300°C, exhibit excellent tensile properties and combine excellent breaking strain and excellent toughness. On the other hand, the cyclic olefin copolymers of Comparative Examples 1 to 5, in which the ratio of the number of moles of structural units derived from α-olefins to the number of moles of all structural units was outside the range of 10 mol % or more and 40 mol % or less, or which had only one glass transition temperature measured by viscoelasticity within the range of 0°C to 300°C, were inferior in at least one of tensile strength, breaking strain, and tensile modulus.

Claims

1. A cyclic olefin copolymer which is an addition type polymer of a cyclic olefin monomer and an α-olefin having 3 to 20 carbon atoms, the ratio of the number of moles of structural units derived from the α-olefin to the number of moles of all structural units is 10 mol % or more and 40 mol % or less; A cyclic olefin copolymer having at least one glass transition temperature measured by viscoelasticity below 0°C, at least one glass transition temperature in the range of 0°C to 100°C, and at least one glass transition temperature in the range of 160°C to 300°C.

2. A method for producing the cyclic olefin copolymer according to claim 1, comprising the steps of: The method includes addition polymerizing the cyclic olefin monomer and the α-olefin in the presence of a titanocene catalyst represented by the following formula (1) and a co-catalyst, the cocatalyst comprises an alkylaluminum compound, a borate compound, and a hindered phenol; The cyclic olefin monomer and the α-olefin monomer are each added in two or more portions to a reaction system in which addition polymerization is carried out, in the divided addition, the amounts of the cyclic olefin monomer and the α-olefin added per one addition are, where TA is the mass of the total amount added and N is the number of divisions, TA / N×0.9 or more and TA / N×1.1 or less, The production method, wherein the timing of addition of the cyclic olefin monomer and the timing of addition of the α-olefin are simultaneous in the divided addition. 【Chemistry 1】 (In formula (1), R 1 ~R 3 each independently represents an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms; R 4 and R 5 each independently represents an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, or a halogen atom; R 6 ~R 13 are each independently a hydrogen atom, an alkyl group having from 1 to 12 carbon atoms, an aryl group having from 6 to 12 carbon atoms, or a silyl group which may have a monovalent hydrocarbon group having from 1 to 12 carbon atoms as a substituent.

Citation Information

Patent Citations

  • Olefinic polymer and manufacturing process therefor

    JP2004359798A

  • Copolymer and method for producing the same, and sheet molding

    JP2016056275A

  • Cyclic olefin resin composition, method for producing the same, and molding

    JP2018145425A

  • Norbornene-type polymer solution

    WO2014141957A1

  • Cyclic olefin resin composition for molding, molded body, and resin

    WO2018181781A1