Hydraulic materials

A hydraulic material with blast furnace slag, copper slag, and an alkali stimulant produces high-strength mortar, addressing the challenge of cement-free production and waste utilization.

JP7586752B2Active Publication Date: 2024-11-19MITSUBISHI UBE CEMENT CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021057275
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-11-19
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

The production of high-strength mortar without using cement is challenging, and the cement firing process emits large amounts of carbon dioxide, while copper slag, a by-product of copper smelting, is underutilized and often disposed of in landfills.

Method used

A hydraulic material comprising blast furnace slag powder, copper slag powder, and an alkali stimulant is used to produce high-strength mortar, with specific ratios and surface areas enhancing the synergistic effects of these components.

Benefits of technology

The proposed solution enables the production of high-strength mortar using copper slag without cement, reducing carbon emissions and effectively utilizing a waste material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586752000006
    Figure 0007586752000006
  • Figure 0007586752000007
    Figure 0007586752000007
  • Figure 0007586752000008
    Figure 0007586752000008
Patent Text Reader

Abstract

To provide a hydraulic material which employs a copper slag and can elevate hardness of mortar by synergic effect of a blast furnace slag powder and a copper slag powder without using cement.SOLUTION: A hydraulic material involves a blast furnace slag powder, a copper slag powder, and an alkali stimulant. A mass ratio of the copper slag powder to a total mass of 100 mass% of the blast furnace slag powder and the copper slag powder is preferably 1% or over and 99% or under. The hydraulic material may further involve fly ash. In this case, a mass ratio of the copper slag powder to a total mass of 100 mass% of the blast furnace slag powder, the copper slag powder, and the fly ash is preferably 1% or over and 99% or under. A specific surface area of the blast furnace slag powder is preferably 3500 cm2 / g or over.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydraulic material. [Background technology]

[0002] The following Patent Document 1 describes the production of mortar by adding water to a cement composition containing cement, blast furnace slag, fly ash, and an alkali.

[0003] However, a cement burning process is necessary to produce cement. A large amount of carbon dioxide is emitted from this cement burning process. For this reason, in the technology described in the following Patent Document 1, a large amount of carbon dioxide is emitted from the cement burning process because it is necessary to produce cement. However, there is also the problem that it is difficult to produce high-strength mortar without using cement.

[0004] On the other hand, copper slag is a by-product that contains a lot of iron and is produced during copper refining. Although some of the copper slag is used domestically as heavy aggregate for heavy concrete and as a filler for caissons, the majority of it is currently exported overseas and disposed of in landfills. Therefore, there is a need to establish a method to effectively utilize copper slag and expand its uses. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-104266 A Summary of the Invention [Problem to be solved by the invention]

[0006] The inventors of the present invention have conducted extensive research into a method for producing high-strength mortar using copper slag without using cement, and as a result have discovered that high-strength mortar can be produced by kneading a hydraulic material containing blast furnace slag powder, copper slag powder, and an alkaline stimulant with water. The present invention has been made based on this knowledge, and aims to provide a hydraulic material that can be used to produce high-strength mortar using copper slag without using cement. [Means for solving the problem]

[0007] The hydraulic material according to the first aspect of the present invention contains blast furnace slag powder, copper slag powder, and an alkaline stimulant. According to the first aspect, it is possible to manufacture high-strength mortar using copper slag without using cement. This point will be described in detail in the test examples described later.

[0008] The hydraulic material according to the second aspect of the present invention is one in which the mass ratio of the copper slag powder to the total mass 100% of the blast furnace slag powder and the copper slag powder is 1% or more and 99% or less. Here, the mass ratio of the alkali stimulant to this total mass 100% is, for example, 5% or more by external ratio. According to the second aspect, a high-strength mortar can be produced using a large amount of copper slag. This point will be explained in detail in the test example described later.

[0009] The hydraulic material according to the first aspect of the present invention may contain fly ash. The hydraulic material according to the third aspect of the present invention is one in which the mass ratio of the copper slag powder to the total mass 100% of the blast furnace slag powder, the copper slag powder, and the fly ash is 1% or more and 99% or less. Here, the mass ratio of the alkali stimulant to this total mass 100% is, for example, 5% or more by external ratio. According to the third aspect, a high-strength mortar can be produced using a large amount of copper slag. This point will be explained in detail in the test example described later.

[0010] The hydraulic material according to the fourth aspect of the present invention is characterized in that the specific surface area of ​​the blast furnace slag powder is 3500 cm2 / g or more. According to the fourth item, a mortar with even higher strength can be produced.

[0011] In each of the above items, the alkaline irritant may be, for example, one or more of an alkali hydroxide, an alkali silicate, an alkali carbonate, and an alkali borate. Effect of the Invention

[0012] As described above, according to the present invention, high-strength mortar can be produced by using copper slag without using cement. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a graph showing the results of examples and comparative examples of the hydraulic material according to the first embodiment of the present invention, and shows the relationship between the copper slag powder content and the compressive strength of the mortar. [Diagram 2] FIG. 2 is a graph showing the results of examples and comparative examples of the hydraulic material according to the second embodiment of the present invention, showing the relationship between the copper slag powder content and the compressive strength of the mortar. [Diagram 3] FIG. 3 is a graph showing the results of examples and comparative examples of the hydraulic material according to the second embodiment of the present invention, showing the relationship between the copper slag powder content and the compressive strength of the mortar. [Figure 4] FIG. 4 is a graph showing the results of examples and comparative examples of the hydraulic material according to the second embodiment of the present invention, and shows the relationship between the specific surface area of ​​blast furnace slag powder and the compressive strength of mortar. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] A hydraulic material according to a first embodiment of the present invention will be described. The hydraulic material according to the first embodiment contains blast furnace slag powder, copper slag powder, and an alkaline stimulant. As the alkaline stimulant, for example, one or more of an alkali hydroxide, an alkali silicate, an alkali carbonate, and an alkali borate can be used. Specifically, for example, sodium hydroxide or water glass can be used as the alkaline stimulant, but the type of the alkaline stimulant that can be used is not limited to these.

[0015] In the hydraulic material according to the first embodiment, the ratio of the mass of the copper slag powder to the total mass 100% of the blast furnace slag powder and the copper slag powder is preferably 1% or more and 99% or less. This ratio is more preferably 1% or more and 55% or less, more preferably 15% or more and 30% or less, and particularly preferably 15% or more and 20% or less. In this way, a high-strength mortar can be manufactured using a large amount of copper slag. The ratio of the mass of the alkali stimulant to the total mass 100% is, for example, 5% or more, specifically 10%.

[0016] The hydraulic material according to the second embodiment of the present invention will be described. The hydraulic material according to the second embodiment further contains fly ash in addition to the blast furnace slag powder, copper slag powder, and alkaline activator used in the first embodiment.

[0017] The ratio of the mass of the copper slag powder to the total mass 100% of the blast furnace slag powder, the copper slag powder, and the fly ash is preferably 1% or more and 99% or less. This ratio is more preferably 10% or more and 50% or less, more preferably 10% or more and 40% or less, and particularly preferably 10% or more and 30% or less. In this way, a high-strength mortar can be produced using a large amount of copper slag. The ratio of the mass of the alkali irritant to the total mass 100% is, for example, 5% or more, specifically 10%.

[0018] In order to manufacture a high-strength mortar by mixing the hydraulic material according to the first or second embodiment with water, the specific surface area of ​​the blast furnace slag powder must be 3500 cm 2 / g or more, and this specific surface area is preferably 4000 cm 2 / g or more (or 5000cm 2 / g or more), and this specific surface area is preferably 7500 cm 2 / g or more, and the specific surface area is preferably 7970 cm 2 / g or more is particularly preferred. In this specification, the specific surface area means the specific surface area measured using a Blaine air permeation device. A specific method for measuring this specific surface area is specified in the Japanese Industrial Standard JIS R 5201 "Physical Testing Methods for Cement."

[0019] Next, examples of the hydraulic material according to the first embodiment of the present invention and comparative examples thereof will be described. In these examples and comparative examples, the compressive strength of test specimens obtained from a mixture of hydraulic material, fine aggregate, and water was measured with reference to JIS R 5201 "Physical Testing Methods for Cement." Standard sand specified in JIS R 5201 "Physical Testing Methods for Cement" was used as the fine aggregate.

[0020] Specifically, the test was carried out as follows. First, an alkaline irritant (specifically, sodium hydroxide) dissolved in water was put into a Hobart-type mixer (manufactured by Hobart Japan Co., Ltd.). Next, powder (materials constituting the hydraulic material excluding the alkaline irritant) was put into the Hobart-type mixer to prepare the hydraulic material.

[0021] Then, the Hobart mixer was operated in low-speed mode (rotation speed: 140 rpm for rotation, 62 rpm for revolution) for 30 seconds to mix the hydraulic material and water. Immediately after 30 seconds, fine aggregate was added to the Hobart mixer while it was operating in low-speed mode. Furthermore, the Hobart mixer was operated in medium-speed mode (rotation speed: 285 rpm for rotation, 125 rpm for revolution) for 30 seconds to mix the hydraulic material, fine aggregate, and water. After 30 seconds, the Hobart mixer was stopped. Then, the kneaded material (mixture of hydraulic material, fine aggregate, and water) attached to the paddle of the Hobart mixer was scraped off from the paddle and the system was left on standby for 75 seconds. Then, the Hobart mixer was operated in medium-speed mode for 1 minute to mix the hydraulic material, fine aggregate, and water. After 1 minute, the Hobart mixer was stopped and the kneaded material was removed from the Hobart mixer.

[0022] Further, the triple-part frame was placed on the table vibrator. Each frame in the triple-part frame was formed into a rectangular parallelepiped with a length of 16 cm, a width of 4 cm, and a height of 4 cm. In addition, only the top surface of each frame was open. Next, while vibrating the table vibrator, the kneaded material taken out from the Hobart mixer was filled into each frame in the triple-part frame with a spoon to a height of 2 cm in 15 seconds. After that, the table vibrator was kept vibrating and the frame was left waiting for 15 seconds. After 15 seconds, the kneaded material taken out from the Hobart mixer was filled into each frame in the triple-part frame with a spoon to a height of 4 cm in 15 seconds. As a result, the kneaded material filled into each frame in the triple-part frame became two layers. Then, the table vibrator was kept vibrating and the frame was left waiting for 75 seconds.

[0023] After 75 seconds, the vibration of the table vibrator was stopped. Then, the kneaded material that protruded upward from the upper surface of each formwork in the triple formwork was scraped off using a trowel. Furthermore, the upper surface of each formwork in the triple formwork was blocked with a flat plastic plate. Then, the kneaded material filled in the triple formwork was cured for 24 hours in an environment of 20°C. Then, the hardened kneaded material was steam cured and then demolded to obtain a geopolymer hardened body. Specifically, for the steam curing, the hardened kneaded material was heated from room temperature to 80°C over 3 hours, held in an environment of 80°C for 5 hours, and cooled from 80°C to room temperature over 3 hours. Furthermore, this geopolymer hardened body was autoclave cured. Specifically, for the autoclave curing, the geopolymer hardened body was heated from room temperature to 180°C over 3 hours, held in an environment of 180°C and 10 atm for 5 hours, and cooled from 180°C to room temperature over 3 hours. The compressive strength of the hardened geopolymer (specimen) after autoclave curing was measured with reference to JIS R 5201 "Physical testing methods for cement".

[0024] The materials used in these Examples and Comparative Examples are shown in Table 1. In Table 1, the density and specific surface area are shown as values ​​measured in accordance with JIS R 5201 "Physical Testing Methods for Cement."

[0025] [Table 1]

[0026] Table 2 shows the relationship between the composition of the powder and the compressive strength of the test specimen in Examples A1-A3 and Comparative Examples A1-A2. In Examples A1-A3, blast furnace slag powder (B2-8 shown in Table 1) and copper slag powder (C-5 shown in Table 1) were used as the powder. In Comparative Example A1, only the blast furnace slag powder was used as the powder, without using copper slag powder. In Comparative Example A2, only the copper slag powder was used as the powder, without using blast furnace slag powder.

[0027] [Table 2]

[0028] In Examples A1-A3 and Comparative Examples A1-A2, the mass ratio of the alkaline irritant to 100% by mass of the powder was 10%, and the mass ratios of the fine aggregate and the water to 100% by mass of the powder were 300% and 50%, respectively.

[0029] FIG. 1 is a graph showing the relationship between the copper slag powder content shown in Table 2 and the compressive strength of the above test specimens. The plots in FIG. 1 relate to Examples A1-A3 and Comparative Examples A1-A2 shown in Table 2. The dashed line shown in FIG. 1 is a straight line connecting the plots of Comparative Examples A1 and A2. This dashed line represents the strength of the above test specimens predicted from the mass ratio of the copper slag powder in the hydraulic material (i.e., the copper slag powder content in the powder). The solid line shown in FIG. 1 is a straight line connecting the plots of Comparative Example A1, Examples A1-A3, and Comparative Example A2 in order.

[0030] If it is assumed that there is no synergistic effect between the powdered blast furnace slag and the powdered copper slag in Examples A1-A3, the dashed line and the solid line in Figure 1 should coincide. However, the solid line is located above the dashed line in Figure 1. In other words, it is considered that the compressive strength of the test specimens in Examples A1-A3 was increased by the synergistic effect between the powdered blast furnace slag and the powdered copper slag.

[0031] As shown in Fig. 1, the difference in compressive strength between the solid line and the broken line is larger when the copper slag powder content is in the range of 1% to 99% than when the copper slag powder content is outside this range. Furthermore, this difference is larger when the copper slag powder content is in the range of 1% to 55%, even larger when the copper slag powder content is in the range of 15% to 30%, and particularly large when the copper slag powder content is in the range of 15% to 20%. Note that, as shown in Fig. 1, when the copper slag powder content is 45.3% or less, the compressive strength is 60 N / mm 2 That's all.

[0032] Next, examples and comparative examples of the hydraulic material according to the second embodiment of the present invention will be described. The test contents in these examples and comparative examples are the same as those in the examples and comparative examples of the hydraulic material according to the first embodiment of the present invention, except for the points described below.

[0033] Table 3 shows the relationship between the composition of the powder and the compressive strength of the test specimen in Examples B1-B5 and Comparative Examples B1-B2. In Examples B1-B5, in addition to the blast furnace slag powder and copper slag powder used in Examples A1-A3, fly ash (F1-5 shown in Table 1) was used as the powder. In Comparative Example B1, the blast furnace slag powder and the fly ash were used as the powder, without using the copper slag powder. In Comparative Example B2, only the copper slag powder was used as the powder, without using the blast furnace slag powder and the fly ash.

[0034] [Table 3]

[0035] FIG. 2 is a graph showing the relationship between the copper slag powder content shown in Table 3 and the compressive strength of the above test specimens. The plots in FIG. 2 relate to Examples B1-B5 and Comparative Examples B1-B2 shown in Table 3. The dashed line shown in FIG. 2 is a straight line connecting the plots of Comparative Example B1 and Comparative Example B2. This dashed line is the strength of the above test specimen predicted from the mass ratio of the copper slag powder in the hydraulic material (i.e., the copper slag powder content in the above powder). The solid line shown in FIG. 2 is a straight line connecting the plots of Comparative Example B1, Examples B1-B5, and Comparative Example B2 in order.

[0036] If it is assumed that there is no synergistic effect between the powdered blast furnace slag and the powdered copper slag in Examples B1-B5, the dashed line and the solid line in Figure 2 should coincide. However, the solid line is located above the dashed line in Figure 2. In other words, it is considered that the compressive strength of the test specimens in Examples B1-B5 was increased by the synergistic effect between the powdered blast furnace slag and the powdered copper slag.

[0037] As shown in Fig. 2, the difference in compressive strength between the solid line and the broken line is larger when the copper slag powder content is in the range of 1% to 99% than when the copper slag powder content is outside this range. Furthermore, this difference is larger when the copper slag powder content is in the range of 10% to 50%, even larger when the copper slag powder content is in the range of 10% to 40%, and particularly large when the copper slag powder content is in the range of 10% to 30%. As shown in Fig. 2, when the copper slag powder content is 54.4% or less, the compressive strength is 60 N / mm 2 That's all.

[0038] Table 4 shows the relationship between the composition of the powder and the compressive strength of the test specimens in Examples C1-C3 and Comparative Examples C1 and B2. Comparative Example C1 differs from Comparative Example B1 only in that B2-4 shown in Table 1 was used as the blast furnace slag powder. Examples C1 and C2 differ from Examples B1 and B2 only in that B2-4 shown in Table 1 was used as the blast furnace slag powder. Example C3 differs from Examples C1 and C2 only in the blast furnace slag content, fly ash content, and copper slag powder content in the powder.

[0039] [Table 4]

[0040] Fig. 3 is a graph showing the relationship between the copper slag powder content shown in Table 4 and the compressive strength of the above test specimens. The plots in Fig. 3 relate to Examples C1-C3 and Comparative Examples C1 and B2 shown in Table 4. The dashed line shown in Fig. 3 is a straight line connecting the plots of Comparative Examples C1 and B2. The solid line shown in Fig. 3 is a straight line connecting the plots of Comparative Example C1, Examples C1-C3, and Comparative Example B2 in order.

[0041] If it is assumed that there is no synergistic effect between the blast furnace slag powder and the copper slag powder in Examples C1-C3, the dashed line and the solid line in Figure 3 should coincide. However, in Figure 3, the solid line is located above the dashed line. In other words, it is considered that the compressive strength of the test specimens in Examples C1-C3 was increased by the synergistic effect between the blast furnace slag powder and the copper slag powder.

[0042] As shown in Fig. 3, the difference in compressive strength between the solid line and the broken line is larger when the copper slag powder content is in the range of 1% to 99% than when the copper slag powder content is outside this range. This difference is larger when the copper slag powder content is in the range of 5% to 50%, and even larger when the copper slag powder content is in the range of 5% to 40%, and is particularly large when the copper slag powder content is in the range of 5% to 30%. As shown in Fig. 3, when the copper slag powder content is 22.6% or less, the compressive strength is 60 N / mm 2 That's all.

[0043] Table 5 shows the relationship between the specific surface area of ​​the blast furnace slag powder contained in the powder and the compressive strength of the test specimen in Examples D1-D3. In Examples D1-D3, blast furnace slag powder, fly ash, and copper slag powder were used as the powder. In Examples D1-D3, the fly ash and copper slag powder used were the same as those in Examples B1-B5. In Examples D1-D3, B2-5, B2-8, and B1-10 shown in Table 1 were used as the blast furnace slag powder. In Examples D1-D3, the blast furnace slag powder content in the powder was 60%, the fly ash content in the powder was 30%, and the copper slag powder content in the powder was 10%.

[0044] [Table 5]

[0045] In Examples D1 to D3, the ratio of the mass of the alkaline irritant to the mass of the powder was 10%, and the ratio of the mass of the water to the mass of the powder was 50%.

[0046] 4 is a graph showing the relationship between the specific surface area of ​​the blast furnace slag powder and the compressive strength of the above test specimens shown in Table 5. The plots in FIG. 4 relate to Examples D1-D3 shown in Table 5.

[0047] In FIG. 4, the specific surface area is 5000 cm 2 / g or more, the compressive strength is 65N / mm 2 The specific surface area is increased to about 7500 cm 2 / g or more, the compressive strength is 90N / mm 2 The specific surface area is increased to 7970 cm 2 / g or more, the compressive strength is 90N / mm 2 Exceed.

[0048] From the above, the following conclusion can be drawn: As can be seen from the results shown in Fig. 1, when a hydraulic material containing blast furnace slag powder, copper slag powder, and an alkaline activator is used, the strength of the mortar actually produced can be increased by the synergistic effect of the blast furnace slag powder and the copper slag powder, compared to the strength of the mortar predicted from the mass ratio of the copper slag powder in the hydraulic material.

[0049] Furthermore, as can be seen from the results shown in Figure 1, when the ratio of the mass of copper slag powder to the total mass of blast furnace slag powder and copper slag powder (100 mass%) is 1% or more and 99% or less, the strength of the mortar can be further increased by the synergistic effect of the blast furnace slag powder and the copper slag powder.

[0050] Furthermore, as can be seen from the results shown in Figures 2 and 3, when a hydraulic material containing blast furnace slag powder, fly ash, copper slag powder, and an alkaline activator is used, the strength of the mortar actually produced can be increased due to the synergistic effect of the blast furnace slag powder and the copper slag powder, compared to the strength of the mortar predicted from the mass ratio of the copper slag powder in the hydraulic material.

[0051] Furthermore, as can be seen from the results shown in Figures 2 and 3, when the ratio of the mass of copper slag powder to the total mass (100 mass%) of blast furnace slag powder, copper slag powder, and fly ash is 1% or more and 99% or less, the strength of the mortar can be further increased by the synergistic effect of the blast furnace slag powder and the copper slag powder.

[0052] Furthermore, as can be seen from the results shown in Figure 4, the specific surface area of ​​the blast furnace slag powder is 5000 cm 2 / g or more, a mortar with even higher strength can be produced. However, if the specific surface area of ​​the blast furnace slag powder is 3500 cm 2 / g or more, the strength of the mortar is increased to 50N / mm 2 It can be assumed that the strength of the mortar can be increased to a certain degree, and it is believed that a mortar with sufficiently high strength can be produced.

Claims

1. Contains blast furnace slag powder, copper slag powder and alkaline stimulant, The ratio of the mass of the copper slag powder to the total mass (100 mass%) of the blast furnace slag powder and the copper slag powder is 15% or more and 20% or less; And does not contain cement A hydraulic material characterized by:

2. 2. The hydraulic material according to claim 1, characterized in that the mass ratio of the alkaline irritant to the total mass of the blast furnace slag powder and the copper slag powder (100 mass%) is 5% or more.

3. A composition comprising blast furnace slag powder, copper slag powder, fly ash and an alkaline stimulant, The ratio of the mass of the copper slag powder to the total mass (100 mass%) of the blast furnace slag powder, the copper slag powder, and the fly ash is 10% or more and 30% or less. And does not contain cement A hydraulic material characterized by:

4. 4. The hydraulic material according to claim 3, characterized in that the mass ratio of the alkaline irritant to the total mass of the blast furnace slag powder, the copper slag powder and the fly ash (100 mass%) is 5% or more.

5. The specific surface area of ​​the blast furnace slag powder is 3500 cm 2 / g or more of the hydraulic material according to any one of claims 1 to 4.

6. 6. The hydraulic material according to claim 1, wherein the alkaline irritant is one or more of an alkali hydroxide, an alkali silicate, an alkali carbonate, and an alkali borate.

Citation Information

Patent Citations

  • Composition, hardened body, concrete cask and method for producing hardened body

    JP2004099425A

  • Method for producing set object

    JP2004299922A

  • Cement-based solidifying material

    JP2011093738A

  • Slag hardening composition and creating method thereof

    JP2012214317A

  • Cement composition and production method thereof, and production method of cement mortar or concrete

    JP2018104266A