Solidified powder containing acrylic crosslinked rubber particles, method for producing same, resin composition, and molded article

The coagulated powder with a crosslinked acrylic rubber structure addresses the impact resistance and dispersibility issues in methacrylic resin, enhancing the toughness and reducing surface defects of molded articles.

JP7586771B2Active Publication Date: 2024-11-19KURARAY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021091130
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-31
Publication Date
2024-11-19
Estimated Expiration
2041-05-31

AI Technical Summary

Technical Problem

Methacrylic resin molded articles suffer from insufficient impact resistance and surface defects due to the formation of particle aggregates when multilayer polymer particles are blended, and existing methods limit the types of resins that can be used and result in poor dispersibility and low impact resistance.

Method used

A coagulated powder containing crosslinked acrylic rubber particles with a specific structure and properties, including a crosslinked rubber inner layer and a thermoplastic resin outermost layer, is produced through emulsion polymerization, aggregation, and granulation, ensuring excellent dispersibility and impact resistance in a matrix resin.

Benefits of technology

The coagulated powder achieves excellent dispersibility and impact resistance in methacrylic resin, reducing surface defects and improving the toughness of molded products without compromising surface hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586771000004
    Figure 0007586771000004
  • Figure 0007586771000001
    Figure 0007586771000001
  • Figure 0007586771000002
    Figure 0007586771000002
Patent Text Reader

Abstract

To provide a coagulated powder including an acrylic cross-linked rubber particle excellent in dispersibility in a matrix resin (base resin), and excellent in impact resistance.SOLUTION: A coagulated powder includes an acrylic cross-linked rubber particle having an inner layer composed of a cross-linked rubber including an acrylic acid ester unit, an outermost layer composed of a thermoplastic resin including a (meth)acrylic acid unit and graft-bonding to the inner layer, and having an average particle size of 0.08-0.3 μm, where the consumed shear energy E necessary for dispersing the acrylic cross-linked rubber particle to monomodality of a dispersed particle size of 1 μm or under is 180 MJ / m3 or less in a 0.1 mass% acetone dispersion of a melt-kneaded composition of the coagulated powder and the (meth)acrylic resin when melt-kneading 60 pts.mass of a (meth)acrylic resin having an MFR at 230°C, 37.3 N of 8±1 g / 10 min. and 40 pts. mass of the coagulated powder, as measured by a kneading extrusion molding evaluation testing machine with a consumed shear energy measuring device at 230°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coagulated powder containing acrylic crosslinked rubber particles, a method for producing the same, a resin composition, and a molded article. [Background technology]

[0002] Methacrylic resin has excellent transparency, and its molded articles have a beautiful appearance and weather resistance, so it is used in a variety of applications, including lighting fixtures, display materials such as signs, optical materials such as display parts, interior materials, building materials, electronic and electrical materials, and medical materials. However, molded articles made of methacrylic resin have insufficient impact resistance, and there has been a problem in that they are prone to cracking and chipping when subjected to stress such as dropping, collision, and vibration.

[0003] To improve the impact strength of methacrylic resin, a method of adding multilayered polymer particles having a rubber component layer in the middle and a thermoplastic resin component layer as the outermost layer is preferably used, and this method is currently most widely used industrially.

[0004] However, in the conventional methacrylic impact-resistant resin in which the multilayered polymer particles are blended in the methacrylic resin, although the impact resistance is improved, the aggregates of the particles are observed as bumps on the surface of the molded product obtained from the resin, and there is a problem that the appearance defect with unevenness occurs. Patent Document 1 discloses a manufacturing method in which the impact modifier obtained by uniformly mixing the multilayered polymer obtained by emulsion polymerization and the rigid thermoplastic polymer in a latex state, and then solidifying and extracting the impact modifier has good dispersibility when melt-mixed with the rigid methacrylic resin, and can significantly improve the occurrence of bumps. However, since the impact modifier contains the rigid thermoplastic polymer, the proportion of the soft polymer layer is small, and the impact resistance relative to the amount added is poor. Patent Document 2 discloses a manufacturing method in which the multilayered polymer is dispersed in an organic solvent, and then the aqueous phase is separated to obtain aggregates, and the organic solvent is added to the aggregates, and the obtained dispersion is mixed with a polymerizable organic compound, thereby obtaining a good dispersion state of the multilayered polymer, but the resin that can be added is limited to a polymerizable organic compound having a reactive group such as an epoxy resin. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 3145864 [Patent Document 2] WO2005 / 028546 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a coagulated powder containing acrylic crosslinked rubber particles that has excellent dispersibility in a matrix resin (base resin) and excellent impact resistance. [Means for solving the problem]

[0007] In order to achieve the above object, the present invention provides a coagulated powder containing acrylic crosslinked rubber particles that satisfies the following conditions, a method for producing the same, and a resin composition and molded article each containing the coagulated powder. [1] A coagulated powder comprising an inner layer containing a crosslinked rubber containing an acrylic acid alkyl ester unit, and an outermost layer made of a thermoplastic resin containing a methyl methacrylate unit and graft-bonded to the inner layer, the thermoplastic resin of the outermost layer having a glass transition temperature of 60 to 85°C, a weight average molecular weight of 40,000 to 80,000, and an average particle size of 0.08 to 0.3 μm, When 60 parts by mass of methyl methacrylate resin having a melt flow rate of 8±1 g / 10 min at 230°C and 37.3 N and 40 parts by mass of the solidified powder were melt-kneaded at a temperature of 230°C using a kneading and extrusion molding evaluation test device equipped with a consumption shear energy measurement device, The consumed shear energy E required for the acrylic crosslinked rubber particles to be dispersed unimodally to a dispersed particle size of 1 μm or less in a 0.1 mass % acetone dispersion of the melt-kneaded composition of the solidified powder and the methyl methacrylate resin is 180 MJ / m 3 The coagulated powder is: [2] The coagulated powder according to [1], wherein the average particle size of the acrylic crosslinked rubber particles is 0.2 to 0.3 μm. [3] A polymerization step of producing a latex containing acrylic crosslinked rubber particles by an emulsion polymerization method; aggregating the latex at 35 to 65°C; The method for producing a coagulated powder according to [1] or [2], further comprising a granulation step of granulating at 100 to 130°C. [4] A resin composition comprising the coagulated powder according to [1] or [2] and a matrix resin. [5] The resin composition according to [4], wherein the thermoplastic resin is a methacrylic resin. [6] A molded article comprising the resin composition according to [4] or [5]. Effect of the Invention

[0008] According to the present invention, it is possible to provide a coagulated powder containing acrylic crosslinked rubber particles that has excellent dispersibility in a matrix resin (base resin) such as a thermoplastic resin and has excellent impact resistance. [Brief description of the drawings]

[0009] [Figure 1] 4 shows the results of measuring the dispersed particle size distribution of the coagulated powder in acetone. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Acrylic crosslinked rubber particles> The acrylic crosslinked rubber particles constituting the coagulated powder of the present invention are particles containing an acrylic crosslinked rubber polymer obtained by emulsion polymerization, and are preferably multi-layered rubber particles containing an outermost layer made of a thermoplastic polymer (P) and a crosslinked rubber polymer (Q) in contact with and covering the outermost layer. Examples of the multi-layered rubber particles include a two-layer structure (QP) in which the core is a crosslinked rubber polymer (Q) and the outer shell (outermost layer) is a thermoplastic polymer (P), a three-layer structure (RQP) in which the core is a crosslinked polymer (R) and the inner shell is a crosslinked rubber polymer (Q) and the outer shell (outermost layer) is a thermoplastic polymer (P), and a four-layer structure (QRQP) in which the core is a crosslinked rubber polymer (Q) and the first inner shell is a crosslinked polymer (R) and the second inner shell is a crosslinked rubber polymer (Q) and the outer shell (outermost layer) is a thermoplastic polymer (P).

[0011] The mass ratio of a layer other than the outermost layer in the acrylic crosslinked rubber particle (hereinafter, a layer other than the outermost layer may be referred to as an "inner layer", for example, the above Q, R+Q, and Q+R+Q each correspond to an inner layer) to the outermost layer is preferably 60 / 40 to 95 / 5, more preferably 70 / 30 to 90 / 10, for inner layer / outermost layer. The proportion of the layer containing the crosslinked rubber polymer (Q) in the inner layer is preferably 20 to 70 mass%, more preferably 30 to 50 mass%.

[0012] The average particle size of the acrylic crosslinked rubber particles is 0.08 to 0.3 μm, preferably 0.2 to 0.3 μm. When the acrylic crosslinked rubber particles having an average particle size within this range, particularly an average particle size of 0.2 to 0.3 μm, are used, toughness can be exhibited even with a small amount of incorporation, and therefore the rigidity and surface hardness of the molded product are not impaired. In this specification, the average particle size is the average value in the volume-based particle size distribution measured by the light scattering method (volume average particle size), or the average particle size measured from an electron microscope photograph. In one embodiment of the present invention, the glass transition temperature of the thermoplastic resin of the outermost layer is 60 to 85° C., and preferably 65 to 80° C. If the glass transition temperature of the thermoplastic resin is within this range, it is preferable in that the shear energy consumed during melt-kneading with the matrix resin is reduced. In another embodiment of the present invention, the weight average molecular weight (Mw) of the thermoplastic resin of the outermost layer is 40,000 to 80,000, and preferably 50,000 to 70,000. If the weight average molecular weight of the thermoplastic resin is within this range, it is preferable in terms of impact resistance and dispersibility.

[0013] The thermoplastic polymer (P) constituting the outermost layer is preferably a methacrylic acid alkyl ester having an alkyl group having 1 to 8 carbon atoms (hereinafter referred to as "methacrylic acid C 1~8 It is a polymer containing a methacrylic acid alkyl ester (sometimes referred to as "methacrylic acid alkyl ester") unit and, if necessary, a monofunctional monomer unit other than the methacrylic acid alkyl ester. It is preferable that the thermoplastic polymer (P) does not contain a polyfunctional monomer unit.

[0014] The amount of the methacrylic acid alkyl ester units having an alkyl group having 1 to 8 carbon atoms constituting the thermoplastic polymer (P) is preferably 75 to 100 mass %, more preferably 80 to 95 mass %, based on the mass of the thermoplastic polymer (P).

[0015] Methacrylic acid alkyl esters having an alkyl group with 1 to 8 carbon atoms (hereinafter referred to as methacrylic acid C 1~8A preferred example of the alkyl ester is methyl methacrylate (MMA).

[0016] Methacrylic acid C that constitutes the thermoplastic polymer (P) 1~8 The amount of the monofunctional monomer units other than the alkyl ester is preferably from 0 to 25% by mass, more preferably from 5 to 20% by mass, based on the mass of the thermoplastic polymer (P). Methacrylic acid C 1~8 Preferred examples of the monofunctional monomer other than alkyl esters include acrylic esters such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and propyl acrylate, and aromatic vinyl compounds such as styrene.

[0017] The outermost layer may be a single layer made of one type of thermoplastic polymer (P), or may be a multilayer made of two or more types of thermoplastic polymers (P).

[0018] In one preferred embodiment of the present invention, the inner layer has an intermediate layer made of a crosslinked rubber polymer (Q) and a core made of a crosslinked polymer (R) and covered in contact with the intermediate layer (inner layer = R + Q).

[0019] The crosslinked polymer (R) is composed of methyl methacrylate units, monofunctional monomer units other than methyl methacrylate, and polyfunctional monomer units.

[0020] The amount of methyl methacrylate units constituting the crosslinked polymer (R) is preferably 40 to 98.5% by mass, more preferably 80 to 95% by mass, based on the mass of the crosslinked polymer (R).

[0021] The amount of the monofunctional monomer units other than methyl methacrylate constituting the crosslinked polymer (R) is 1 to 59.5% by mass, preferably 5 to 20% by mass, based on the mass of the crosslinked polymer (R). Preferred examples of the monofunctional monomer other than methyl methacrylate include acrylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and propyl acrylate, and aromatic vinyl compounds such as styrene.

[0022] The amount of the polyfunctional monomer unit constituting the crosslinked polymer (R) is preferably 0.05 to 0.4 mass %, more preferably 0.1 to 0.3 mass %, based on the mass of the crosslinked polymer (R).

[0023] The amount of the crosslinked polymer (R) is preferably 5 to 40% by mass, more preferably 7 to 35% by mass, and further preferably 10 to 30% by mass, based on the amount of the multi-layered rubber particles.

[0024] The crosslinked rubber polymer (Q) comprises acrylate units having an alkyl group having 1 to 8 carbon atoms, monofunctional monomer units other than acrylate esters, and polyfunctional monomer units.

[0025] The amount of the acrylic ester unit having an alkyl group having 1 to 8 carbon atoms in the crosslinked rubber polymer (Q) is preferably 10 to 90 mass %, more preferably 20 to 85 mass %, based on the mass of the crosslinked rubber polymer (Q). The content of the monofunctional monomer units other than the acrylic acid ester in the crosslinked rubber polymer (Q) is preferably 10 to 90 mass %, more preferably 15 to 80 mass %, based on the mass of the crosslinked rubber polymer (Q).

[0026] The content of the polyfunctional monomer unit in the crosslinked rubber polymer (Q) is preferably from 0.01 to 3 mass %, more preferably from 0.1 to 2 mass %, based on the mass of the crosslinked rubber polymer (Q).

[0027] Examples of the acrylic acid esters used in the thermoplastic polymer (P), the crosslinked rubber polymer (Q), and the crosslinked polymer (R) include acrylic acid alkyl esters such as methyl acrylate (MA), ethyl acrylate, n-propyl acrylate, n-butyl acrylate (BA), s-butyl acrylate, t-butyl acrylate, n-butylmethyl acrylate, n-heptyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate. These acrylic acid esters can be used alone or in combination of two or more. Among these, methyl acrylate and / or n-butyl acrylate are preferred.

[0028] Examples of the polyfunctional monomer unit used in the crosslinked rubber polymer (Q) and the crosslinked polymer (R) include ethylene glycol dimethacrylate, propylene glycol dimethacrylate, triethylene glycol dimethacrylate, hexanediol dimethacrylate, ethylene glycol diacrylate, propylene glycol diacrylate, triethylene glycol diacrylate, allyl methacrylate (ALMA), and triallyl isocyanurate. The monofunctional monomer units other than methyl methacrylate in the crosslinked polymer (R) and the monofunctional monomer units other than acrylic acid esters in the crosslinked rubber polymer (Q) may be any vinyl monomer that can be copolymerized with a methacrylic acid ester or an acrylic acid ester, and examples thereof include aromatic vinyl monomers such as styrene, p-methylstyrene, o-methylstyrene, and vinylnaphthalene, unsaturated nitrile monomers such as acrylonitrile, olefin monomers such as ethylene and propylene, halogenated vinyl monomers such as vinyl chloride, vinylidene chloride, and vinylidene fluoride, unsaturated carboxylic acid monomers such as acrylic acid, methacrylic acid, and maleic anhydride, and maleimide monomers such as vinyl acetate, N-propylmaleimide, N-cyclohexylmaleimide, and No-chlorophenylmaleimide, and these compounds may be used alone or in combination of two or more.

[0029] <Polymerization process> The latex of the acrylic crosslinked rubber particles, which comprises an outermost layer composed of a thermoplastic polymer (P), an inner shell composed of a crosslinked rubber polymer (Q) in contact with and covering the outermost layer, and a core composed of a crosslinked polymer (R) as required, can be produced according to a conventional method by polymerizing each of them in multiple stages using a monomer mixture, a polymerization initiator, an emulsifier, etc. The polymerization initiator used in each polymerization is not particularly limited. Examples of the polymerization initiator include water-soluble inorganic initiators such as potassium persulfate and ammonium persulfate; redox initiators obtained by combining an inorganic initiator with a sulfite or thiosulfate; and redox initiators obtained by combining an organic peroxide with a ferrous salt or sodium sulfoxylate. The polymerization initiator may be added to the reaction system all at once at the start of polymerization, or may be added to the reaction system in portions at the start of polymerization and during polymerization, taking into account the reaction rate. The amount of the polymerization initiator used may be appropriately set so that the average particle size of the granular material contained in the acrylic crosslinked rubber particles falls within the above-mentioned range.

[0030] The emulsifier used in each polymerization is not particularly limited. Examples of the emulsifier include anionic emulsifiers such as long-chain alkyl sulfonates, sulfosuccinic acid alkyl ester salts, and alkylbenzene sulfonates; nonionic emulsifiers such as polyoxyethylene alkyl ethers and polyoxyethylene nonylphenyl ether; nonionic and anionic emulsifiers such as polyoxyethylene nonylphenyl ether sulfates such as sodium polyoxyethylene nonylphenyl ether sulfate, polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene alkyl ether sulfate, and alkyl ether carboxylates such as sodium polyoxyethylene tridecyl ether acetate. The amount of the emulsifier used can be appropriately set so that the average particle size of the granular material contained in the acrylic crosslinked rubber particles is within the above-mentioned range.

[0031] A preferred method for producing the coagulated powder of the present invention includes a polymerization step of producing a latex containing acrylic crosslinked rubber particles by an emulsion polymerization method, an aggregation step of aggregating the latex at 35 to 65°C to obtain a slurry, and a granulation step of granulating the slurry at 100 to 130°C.

[0032] The production of coagulated powder from the latex containing the acrylic crosslinked rubber particles of the present invention can be carried out by a freeze coagulation method, a salting-out coagulation method, an acid precipitation coagulation method, etc. Among these, the salting-out coagulation method is preferred because it is possible to adjust the coagulation force of the coagulated powder and to continuously produce a high-quality coagulated product.

[0033] <Agglomeration process> The aggregation process is a reaction that causes slow aggregation, in which the emulsified latex and the coagulant solution are mixed in a heated state, and the aggregation is allowed to proceed at a slow rate in order to improve the dispersibility of the acrylic crosslinked rubber particles during the subsequent melt-kneading.

[0034] The coagulant that can be used in the present invention may be an aqueous solution of an inorganic acid or a salt thereof, or an organic acid or a salt thereof, that has the property of being able to coagulate or solidify the emulsion polymerized latex.

[0035] Specific examples of the inorganic acid solution, inorganic acid salt solution, organic acid solution, or organic acid salt solution include alkali metal halides such as sodium chloride, potassium chloride, lithium chloride, sodium bromide, potassium bromide, lithium bromide, potassium iodide, and sodium iodide; alkali metal sulfates such as potassium sulfate and sodium sulfate; ammonium sulfate; ammonium chloride; alkali metal nitrates such as sodium nitrate and potassium nitrate; calcium chloride, ferrous sulfate, magnesium sulfate, calcium acetate, zinc sulfate, copper sulfate, barium chloride, ferrous chloride, ferric chloride, magnesium chloride, ferric sulfate, aluminum sulfate, potassium alum, and iron alum, and other inorganic salt solutions, either alone or in combination. Among these, aqueous solutions of monovalent or divalent inorganic acid salts such as sodium chloride, potassium chloride, sodium sulfate, ammonium chloride, calcium chloride, magnesium chloride, magnesium sulfate, barium chloride, and calcium acetate can be preferably used. There is no particular limitation on the method of adding the coagulant, and it can be added all at once, in portions, or continuously.

[0036] The polymer concentration of the emulsified latex in the aggregation step is preferably 5 to 25% by mass, more preferably 7.5 to 22.5% by mass, and further preferably 10 to 20% by mass. The lower the polymer concentration of the emulsified latex, the more difficult the aggregation will be, while the higher the polymer concentration, the more easily the aggregation will proceed, but the higher the viscosity will make it more difficult to control.

[0037] The concentration of the coagulant added in the aggregation step is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7.5 parts by mass, and even more preferably 1.0 to 7.0 parts by mass, based on 100 parts by mass of the polymer in the emulsified latex. If the concentration of the coagulant added is low, aggregation becomes difficult to proceed, and if the concentration is high, aggregation proceeds more easily, but the obtained coagulated product tends to have poor resistance to whitening in hot water or boiling water.

[0038] The residence time in the aggregation step is preferably 0.25 to 2.0 hours, more preferably 0.5 to 1.75 hours, and further preferably 0.75 to 1.6 hours. The shorter the residence time, the more insufficient the aggregation becomes and the smaller the particle size of the obtained coagulum becomes. The longer the residence time, the more likely the aggregation progresses, but the hot water or boiling water whitening resistance of the obtained coagulum tends to deteriorate.

[0039] <Granulation process> In the granulation step, the slurry obtained in the first solidification (aggregation step) is further heated to reduce the number of fine particles that do not completely aggregate and to increase the bulk density of the aggregate.

[0040] The residence time in the granulation step is preferably 0.5 to 3 hours, more preferably 0.75 to 2.75 hours, and further preferably 1.0 to 2.5 hours. The shorter the residence time, the more insufficient the granulation becomes and the smaller the particle size of the obtained coagulated product becomes. The longer the residence time, the easier the granulation proceeds, but the more likely the obtained coagulated product is to have poor resistance to whitening in hot water or boiling water.

[0041] The washing and dehydration of the slurry can be carried out, for example, by a filter press, a belt press, a Ginner centrifuge, a screw decanter centrifuge, etc. From the viewpoint of productivity and washing efficiency, it is preferable to use a screw decanter centrifuge. It is preferable to wash and dehydrate the slurry at least twice. The more times the washing and dehydration are carried out, the lower the remaining amount of water-soluble components. However, from the viewpoint of productivity, it is preferable to wash and dehydrate the slurry three times or less.

[0042] The moisture content of the coagulum after dehydration is preferably 5 to 50% by mass, more preferably 5 to 45% by mass, and even more preferably 5 to 40% by mass. The higher the moisture content, the less sufficient the drying can be, and the more difficult it becomes to obtain a coagulum with a suitable moisture content after drying. The turbidity of the wastewater discharged during dehydration is preferably not more than 1000, more preferably not more than 700, and even more preferably not more than 400. High turbidity of the wastewater indicates insufficient solid-liquid separation, which not only reduces the product yield but also causes problems such as clogging of the strainer of the discharge pump, making stable operation difficult.

[0043] The coagulum is dried so that the moisture content is preferably less than 0.2% by mass, more preferably less than 0.1% by mass. The higher the moisture content, the more likely it is that an ester hydrolysis reaction will occur in the acrylic crosslinked rubber particles during melt extrusion molding, resulting in the formation of carboxyl groups in the molecular chains.

[0044] The solidified powder of the present invention is defined by a series of melt-kneaded compositions obtained by melt-kneading 60 parts by mass of a methyl methacrylate resin having a melt flow rate of 8±1 g / 10 min according to JIS K7210 at 230°C and 37.3 N and 40 parts by mass of the solidified powder at a temperature of 230°C and 40 rpm using a kneading / extrusion molding evaluation tester equipped with a consumption shear energy measurement device, and sampling every minute. The methyl methacrylate resin has a weight average molecular weight in the range of 70,000 to 120,000, and a mass ratio of methyl methacrylate units:methyl acrylate units is 90:10 to 100:0. The series of melt-kneaded compositions are each stirred in acetone at a ratio of 0.1% by mass for 2 hours at room temperature, and the acetone dispersion in which the soluble components are dissolved and the insoluble components are dispersed is measured for particle size distribution using a laser diffraction / scattering particle size distribution measurement device. Samples with short melt-kneading times have multimodal or broad particle size distributions, whereas samples with advanced melt-kneading times have a unimodal distribution. In the solidified powder of the present invention, the consumed shear energy E required for the acrylic crosslinked rubber particles to initially form a monomodal distribution with a dispersed particle size of 1 μm or less in a series of melt-kneaded compositions sampled every minute was 180 MJ / m 3 Less than or equal to 150MJ / m 3 The following is the result. The solidified powder of the present invention, in which the consumed shear energy E is equal to or less than the upper limit, has excellent dispersibility of acrylic crosslinked rubber particles when melt-kneaded into a methacrylic resin, and the composition with the methacrylic resin has reduced agglomeration defects and is excellent in impact resistance.

[0045] <Resin composition> Examples of the matrix resin contained in the resin composition of the present invention include methacrylic resins which are homopolymers or copolymers mainly composed of methacrylic acid esters such as polymethyl methacrylate, olefin resins such as polyethylene, polypropylene, polybutene-1, poly-4-methylpentene-1, and polynorbornene, styrene resins such as ethylene ionomers, polystyrene, styrene-maleic anhydride copolymers, high impact polystyrene, AS resins, ABS resins, AES resins, AAS resins, ACS resins, and MBS resins, and methyl methacrylate-styrene resins such as styrene- ... Examples of the matrix resin include ethylene copolymers, ester resins such as polyethylene terephthalate and polybutylene terephthalate, amide resins such as nylon 6, nylon 66, and polyamide elastomers, polyphenylene sulfide, polyether ether ketone, polysulfone, polyphenylene oxide, polyimide, polyetherimide, polycarbonate, polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, polyvinyl alcohol, ethylene-vinyl alcohol copolymers, polyacetal, and phenoxy resins, with methacrylic resins being preferred. One or more types of matrix resins may be used.

[0046] The resin composition of the present invention may contain various additives as necessary. Examples of additives include antioxidants, heat deterioration inhibitors, ultraviolet absorbers, light stabilizers, lubricants, mold release agents, polymer processing aids, antistatic agents, flame retardants, dyes and pigments, light diffusing agents, matting agents, anti-sticking agents, impact resistance modifiers, and phosphors. The content of these additives can be appropriately set within a range that does not impair the effects of the present invention. For example, the content of the antioxidant is preferably 0.01 to 1 part by mass, the content of the ultraviolet absorber is preferably 0.01 to 3 parts by mass, the content of the light stabilizer is preferably 0.01 to 3 parts by mass, the content of the lubricant is preferably 0.01 to 3 parts by mass, the content of the dyes and pigments is preferably 0.01 to 3 parts by mass, and the anti-sticking agent is preferably 0.001 to 1 part by mass, relative to 100 parts by mass of the resin composition. Other additives can also be added in the range of 0.01 to 3 parts by mass.

[0047] The antioxidant is effective in preventing the oxidation degradation of the resin by itself in the presence of oxygen. Examples of the antioxidant include phosphorus-based antioxidants, phenol-based antioxidants, sulfur-based antioxidants, and amine-based antioxidants. Among them, from the viewpoint of the effect of preventing the degradation of optical properties due to coloring, phosphorus-based antioxidants and phenol-based antioxidants are preferred, and it is more preferred to use a phenol-based antioxidant alone or in combination with a phosphorus-based antioxidant and a phenol-based antioxidant. When a phosphorus-based antioxidant and a phenol-based antioxidant are used in combination, it is preferred to use the phosphorus-based antioxidant / phenol-based antioxidant in a mass ratio of 0.2 / 1 to 2 / 1, and more preferably 0.5 / 1 to 1 / 1.

[0048] Preferred examples of the phosphorus-based antioxidant include 2,2-methylenebis(4,6-di-t-butylphenyl)octylphosphite (ADEKA CORPORATION, "ADEKA STAB HP-10"), tris(2,4-di-t-butylphenyl)phosphite (BASF Japan Ltd., "IRGAFOS168"), and 3,9-bis(2,6-di-t-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (ADEKA CORPORATION, "ADEKA STAB PEP-36")).

[0049] Preferred phenol-based antioxidants include pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (BASF Japan Ltd., "IRGANOX1010") and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (BASF Japan Ltd., "IRGANOX1076"), etc. As the sulfur-based antioxidant, dilauryl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, pentaerythritol tetrakis(3-laurylthiopropionate), and the like are preferred. As the amine-based antioxidant, octylated diphenylamine and the like are preferred.

[0050] The heat deterioration inhibitor can prevent the heat deterioration of the resin by capturing the polymer radicals generated when exposed to high temperatures under substantially oxygen-free conditions. Preferred heat deterioration inhibitors include 2-t-butyl-6-(3'-t-butyl-5'-methyl-hydroxybenzyl)-4-methylphenyl acrylate (Sumitomo Chemical Co., Ltd.'s "Sumilizer GM") and 2,4-di-t-amyl-6-(3',5'-di-t-amyl-2'-hydroxy-α-methylbenzyl)phenyl acrylate (Sumitomo Chemical Co., Ltd.'s "Sumilizer GS"), etc.

[0051] The ultraviolet absorbent is a compound that has ultraviolet absorbing ability and is said to have the function of converting light energy into heat energy.The ultraviolet absorbent includes benzophenones, benzotriazoles, triazines, benzoates, salicylates, cyanoacrylates, oxalic acid anilides, malonic acid esters, and formamidines.Among them, benzotriazoles and triazines are preferred.The ultraviolet absorbent can be used alone or in combination of two or more kinds.

[0052] A light stabilizer is a compound that is said to have the function of capturing radicals generated mainly by oxidation due to light. Suitable light stabilizers include hindered amines such as compounds having a 2,2,6,6-tetraalkylpiperidine skeleton. For example, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate ("Adeka STAB LA-77Y" manufactured by ADEKA CORPORATION) can be mentioned.

[0053] A lubricant is a compound that is said to have the effect of improving releasability and processability by adjusting the slip between the resin and the metal surface and preventing adhesion or sticking. Examples of lubricants include higher alcohols, hydrocarbons, fatty acids, fatty acid metal salts, aliphatic amides, and fatty acid esters. Among them, from the viewpoint of compatibility with the resin composition of the present invention, aliphatic monohydric alcohols and aliphatic amides having 12 to 18 carbon atoms are preferred, and aliphatic amides are more preferred. Aliphatic amides are classified into saturated aliphatic amides and unsaturated aliphatic amides, and unsaturated aliphatic amides are more preferred because they are expected to have a slip effect due to anti-adhesion. Examples of unsaturated aliphatic amides include N,N'-ethylenebisoleic acid amide ("Slipax O" manufactured by Nippon Kasei Co., Ltd.) and N,N'-dioleyl adipamide ("Slipax ZOA" manufactured by Nippon Kasei Co., Ltd.).

[0054] Examples of the release agent include higher alcohols such as cetyl alcohol and stearyl alcohol; and higher fatty acid esters of glycerin such as monoglyceride stearate and diglyceride stearate. In the present invention, it is preferable to use higher alcohols and glycerin fatty acid monoesters in combination as the release agent. When higher alcohols and glycerin fatty acid monoesters are used in combination, the ratio is not particularly limited, but the amount of higher alcohols used: the amount of glycerin fatty acid monoester used is preferably 2.5:1 to 3.5:1, more preferably 2.8:1 to 3.2:1, by mass ratio. The polymer processing aid is a compound that is effective in achieving thickness accuracy and thinning when molding a resin composition. The polymer processing aid is usually a polymer particle having a particle size of 0.05 to 0.5 μm, which can be produced by emulsion polymerization.

[0055] Examples of the antistatic agent include alkylsulfonates such as sodium heptyl sulfonate, sodium octyl sulfonate, sodium nonyl sulfonate, sodium decyl sulfonate, sodium dodecyl sulfonate, sodium cetyl sulfonate, sodium octadecyl sulfonate, sodium diheptyl sulfonate, potassium heptyl sulfonate, potassium octyl sulfonate, potassium nonyl sulfonate, potassium decyl sulfonate, potassium dodecyl sulfonate, potassium cetyl sulfonate, potassium octadecyl sulfonate, potassium diheptyl sulfonate, lithium heptyl sulfonate, lithium octyl sulfonate, lithium nonyl sulfonate, lithium decyl sulfonate, lithium dodecyl sulfonate, lithium cetyl sulfonate, lithium octadecyl sulfonate, and lithium diheptyl sulfonate.

[0056] Examples of the flame retardant include metal hydrates having a hydroxyl group or crystal water, such as magnesium hydroxide, aluminum hydroxide, hydrated aluminum silicate, hydrated magnesium silicate, and hydrotalcite; phosphate compounds, such as polyamine phosphoric acid esters; and silicon compounds. Of these, preferred are phosphate ester-based flame retardants, such as trimethyl phosphate, triethyl phosphate, tripropyl phosphate, tributyl phosphate, tripentyl phosphate, trihexyl phosphate, tricyclohexyl phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, dimethylethyl phosphate, methyl dibutyl phosphate, ethyl dipropyl phosphate, and hydroxyphenyl diphenyl phosphate.

[0057] Examples of dyes and pigments include red organic pigments such as Para Red, Fire Red, Pyrazolone Red, Thioindigo Red, and Perylene Red; blue organic pigments such as Cyanine Blue and Indanthrene Blue; and green organic pigments such as Cyanine Green and Naphthol Green. One or more of these can be used. Examples of the light diffusing agent and the matting agent include glass particles, polysiloxane-based crosslinked particles, crosslinked polymer particles, talc, calcium carbonate, barium sulfate, etc. The copolymer of the present invention preferably does not contain an acid generator.

[0058] Examples of the anti-sticking agent include fatty acids such as stearic acid and palmitic acid; fatty acid metal salts such as calcium stearate, zinc stearate, magnesium stearate, potassium palmitate, and sodium palmitate; waxes such as polyethylene wax, polypropylene wax, and montanic acid wax; low molecular weight polyolefins such as low molecular weight polyethylene and low molecular weight polypropylene; acrylic resin powder; polyorganosiloxane such as dimethylpolysiloxane; amide resin powders such as octadecylamine, alkyl phosphate, fatty acid ester, and ethylene bisstearylamide, fluororesin powders such as tetrafluoroethylene resin, molybdenum disulfide powder, silicone resin powder, silicone rubber powder, and silica. Examples of impact resistance modifiers include core-shell type modifiers that contain a diene rubber as a core layer component; modifiers that encapsulate a plurality of rubber particles; and the like. Examples of fluorescent substances include fluorescent pigments, fluorescent dyes, fluorescent white dyes, fluorescent brighteners, and fluorescent bleaches.

[0059] When a matrix resin and / or additives are contained in the resin composition of the present invention, they may be added during polymerization of the matrix resin and / or the acrylic crosslinked rubber particles, or they may be added when mixing with the matrix resin and / or the acrylic crosslinked rubber particles, or they may be added after mixing with the matrix resin and / or the acrylic crosslinked rubber particles.

[0060] The resin composition of the present invention can be molded using a molding method and molding apparatus generally used for matrix resins. For example, molded products can be produced by molding methods involving heating and melting, such as injection molding, extrusion molding, compression molding, blow molding, calendar molding, and vacuum molding, and solution casting methods.

[0061] The resin composition of the present invention is also useful as a film, and can be well processed by, for example, the inflation method, T-die extrusion method, which are common melt extrusion methods, or the calendar method, or further the solution casting method. If necessary, it is also possible to obtain a film with better surface properties by simultaneously contacting both sides of the film with a roll or a metal belt, particularly by simultaneously contacting the roll or metal belt heated to a temperature equal to or higher than the glass transition temperature. In addition, it is also possible to modify the film by lamination molding or biaxial stretching depending on the purpose.

[0062] The film obtained from the resin composition of the present invention can be used by laminating it to metal, plastic, etc. Examples of lamination methods include wet lamination, in which an adhesive is applied to a metal plate such as a steel plate, and then a film is placed on the metal plate and dried to adhere to the metal plate, dry lamination, extrusion lamination, hot melt lamination, etc.

[0063] Methods for laminating a film onto a plastic part include film insert molding, in which the film is placed in a mold and then filled with resin by injection molding, and laminate injection press molding, as well as film in-mold molding, in which the film is preformed, then placed in a mold and then filled with resin by injection molding.

[0064] The resin composition of the present invention and the molded product containing the same can be used as a member for various applications.Specific applications include, for example, signboard parts and marking films; display parts; lighting parts; interior parts; building parts; automobile side visors, rear visors, head wings, headlight covers, sunroofs, glazing, automobile interior parts, automobile exterior parts such as bumpers, and other transport-related parts; electronic equipment parts; medical equipment parts; machine-related parts; liquid crystal protection plates, light guide plates, light guide films, Fresnel lenses, lenticular lenses, front panels of various displays, diffusion plates, and other optical parts; transportation-related parts; and other various surface materials. On the other hand, laminated products of films obtained from the resin composition of the present invention can be used for automobile interior and exterior materials, daily necessities, wallpaper, paint replacement applications, housings for furniture and electrical equipment, housings for office automation equipment such as facsimiles, flooring materials, parts for electrical or electronic devices, bathroom equipment, etc. EXAMPLES

[0065] Production examples and examples according to the present invention, as well as comparative examples, will be described below.

[0066] [Evaluation items and evaluation methods] The evaluation items and evaluation methods in the Production Examples, Examples, and Comparative Examples are as follows. (Weight average molecular weight (Mw)) The weight average molecular weight (Mw) of the resin was determined by the GPC method. Tetrahydrofuran was used as the eluent. Two TSKgel SuperMultipore HZM-M columns manufactured by Tosoh Corporation and a SuperHZ4000 were connected in series as the column. The GPC device used was an HLC-8320 (product number) manufactured by Tosoh Corporation equipped with a differential refractive index detector (RI detector). A sample solution was prepared by dissolving 4 mg of the resin to be measured in 5 mL of tetrahydrofuran. The temperature of the column oven was set to 40°C, and 20 μL of the sample solution was injected into the device at an eluent flow rate of 0.35 mL / min to measure the chromatogram. Ten standard polystyrene points with molecular weights in the range of 400 to 5,000,000 were measured by GPC, and a calibration curve showing the relationship between retention time and molecular weight was created. The Mw of the resin to be measured was determined based on this calibration curve.

[0067] (Volume average particle size) For the latex containing acrylic crosslinked rubber particles, the volume average particle size was determined by a light scattering method using a laser diffraction / scattering type particle size distribution measuring device LA-950V2 manufactured by Horiba, Ltd.

[0068] (shear energy consumed) 60 parts by mass of methyl methacrylate resin (Parapet G manufactured by Kuraray Co., Ltd.) with a melt flow rate of 8 g / 10 min at 230 ° C and 37.3 N was kneaded for 3 minutes at 230 ° C, 80 rpm using a Sigma Mixer in a kneading and extrusion molding evaluation tester equipped with a consumption shear energy measuring device (Labo Plastomill 4C150 manufactured by Toyo Seiki Co., Ltd.), and then 40 parts by mass of the solidified powder was added and further kneaded at 40 rpm. During kneading, samples were taken every minute to obtain melt-kneaded compositions with different consumption shear energy. 0.10 parts by mass of each of the obtained melt-kneaded compositions was dissolved in 100 parts by mass of acetone for 2 hours, and the volume average dispersed particle size of the acrylic crosslinked rubber particles dispersed in the methacrylic resin was measured by a light scattering method using a laser diffraction / scattering type particle size distribution measuring device LA-950V2 manufactured by Horiba, Ltd. When the particle size was within 1 μm and a single distribution peak (unimodal) appeared, it was considered to be dispersed into primary particles, and the shear energy consumed by the resin composition was adopted as the shear energy consumed by the solidified powder.

[0069] (Charpy impact value) The impact value (with notch) of the press-molded sample was measured at a temperature of 23°C and a relative humidity of 50% according to a method in accordance with JIS-K7111. Five measurements were performed, and the average value was used as the Charpy impact value.

[0070] (Number of defects) The pellets of the acrylic resin composition obtained in the Examples or Comparative Examples were extruded at a cylinder temperature of 240-250°C and a 150 mm wide T-die temperature of 260°C using an extruder ME-20 / 26V2 and a winder CR-8 attached to a polymer quality inspection device manufactured by OCS, and the film was wound on a cooling roll at a speed of 4.2 m / min to obtain a film having a thickness of 30-70 mm. The obtained film was measured for defects of 40 μm or more using the polymer quality inspection device FSA-100, and the number of defects was measured for defects of 1 m. 2 The number of hits was used as the number of different defects (number of defects).

[0071] (Production Example 1) In a reactor equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, a monomer inlet tube and a reflux condenser, 750 parts by mass of ion-exchanged water, 0.14 parts by mass of sodium polyoxyethylene tridecyl ether acetate and 0.1 parts by mass of sodium carbonate were charged, and the inside of the reactor was fully replaced with nitrogen gas. The inside temperature was then set to 80°C. 0.10 parts by mass of potassium persulfate was added thereto and stirred for 5 minutes. 262.5 parts by mass of a monomer mixture consisting of 93.8% by mass of methyl methacrylate (MMA), 6.0% by mass of methyl acrylate (MA) and 0.2% by mass of allyl methacrylate (ALMA) were continuously dripped into the mixture over a period of 45 minutes. After the dripping was completed, the polymerization reaction was continued for another 60 minutes so that the polymerization conversion rate was 98% or more (first layer (R)). Next, 0.10 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. After that, 337.5 parts by mass of a monomer mixture consisting of 80.6% by mass of butyl acrylate (BA), 17.4% by mass of styrene (St) and 2% by mass of allyl methacrylate (ALMA) were continuously dripped over 60 minutes. After the dripping was completed, the polymerization reaction was carried out for another 80 minutes so that the polymerization conversion rate was 98% or more (first layer (R) + second layer (Q)). Next, 0.10 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. After that, 150 parts by mass of a monomer mixture consisting of 80.0% by mass of methyl methacrylate (MMA) and 20.0% by mass of methyl acrylate (MA) and 0.3 parts by mass of n-octyl mercaptan were continuously dripped over 25 minutes. After the dripping was completed, the polymerization reaction was carried out for another 60 minutes so that the polymerization conversion rate was 98% or more. By the above operations, a latex containing acrylic crosslinked rubber particles was obtained (first layer (R) + second layer (Q) + third layer (P)). The volume average particle diameter of the acrylic crosslinked rubber particles in the latex was 0.26 μm.

[0072] (Production Example 2) For the first and second layers, a latex containing a crosslinked rubber polymer was obtained in the same manner as in Production Example 1. Next, 0.10 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. Then, 150 parts by mass of a monomer mixture consisting of 94.0% by mass of methyl methacrylate and 6.0% by mass of methyl acrylate and 0.3 parts by mass of n-octyl mercaptan were continuously added dropwise over 25 minutes. After the dropwise addition was completed, the polymerization reaction was continued for another 60 minutes so that the polymerization conversion rate was 98% or more. Through the above operations, a latex containing acrylic crosslinked rubber particles (three-layer structure: RQP) was obtained. The volume average particle diameter of the acrylic crosslinked rubber particles in the latex was 0.23 μm.

[0073] (Production Example 3) For the first and second layers, a latex containing a crosslinked rubber polymer was obtained in the same manner as in Production Example 1. Next, 0.10 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. Then, 150 parts by mass of a monomer mixture consisting of 94.0% by mass of methyl methacrylate and 6.0% by mass of methyl acrylate and 1.125 parts by mass of n-octyl mercaptan were continuously dropped over 25 minutes. After the dropwise addition was completed, the polymerization reaction was continued for another 60 minutes so that the polymerization conversion rate was 98% or more. By the above operations, a latex containing acrylic crosslinked rubber particles (three-layer structure: RQP) was obtained. The volume average particle diameter of the acrylic crosslinked rubber particles in the latex was 0.29 μm.

[0074] (Production Example 4) For the first and second layers, a latex containing a crosslinked rubber polymer was obtained in the same manner as in Production Example 1. Next, 0.10 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. After that, 150 parts by mass of a monomer mixture consisting of 86.0% by mass of methyl methacrylate and 14.0% by mass of butyl acrylate and 0.3% by mass of n-octyl mercaptan were continuously dropped over 25 minutes. After the dropwise addition was completed, the polymerization reaction was continued for another 60 minutes so that the polymerization conversion rate was 98% or more. By the above operations, a latex containing acrylic crosslinked rubber particles (three-layer structure: RQP) was obtained. The volume average particle diameter of the acrylic crosslinked rubber particles in the latex was 0.29 μm.

[0075] (Production Example 5) For the first and second layers, a latex containing a crosslinked rubber polymer was obtained in the same manner as in Production Example 1. Next, 0.10 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. Then, 150 parts by mass of a monomer mixture consisting of 86.0% by mass of methyl methacrylate and 14.0% by mass of butyl acrylate and 1.125 parts by mass of n-octyl mercaptan were continuously dropped over 25 minutes. After the dropwise addition was completed, the polymerization reaction was continued for another 60 minutes so that the polymerization conversion rate was 98% or more. By the above operations, a latex containing acrylic crosslinked rubber particles (three-layer structure: RQP) was obtained. The volume average particle diameter of the acrylic crosslinked rubber particles in the latex was 0.29 μm.

[0076] [Example 1] The latex obtained in Production Example 1 was coagulated under the following conditions. 484.8 parts of ion-exchanged water and 5.25 parts of magnesium sulfate were added to 210 parts of latex, and the liquid temperature was raised to 40°C while stirring. Stirring was continued for 1.1 hours while maintaining the liquid temperature at 40°C to obtain an aggregated slurry. The slurry was further heated to 115°C and stirred for 1.6 hours while maintaining the temperature to obtain a granulated slurry. The obtained granulated slurry was washed and dehydrated using a screw decanter centrifuge, and dried to obtain a coagulated powder. The volume average particle size of the coagulated powder was 239 μm. 40 parts by mass of the obtained solidified powder and 60 parts by mass of a methacrylic resin were melt-kneaded in a Φ40 mm single screw extruder at a cylinder temperature of 170 to 235° C. Thereafter, the molten resin composition was extruded to obtain a pellet-shaped acrylic resin composition, and the number of defects was measured by the above-mentioned method. In addition, 40 parts by mass of the obtained solidified powder and 60 parts by mass of methacrylic resin were kneaded in a Labo Plastomill (4C150 manufactured by Toyo Seiki) at 230°C for 3 minutes to obtain an acrylic resin composition, and the dispersed particle size distribution in acetone shown in Figure 1 was measured. Furthermore, a molded product having a thickness of 3 mm was obtained by hot press molding at 230°C for 4 minutes and 30 seconds, and the Charpy impact value was measured. The physical property evaluation results are shown in Table 2.

[0077] [Examples 2 to 4] A coagulated powder was obtained in the same manner as in Example 1, except that the temperature and acrylic crosslinked rubber particles were changed as shown in Table 2. In each Example, a molded product was obtained using the obtained coagulated powder in the same manner as in Example 1. The physical property evaluation results in each Example are shown in Table 2.

[0078] [Comparative Examples 1 to 6] A coagulated powder was obtained in the same manner as in Example 1, except that the temperature, acrylic crosslinked rubber particles, and dispersion particles were changed as shown in Table 3. In each comparative example, a molded product was obtained using the obtained coagulated powder in the same manner as in Example 1. The physical property evaluation results in each comparative example are shown in Table 3. In addition, 40 parts by mass of the coagulated powder obtained in Comparative Example 1 and 60 parts by mass of a methacrylic resin were kneaded in a Labo Plastomill at 230°C for 3 minutes to obtain an acrylic resin composition, and the dispersed particle size distribution in acetone shown in Figure 1 was measured.

[0079] [Table 1]

[0080] [Table 2]

[0081] [Table 3]

[0082] The molded articles obtained in Examples 1 to 4, which were made of the coagulated powder containing the acrylic crosslinked rubber particles of the present invention, had good dispersibility and impact resistance.

[0083] In contrast, the molded products obtained in Comparative Examples 1 and 2, which were made of coagulated powder containing acrylic crosslinked rubber particles having a high third layer glass transition temperature, had a large number of defects and poor impact strength compared to the Examples.

[0084] The molded product obtained in Comparative Example 3, which was made of coagulated powder containing acrylic crosslinked rubber particles produced by increasing the agglomeration temperature in the process of obtaining the coagulated powder, had a larger number of defects and poor impact strength compared to the Examples.

[0085] The molded article obtained in Comparative Example 4, in which the outermost layer was made of coagulated powder containing low molecular weight acrylic crosslinked rubber particles, had poor impact strength compared to the Examples.

[0086] The molded product obtained in Comparative Example 5, which was made of a coagulated powder containing acrylic crosslinked rubber particles produced by lowering the molecular weight of the outermost layer and increasing the granulation temperature in the process of obtaining the coagulated powder, had a larger number of bumps and poorer impact strength than the Examples.

[0087] The molded product obtained in Comparative Example 6, which was made of a coagulated powder containing acrylic crosslinked rubber particles obtained by adding dispersing particles, had poor impact strength compared to the Examples due to a decrease in the overall rubber content.

Claims

1. A coagulated powder comprising an inner layer containing a crosslinked rubber containing acrylic acid alkyl ester units, and an outermost layer made of a thermoplastic resin containing methyl methacrylate units and graft-bonded to the inner layer, the thermoplastic resin of the outermost layer having a glass transition temperature of 60 to 85°C, a weight average molecular weight of 40,000 to 80,000, and an average particle size of 0.08 to 0.3 μm, the coagulated powder comprising acrylic crosslinked rubber particles, When 60 parts by mass of a methyl methacrylate resin having a melt flow rate of 8±1 g / 10 min at 230 ° C. and 37.3 N and 40 parts by mass of the coagulated powder are melt-kneaded at a temperature of 230 ° C. using a kneading / extrusion molding evaluation test device equipped with a consumption shear energy measuring device, The consumed shear energy E required for the acrylic crosslinked rubber particles to be dispersed unimodally to a dispersed particle diameter of 1 μm or less in a 0.1 mass % acetone dispersion of the melt-kneaded composition of the coagulated powder and the methyl methacrylate resin is 180 MJ / m 3 The coagulated powder is:

2. 2. The coagulated powder according to claim 1, wherein the average particle size of the acrylic crosslinked rubber particles is 0.2 to 0.3 μm.

3. A polymerization step of producing a latex containing acrylic crosslinked rubber particles by an emulsion polymerization method; aggregating the latex at 35 to 65° C.; The method for producing a solidified powder according to claim 1 or 2, further comprising a granulation step of granulating at 100 to 130°C.

4. A resin composition comprising the coagulated powder according to claim 1 or 2 and a matrix resin.

5. 5. The resin composition according to claim 4, wherein the matrix resin is a methacrylic resin.

6. A molded article comprising the resin composition according to claim 4 or 5.

Citation Information

Patent Citations

  • Production of polymer flocculate

    JP1995157513A

  • METHOD FOR MANUFACTURING METHACRYLIC IMPACT RESISTANT RESIN COMPOSITION

    JP3145864B2

  • Process for producing rubbery polymer particle and process for producing resin composition containing the same

    WO2005028546A1

  • Acrylic polymer coagulates

    WO2019146782A1

  • Multilayer-structured polymer particle, and thermoplastic resin composition, molded body, and film including same

    WO2020138501A1