Resin additive composition for thermosetting resin and manufacturing method thereof, thermosetting resin composition and manufacturing method thereof, and cured product of thermosetting resin composition
By mixing fullerenes with a resin medium and heat-treating in a low-oxygen atmosphere, the method addresses the limitations of existing dispersal methods, resulting in a resin composition with enhanced heat resistance, surface smoothness, and voltage resistance through fullerene adduct formation.
Patent Information
- Application Number
- JP2020563235
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-27
- Filing Date
- 2019-12-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-12-23
AI Technical Summary
Existing methods for dispersing fullerenes in resins are limited by the use of specific solvents and resins, leading to insufficient affinity and dispersibility, particularly with polyester and epoxy resins, which affects heat resistance, surface smoothness, and voltage resistance.
A method involving the use of a thermoplastic or thermosetting resin medium, mixed with fullerenes and subjected to heat-treatment in a low-oxygen atmosphere, forming fullerene adducts that improve solubility and affinity with the resin, enhancing heat resistance, surface smoothness, and voltage resistance.
The method results in a resin composition with improved heat resistance, surface smoothness, and voltage resistance by forming fullerene adducts that enhance the resin's properties.
Smart Images

Figure 0007586710000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin additive composition and a method for producing the same, and a resin composition and a method for producing the same. This application claims priority based on Japanese Patent Application No. 2018-246101, filed on December 27, 2018, the contents of which are incorporated herein by reference. [Background technology]
[0002] It is known that sufficient dispersion of fullerene in a resin improves the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin. Patent Document 1 discloses a method for producing a polyester resin composition by uniformly dispersing fullerenes in a polyester resin. One embodiment of this production method includes a step of dissolving fullerenes in a solvent to prepare a fullerene solution, a step of adding a polyester resin to the fullerene solution to prepare a polymer dope solution, and a step of removing the solvent from the polymer dope solution. Another embodiment of this production method includes a step of dissolving fullerenes in a solvent to prepare a fullerene solution, and a step of adding a polyester raw material or an oligomer thereof to the fullerene solution, performing a polymerization reaction, and producing a polyester resin composition. The polyester resin composition obtained by this production method improves the heat resistance, surface smoothness, and mechanical properties of the polyester resin. Patent Document 2 discloses a technique for improving the dielectric breakdown voltage of a resin sheet by producing the resin sheet using a resin composition in which fullerene is dispersed in polyolefin. Patent Document 3 discloses a technique for improving the dispersibility of fullerene in a resin by mixing an organic solvent solution containing a fullerene derivative with the resin. The fullerene derivative is a fullerene derivative obtained by introducing a substituent into the fullerene that improves the solubility in an organic solvent having a high affinity with the resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-117760 A [Patent Document 2] JP 2018-104549 A [Patent Document 3] International Publication No. 2016 / 063972 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the method described in Patent Document 1, the solvents that can be used for dissolving fullerenes to prepare a fullerene solution, mixing the fullerene solution with a polyester resin, or polymerizing the polyester resin in the fullerene solution are limited to some aromatic solvents such as benzene and toluene. In the method described in Patent Document 2, the resin capable of dispersing fullerenes is limited to a polyester-based resin. In the method described in Patent Document 3, an indene adduct is disclosed as a fullerene derivative. Since the indene adduct has a fundamentally different structure from the skeleton of resins such as polyester and epoxy resins, it does not have sufficient affinity with these resins and is not sufficiently dispersible in these resins.
[0005] The present invention has been made in consideration of the above circumstances, and aims to provide a resin additive composition and a method for producing the same, and a resin composition and a method for producing the same, which improve the heat resistance, surface smoothness, mechanical properties, and voltage resistance of a resin. [Means for solving the problem]
[0006] [1] A method for producing a resin additive composition, comprising the steps of: mixing a medium A with a fullerene to obtain a fullerene dispersion containing the medium A and the fullerene; and heat-treating the fullerene dispersion, wherein the medium A is at least one selected from the group consisting of a thermoplastic resin, a raw material for a thermoplastic resin, and a raw material for a thermosetting resin. [2] The method for producing the resin additive composition according to [1], wherein an organic solvent is mixed in the step of obtaining the fullerene dispersion. [3] The method for producing a resin additive composition according to [1] or [2], wherein the step of heat-treating the fullerene dispersion is carried out in a low-oxygen atmosphere. [4] The method for producing the resin additive composition according to [3], wherein the oxygen concentration in the fullerene dispersion is 10 ppm by mass or less. [5] The step of heat-treating the fullerene dispersion includes a step of determining a heating temperature and a heating time of the fullerene dispersion, the step of determining the heating temperature and the heating time of the fullerene dispersion includes a step of measuring the fullerene concentration in the fullerene dispersion in a heated state at regular intervals to create a calibration curve showing the relationship between the fullerene concentration in the fullerene dispersion and the heating time of the fullerene dispersion; The method for producing the resin additive composition according to any one of [1] to [4], further comprising a step of determining a heating temperature and a heating time of the fullerene dispersion based on the calibration curve. [6] The fullerene is C 60 , C 70 And C 60 and C 70 The method for producing the resin additive composition according to any one of [1] to [5], wherein the resin additive composition is any one of a mixture containing: [7] A method for producing the resin additive composition according to any one of [1] to [6], comprising a step of removing insoluble components from the fullerene dispersion. [8] A method for producing the resin additive composition according to any one of [1] to [7], comprising a step of removing volatile components from the resin additive composition. [9] A resin additive composition produced by the method for producing a resin additive composition according to any one of [1] to [8].
[10] A method for producing a resin composition, comprising: obtaining a resin additive composition by the method for producing a resin additive composition according to any one of [1] to [8]; and mixing the obtained resin additive composition with a medium B, wherein the medium B is a raw material for a thermosetting resin, a curing agent for a thermosetting resin, or a thermoplastic resin.
[11] A resin composition produced by the method for producing a resin composition according to
[10] .
[12] When the medium B is a raw material for a thermosetting resin or a curing agent for a thermosetting resin, a cured product of the resin composition described in
[11] . Effect of the Invention
[0007] According to the present invention, it is possible to provide a resin additive composition and a method for producing the same, and a resin composition and a method for producing the same, which improve the heat resistance, surface smoothness, mechanical properties, and voltage resistance of a resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of a resin additive composition and a method for producing the same, and a resin composition and a method for producing the same to which the present invention is applied will be described. It should be noted that the present embodiment is specifically described to allow a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified.
[0009] [Resin additive composition] The resin additive composition of this embodiment is produced by a method for producing a resin additive composition described later, and includes a medium A, a fullerene, and a fullerene adduct. The fullerene adduct is a compound formed by adding a structure derived from a component contained in the medium A to the fullerene. The resin additive composition of this embodiment is produced by heat-treating a mixture of the medium A and the fullerene (fullerene dispersion) in the method for producing a resin additive composition of this embodiment described later.
[0010] (Media A) The medium A contained in the resin additive composition of this embodiment is at least one selected from the group consisting of a thermoplastic resin, a raw material for a thermoplastic resin, and a raw material for a thermosetting resin. More specifically, when the resin additive composition of this embodiment is used for a thermoplastic resin, the medium A is a thermoplastic resin or a raw material for a thermoplastic resin. Examples of raw materials for a thermoplastic resin include at least one selected from the group consisting of a monomer for a thermoplastic resin, a thermoplastic resin additive, and a reactive component. In addition, when the resin additive composition of this embodiment is used for a thermosetting resin, the medium A is a raw material for a thermosetting resin. Examples of raw materials for a thermosetting resin include at least one selected from the group consisting of a polymerizable monomer, a polymerizable oligomer, and a reactive component.
[0011] In general, when the temperature of a thermoplastic resin exceeds the melting temperature, the chemical bonds constituting the molecule, which mainly has carbon, oxygen, nitrogen, and silicon atoms in the main chain, are gradually cleaved, and the molecular weight is reduced. Examples of such thermoplastic resins include polymers of monomers such as methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, methyl acrylate, ethyl allyl, butyl acrylate, vinyl acetate, styrene, ethylene glycol, propylene glycol, ethylene, propylene, and butadiene, and copolymers of these monomers.
[0012] Examples of monomers that are raw materials for thermoplastic resins include those mentioned above.
[0013] The thermoplastic resin additive, which is the raw material of the thermoplastic resin, is not particularly limited. For example, the thermoplastic resin additive may be a commercially available antioxidant. These additives may be used alone or in combination of two or more. The thermoplastic resin additive is more preferably one having an aromatic ring. Examples of antioxidants having an aromatic ring include dibutylhydroxytoluene (BHT), butylhydroxyanisole (BHA), 2,6-butylphenol (DTP), bis(3,5-dibutyl-4-hydroxyphenyl)methane (BDBA), 2,4,6-tributylphenol (TBP), 3-arylbenzofuran-2-one (intramolecular cyclic ester of hydroxycarboxylic acid), phenyl-α-naphthylamine, dialkyldiphenylamine, and benzotriazole.
[0014] As the polymerizable monomer or oligomer that is the raw material of the thermosetting resin, any raw material monomer or oligomer such as the following can be used without any particular limitation. This raw material monomer or oligomer is polymerized by heating or light irradiation in the presence of a curing agent or a photocuring agent to produce a phenolic resin, an epoxy resin, a melamine resin, a urea resin, an unsaturated polyester resin, an alkyd resin, a polyurethane, a polyimide, or the like. The thermosetting resin is preferably an epoxy resin. Specific examples of the epoxy resin include phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol type epoxy resin, biphenol type epoxy resin, naphthalene skeleton-containing epoxy resin, heterocyclic epoxy resin, silicon epoxy resin, etc.
[0015] The reactive components that are the raw materials of the thermoplastic resin and the thermosetting resin are preferably compounds that have high affinity in terms of solubility with the medium A and the medium B described below. It is more preferable that the reactive component is a compound having a similar chemical structure to the main components of medium A and medium B, in terms of having a high affinity with medium A and medium B in terms of solubility. Furthermore, from the viewpoint of ease of production, the reactive component is preferably a component contained in medium B, and is preferably a compound that chemically bonds to fullerenes, which will be described later, at approximately 200° C. or less. As the reactive component, for example, a compound having a skeleton such as a hydrocarbon, ether, or ester, such as paraffin, olefin, naphthene, or aromatic, is preferable.
[0016] In addition, the reactive component is preferably, for example, a saturated hydrocarbon having a side chain or ring, or an unsaturated hydrocarbon such as a diene or aromatic, in terms of being chemically bonded to fullerene at about 200° C. or less. The aromatic may have multiple rings or an alkyl side chain. Other preferred examples of such reactive components include a compound having an ether bond, a compound having an ester bond, a compound having a phosphate ester bond, a compound having a disulfide bond, a compound having a phenolic hydroxyl group, and silicone.
[0017] Specific examples of such reactive components include linear or branched hydrocarbons, hydrocarbons having unsaturated double bonds, aromatic hydrocarbons having alkyl groups, polycyclic aromatic hydrocarbons, compounds having ether bonds, compounds having ester groups, compounds having disulfide bonds, di-p-tolyl disulfide, compounds having phenolic hydroxyl groups, diazo compounds, silicones, and combinations of these. It is believed that the molecules of these compounds are cleaved by heating and react with fullerene to form a fullerene adduct. Examples of linear or branched hydrocarbons include hexane, decane, cyclohexane, isobutane, decalin, etc. Examples of hydrocarbons with unsaturated double bonds include hexacene, pentacene, cyclohexene, decene, turpentine oil, terpene derivatives, α-olefins, etc. Examples of aromatic hydrocarbons with alkyl groups include dodecylbenzene, hexabenzene, ethylbenzene, trimethylbenzene, tetramethylbenzene, cumene, methylnaphthalene. Examples of polycyclic aromatic hydrocarbons include anthracene, butacene, hexacene, etc. Examples of compounds with ether bonds include tripropylene glycol, dipropylene glycol, triethylene glycol, tetrahydrofuran, etc. Examples of compounds with ester groups include ethyl acetate, octyl acetate, γ-butyrolactone, fats (fatty acid glycerin esters), etc. Examples of compounds with phosphate ester bonds include tricresyl phosphate (TCP), triphenyl phosphate (TPP), 2,6-di-tert-butylphenol (DTP), etc. Examples of compounds having a disulfide bond include dibenzyl disulfide (DBDS), di-p-tolyl disulfide (DTDS), etc. Examples of compounds having a phenolic hydroxyl group include 3,5-di-tert-butyl-4-hydroxytoluene (BHT), butylhydroxyanisole (BHA), 2,6-butylphenol (DTP), bis(3,5-di-tert-butyl-4-hydroxyphenyl)methane (BDBA), 2,4,6-tributylphenol (TBP), etc.
[0018] The reactive component is chemically bonded (added) to the fullerene to form a fullerene adduct. In such a fullerene adduct, the molecule (group) of the reactive component is present on the surface of the fullerene skeleton. Therefore, the fullerene adduct has excellent affinity with the resin due to the group obtained from the reactive component present on the surface. Therefore, by including the fullerene adduct in the resin additive composition, the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin can be improved.
[0019] It can be confirmed by liquid chromatography mass spectrometry (LC-MS) that the reactive component is chemically bonded to the fullerene to form a fullerene adduct.
[0020] An organic solvent may be used in the process of obtaining a fullerene dispersion containing the medium A and fullerene. By using an organic solvent, when the thermoplastic resin additive of the medium A is solid at room temperature, it can be dissolved in the organic solvent to make it liquid, making it possible to handle it as a liquid, and facilitating the production of the resin additive composition described below. In addition, the use of an organic solvent can enhance the dispersion of fullerene, facilitating the production of the resin additive composition described below. When it is difficult to disperse fullerene in the thermoplastic resin additive, polymerizable monomer, polymerizable oligomer, etc. of medium A, the addition of an organic solvent to the mixture of these can enhance the dispersion of fullerene.
[0021] Examples of organic solvents include aromatic solvents, decalin, N-methylpyrrolidone, polypropylene glycol, etc. Among them, aromatic solvents are particularly preferred. Examples of aromatic solvents include benzene, toluene, xylene, trimethylbenzene, chlorobenzene, dichlorobenzene, methylnaphthalene, etc.
[0022] (Fullerene) The fullerene contained in the resin additive composition of the present embodiment is not particularly limited in structure or production method, and various fullerenes can be used. For example, C 60 Or C 70 , higher fullerenes, or mixtures of these. Among fullerenes, C 60 and C 70 is preferable, and C is preferable because it has little coloring. 60 is more preferable. In the case of a mixture, C 60 It is preferable that the content is 50 mass % or more.
[0023] (Fullerene adduct) In the manufacturing process of the resin additive composition of this embodiment, the concentration of fullerene in the fullerene dispersion containing the medium A and fullerene after heat treatment is lower than the concentration of fullerene before heat treatment. That is, the resin additive composition of this embodiment contains a fullerene adduct formed by chemically bonding a reactive component that may be contained in the medium A to the fullerene through heat treatment. The fullerene adduct is preferably the following compound added to the fullerene. This compound is at least one compound selected from the group consisting of hydrocarbons, compounds having an ether bond, compounds having an ester bond, compounds having a phosphate ester bond, compounds having a disulfide bond, compounds having a phenolic hydroxyl group, and silicone.
[0024] The resin additive composition of the present embodiment is a resin additive composition produced by a method for producing a resin additive composition described below.
[0025] The resin additive composition of the present embodiment contains a medium A, a fullerene, and a fullerene adduct, and is obtained by heat-treating a dispersion of the medium A and the fullerene. Therefore, the solubility of the fullerene in the resin is improved, and the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin can be improved.
[0026] The resin additive composition of this embodiment can be used for various applications such as thermosetting fiber reinforced plastics (FRP), thermoplastic fiber reinforced plastics (FRTP), thermosetting carbon fiber reinforced plastics (CFRP), thermoplastic carbon fiber reinforced plastics (CFRTP), heat dissipating resins, electrical insulating resins, O-ring packings, and wire coating materials.
[0027] For example, in applications of FRP, FRTP, CFRP, CFRTP, heat dissipation resin, and electrical insulating resin, if a resin serving as a base material (hereinafter also referred to as a "resin base material") is produced by the method of this embodiment, the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained FRP, CFRP, heat dissipation resin, and electrical insulating resin can be improved. In this case, the resin substrate is made of a thermosetting resin, such as an epoxy resin.
[0028] For example, in applications of sealing resins such as CFRTP, FRTP, O-ring packing, and wire coating materials, if a resin serving as a base material (hereinafter also referred to as a "resin base material") is produced by the method of this embodiment, the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resulting FRP and sealing materials can be improved. In this case, the resin substrate is made of a thermoplastic resin, such as polyethylene, polypropylene, methyl methacrylate, methyl acrylate, polystyrene, butyl rubber, butadiene rubber, or fluororubber.
[0029] [Method of manufacturing resin additive composition] The manufacturing method of the resin additive composition of this embodiment is the manufacturing method of the resin additive composition of this embodiment described above, and includes a step of mixing medium A and fullerene, dissolving the soluble components of the fullerene in medium A, and obtaining a mixture of medium A and fullerene (hereinafter referred to as the "first step"), and a step of heat-treating the fullerene dispersion (hereinafter referred to as the "second step"). Furthermore, the method for producing the resin additive composition of this embodiment may include a step (hereinafter referred to as "third step") of removing insoluble components contained in the mixture after the first step to obtain a fullerene mixture. A fullerene dispersion (hereinafter sometimes simply referred to as "fullerene dispersion") is obtained from the mixture of fullerene and medium A that has been subjected to the first or second step. Furthermore, the method for producing the resin additive composition of this embodiment may include, after the third step, a step of removing volatile matters such as the organic solvent contained in the resin additive composition (hereinafter referred to as the "fourth step").
[0030] The method for producing the resin additive composition of this embodiment will be described in detail below.
[0031] (first step) When medium A is liquid at room temperature, or when medium A is solid and in a solution state dissolved in an organic solvent, the raw fullerene is put into medium A (solution) and a dispersion means such as a stirrer is used to perform a dispersion treatment for 1 hour to 48 hours at about room temperature or while heating as necessary. When medium A is solid at room temperature and melts by heating, a dispersion means such as a stirrer or kneader is used to perform a dispersion treatment for 1 hour to 48 hours at the melting temperature. The amount of fullerene to be charged as the raw material is, for example, 1.1 to 200 times, more preferably 1.1 to 20 times, the amount of fullerene calculated to obtain the desired fullerene concentration relative to the medium A, taking into consideration the fullerene concentration of the resin additive composition to be finally prepared. If it is less than 1.1 times, the amount of soluble components that can be extracted is small, and the desired fullerene concentration may not be achieved. If it is more than 200 times, the filtration speed decreases during the second step of removing insoluble components, and the execution time becomes long. Furthermore, the raw material cost of fullerene increases.
[0032] Examples of dispersing means for dispersing fullerene in medium A include a stirrer, an ultrasonic dispersing device, a homogenizer, a ball mill, a bead mill, a triple roll mill, and a kneader. The fullerene dispersion preferably has a fullerene concentration of 1 ppm by mass (0.0001% by mass) or more and 10,000 ppm by mass (1.0% by mass) or less, more preferably 5 ppm by mass (0.0005% by mass) or more and 2,000 ppm by mass (0.2% by mass) or less, and even more preferably 10 ppm by mass (0.001% by mass) or more and 500 ppm by mass (0.05% by mass) or less. If the concentration of fullerene is within the above range, the effects of heat resistance, surface smoothness, mechanical properties, and voltage resistance due to the addition of fullerene can be maintained for a long period of time. In addition, the decrease in the concentration of fullerene due to degradation of fullerene can be compensated for.
[0033] (Second process) The fullerene dispersion obtained in the first step is heat-treated to obtain a resin additive composition. Note that, before the second step, a third step may be performed to remove insoluble components contained in the fullerene dispersion and obtain a fullerene mixture. Specifically, a third step may be performed to filter the fullerene dispersion obtained in the first step.
[0034] The fullerene dispersion obtained in the first step (or the third step) is exposed to the atmosphere in the first step (or the third step), and therefore the oxygen concentration inside is in equilibrium with the oxygen in the atmosphere. Therefore, the second step preferably includes an operation for lowering the oxygen concentration in the mixture to a level lower than that in the state in which the mixture is left in the atmosphere. Specifically, the oxygen concentration in the mixture is preferably 10 ppm by mass or less, more preferably 5 ppm by mass or less, and even more preferably 1 ppm by mass or less. Thereafter, the fullerene dispersion with the reduced oxygen concentration is heat-treated without being exposed to the atmosphere again.
[0035] In the second step, the fullerene dispersion is heat-treated to chemically bond reactive components to fullerenes to form fullerene adducts. Therefore, the concentration of fullerenes in the resin additive composition obtained after heat treatment is lower than the concentration of fullerenes in the fullerene dispersion before heat treatment. In other words, after heat treatment, fullerene adducts are formed, so fullerenes are consumed and the concentration is lower than before heat treatment.
[0036] The heat treatment in the second step is desirably carried out in a low oxygen concentration atmosphere (O2 concentration of 1% by volume or less). For this purpose, it is preferable to reduce the oxygen concentration as described above before the heat treatment. More preferable methods for reducing the oxygen concentration include, for example, the following four methods.
[0037] The first method will be described. The fullerene dispersion obtained in the first step (or the third step) is placed in an airtight metallic container made of stainless steel or the like, and the container is then sealed. Next, the inside of the container is replaced with an inert gas such as nitrogen gas or argon gas, or the fullerene dispersion in the container is further bubbled with the inert gas to bring the fullerene dispersion into equilibrium with the inert gas. The fullerene dispersion is then heat-treated by heating the container while maintaining an equilibrium state between the fullerene dispersion and the inert gas. In the first method, the heat treatment of the fullerene dispersion is carried out in a low-oxygen atmosphere by heating the container while maintaining an equilibrium state between the fullerene dispersion and the inert gas.
[0038] The second method will now be described. The fullerene dispersion obtained in the second step is placed in an airtight container made of a metal such as stainless steel, and the container is then sealed. The vessel is then vacuumed to reduce the oxygen concentration in the fullerene dispersion. Next, the container is heated while maintaining the state in which the oxygen concentration in the fullerene dispersion is reduced, thereby heat-treating the fullerene dispersion. In the second method, the container is heated while maintaining the oxygen concentration in the fullerene dispersion at a reduced level, thereby carrying out the heat treatment of the fullerene dispersion in a low-oxygen atmosphere.
[0039] A third method will now be described. The fullerene dispersion obtained in the second step is placed in an airtight container made of a metal such as stainless steel, and the container is then sealed. The vessel is then vacuumed to reduce the oxygen concentration in the fullerene dispersion. Next, the inside of the container is replaced with an inert gas such as nitrogen gas, or the fullerene dispersion in the container is further bubbled with the inert gas, thereby bringing the fullerene dispersion into equilibrium with the inert gas. The fullerene dispersion is then heat-treated by heating the container while maintaining an equilibrium state between the fullerene dispersion and the inert gas. In the third method, the heat treatment of the fullerene dispersion is carried out in a low-oxygen atmosphere by heating the container while maintaining an equilibrium state between the fullerene dispersion and the inert gas.
[0040] The higher the heating temperature of the fullerene dispersion, the shorter the heating time. However, if the heating temperature is too high, the components of medium A may evaporate, or medium A may deteriorate or change in quality. Therefore, the upper limit of the heating temperature of the fullerene dispersion is the upper limit of the temperature at which the weight of the fullerene dispersion does not decrease too much due to the evaporation of medium A. However, even if this temperature is exceeded, the heating temperature of the fullerene dispersion can be higher than the temperature at which medium A evaporates if the evaporated components are recovered using a cooling tube or the like and returned to medium A, or if the heat treatment is performed in a pressure vessel under pressure to suppress evaporation.
[0041] When the fullerene dispersion is solid at room temperature, it is preferable that it is brought into a molten state by heating, and the heating temperature is preferably higher than the melting temperature. The heating temperature of the mixture is preferably 100°C or higher and 250°C or lower, more preferably 100°C or higher and 150°C or lower, and even more preferably 120°C or higher and 150°C or lower.
[0042] The lower the heating temperature of the fullerene dispersion, the longer the heating time. If the heating temperature is 100° C. or higher, the resin additive composition exhibits improved heat resistance, surface smoothness, mechanical properties, and voltage resistance. When the resin additive composition is produced industrially, the heating temperature of the fullerene dispersion is more preferably 100° C. or higher, and even more preferably 120° C. or higher. The higher the heating temperature, the faster the heat treatment of the fullerene dispersion proceeds, and therefore the shorter the heating time.
[0043] The higher the oxygen concentration in the fullerene dispersion, the more the thermal deterioration of the medium A advances during the heat treatment of the fullerene dispersion, making it difficult to improve the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin additive composition. If the oxygen concentration in the fullerene dispersion is high, the medium A deteriorates due to oxidation during the heat treatment of the fullerene dispersion. This may cause the medium A to become colored, the viscosity of the medium A to increase or decrease, or the amount of volatile components to increase volatility, resulting in a decrease in the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin.
[0044] In addition, when the fullerene dispersion is exposed to the air for 10 minutes or more, the oxygen concentration in the fullerene dispersion approaches the concentration in equilibrium with the air. When such a fullerene dispersion is heat-treated, deterioration due to oxidation of the medium A occurs, and the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin additive composition decrease. That is, the lower the oxygen concentration in the fullerene dispersion, the more the thermal deterioration of the medium A is suppressed, and the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin additive composition improve. The oxygen concentration in the fullerene dispersion is preferably lower than the oxygen concentration in the air, and more preferably 1 / 10 or less of the oxygen concentration in the air. Specifically, the oxygen concentration in the fullerene dispersion is preferably 10 ppm by mass or less, more preferably 5 ppm by mass or less, and even more preferably 1 ppm by mass or less.
[0045] The oxygen concentration in the fullerene dispersion can be measured using a dissolved oxygen meter. When the oxygen concentration is low, it is difficult to accurately measure the oxygen concentration industrially, so the oxygen concentration in the fullerene dispersion is adjusted to a predetermined range by adjusting the production conditions.
[0046] In the second step, the concentration of fullerene in the resin additive composition obtained after the heat treatment is lower than the concentration of fullerene in the fullerene dispersion before the heat treatment. The reason for this decrease in concentration is believed to be that the chemical bonds constituting the molecules contained in medium A are gradually cleaved, and the cleaved molecules are added to fullerenes, converting the fullerene molecules into fullerene adducts. It is presumed that the production of the reaction products improves the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resulting resin additive composition.
[0047] The fullerene concentrations in the fullerene dispersion before the heat treatment and in the resin additive composition immediately after the heat treatment can be measured by a method using high performance liquid chromatography (HPLC) described in the Examples.
[0048] The amount of fullerene lost by heat treatment of a fullerene dispersion can be calculated from the difference in fullerene concentration before and after heat treatment, i.e., fullerene concentration difference before and after heat treatment = [fullerene concentration before heat treatment] - [fullerene concentration after heat treatment].
[0049] The concentration difference is preferably 5 mass ppm or more, more preferably 10 mass ppm or more, and even more preferably 50 mass ppm or more. That is, in a fullerene dispersion having a fullerene content of 50 mass ppm or less, fullerenes may not be detected by heat treatment. Even if the fullerene content exceeds 50 mass ppm, the loss of fullerenes may exceed 50 mass ppm by continuing heat treatment, so that fullerenes may not be detected. If the amount of fullerene lost is 5 ppm or more, the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin additive composition can be improved.
[0050] When the amount of fullerene disappearance exceeds 500 ppm by mass, or even if it is less than 500 ppm by mass, the heat treatment can be continued even after the state where the fullerene that has disappeared is reached and no fullerene remains. However, the heat treatment time makes it difficult to further improve the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained resin additive composition. Therefore, the amount of fullerene disappearance is preferably 500 ppm by mass or less, more preferably 100 ppm by mass or less, and even more preferably 50 ppm by mass or less.
[0051] In order to determine the heat treatment conditions of the fullerene dispersion, a graph (calibration curve) is created by the following method. Using the device in Example 1 described later, a fullerene dispersion in a heated state is sampled at regular intervals. The concentration of fullerene contained in the solution is then quantified, and a graph (calibration curve) is created showing the relationship between the concentration of fullerene in the fullerene dispersion and the heating time of the mixture. From this graph, the heating temperature and heating time of the fullerene dispersion can be determined. Note that if the determined heating time is shorter than desired from the standpoint of ease of operation, etc., a calibration curve may be created again at a lower heating temperature, and conversely, if the determined heating time is longer than desired, a calibration curve may be created again at a higher heating temperature to determine the heating temperature and heating time.
[0052] (Third step) The mixture obtained in the first step may contain, as insoluble components, fullerene aggregates, which are impurities derived from the raw fullerene, undissolved fullerene, impurities in the medium A, particles mixed in during the manufacturing process, etc. Therefore, if the mixture is used as is, problems such as wear of the sliding parts in contact with the resin additive composition may occur. Therefore, after the first step, a third step (filtering) for removing the insoluble components may be provided.
[0053] Examples of the third step include (1) a removal step using a membrane filter, (2) a removal step using a centrifuge, and (3) a removal step using a combination of a membrane filter and a centrifuge. Among these removal steps, in terms of filtration time, (1) the removal step using a membrane filter is preferred when a small amount of the resin additive composition is to be obtained, and (2) the removal step using a centrifuge is preferred when a large amount of the resin additive composition is to be obtained.
[0054] (1) In the removal step using a membrane filter, for example, the mixture of medium A and fullerene obtained in the first step is filtered using a filter with a small mesh (for example, a membrane filter with a mesh of 0.1 μm to 1 μm) and collected as a fullerene dispersion. In order to shorten the filtration time, it is preferable to reduce the pressure during filtration. (2) In the removal step using a centrifuge, for example, the mixture of medium A and fullerene obtained in the first step is subjected to a centrifugal separation process, and the supernatant is collected as a fullerene dispersion.
[0055] (Fourth step) In the fourth step, after the third step, volatile matters such as organic solvents contained in the resin additive composition are removed. Examples of methods for removing volatile components include a method in which the volatile components are evaporated by heating or heating under reduced pressure. The fourth step can be carried out continuously after the third step. For example, in the first to third methods of the third step, after the heating is completed, the pressure in the container can be reduced to less than atmospheric pressure using a vacuum pump or the like, thereby removing volatile matters such as organic solvents contained in the resin additive composition.
[0056] According to the method for producing a resin additive composition of the present embodiment, a resin additive composition capable of improving heat resistance, surface smoothness, mechanical properties, and voltage resistance can be obtained.
[0057] [Resin composition and its manufacturing method] The resin composition of this embodiment contains medium B and the resin additive composition, and is obtained by mixing medium B with the resin additive composition. Medium B contained in the resin composition of this embodiment is a raw material for a thermosetting resin, a curing agent for a thermosetting resin, or a thermoplastic resin. More specifically, when medium A used in the resin additive composition is a thermoplastic resin or a raw material for a thermoplastic resin, medium B is a thermoplastic resin. In addition, when medium A used in the resin additive composition is a raw material for a thermosetting resin, medium B is a polymerizable monomer, a polymerizable oligomer, a heat curing accelerator, a curing agent for a thermosetting resin, and a mixture thereof.
[0058] The method for mixing the medium B with the resin additive composition is not particularly limited, and a method such as a hot kneading method can be used.
[0059] When using a thermosetting resin, a commonly used curing agent can be used without any restrictions. For example, an aliphatic polyamine such as triethylenetetramine, an aromatic polyamine such as diaminodiphenylmethane, an acid anhydride such as 4-methylhexahydrophthalic anhydride, a phenol novolac resin such as phenol novolac resin, and a dicyandiamide such as dicyandiamide can be used.
[0060] When using a curable resin, the curing accelerator can be any commonly used one without any restrictions. For example, amine-based accelerators include tris(dimethylaminomethylphenol), imidazole-based accelerators include 1-cyanoethyl-2-ethyl-4-methylimidazole, and phosphine-based accelerators include triphenylphosphine and tetraphenylphosphonium tetraphenylborate.
[0061] According to the method for producing a resin composition of the present embodiment, a resin composition having excellent heat resistance, surface smoothness, mechanical properties, and voltage resistance can be obtained. [Cured product of resin composition] When the medium B contained in the resin composition of this embodiment is a raw material for a thermosetting resin, a cured product of the resin composition is obtained by heat curing treatment. The conditions of the heat curing treatment are not particularly limited, and for example, a method of heating in an air atmosphere at 50 to 150°C for 2 to 20 hours is included. The shape of the cured product is not particularly limited, and for example, a sheet shape is included.
[0062] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to the specific embodiment, and various modifications and changes are possible within the scope of the gist of the present invention described in the claims. EXAMPLES
[0063] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0064] [Example 1] (Preparation of Resin Additive Composition) <First step> As the medium A, 10 g of epoxy resin A (bisphenol F (JER806, manufactured by Mitsubishi Chemical Corporation)) was mixed with 40 g of toluene as an organic solvent and stirred at room temperature for 1 hour. Next, the obtained solution was mixed with Nanom (registered trademark) Mix (C, manufactured by Frontier Carbon Corporation), which is a fullerene. 60 61% by mass, C 70 28% by mass, C 70 The mixture was mixed with 0.05 g of a mixture containing 11 mass % of larger higher-order fullerenes, and stirred at room temperature for 6 hours to obtain a fullerene dispersion. This fullerene dispersion contains C 60 600 mass ppm, C 70 It was confirmed by HPLC that the content was 250 ppm by mass.
[0065] <Second process> This fullerene dispersion was transferred into a pressure-resistant stainless steel container. Two gas inlets were attached to the lid of this container. The container had a capacity of 250 mL. Nitrogen gas was allowed to flow into the inside of this container from one of the gas inlets, and the gas inside the container was evacuated from the other, and the container was left for 10 minutes. Thereafter, the nitrogen injection was stopped and the container was sealed. In this state, the container was left in an oil bath at 140°C. Here, the concentration of oxygen dissolved in the fullerene dispersion was measured by the following procedure. First, 100 mL of n-dodecane (manufactured by Wako Pure Chemical Industries, Ltd.) was placed in a 250 mL beaker, and air was bubbled into the beaker for 10 minutes. Next, the oxygen concentration of this solution was set to the standard (100% saturation) using a dissolved oxygen meter (product name: B-506, manufactured by Iijima Electronics Co., Ltd.). Next, the saturated oxygen concentration of the fullerene dispersion in the stainless steel container was measured, and the result was that the saturated oxygen concentration was 150% before the nitrogen gas was introduced and 7% after the nitrogen gas was introduced. Next, the saturated oxygen concentration of dodecane in air was set to 73 ppm by mass, and from this value and the above values of 150% and 7%, the dissolved oxygen concentrations in the fullerene dispersion were calculated to be 110 ppm by mass and 5 ppm, respectively. 0.1 mL of the fullerene dispersion in the reaction vessel was withdrawn every 2 hours, and the C 60 and C. 70 The amount of was quantified by HPLC. 60 is 60 ppm, C 70 When the concentration decreased to 20 ppm, the temperature of the oil bath was lowered to 100°C. The fullerene dispersion was treated with C 60 600 mass ppm, C 70 After heat treatment, 60 is 60 mass ppm, C 70 The amount of fullerene was reduced to 1 / 10 or less because a part of the epoxy resin was cleaved by heating and added to the fullerene.
[0066] As a fourth step, a vacuum pump was connected to one of the gas inlets of the container to reduce the pressure inside the container. The container was left in this state for 1 hour to remove volatile components such as toluene from inside the container. A highly viscous liquid was taken out from inside the container to obtain a resin additive composition. The mass of the obtained resin additive composition was 10 g, and the organic solvent toluene was removed.
[0067] (Preparation of resin composition) The resin additive composition was mixed with 8 g of HN-2200 (manufactured by Hitachi Chemical Co., Ltd.), which is an epoxy resin curing agent, and 1 g of 1-cyanoethyl-2-ethyl-4-methylimidazole (manufactured by Wako Pure Chemical Industries, Ltd.), which is an initiation curing accelerator, as a medium B. The resin composition of this example was obtained. The resin composition of this example was poured into a frame capable of producing a 1 mm thick sheet, and was heated in an air atmosphere at 70° C. for 12 hours to harden it, producing a sheet-like hardened resin composition.
[0068] (Evaluation of withstand voltage) The withstand voltage was measured using a dielectric breakdown tester YST-243-100RH0 (manufactured by Yamayo Test Instruments Co., Ltd.) in accordance with JIS C2110-1 using a 20-second step method. First, the sheet was placed in a silicon oil bath at room temperature and sandwiched between electrodes with a diameter of 25 mm from above and below the thickness direction of the sheet. Next, if no dielectric breakdown occurred at the specified voltage for 20 seconds, the voltage increase step was repeated, and the voltage set before dielectric breakdown was regarded as the withstand voltage. The voltage was increased by 1 kV increments up to 20 kV, and by 2 kV increments after 20 kV. The obtained withstand voltages are shown in Table 1.
[0069] (Evaluation of heat resistance) The heat resistance of the sheet was measured by a thermogravimetric method using a thermobalance (Shimadzu Corporation, DTG-60A). First, a 0.5 mm square piece of resin was cut from the sheet and placed on a balance. Next, the temperature of the balance was raised from room temperature to 500°C at a rate of 10°C per minute, and the change in weight of the resin piece was measured. When heated, the resin piece was burned by oxygen in the air, causing it to lose weight. The temperature at which the weight of the resin had decreased by 10% was taken as the heat resistance temperature. The heat resistance values obtained are shown in Table 1.
[0070] (Mechanical strength evaluation) The strength of the sheet was measured by a tensile test method using a tensile tester (RTF-1210, manufactured by A&T Corporation). First, a resin piece 10 mm wide and 100 mm long was cut from the sheet and placed in a tensile test device. The resin piece was then pulled at 1 mm per minute, and the tensile strength was measured until it broke. The maximum tensile strength was recorded as the tensile strength. The tensile strengths obtained are shown in Table 1.
[0071] (Evaluation of surface smoothness) The surface smoothness of the sheet was measured by arithmetic mean height (Ra) using a surface roughness meter (DektakXT, manufactured by Bruker Corporation). First, a resin piece 10 mm wide and 10 mm long was cut out from the sheet and set in a surface roughness meter. Next, a length of 5 mm was measured and the arithmetic average height (Ra) was calculated. The obtained surface smoothness is shown in Table 1.
[0072] (Quantitative method for fullerene determination by HPLC) The fullerene concentration was measured using a high performance liquid chromatograph under the following measurement conditions to quantitatively determine the amount of fullerene contained in the resin additive composition. Equipment: Agilent Technologies 1200 Series Column: YMC-Pack ODS-AM (150mm x 4.6) manufactured by YMC Co., Ltd. Developing solvent: 1:1 (volume ratio) mixture of toluene and methanol Detection: absorbance (wavelength 309 nm).
[0073] [Example 2] A resin additive composition was prepared by the same procedure as in Example 1, except that the step of flowing nitrogen gas in the step of heat-treating the fullerene dispersion in Example 1 was omitted. Using the obtained resin additive composition, a resin composition was prepared in the same manner as in Example 1, and a cured product of the sheet-shaped resin composition was prepared. The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained sheet are shown in Table 1.
[0074] [Comparative Example 1] As a comparative sample, a resin additive composition was prepared by the same procedure as in Example 1, except that the step of heat-treating the fullerene dispersion was omitted. Using the obtained resin additive composition, a resin composition was prepared in the same manner as in Example 1, and a cured product of the sheet-shaped resin composition was prepared. The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained sheet are shown in Table 1. From the results in Table 1, Example 1 and Example 2 were compared with Comparative Example 1. The resin compositions prepared in Example 1 and Example 2 had improved heat resistance, surface smoothness, mechanical properties, and voltage resistance compared to the resin composition prepared in Comparative Example 1. In Example 1 and Example 2, the resin composition was prepared after processing fullerene into a resin additive composition. In contrast, in Comparative Example 1, the resin composition was prepared without processing fullerene into a resin additive composition. Comparing Example 2 with Example 1, by using a nitrogen atmosphere during the heat treatment, the heat resistance, surface smoothness, mechanical properties, and voltage resistance were improved compared to the resin composition prepared without using a nitrogen atmosphere. In the resin additive compositions of Examples 1 and 2, the epoxy monomer molecules contained in medium A were cleaved by heating and added to the fullerenes, which increased the affinity of the fullerenes to the epoxy resin, thereby improving the fullerene solubility in the resin composition.
[0075] [Example 3] In Example 1, the resin composition and its sheet-shaped cured product were obtained by the method shown in Example 1, except that the medium A was 20 g of polyoxyethylene (Unistar MB-881, NOF Corp.), and toluene was not added to obtain a resin additive composition; the fourth step (removal of volatiles = toluene) was not performed; and the medium B was a mixture of 100 g of epoxy resin B (Mitsubishi Chemical Corp., JER828), 100 g of HN-2200 (Hitachi Chemical Co., Ltd.) as a curing agent, and 10 g of 1-cyanoethyl-2-ethyl-4-methylimidazole (Wako Pure Chemical Industries, Ltd.) as an initial curing accelerator. The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained sheet are shown in Table 1.
[0076] [Comparative Example 2] As a comparative sample, a resin additive composition was prepared by the same procedure as in Example 2, except that the step of heat-treating the fullerene dispersion was omitted. Using the obtained resin additive composition, a resin composition was prepared in the same manner as in Example 1, and a cured product of the sheet-shaped resin composition was prepared. The voltage resistance, heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained sheet are shown in Table 1. Comparing Example 3 and Comparative Example 2 from the results in Table 1, the resin composition prepared in Example 3 had improved heat resistance, surface smoothness, mechanical properties, and voltage resistance compared to the resin composition prepared in Comparative Example 2. In Example 3, the resin composition was prepared after processing fullerene into a resin additive composition. In contrast, in Comparative Example 2, the resin composition was prepared without processing fullerene into a resin additive composition. In the resin additive composition of Example 3, the chemical bonds constituting the polyoxyethylene molecules contained in medium A were gradually cleaved and attached to the fullerenes, which increased the affinity of the fullerenes to the epoxy resin, thereby improving the fullerene solubility in the resin composition.
[0077] [Example 4] A resin composition and a sheet-shaped cured product thereof were obtained by the method shown in Example 1, except that in Example 1, medium A was obtained by using 5 g of epoxy resin C (manufactured by Kyoeisha Chemical Co., Ltd., neopentyl glycol diglycidyl ether, Epolite 1500NP) and 45 g of xylene as a solvent to obtain a resin additive composition; and medium B was obtained by using 5 g of epoxy resin C. The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin composition are shown in Table 1.
[0078] [Comparative Example 3] As a comparative sample, a resin composition and a sheet-like cured product thereof were prepared by the same procedure as in Example 3, except that the step of heat-treating the fullerene dispersion was omitted. The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained sheet are shown in Table 1. Comparing Example 4 and Comparative Example 3 from the results in Table 1, the resin composition prepared in Example 4 had improved heat resistance, surface smoothness, mechanical properties, and voltage resistance compared to the resin composition prepared in Comparative Example 3. In Example 4, the resin composition was prepared after processing fullerene into a resin additive composition. In contrast, in Comparative Example 3, the resin composition was prepared without processing fullerene into a resin additive composition. In the resin additive composition of Example 4, the chemical bonds constituting the neopentyl glycol diglycidyl ether molecule contained in the medium A were gradually cleaved and added to the fullerene. This increased the affinity of the fullerene to the epoxy resin. This is believed to be due to the improved solubility of the fullerene in the resin composition.
[0079] [Example 5] (thermoplastic resin) A resin additive composition was obtained by the procedure of Example 1, except that medium A was 75 g of polymethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) and 25 g of paradichlorobenzene (manufactured by Tokyo Chemical Industry Co., Ltd.). The resin composition was prepared by taking out the resin additive composition and kneading it with 350 g of polymethyl methacrylate (manufactured by Tokyo Kasei Co., Ltd.) as medium B using a twin-screw extruder (Toyo Seiki Seisakusho Co., Ltd., Labo Plastomill 4C150). The kneading conditions were a small twin-screw segment extruder (model: 2D15W), intermeshing type synchronous rotation, L / D=17 (D is screw diameter, L is screw length, D=15 mm), and kneading at 140°C to obtain a resin composition. The obtained resin composition was molded into a sheet with a thickness of 1 mm to obtain a sheet-shaped cured product. The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained sheet are shown in Table 1.
[0080] [Comparative Example 4] As a comparative sample, a resin composition and a sheet-like cured product thereof were prepared by the same procedure as in Example 5, except that the step of heat-treating the fullerene dispersion was omitted. The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained sheet are shown in Table 1. Comparing the results of Table 1 between Example 5 and Comparative Example 4, the resin composition prepared in Example 5 had improved surface smoothness, mechanical properties, and voltage resistance compared to the resin composition prepared in Comparative Example 4. In addition, the heat resistance was slightly improved. In Example 5, the resin composition was prepared after processing fullerene into a resin additive composition. In contrast, in Comparative Example 4, the resin composition was prepared without processing fullerene into a resin additive composition. The following is considered for the resin additive composition of Example 5. The chemical bonds constituting the polymethyl methacrylate molecules contained in the medium A were gradually cleaved, and these were added to the fullerene. As a result, the affinity of the fullerene to the methyl methacrylate resin was increased. As a result, the fullerene solubility in the resin composition was improved.
[0081] [Example 6] (thermoplastic resin) A resin composition was obtained by the method shown in Example 5, except that in Example 5, the medium A was 10 g of trimethylbenzene (manufactured by Tokyo Chemical Industry Co., Ltd.) and the resin additive composition was obtained without using paradichlorobenzene; and the medium B was the resin additive composition and 25 g of polymethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.). The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained resin composition are shown in Table 1.
[0082] [Comparative Example 5] As a comparative sample, a resin additive was prepared by the same procedure as in Example 6, except that the step of heat-treating the fullerene dispersion was omitted. The heat resistance, surface smoothness, mechanical properties, and voltage resistance of the obtained resin composition are shown in Table 1. Comparing Example 6 and Comparative Example 5 from the results in Table 1, the resin composition prepared in Example 6 had improved surface smoothness, mechanical properties, and voltage resistance compared to the resin composition prepared in Comparative Example 5. Also, the heat resistance was slightly improved. In Example 6, the resin composition was prepared after processing fullerene into a resin additive composition. In contrast, in Comparative Example 5, the resin composition was prepared without processing fullerene into a resin additive composition. In the resin additive composition of Example 6, the chemical bonds constituting the trimethylbenzene molecules contained in the medium A were gradually cleaved and added to the fullerenes. This increased the affinity of the fullerenes to the methyl methacrylate resin. This is believed to be due to the improved solubility of the fullerenes in the resin composition.
[0083] [Table 1] [Industrial Applicability]
[0084] According to the present invention, the heat resistance, surface smoothness, mechanical properties, and voltage resistance of the resin can be improved by using a fullerene-containing resin additive composition that contains a medium A and a fullerene and is heat-treated.
Claims
1. A step of mixing a medium A and a fullerene to obtain a fullerene dispersion containing the medium A and the fullerene; and heat-treating the fullerene dispersion at 100° C. or more and 250° C. or less. A method for producing a resin additive composition for a thermosetting resin to be added to a thermosetting resin, comprising the steps of: The medium A is a raw material of a thermosetting resin, the raw material of the thermosetting resin is at least one selected from the group consisting of a polymerizable monomer, a polymerizable oligomer, and a reactive component; The polymerizable monomer or the polymerizable oligomer is polymerized by heating or light irradiation in the presence of a curing agent or a photocuring agent to produce a phenolic resin, an epoxy resin, a melamine resin, a urea resin, an unsaturated polyester resin, an alkyd resin, a polyurethane, or a polyimide; The method for producing a resin additive composition for thermosetting resins, wherein the reactive component is at least one selected from the group consisting of linear or branched hydrocarbons, hydrocarbons having an unsaturated double bond, aromatic hydrocarbons having an alkyl group, hydrocarbons having a polycyclic aromatic ring, compounds having an ether bond, compounds having an ester group, compounds having a disulfide bond, di-p-tolyl disulfide, compounds having phenolic hydroxyl group, diazo compounds, and silicones.
2. The method for producing a resin additive composition for thermosetting resins according to claim 1, wherein an organic solvent is mixed in the step of obtaining the fullerene dispersion.
3. 3. The method for producing a resin additive composition for thermosetting resins according to claim 1, wherein the step of heat-treating the fullerene dispersion is carried out in a low-oxygen atmosphere.
4. The method for producing a resin additive composition for thermosetting resins according to claim 3, wherein the oxygen concentration in the fullerene dispersion is 10 ppm by mass or less.
5. In the step of heat treating the fullerene dispersion, determining a heating temperature and a heating time of the fullerene dispersion; The step of determining the heating temperature and heating time of the fullerene dispersion includes: measuring the concentration of the fullerene in the fullerene dispersion in a heated state at regular intervals to prepare a calibration curve showing the relationship between the concentration of the fullerene in the fullerene dispersion and the heating time of the fullerene dispersion; The method for producing the resin additive composition for thermosetting resins according to any one of claims 1 to 4, further comprising a step of determining a heating temperature and a heating time of the fullerene dispersion based on the calibration curve.
6. The method for producing a resin additive composition for thermosetting resins according to any one of claims 1 to 5, wherein the fullerene is any one of C60, C70, and a mixture containing C60 and C70.
7. The method for producing a resin additive composition for thermosetting resins according to any one of claims 1 to 6, further comprising a step of removing insoluble components from the fullerene dispersion.
8. The method for producing a resin additive composition for thermosetting resins according to any one of claims 1 to 7, further comprising a step of removing volatile components from the resin additive composition.
9. A medium A and a fullerene adduct are included, The medium A is a raw material of a thermosetting resin, the raw material of the thermosetting resin is at least one selected from the group consisting of a polymerizable monomer, a polymerizable oligomer, and a reactive component; The polymerizable monomer or the polymerizable oligomer is polymerized by heating or light irradiation in the presence of a curing agent or a photocuring agent to produce a phenolic resin, an epoxy resin, a melamine resin, a urea resin, an unsaturated polyester resin, an alkyd resin, a polyurethane, or a polyimide; the reactive component is at least one selected from the group consisting of linear or branched hydrocarbons, hydrocarbons having an unsaturated double bond, aromatic hydrocarbons having an alkyl group, polycyclic aromatic hydrocarbons, compounds having an ether bond, compounds having an ester group, compounds having a disulfide bond, di-p-tolyl disulfide, compounds having a phenolic hydroxyl group, diazo compounds, and silicones; The fullerene adduct is a compound in which a structure derived from a component contained in the medium A is added to a fullerene, and is a resin additive composition for thermosetting resins to be added to a thermosetting resin.
10. The method includes the steps of obtaining a resin additive composition by the method for producing a resin additive composition for a thermosetting resin according to any one of claims 1 to 8, and mixing the obtained resin additive composition with a medium B, The medium B includes a curing agent for a thermosetting resin.
11. The method for producing a thermosetting resin composition according to claim 10 , wherein the medium B contains a raw material for a thermosetting resin.
12. A mixture of the resin additive composition for thermosetting resins according to claim 9 and a medium B, The medium B is a thermosetting resin composition containing a curing agent for a thermosetting resin.
13. The thermosetting resin composition according to claim 12 , wherein the medium B contains a raw material of a thermosetting resin.
14. A cured product of the thermosetting resin composition according to claim 13.
Citation Information
Patent Citations
Resin composition and method for producing the same
JP2004182771A
Method of compounding a nanocarbon
JP2004331929A
Resin composition
JP2006016466A
Polyester resin composition and its manufacturing method
JP2006117760A
Resin composition, wire cable and master batch
JP2018104549A
Cited By
Reactive composition for highly transparent thermosetting resin, and glass fiber composite comprising same
WO2026206048A1