Polyurethane foams having improved combustion behavior

By integrating halogen-free flame retardants and transition metals into the isocyanate-reactive composition of polyurethane foams, the emissions of HCN and CO are substantially reduced, enhancing combustion behavior and maintaining thermal stability.

JP7586887B2Active Publication Date: 2024-11-19DOW GLOBAL TECHNOLOGIES LLC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022501241
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2020-07-09
Publication Date
2024-11-19
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Existing polyurethane-based foams do not adequately address smoke opacity and toxin emissions during combustion, particularly hydrogen cyanide (HCN) and carbon monoxide (CO), despite their inherent char formation and thermal stability.

Method used

Incorporating a halogen-free flame retardant compound and transition metal compounds into the isocyanate-reactive composition of polyurethane-based foams, with specific weight percentages and molar ratios, to form a combustion modifier composition that reduces HCN and CO emissions.

Benefits of technology

The modified foams exhibit significant reductions in HCN and CO emissions during pyrolysis events, maintaining low smoke production and high thermal stability, as demonstrated by ASTM E662 and NBS/FTIR tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586887000001
    Figure 0007586887000001
  • Figure 0007586887000002
    Figure 0007586887000002
  • Figure 0007586887000003
    Figure 0007586887000003
Patent Text Reader

Abstract

The present disclosure provides an isocyanate-reactive composition capable of reacting with an isocyanate compound in a reaction mixture to form a polyurethane-based foam. The isocyanate-reactive composition includes an isocyanate-reactive compound and a flame modifier composition. The isocyanate-reactive compound has an isocyanate-reactive moiety and an aromatic moiety. The flame modifier composition includes both phosphorus from the halogen-free flame retardant compound and a transition metal from the transition metal compound. The flame modifier composition can have a molar ratio of transition metal to phosphorus (molar transition metal:molar phosphorus) of 0.05:1 to 5:1.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates generally to polyurethane-based foams, and more specifically to polyurethane-based foams having improved burn behavior. [Background technology]

[0002] Polyurethane rigid (PUR) foams have been used in construction since the 1960s as high-performance insulation materials. Continuing technological developments in Europe and the United States have resulted in the next product generation, called polyisocyanurate rigid (PIR) foams. Both PUR and PIR are polyurethane-based foams made from two reactants, isocyanates (e.g., methyldiphenyl diisocyanate, MDI) and polyols. For PUR, the isocyanates and polyols are implemented in a nearly balanced ratio compared to the equivalent weight, while the isocyanates are used in excess during the production of PIR. The isocyanates partially react with themselves, and the resulting PIR is a highly cross-linked synthetic material with ring-like isocyanurate structures. The advanced bonds and ring structure ensure the high thermal stability of rigid PIR foams. PIR also has excellent dimensional stability.

[0003] PIR foams also feature a very good response to fire behavior due to their inherent charring behavior, which is also related to the outstanding thermal stability of the isocyanurate chemical structure. It is common to add phosphorus-based flame retardants to further promote char formation. When a building product such as an insulated metal panel or insulation board is exposed to fire, the insulating PIR core rapidly forms a coherent char that helps protect the underlying material. It follows that only a limited portion of the available combustible insulation material exposed to the fire actually contributes in terms of heat release and smoke. Summary of the Invention [Problem to be solved by the invention]

[0004] The fire behavior of combustible thermosetting materials is a complex issue. As an example, halogenated flame retardants are very effective in reducing heat release, but can worsen smoke opacity. Dow Patent Publication US2014 / 0206786A1 describes the use of triethyl phosphate (TEP) as a smoke suppression additive when compared to traditional halogenated flame retardants such as tris(2-chloroisopropyl)phosphate (TCPP). Furthermore, as is well known, the composition of the combustion effluent (even more than the material itself) is highly dependent on the fire conditions, especially temperature, geometry, and ventilation, including oxygen availability. As mentioned above, even if the inherent charring behavior of polyisocyanurates limits and / or delays the amount of polymer that burns (and thus limits and / or delays the release of heat and smoke), it is still desirable to further modify the combustion / burning behavior, thus reducing smoke opacity and smoke toxics as much as possible.

[0005] The present disclosure provides polyurethane-based foams having improved combustion behavior with respect to hydrogen cyanide (HCN) and carbon monoxide (CO) emissions during a pyrolysis event (e.g., fire). The polyurethane-based foams are formed with a reaction mixture that includes both an isocyanate compound and an isocyanate-reactive composition. The isocyanate-reactive composition of the polyurethane-based foam includes, among other things, phosphorus from the halogen-free flame retardant compound and a transition metal from the transition metal compound that together help to provide a significant reduction in both HCN and CO during pyrolysis of the polyurethane-based foam.

[0006] For an embodiment of the present disclosure, an isocyanate-reactive composition for forming a polyurethane-based foam includes an isocyanate-reactive compound and a flame modifier composition. The isocyanate-reactive compound has an isocyanate-reactive moiety and an aromatic moiety, the aromatic moiety being 5 weight percent (wt%) to 80 wt% of the isocyanate-reactive compound based on the total weight of the isocyanate-reactive compound. The flame modifier composition includes both 0.1 wt% to 7.0 wt% phosphorus from the halogen-free flame retardant compound and 0.05 wt% to 14.0 wt% transition metal from the transition metal compound, the wt% transition metal and the wt% phosphorus are each based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound). For these given wt% values, the flame modifier composition may have a molar ratio of transition metal to phosphorus (mol transition metal:mol phosphorus) of 0.05:1 to 5:1.

[0007] For embodiments provided herein, the halogen-free flame retardant compound may be selected from the group consisting of phosphates, phosphonates, phosphinates, and combinations thereof. For embodiments provided herein, the transition metal compound may be selected from the group consisting of oxides, carboxylates, salts, coordination compounds, and combinations thereof, and the transition metal may be selected from the group consisting of copper, iron, manganese, cobalt, nickel, zinc, and combinations thereof. Preferably, the transition metal compound is selected from the group consisting of copper(I) oxide, copper(II) oxide, ethylenediaminetetraacetic acid (EDTA) copper disodium salt, and combinations thereof. For various embodiments, the transition metal compound preferably has a median particle diameter (D50) of 10 nm to 10 μm. For embodiments provided herein, the isocyanate-reactive moiety of the isocyanate-reactive compound may be a hydroxyl moiety, and the isocyanate-reactive compound is selected from the group consisting of polyether polyols, polyester polyols, polycarbonate polyols, polyester carbonate polyols, polyether carbonate polyols, and combinations thereof. For the various embodiments, the isocyanate-reactive compositions provided herein may also include a catalyst, a surfactant, a blowing agent, or a combination thereof.

[0008] The reaction mixture for forming the polyurethane-based foam, as provided herein, includes both an isocyanate compound having an isocyanate moiety and an isocyanate-reactive compound having an isocyanate moiety and an aromatic moiety that constitutes 5% to 80% by weight of the isocyanate-reactive compounds, based on the total weight of the isocyanate-reactive compounds. For embodiments herein, the reaction mixture may have a molar ratio of isocyanate moieties to isocyanate-reactive moieties of 1.2:1 to 7:1. For example, the isocyanate-reactive moieties of the isocyanate-reactive composition are hydroxyl moieties, and the reaction mixture has a molar ratio of isocyanate moieties to hydroxyl moieties of 1.2:1 to 7:1. The reaction mixture also includes 0.1% to 7.0% by weight phosphorus from the halogen-free flame retardant compound and 0.05% to 14.0% by weight transition metal from the transition metal compound, the weight percent values ​​of phosphorus and transition metal being based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound. The reaction mixture may further optionally include a catalyst, a surfactant, and a blowing agent for forming a polyurethane-based foam. As discussed herein, a polyurethane-based foam is formed using the reaction mixture.

[0009] The present disclosure also provides a process for preparing a reaction mixture for producing a polyurethane-based foam. The process may include providing an isocyanate compound having an isocyanate moiety, providing an isocyanate-reactive compound having an isocyanate-reactive moiety and an aromatic moiety constituting 5% to 80% by weight of the isocyanate-reactive compound based on the total weight of the isocyanate-reactive compound, providing 0.1% to 7.0% by weight of phosphorus from a halogen-free flame retardant compound and 0.05% to 14.0% by weight of a transition metal from a transition metal compound, the phosphorus and transition metal weight percentage values ​​being based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound and the transition metal compound, providing a catalyst, a surfactant and a blowing agent, if necessary, and mixing the isocyanate compound, the isocyanate-reactive compound, the halogen-free flame retardant compound, the transition metal compound, the optional catalyst, the surfactant and the blowing agent to form a reaction mixture. For various embodiments, the reaction mixture may have a molar ratio of isocyanate moieties to isocyanate-reactive moieties of from 1.2:1 to 7:1. The mixing to form the reaction mixture may also include providing a molar ratio of transition metal to phosphorus (molar transition metal:mol phosphorus) in the reaction mixture of from 0.05:1 to 5:1. Additional embodiments of the process further include mixing the transition metal compound with a liquid carrier in providing the transition metal from the transition metal compound. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present disclosure provides polyurethane-based foams with improved combustion behavior with respect to hydrogen cyanide (HCN) and carbon monoxide (CO) emissions during a pyrolysis event (e.g., fire). The polyurethane-based foams are formed with a reaction mixture that includes both an isocyanate compound and an isocyanate-reactive composition. For embodiments of the present disclosure, the isocyanate-reactive composition for forming the polyurethane-based foam includes an isocyanate-reactive compound having an isocyanate-reactive moiety and an aromatic moiety as provided herein. The isocyanate-reactive composition also includes, among other things, phosphorus from the halogen-free flame retardant compound and a transition metal from the transition metal compound, which together help to provide a significant reduction in both HCN and CO during pyrolysis of the polyurethane-based foam.

[0011] For various embodiments, the isocyanate-reactive moieties of the isocyanate-reactive compound are hydroxyl moieties, and the isocyanate-reactive compound may be selected from the group consisting of polyether polyols, polyester polyols, polycarbonate polyols, polyester carbonates, polyether carbonate polyols, and combinations thereof. For various embodiments, the isocyanate-reactive compound may contain two or more hydroxyl moieties, and the active hydrogen atoms are reactive with the carbon atoms of the isocyanate groups (-N=C=O) of the isocyanate compound. The isocyanate-reactive compound may have a number average molecular weight of 100 g / mol to 2,000 g / mol. Other number average molecular weight values ​​may also be possible. For example, the isocyanate-reactive compound may have a number average molecular weight of a low value of 100, 200, 300, 350, or 400 g / mol to an upper value of 500, 750, 1,000, 1,500, or 2,000 g / mol. Number average molecular weight values ​​reported herein are determined by end group analysis, gel permeation chromatography, and other methods known in the art.

[0012] The isocyanate-reactive compound also includes an aromatic moiety. For various embodiments, the aromatic moiety is between 5 weight percent (wt%) and 80 wt% of the isocyanate-reactive compound, based on the total weight of the isocyanate-reactive compound. Preferably, the aromatic moiety comprises between 8 wt% and 50 wt% of the isocyanate-reactive compound, based on the total weight of the isocyanate-reactive compound. More preferably, the aromatic moiety comprises between 10 wt% and 40 wt% of the isocyanate-reactive compound, based on the total weight of the isocyanate-reactive compound. As used herein, an "aromatic moiety" is at least one cyclically conjugated molecular moiety in the form of a planar unsaturated ring of carbon atoms that is covalently bonded to the isocyanate-reactive compound. The planar unsaturated ring of carbon atoms may have at least six carbon atoms. To illustrate, C 12 H 14 The isocyanate-reactive compound bis(2-hydroxyethyl) terephthalate has a molecular formula of O6 and a formula weight of 254.2 grams / mole, and an aromatic content corresponding to a molecular formula of CH4 with a corresponding formula weight of 76.1 grams / mole, resulting in an aromatic portion of 29.9 weight percent (wt %) of bis(2-hydroxyethyl) terephthalate.

[0013] In some embodiments, polyether polyols may include those with at least two hydroxyl groups per molecule, such as two or three, and may be prepared, for example, by polymerization of oxiranes / cyclic ethers, such as ethylene oxide, propylene oxide, butylene oxide, styrene oxide, or epichlorohydrin, either by themselves, in the presence of BF3, or by the process of chemical addition of these oxiranes to starting components with reactive hydrogen atoms, such as water, ammonia, alcohols, or amines, optionally as mixtures (such as mixtures of ethylene oxide and propylene oxide) or in succession. Examples of suitable starting components include ethylene glycol, propylene glycol-(1,3) or -(1,2), glycerol, trimethylolpropane, 4,4'-dihydroxy-diphenylpropane, novolac, aniline, ethanolamine, o-tolueneamine, or ethylenediamine. Sucrose-based polyether polyols may also be used. In many cases it will be preferred to use polyethers which contain a predominant amount of primary OH groups (up to 100% by weight of the OH groups present in the polyether).

[0014] For some embodiments, polyester polyols may include those having at least 1.8 to 3 hydroxyl groups (average number) per molecule. Examples of such polyester polyols may include those formed as reaction products of polyhydric, such as dihydric and / or trihydric alcohols, with polybasic, such as dibasic and / or tribasic, carboxylic acids. Instead of free polycarboxylic acids, the corresponding polycarboxylic acid anhydrides or corresponding polycarboxylic acid esters of lower alcohols or mixtures thereof may be used, as well as mixtures thereof with free polycarboxylic acids. The polycarboxylic acids may be aliphatic, cycloaliphatic, aromatic and / or heterocyclic, and they may be substituted, for example, by halogen atoms and / or unsaturated. Suitable exemplary polycarboxylic acids, anhydrides, and polycarboxylic acid esters of lower alcohols include, but are not limited to, succinic acid, adipic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, terephthalic acid, isophthalic acid, trimellitic acid, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, tetrachlorophthalic anhydride, endomethylenetetrahydrophthalic anhydride, glutaric anhydride, maleic acid, maleic anhydride, fumaric acid, dimeric and trimeric fatty acids, optionally mixed with monomeric fatty acids, dimethyl terephthalate, and terephthalic acid-bis-glycol esters. Other suitable examples of polyester polyols include modified aromatic polyester polyols, such as those offered under the trade designation STEPANPOL PS-2352 (acid number, max. 0.6-1.0 mg KOH / g, hydroxyl number 230-250 mg KOH / g, functionality 2.0, Stepan Company).

[0015] Exemplary suitable polyhydric alcohols include, but are not limited to, ethylene glycol, propylene glycol-(1,2) and-(1,3), butylene glycol-(1,4) and-(2,3), hexanediol-(1,6), octanediol-(1,8), neopentyl glycol, cyclohexanedimethanol (1,4-bis-hydroxy-methylcyclohexane and other isomers), 2-methyl-1,3-propane-diol, glycerol, trimethylolpropane, hexanetriol-(1,2,6), butanetriol-(1,2,4), trimethylolethane, pentaerythritol, quinitol, mannitol and sorbitol, methylglycosides, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, dibutylene glycol and polybutylene glycol. The polyesters may also contain a percentage of carboxyl end groups. Polyesters of lactones, such as ε-caprolactone, or hydroxycarboxylic acids, such as co-hydroxycaproic acid, may also be used.

[0016] In some embodiments, the polyester polyol is an aromatic polyester polyol. Examples of aromatic polyester polyols include those formed from the reaction product of an aromatic polybasic acid and an aliphatic polyhydric alcohol. Other examples include reaction products formed from the reaction of a polybasic acid comprising at least one of terephthalic acid, isophthalic acid, phthalic acid, phthalic anhydride, trimellitic acid, or trimellitic anhydride with an aliphatic polyhydric alcohol comprising at least one of ethylene glycol, propylene glycol, diethylene glycol, polyethylene glycol, polypropylene glycol, or glycerol. In an additional example, the aromatic polyester polyol is a reaction product formed from a polybasic acid of terephthalic acid and an aliphatic polyhydric alcohol comprising diethylene glycol, polyethylene glycol, and / or glycerol. For various embodiments, the aromatic polyester polyol has an aromatic content from a low of 8, 10, 12, or 14 weight percent (wt%) and a high of 18, 20, 30, or 40 wt%, based on the total weight of the polyester polyol, with any combination of the low and high values ​​provided being possible (e.g., the aromatic content of the aromatic polyester polyol is 8 wt% to 40 wt%). In some embodiments, the aromatic polyester polyol has an average hydroxyl functionality of at least 1.8, 1.9, or 2.0 and at most 2.4. 2.7, or 3.0, with any combination of the low and high values ​​provided being possible (e.g., the average hydroxyl functionality is 1.8 to 3.0). For some embodiments, the aromatic polyester polyol has a number average molecular weight of at least 300, 350, 400, or 425 and at most 525, 550, 600, or 800, with any combination of the lower and higher values ​​provided being possible (e.g., the number average molecular weight of the aromatic polyester polyol is from 300 to 800).

[0017] Such polyol components may also include polycarbonate polyols such as the reaction products of diols such as propanediol-(1,3), butanediol-(1,4) and / or hexanediol-(1,6), diethylene glycol, triethylene glycol or tetraethylene glycol with diaryl carbonates such as diphenyl carbonate, dialiphatic carbonates such as dimethyl carbonate or phosgene, or from the reaction of oxirane and carbon dioxide.

[0018] Other examples of suitable isocyanate-reactive compounds include those polymers or copolymers formed with propylene oxide having a hydroxyl equivalent of at least 75. The propylene oxide may be 1,3-propylene oxide, but is more commonly 1,2-propylene oxide. In the case of copolymers, the comonomer is another copolymerizable alkylene oxide, such as ethylene oxide, 2,3-butylene oxide, tetrahydrofuran, 1,2-hexane oxide, and the like. The copolymers may contain 25% or more, 50% or more, and preferably 75% or more by weight of polymerized propylene oxide. The isocyanate-reactive compounds may also include those polymers formed with 100% propylene oxide based on the total weight of polymerized alkylene oxide. The copolymers preferably contain 75% or less, especially 50% or less by weight of polymerized ethylene oxide. The polymers or copolymers of propylene oxide should have a nominal functionality of at least 2.0. The nominal functionality is preferably 2.5 to 8, more preferably 2.5 to 7 or 2.5 to 6. The hydroxyl equivalent weight of the propylene oxide polymer or copolymer is at least 100, preferably at least 150, more preferably 150 to 1,000, and in some embodiments 150 to 750. The isocyanate-reactive compound may be formed in a blend, and the polyol blend may include a blend of a diol and a triol. The diol has an average molecular weight (Mw) of 300 to 8,000 grams / mole, and the triol has an average molecular weight (Mw) of 500 to 6,500 grams / mole.

[0019] In various embodiments, suitable isocyanate-reactive compounds without aromatic moieties may be formed as blends with suitable isocyanate-reactive compounds with aromatic moieties. In isocyanate-reactive compounds that are blends of non-aromatic isocyanate-reactive compounds and aromatic-containing isocyanate-reactive compounds, the isocyanate-reactive compounds containing aromatic moieties have an aromatic content of 5 weight percent (wt%) to 80 wt%. Preferably, the aromatic moieties comprise 8 wt% to 50 wt% of the isocyanate-reactive compounds containing aromatic moieties. More preferably, the aromatic moieties comprise 10 wt% to 40 wt% of the isocyanate-reactive compounds containing aromatic moieties.

[0020] In various embodiments, the isocyanate-reactive compound may have a hydroxyl value of 10 mg KOH / g to 700 mg KOH / g. In yet other embodiments, the isocyanate-reactive compound may have a hydroxyl value of 100 mg KOH / g to 500 mg KOH / g, or 150 mg KOH / g to 400 mg KOH / g, or 190 mg KOH / g to 350 mg KOH / g. As used herein, hydroxyl value is the number of milligrams of potassium hydroxide equivalent to the hydroxyl content in one gram of polyol or other hydroxyl compound. The polyol may also have a number average isocyanate-reactive group functionality of 1.8 to 3, such as 2 to 2.7 or 2 to 2.5.

[0021] For the various embodiments, the polyether polyols and / or polyester polyols can also be uncapped or capped using ethylene oxide (EO) and / or propylene oxide (PO) as known in the art to provide hydrophilic or hydrophobic structures.

[0022] In the present disclosure, other isocyanate-reactive compositions can be used in forming the isocyanate-reactive compositions of the present disclosure besides the polyol component. This allows for a two-component system of isocyanate-reactive compositions, where an amine can be used as a curing agent in place of or in addition to a polyol as provided herein. Such isocyanate-reactive compositions can include aromatic diamines, such as those containing at least one alkyl substituent ortho to the first amino group and two alkyl substituents ortho to the second amino group, or mixtures thereof. In some embodiments, at least two of the alkyl substituents contain at least two carbon atoms. In certain embodiments, the reactivity of the diamine towards isocyanates is not reduced by electron-withdrawing substituents such as halogens, esters, ethers or disulfide groups, as in the case of, for example, methylene-bis-chloroaniline (MOCA). In certain embodiments, such diamines do not contain other functional groups that react with isocyanates. In certain embodiments, the aforementioned alkyl substituents can have up to 20 carbon atoms and can be linear or branched long chain.

[0023] The isocyanate-reactive composition for forming a polyurethane-based foam also includes a flame modifier composition. For various embodiments, the flame modifier composition includes 0.1 wt% to 7.0 wt% phosphorus from the halogen-free flame retardant compound and 0.05 wt% to 14.0 wt% transition metal from the transition metal compound, where the weight percent of phosphorus and transition metal is based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound. Preferably, the flame modifier composition includes 0.3 wt% to 5.0 wt% phosphorus from the halogen-free flame retardant compound, where the weight percent of phosphorus from the halogen-free flame retardant compound is based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound, and 0.1 wt% to 5.0 wt% transition metal from the transition metal compound, based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound. More preferably, the flame modifier composition comprises 1.0 wt% to 3.0 wt% phosphorus from the halogen-free flame retardant compound, where the weight % of phosphorus from the halogen-free flame retardant compound is based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound, and 0.3 wt% to 2.0 wt% transition metal from the transition metal compound, based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound. For a given weight percent value, the flame modifier composition has a molar ratio of transition metal to phosphorus (mol transition metal:mol phosphorus) of 0.05:1 to 5:1. Preferably, the molar ratio of transition metal to phosphorus (mol transition metal:mol phosphorus) is 0.10:1 to 3:1. More preferably, the molar ratio of transition metal to phosphorus (mol transition metal:mol phosphorus) is 0.15:1 to 1:1.

[0024] For the embodiments provided herein, the halogen-free flame retardant compound is selected from the group consisting of phosphates, polyphosphates, phosphonates, phosphinates, biphosphinates, and combinations thereof. Examples of phosphates include trialkyl phosphates, triaryl phosphates, phosphate esters, and resorcinol bis(diphenyl phosphate). As used herein, trialkyl phosphates have at least one alkyl group having 2 to 12 carbon atoms. The other two alkyl groups of the trialkyl phosphate may be independently the same or different from the first alkyl group containing 1 to 8 carbon atoms, and include linear or branched alkyl groups, cyclic alkyl groups, alkoxyethyl, hydroxyl alkyl, hydroxyl alkoxy alkyl groups, and linear or branched alkylene groups. Examples of the other two alkyl groups of the trialkyl phosphate include, for example, methyl, ethyl, propyl, butyl, n-propyl, and isopropyl. n-butyl, isobutyl, sec-butyl, tert-butyl, butoxyethyl, isopentyl, neopentyl, isohexyl, isoheptyl, cyclohexyl, propylene, 2-methylpropylene, neopentylene, hydroxymethyl, hydroxyethyl, hydroxypropyl, or hydroxybutyl. Blends of different trialkyl phosphates may also be used. The three alkyl groups of the trialkyl phosphate may be the same. The trialkyl phosphate is desirably triethyl phosphate (TEP).

[0025] Examples of phosphonates include diethyl (hydroxymethyl) phosphonate, dimethyl methyl phosphonate, and diethyl ethyl phosphonate. Examples of phosphinates include metal salts of organic phosphinates such as aluminum methyl ethyl phosphinate, aluminum diethyl phosphinate, zinc methyl ethyl phosphinate, and zinc diethyl phosphinate. Examples of additional halogen-free flame retardant compounds include 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, ammonium polyphosphate, and combinations thereof.

[0026] For the embodiments provided herein, the transition metal compound is selected from the group consisting of oxides, carboxylates, salts, coordination compounds, and combinations thereof, and the transition metal is selected from the group consisting of copper, iron, manganese, cobalt, nickel, zinc, and combinations thereof. Examples of transition metal compounds include copper(I) oxide, copper(II) oxide, copper(II) acetate, copper(I) acetate, copper butyrate, copper ethylenediaminetetraacetic acid (EDTA) disodium salt, di-μ-hydroxobis[(N,N,N′,N′-tetramethylethylenediamine)copper(II)] chloride, zinc stannate, zinc hydroxystannate, manganese(II) 2-ethylhexanoate, dicyclopentadienyliron (ferrocene), and combinations thereof. Preferably, the transition metal compound is selected from the group consisting of copper(I) oxide, copper(II) oxide, copper ethylenediaminetetraacetic acid (EDTA) disodium salt, and combinations thereof. The transition metal compounds of the present disclosure have little or no effect on the reaction of isocyanates and isocyanate-reactive compositions. The transition metal compounds preferably do not reduce the isocyanurate concentration in the polyurethane foam by 40% or more compared to the same polyurethane foam formulation without the transition metal compound. More preferably, the transition metal compounds do not reduce the isocyanurate concentration in the polyurethane foam by 30% or more compared to the same polyurethane foam formulation without the transition metal compound. Most preferably, the transition metal compounds do not reduce the isocyanurate concentration in the polyurethane foam by 20% or more compared to the same polyurethane foam formulation without the transition metal compound.

[0027] As discussed in the Examples section below, there is a surprising reduction in HCN generation from the pyrolysis of polyurethane-based foams having transition metal compounds of a given size range. Preferably, the transition metal compounds used to form the polyurethane-based foams of the present disclosure have a median particle diameter (D50) of 1 nm to 100 μm. Preferably, the transition metal compounds used to form the polyurethane-based foams of the present disclosure have a median particle diameter (D50) of 10 nm to 10 μm. Other preferred values ​​of the median particle diameter of the transition metal compounds used to form the polyurethane-based foams of the present disclosure include 5 nm to 50 μm and 10 nm to 20 μm.

[0028] For various embodiments, the isocyanate-reactive composition has a molar ratio of moles of isocyanate-reactive moieties from the halogen-free flame retardant compound to moles of phosphorus of 70:1 to 1:1. Preferably, the molar ratio of moles of isocyanate-reactive moieties from the halogen-free flame retardant compound to moles of phosphorus is 35:1 to 2:1. Most preferably, the molar ratio of moles of isocyanate-reactive moieties from the halogen-free flame retardant compound to moles of phosphorus is 10:1 to 3:1.

[0029] For the embodiments provided herein, the isocyanate-reactive composition may further comprise a catalyst, a surfactant, a blowing agent, or a combination thereof. The use of other components known in the art may also be included in the isocyanate-reactive composition to enhance and / or facilitate the use of the isocyanate-reactive composition with an isocyanate compound in a reaction mixture as provided herein to form a polyurethane-based foam.

[0030] Water may be included in the reaction mixture, if desired, to drive the reaction and may be used as a chemical blowing agent. The amount of water present in the reaction mixture may range from 0 to 5 weight percent, based on the total weight of the isocyanate-reactive composition.

[0031] The catalyst may be present in the isocyanate-reactive composition in an amount sufficient to provide the reaction mixture with 0.1 to 3.0 weight percent catalyst based on the total weight of the reaction mixture. The catalyst may be selected from the group consisting of organic tertiary amines, tertiary phosphines, potassium acetate, urethane-based catalysts, and combinations. The catalyst may also include organotin compounds, as known in the art.

[0032] For the various embodiments, the catalyst may be a blowing catalyst, a gelling catalyst, a trimerization catalyst, or a combination thereof. As used herein, blowing catalysts and gelling catalysts may be distinguished by their tendency to favor either a urea (blow) reaction in the case of a blowing catalyst, or a urethane (gel) reaction in the case of a gelling catalyst. A trimerization catalyst may be utilized to promote isocyanurate reactions in the composition.

[0033] Examples of blowing catalysts, such as catalysts that may tend to favor the blowing reaction, include, but are not limited to, short-chain tertiary amines or tertiary amines that contain oxygen. Amine-based catalysts may not be sterically hindered. For example, blowing catalysts include, among others, bis-(2-dimethylaminoethyl)ether, pentamethyldiethylene-triamine, triethylamine, tributylamine, N,N-dimethylaminopropylamine, dimethylethanolamine, N,N,N',N'-tetra-methylethylenediamine, and combinations thereof. An example of a commercially available blowing catalyst is POLYCAT™ 5 from Evonik, among other commercially available blowing catalysts.

[0034] Examples of gelling catalysts, e.g., catalysts that may tend to favor the gelling reaction, include, but are not limited to, organometallic compounds, cyclic tertiary amines and / or long chain amines, e.g., those containing several nitrogen atoms, and combinations thereof. Organometallic compounds include organotin compounds such as tin(II) salts of organic carboxylic acids, e.g., tin(II) diacetate, tin(II) dioctanoate, tin(II) diethylhexanoate, and tin(II) dilaurate, and dialkyltin(IV) salts of organic carboxylic acids, e.g., dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate, and dioctyltin diacetate. Bismuth salts of organic carboxylic acids may also be utilized as gelling catalysts, e.g., bismuth octanoate. Cyclic tertiary amines and / or long chain amines include dimethylbenzylamine, triethylenediamine, and combinations thereof. , and combinations thereof. Examples of commercially available gelling catalysts are POLYCAT™ 8 and DABCO™ T-12 from Evonik, among other commercially available gelling catalysts.

[0035] Examples of trimerization catalysts include, among others, N,N,N',N'',N''-pentamethyldiethylenetriamine (PMDETA), N,N',N''-tris(3-dimethylaminopropyl)hexahydro-s-triazine, N,N-dimethylcyclo-hexylamine, 1,3,5-tris(N,N-dimethylaminopropyl)-s-hexahydrotriazine, [2,4,6-tris(dimethylaminomethyl)phenol], potassium acetate, potassium octanoate, tetraalkylammonium hydroxides such as tetramethylammonium hydroxide, alkali metal hydroxides such as sodium hydroxide, alkali metal alkoxides such as sodium methoxide and potassium isopropoxide, and alkali metal salts of long chain fatty acids having 10 to 20 carbon atoms, and combinations thereof. Some commercially available trimerization catalysts include DABCO™ TMR-2, TMR-7, DABCO™ K 2097, DABCO™ K15, POLYCAT™ 41, and POLYCAT™ 46, each from Evonik, among other commercially available trimerization catalysts.

[0036] For the various embodiments, the blowing agent may be present in the isocyanate-reactive composition in an amount sufficient to provide the reaction mixture with 1.0 to 15 weight percent blowing agent based on the total weight of the reaction mixture. The blowing agent may be selected from the group consisting of water, volatile organic materials, dissolved inert gases, and combinations thereof, as known in the art. Examples of blowing agents include hydrocarbons such as butane, isobutane, 2,3-dimethylbutane, n- and i-pentane isomers, hexane isomers, heptane isomers, and cycloalkanes, including cyclopentane, cyclohexane, cycloheptane; HCFC-142b (1-chloro-1,1-difluoroethane), HCFC-141b (1,1-dichloro-1-fluoroethane), HCFC-22 (chlorodifluoro-methane), HFC-245fa (1,1,1,3,3-pentafluoropropane), HFC-365mfc (1,1,1,3,3-penta-fluorobutane), HFC 227ea (1,1,1,2,3,3,3-heptafluoropropane), HFC-134a (1,1,1,2-tetrafluoroethane), HFC-125 (1,1,1,2,2-pentafluoroethane), HFC-143 (1,1,2-trifluoroethane), HFC 143A (1,1,1-trifluoroethane), HFC-152 (1,1-difluoroethane), HFC-227ea (1,1,1,2,3,3,3-heptafluoropropane), HFC-236ca (1,1,2,2,3,3-hexafluoropropane), HFC 236fa (1,1,1,3,3,3-hexafluoroethane), HFC 245ca (1,1,2,2,3-pentafluoropentane), HFC hydrofluorocarbons such as HFC 356mff (1,1,1,4,4,4-hexafluorobutane), HFC 365mfc (1,1,1,3,3-pentafluorobutane); hydrofluoroolefins such as cis-1,1,1,4,4,4-hexafluoro-2-butene, 1,3,3,3-tetrafluoropropene, trans-1-chloro-3,3,3-trifluoropropene; and chemical blowing agents such as formic acid and water.Blowing agents also include other volatile organics such as ethyl acetate; methanol; ethanol; halogen-substituted alkanes such as methylene chloride, chloroform, ethylidene chloride, vinylidene chloride, monofluorotrichloromethane, chlorodifluoromethane, dichlorodifluoromethane; butane; hexane; heptane; diethyl ether as well as gases such as nitrogen; air; and carbon dioxide.

[0037] For various embodiments, the surfactant may be present in the isocyanate-reactive composition in an amount sufficient to provide a reaction mixture with 0.1-10 wt. % surfactant based on the total weight of the reaction mixture. Examples of suitable surfactants include silicone-based surfactants and organic-based surfactants. Some representative materials are generally polysiloxane polyoxyl alkylene block copolymers, such as those disclosed in U.S. Pat. Nos. 2,834,748, 2,917,480, and 2,846,458, the disclosures of which are incorporated herein by reference in their entirety. Also included are organic surfactants containing polyoxyethylene-polyoxybutylene block copolymers, as described in U.S. Pat. No. 5,600,019, the disclosure of which is incorporated herein by reference in its entirety. Other surfactants include polyethylene glycol ethers of long chain alcohols, tertiary amine or alkanolamine salts of long chain aryl acid sulfates, alkyl sulfonates, alkylaryl sulfonic acids, and combinations thereof.

[0038] The reaction mixture may further include a filler along with other additives in addition to water, catalyst, blowing agent, surfactant, and combinations thereof. The total amount of such other additives present in the isocyanate-reactive composition may be sufficient to provide the reaction mixture with 0.01 to 3.0 weight percent of other additives (e.g., fillers) based on the total weight of the reaction mixture. The use of other additives for polyurethane foams is also known and may be used in the present disclosure.

[0039] The reaction mixture for forming the polyurethane-based foam of the present disclosure, as provided herein, includes an isocyanate compound having an isocyanate moiety and an isocyanate-reactive compound having an isocyanate moiety and an aromatic moiety, the isocyanate-reactive compound constituting 5% to 80% by weight of the isocyanate-reactive compound, based on the total weight of the isocyanate-reactive compound. For embodiments herein, the reaction mixture may have a molar ratio of isocyanate moiety to isocyanate-reactive moiety of 1.2:1 to 7:1. Preferably, the molar ratio of isocyanate moiety to isocyanate-reactive moiety is 1.5:1 to 5:1. More preferably, the molar ratio of isocyanate moiety to isocyanate-reactive moiety is 2:1 to 4:1. Preferably, the isocyanate-reactive moiety of the isocyanate-reactive compound is a hydroxyl moiety, and the reaction mixture has a molar ratio of isocyanate moiety to hydroxyl moiety of 1.2:1 to 7:1, preferably 1.5:1 to 5:1, more preferably 2:1 to 4:1.

[0040] The reaction mixture also includes 0.1 wt% to 7.0 wt% phosphorus from the halogen-free flame retardant compound and 0.05 wt% to 14.0 wt% transition metal from the transition metal compound, the weight percent values ​​of phosphorus and transition metal being based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound. For various embodiments, the halogen-free flame retardant compound and / or the transition metal compound can be included in a mixture with either the isocyanate compound and / or the isocyanate-reactive compound, and when both the halogen-free flame retardant compound and the transition metal compound are included with the isocyanate-reactive compound of the present disclosure, the mixture can provide the isocyanate-reactive composition of the present disclosure. The reaction mixture further optionally includes a catalyst, a surfactant, and a blowing agent, each as provided herein, for forming a polyurethane-based foam. As discussed herein, the polyurethane-based foam is formed using the reaction mixture.

[0041] For various embodiments, the isocyanate compound has a number average molecular weight of 150 g / mol to 750 g / mol. Other number average molecular weight values ​​may also be possible. For example, the isocyanate-reactive compound may have a number average molecular weight as low as 150, 200, 250, or 300 g / mol to an upper limit of 350, 400, 450, 500, or 750 g / mol. In some embodiments, when the isocyanate compound is an isocyanate prepolymer resulting from the reaction of an isocyanate-reactive compound with a molar excess of a polyisocyanate compound or a polymeric isocyanate compound under conditions that do not result in gelation or solidification, the isocyanate prepolymer may have a number average molecular weight higher than 750 g / mol, which may be calculated from the number average molecular weight of each component used in preparing the prepolymer and their relative masses. The number average molecular weight values ​​reported herein are determined by end group analysis, gel permeation chromatography, and other methods known in the art. The isocyanate compound may be monomeric and / or polymeric, as is known in the art. In addition, the isocyanate compound may have an isocyanate equivalent weight of 80 to 400.

[0042] As used herein, a polymeric isocyanate compound contains two or more -NCO groups per molecule. For various embodiments, the polymeric isocyanate compound is selected from aliphatic diisocyanates, cycloaliphatic diisocyanates, aromatic diisocyanates, polyisocyanates, isocyanate prepolymers, and combinations thereof. For various embodiments, the polymeric isocyanate compound has a number average molecular weight of 150 g / mol to 500 g / mol. In addition, the polymeric isocyanate compound may have an isocyanate equivalent weight of 80 to 150, preferably 100 to 145, and more preferably 110 to 140.

[0043] Examples of polymeric isocyanate compounds of the present disclosure include methylene diphenyl diisocyanate (MDI), polymethylene polyphenylisocyanates containing MDI, polymeric MDI (PMDI), 1,6 hexamethylene diisocyanate (HDI), 2,4- and / or 2,6-toluene diisocyanate (TDI), 1,5-naphthalene diisocyanate (NDI), tetramethylene-1,4-diisocyanate, cyclohexane-1,4-diisocyanate, hexahydrotoluene diisocyanate, hydrogenated MDI (HDI), and the like. 12MDI), methoxyphenyl-2,4-diisocyanate, 4,4'-biphenylene diisocyanate, 3,3'-dimethyloxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4',4"-triphenylmethane diisocyanate, polymethylene polyphenyl isocyanate, hydrogenated polymethylene polyphenyl polyisocyanate, toluene-2,4,6-triisocyanate and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate, methylenebicyclohexyl isocyanate (HMDI), isophorone diisocyanate (IPDI) and combinations thereof. Suitable isocyanates may also include, but are not limited to, and other aromatic and / or aliphatic polyfunctional isocyanates. Aromatic diisocyanates include those containing phenyl, tolyl, xylyl, naphthyl, or diphenyl moieties, or combinations thereof, such as the trimethylolpropane adduct of xylylene diisocyanate, the trimethylolpropane adduct of toluene diisocyanate, 4,4'-diphenyldimethane diisocyanate (MDI), xylylene diisocyanate (XDI), 4,4'-diphenyldimethylmethane diisocyanate, di- and tetraalkyldiphenylmethane diisocyanates, 4,4'-dibenzyl diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, and combinations thereof.Suitable aliphatic polymeric isocyanates include trimer of hexamethylene diisocyanate, trimer of isophorone diisocyanate, biuret of hexamethylene diisocyanate, hydrogenated polymeric methylene diphenyl diisocyanate, hydrogenated methylene diphenyl diisocyanate, hydrogenated MDI, tetramethylxylol diisocyanate (TMXDI), 1-methyl-2,4-diisocyanato-cyclohexane, 1,6-diisocyanato-2,2,4-trimethylhexane, 1-isocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane, tetramethoxybutane 1,4-diisocyanate, butane 1,4-diisocyanate, hexane 1,6-diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane 1,4-diisocyanate, and combinations thereof. Examples of other polymeric isocyanate compounds include additional aliphatic, cycloaliphatic, polycyclic or aromatic in nature, such as hydrogenated xylene diisocyanate (HXDI), p-phenylene diisocyanate (PPDI), 3,3'-dimethyldiphenyl-4,4'-diisocyanate (DDDI), 2,2,4-trimethylhexamethylene diisocyanate (TMDI), isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (H12MDI) and norbornane diisocyanate (NDI). As well as the above isocyanates, some modified polyisocyanates may be utilized, including, among others, uretdione, isocyanurate, carbodiimide, uretonimine, allophanate or biuret structures, and combinations thereof.

[0044] In certain embodiments, the isocyanate has a viscosity of 5 to 10,000 mPa·s at 25° C. as measured using a Brookfield DVE viscometer. Other viscosity values ​​may also be possible. For example, the isocyanate compound may have a viscosity of 5, 10, 30, 60 or 150 mPa·s. . Low values ​​of s ~500, 2500, 5000 or 10,000 mPa . The viscosity may have a viscosity value at 25° C. as measured using a Brookfield DVE viscometer of up to 1000 psi.

[0045] For the embodiments provided herein, the reaction mixture optionally includes a catalyst, a surfactant, a blowing agent, or a combination thereof, as discussed herein, and these components may be provided in the isocyanate-reactive composition discussed herein. The reaction mixture may also include other components known in the art to enhance and / or promote the reaction mixture, as provided herein, to form a polyurethane-based foam. It is understood that the catalyst, surfactant, blowing agent, or a combination thereof may be present in any combination of the isocyanate-reactive composition and / or isocyanate compound to arrive at their respective weight percent values ​​provided herein for the reaction mixture. This is also the case for reaction mixtures having other components known in the art to enhance and / or promote the use of the components of the reaction mixture.

[0046] The present disclosure also provides a process for preparing a reaction mixture for producing a polyurethane-based foam. The process may include providing an isocyanate compound having an isocyanate moiety as discussed herein. The process further includes providing an isocyanate-reactive compound having an isocyanate-reactive moiety and an aromatic moiety, the isocyanate-reactive compound constituting 5% to 80% by weight of the isocyanate-reactive compound based on the total weight of the isocyanate-reactive compound. The process also includes providing 0.1% to 7.0% by weight of phosphorus from the halogen-free flame retardant compound as discussed herein, and 0.05% to 14.0% by weight of a transition metal from the transition metal compound as discussed herein, the weight percent values ​​of phosphorus and transition metal being based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound. For these given weight percent values, mixing the isocyanate-reactive composition and the isocyanate compound to form the reaction mixture may include providing a molar ratio of transition metal to phosphorus (molar transition metal:molar phosphorus) in the reaction mixture of 0.05:1 to 5:1. The process optionally further includes providing a catalyst, a surfactant, and a blowing agent.The process then includes mixing the isocyanate compound, the isocyanate-reactive compound, the halogen-free flame retardant compound; the transition metal compound; and the optional catalyst, surfactant, and blowing agent to form a reaction mixture.For various embodiments, the reaction mixture can have a molar ratio of isocyanate moieties to isocyanate-reactive moieties of 1.2:1 to 7:1.

[0047] Additional embodiments of the process further include mixing the transition metal compound with a carrier when providing the transition metal from the transition metal compound. As used herein, a carrier is a liquid that is typically used to mix with the transition metal compound, which is a solid powder, to form a slurry or solution to facilitate providing the transition metal from the transition metal compound (e.g., mixing into an isocyanate-reactive composition). Any of the liquid components used in the reaction mixture for preparing polyurethane foam can be used to disperse the transition metal compound, regardless of whether it is isocyanate-reactive. Examples of such carrier liquids include, but are not limited to, polyols, catalysts, surfactants, flame retardant additives, liquid blowing agents, rheology modifiers, liquid dyes, and the like. It is also known to those skilled in the art that the transition metal compound can even be directly dispersed in the isocyanate compound for making polyurethane foam. For various embodiments, during the process for preparing the reaction mixture for producing the polyurethane-based foam, it is also possible to mix 0.1 wt % to 7.0 wt % phosphorus from the halogen-free flame retardant compound (wt % phosphorus based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound) with the isocyanate compound having an isocyanate moiety, as discussed herein.

[0048] As previously discussed, catalysts, surfactants, blowing agents or combinations thereof for the reaction mixture can be optionally provided in the isocyanate-reactive composition as discussed herein. It is also possible for other components provided herein to be mixed with the isocyanate-reactive composition and isocyanate compound when forming the reaction mixture. It is understood that catalysts, surfactants, blowing agents or combinations thereof can be present in any combination of the isocyanate-reactive composition and / or isocyanate compound to arrive at their respective weight percent values ​​provided herein for the reaction mixture. This is also the case for reaction mixtures having other components known in the art to enhance and / or facilitate the use of the isocyanate-reactive composition with the isocyanate compound in the reaction mixture.

[0049] The process for preparing the reaction mixture for producing polyurethane-based foams can be accomplished through any process technique known in the art. In general, polyurethane foams can be produced by discontinuous or continuous processes, including processes commonly referred to as discontinuous panel process (DCP) and continuous lamination, where the foaming reaction and subsequent curing are carried out in a mold or on a conveyor. The process provided herein can be carried out at a temperature between 15°C and 80°C. Mixing pressures for the process can include values ​​between 80 kPa and 25,000 kPa. Mixing can be carried out using mixing equipment known in the art. The density of the resulting foam can be between 10 kg / m 3 More than 15kg / m 3 More preferably, 25 kg / m 3 More than 35 kg / m 3 At the same time, typically 200 kg / m 3 Less than 100 kg / m 3 Less than or equal to 70 kg / m 3 Less than 50 kg / m 3 It can be the following:

[0050] The polyurethane-based foams of the present disclosure provide low smoke generation and high thermal stability as determined according to ASTM E662 "Test Method for Specific Optical Density of Smoke Generated by Solid Materials". Lower values ​​of maximum specific optical density (Max Ds) mean less smoke generation. Lower values ​​of mass loss % mean greater thermal stability. Max Ds can be 400 or less, preferably 200 or less, more preferably 100 or less, and even most preferably 50 or less. Mass loss % can be 50% or less, preferably 45% or less, more preferably 40% or less, and even most preferably 35% or less.

[0051] The polyurethane-based foams of the present disclosure may have low thermal conductivity for applications such as building insulation. The thermal conductivity of rigid foams is expressed as K-factor. K-factor is a measure of thermal insulation properties. The K-factor of the foams prepared may be 30.0 mW / m·K or less, preferably 27.0 mW / m·K or less, more preferably 24.0 mW / m·K or less, and most preferably 22.0 mW / m·K or less. Thermal conductivity (K-factor) was measured using ASTM C-518-17 at an average temperature of 75°F.

[0052] The applications of polyurethane-based foams produced by the present disclosure are known in the industry. For example, polyurethane-based foams can be used for insulation used in building walls and roofs, garage doors, transportation trucks and railroad cars, and refrigeration facilities. The polyurethane-based foams disclosed herein can have a combination of properties that are desirable for these applications. For example, the polyurethane-based foams disclosed herein can advantageously provide desirable low thermal conductivity, smoke density, thermal stability, and improved combustion properties with reduced HCN and CO emissions.

[0053] Some embodiments of the present disclosure will now be described in detail in the following examples. EXAMPLES

[0054] In the examples, various terms and designations of materials are used, including, for example:

[0055] material Materials used in the examples and / or comparative examples include the following:

[0056] Polyol A is a polyester polyol (aromatic polyester polyol from terephthalic acid, polyethylene glycol, and diethylene glycol) from Dow Inc, with a hydroxyl number of 220 mg KOH / g, a functionality of 2, and a total aromatic moiety content of 14.8 wt %.

[0057] Polyol B is a polyester polyol (aromatic polyester polyol from terephthalic acid, polyethylene glycol, glycerol, and diethylene glycol) from Dow Inc, having a hydroxyl number of 315 mg KOH / g, a functionality of 2.4, and a total content of aromatic moieties of 17.4 wt.%.

[0058] Triethyl phosphate (TEP) is a flame retardant from LANXESS.

[0059] Fyrolflex(TM) resorcinol bis(diphenyl phosphate) (RDP) is an ICL It is a flame retardant from Industrial Products.

[0060] Diethyl(hydroxymethyl)phosphonate (DEHMP) is a product of Tokyo Chemical This is a flame retardant from Industry Co., Ltd.

[0061] POLYCAT™ 5 is a catalyst from Evonik Industries AG.

[0062] POLYCAT™ 46 is a catalyst from Evonik Industries AG.

[0063] The surfactant is a silicone hard foam surfactant from Evonik Industries AG.

[0064] The water is deionized water having a resistivity of 10 MΩ×cm (million ohms) at 25° C.

[0065] Cyclopentane (c-pentane) is a foaming agent from Sigma-Aldrich.

[0066] PAPI™ 580N is a 30.8% methylene diphenyl ether from Dow Inc. It is a polymethylene polyphenylisocyanate containing diisocyanate (MDI).

[0067] Copper disodium ethylenediaminetetraacetate (CuEDTA) from Fluka.

[0068] Copper(II) 2-ethylhexanoate (CuEH) from Sigma-Aldrich.

[0069] Copper(I) oxide (CuO), powder, size ≤ 7 μm, 97% from Sigma-Aldrich.

[0070] Copper(II) oxide (CuO), powder, size ≤10 μm, 98% from Sigma-Aldrich.

[0071] Copper(II) oxide (CuO), powder, size 10 nm, 98% from US Research Nanomaterials, Inc.

[0072] Copper(II) oxide (CuO), powder, size 40 nm, 98% from US Research Nanomaterials, Inc.

[0073] Dicyclopentadienyliron (ferrocene) from Fluka.

[0074] Preparation of polyurethane-based foams for the examples (Ex) and comparative examples (C Ex) The following components are used in the reaction mixture to form polyurethane-based foams for Examples (Ex.) 1-17 and Comparative Examples (C Ex.) A-F. The amount of each component is listed in parts by weight (PBW) based on the total weight of the reaction mixture used to form the polyurethane-based foam. The amount of "Transition Metal Compound" is found in Table 1, while the composition of "Transition Metal Compound" for each Example and Comparative Example is shown in Tables 2-5. [Table 1]

[0075] The polyurethane-based foams are prepared as follows: The components of the isocyanate-reactive composition, except for the cyclopentane and transition metal compound provided in Table 1 for each Example and Comparative Example, are mixed in a plastic beaker at 2000 rpm using a rotary mixer for 1 minute (min). The transition metal compound for each Example and Comparative Example, except for the use of the transition metal compound below, is directly mixed with the isocyanate-reactive composition for an additional minute at 2000 rpm. For CuEH, the CuEH is first dissolved in TEP and mixed with the remaining components of the isocyanate-reactive composition. Cyclopentane for each Example and Comparative Example is then directly mixed with the isocyanate-reactive composition. The isocyanate-reactive composition and isocyanate are then mixed again in the beaker at 3000 rpm for 4 seconds (s). Immediately after mixing, the contents of the beaker are poured into a mold (300 millimeters (mm) x 200 mm x 50 mm) that is preheated to 60°C. After curing at 60°C for 20 minutes, the polyurethane-based foam is removed from the mold. The core density of the moulded polyurethane-based foam is approximately 40 kg / m 3 It was.

[0076] Analysis of smoke gas composition Method 1 - Pyrolysis / GC Pyrolysis tests are performed using a Frontier Labs 2020D pyrolyzer attached to an Agilent 6890 GC with an FID detector. Approximately 200-250 μg of sample is weighed into a Frontier lab silica-lined stainless steel cup. Pyrolysis is performed by single shot mode by dropping the sample cup into an oven for analysis at 600 °C under air conditions for 2 min, followed by another 2 min under helium conditions. Volatile products expelled from the sample are captured at the head of the separation column using a micro-cryotrapping device (MCT). Separation is achieved using a 10 m x 0.32 mm ID x 5 μm PoraBond Q column from Agilent with HP-1 (10 m x 0.53 mm x 2.65 um) as a guard column. Back inlet pressure is used for backflush purposes (0.5 m x 0.53 mm guard column using back inlet as head pressure tee to PoraBond Q and HP-1 column). HCN was detected with a back FID detector. Use the HCN normalized peak area by sample weight for HCN concentration comparison. Define the relative HCN content of a transition metal-containing sample as the ratio of its normalized HCN peak area divided by the normalized HCN peak area for a comparative control without transition metals.

[0077] GC conditions: front injection port: 300 °C; split injector at 1:1; ramp pressure: 4.9 psi for 1.5 min then held at 3.1 psi at 50 psi / min; back injection port: 4 psi; GC oven: 40 °C for 3 min, held at 240 °C at 30 °C / min; FID: 250 °C, H2 flow: 40 mL / min, air flow: 450 mL / min, make-up gas (N2): 30 mL / min, 50 Hz.

[0078] Method 2-NBS / FTIR The NBS Smoke Chamber test protocol is carried out according to ISO 5659:1994, Plastics - Smoke Generation - Part 2: Determination of Optical Density by a Single Chamber Test. The specimens are subjected to a flame exposure mode of 50 kW / m for a test period of 20 minutes. 2 of irradiance. Products of combustion are analyzed using a Fourier transform infrared (FTIR) spectrometer. Gas sampling for toxicity measurements begins at the beginning of the exposure and continues until the end of the test period. Maximum detected concentration is reported in parts per million and % mass loss of the specimen as (initial mass-final mass) / nominal mass*100%. The nominal mass of the specimen is the total mass of a foam specimen with dimensions of 3" x 3" x 1". The relative HCN or CO content of the transition metal containing samples is defined as the ratio of the maximum HCN or maximum CO concentration normalized by the maximum HCN or maximum CO concentration for the comparative control without the transition metal.

[0079] NBS Smoke Density and Mass Loss % Measurements NBS smoke density measurements are performed according to ASTM E-662 Standard Test Method for Specific Optical Density of Smoke Generated by Solid Materials. Samples are subjected to a flame exposure mode of 25 kW / m for a test period of 10 minutes. 2 The average maximum specific optical density (D s,max ) and report the % mass loss of the specimen as (initial mass-final mass) / nominal mass*100%. The nominal mass of the specimen is the total mass of a foam specimen having dimensions of 3" x 3" x 1".

[0080] Relative Isocyanurate Content Determination Attenuated total reflectance Fourier transform infrared spectroscopy (ATR-FTIR) is performed on a Nicolet iS50 FT-IR instrument using a SMART iTX single bounce diamond ATR. Sixteen scans were performed at 4 cm -1 Resolution of 4000~600cm -1A rectangular cross section (10 mm x 60 mm) is cut from the center of the molded polyurethane-based foam sample. Three tests on the cross section are performed by averaging the three measurements for the characteristic peak. The relative isocyanurate content is calculated by the isocyanurate group characteristic peak height (approximately 1409 cm) normalized by this peak height ratio for a comparative control example having no transition metal. -1 ) and the phenyl group characteristic peak height (approximately 1595 cm -1 ) is defined as the ratio of

[0081] result Table 2 shows a significant reduction in HCN production from pyrolysis / GC (relative HCN concentration <0.70) while maintaining excellent smoke density and thermal stability (Max Ds ≤ 45, mass loss value ≤ 35%, and relative isocyanurate content ≥ 0.60) of polyurethane-based foams. [Table 2]

[0082] As seen in Tables 3 and 4, significant reductions in HCN production from pyrolysis / GC, excellent smoke density, and isocyanurate content are achieved with different phosphorus compounds. [Table 3] [Table 4]

[0083] As can be seen in Table 5, significant reductions in HCN production from pyrolysis / GC can be achieved with the addition of different types of transition metal compounds. [Table 5]

[0084] As shown in Table 6, a significant reduction in HCN production from pyrolysis / GC can be achieved by adding transition metal additives of different sizes. [Table 6]

[0085] High heat flux exposure (50kw / m 2 As seen in the NBS / FTIR tests under 0.25 wt. % copper concentration, there was a significant reduction in HCN and CO observed for polyurethane-based foams with CuO at all concentrations (Table 7). Surprisingly, more efficient HCN and CO reduction with higher char yield was achieved at a copper concentration of 0.25 wt. % copper. The copper compound CuEH, which is soluble in the isocyanate-reactive composition, was used and HCN emissions were higher than the control (Comparative Example A). [Table 7] Examples of the invention of this application include the following: [1] An isocyanate-reactive composition for forming a polyurethane-based foam, comprising: an isocyanate-reactive compound having an isocyanate-reactive moiety and an aromatic moiety, the aromatic moiety being between 5 weight percent (wt %) and 80 wt % of the isocyanate-reactive compound, based on the total weight of the isocyanate-reactive compound; 0.1% to 7.0% by weight of phosphorus from a halogen-free flame retardant compound, and and a combustion modifier composition comprising 0.05 wt.% to 14.0 wt.% of a transition metal from a transition metal compound, wherein said weight percent of said transition metal and said weight percent of said phosphorus are each based on the total weight of said isocyanate-reactive compound, said halogen-free flame retardant compound, and said transition metal compound. [2] The isocyanate-reactive composition according to [1] above, wherein the combustion modifier composition has a molar ratio of the transition metal to phosphorus of from 0.05:1 to 5:1. [3] The isocyanate-reactive composition of [1] above, wherein the halogen-free flame retardant compound is selected from the group consisting of phosphates, phosphonates, phosphinates, and combinations thereof. [4] The isocyanate-reactive composition of [1] above, wherein the transition metal compound is selected from the group consisting of oxides, carboxylates, salts, coordination compounds, and combinations thereof, and the transition metal is selected from the group consisting of copper, iron, manganese, cobalt, nickel, zinc, and combinations thereof. [5] The isocyanate-reactive composition of [1] above, wherein the transition metal compound is selected from the group consisting of copper(I) oxide, copper(II) oxide, copper disodium ethylenediaminetetraacetic acid (EDTA), and combinations thereof. [6] The isocyanate-reactive composition according to any one of [1] to [5] above, wherein the transition metal compound has a median particle diameter of 10 nm to 10 μm. [7] A reaction mixture for forming a polyurethane-based foam, comprising: an isocyanate compound having an isocyanate moiety; an isocyanate-reactive compound having an isocyanate-reactive moiety and an aromatic moiety that constitutes 5 weight percent (wt %) to 80 wt % of the isocyanate-reactive compound, based on the total weight of the isocyanate-reactive compound; 0.1 wt % to 7.0 wt % phosphorus from a halogen-free flame retardant compound and 0.05 wt % to 14.0 wt % transition metal from a transition metal compound, the weight percentages of phosphorus and said transition metal being based on the total weight of said isocyanate-reactive compound, said halogen-free flame retardant compound and said transition metal compound; Optionally, a catalyst, a surfactant, a blowing agent, or a combination thereof. [8] The reaction mixture of [7] above, wherein the reaction mixture has a molar ratio of the isocyanate moieties to the isocyanate-reactive moieties of from 1.2:1 to 7:1. [9] A polyurethane-based foam formed using the reaction mixture according to [7] or [8] above.

[10] A process for preparing a reaction mixture for producing a polyurethane-based foam, comprising: Providing an isocyanate compound having an isocyanate moiety; Providing an isocyanate-reactive composition according to any one of the above [1] to [6]; Optionally providing a catalyst, a surfactant, a blowing agent or a combination thereof; mixing said isocyanate compound, said isocyanate-reactive composition and said optional catalyst, surfactant, blowing agent or combination thereof to form said reaction mixture, said reaction mixture having a molar ratio of said isocyanate moieties to said isocyanate-reactive moieties of from 1.2:1 to 7:1.

Claims

1. 1. An isocyanate-reactive composition for forming a polyurethane-based foam, comprising: an isocyanate-reactive compound having an isocyanate-reactive moiety and an aromatic moiety, the aromatic moiety being from 5 weight percent (wt %) to 80 wt % of the isocyanate-reactive compound, based on the total weight of the isocyanate-reactive compound; 0.1% to 7.0% by weight of phosphorus from a halogen-free flame retardant compound, and a combustion modifier composition comprising 0.05 wt.% to 14.0 wt.% of a transition metal from a transition metal compound; wherein the weight percentage of the transition metal and the weight percentage of the phosphorus are each based on the total weight of the isocyanate-reactive compound, the halogen-free flame retardant compound, and the transition metal compound, and the transition metal compound is selected from the group consisting of copper (I) oxide, copper (II) oxide, copper ethylenediaminetetraacetic acid (EDTA) disodium salt, and combinations thereof.

2. 10. The isocyanate-reactive composition of claim 1, wherein the burn modifier composition has a molar ratio of the transition metal to phosphorus of from 0.05:1 to 5:

1.

3. 2. The isocyanate-reactive composition of claim 1, wherein the halogen-free flame retardant compound is selected from the group consisting of phosphates, phosphonates, phosphinates, and combinations thereof.

4. An isocyanate-reactive composition according to any one of claims 1 to 3, wherein the transition metal compound has a median particle diameter of from 10 nm to 10 μm.

5. 1. A reaction mixture for forming a polyurethane-based foam, comprising: an isocyanate compound having an isocyanate moiety; an isocyanate-reactive compound having an isocyanate-reactive moiety and an aromatic moiety that constitute from 5 weight percent (wt %) to 80 wt % of the isocyanate-reactive compound, based on the total weight of the isocyanate-reactive compound; 0.1 wt % to 7.0 wt % phosphorus from a halogen-free flame retardant compound and 0.05 wt % to 14.0 wt % transition metal from a transition metal compound, the weight percent values ​​of phosphorus and said transition metal being based on the total weight of said isocyanate-reactive compound, said halogen-free flame retardant compound and said transition metal compound, said transition metal compound being selected from the group consisting of copper (I) oxide, copper (II) oxide, copper disodium ethylenediaminetetraacetic acid (EDTA) and combinations thereof; Optionally, a catalyst, a surfactant, a blowing agent or a combination thereof; A reaction mixture comprising:

6. 6. The reaction mixture of claim 5, wherein the reaction mixture has a molar ratio of the isocyanate moieties to the isocyanate-reactive moieties of from 1.2:1 to 7:

1.

7. 7. A polyurethane-based foam formed using the reaction mixture of claim 5 or 6.

8. 1. A process for preparing a reaction mixture for producing a polyurethane-based foam, comprising: Providing an isocyanate compound having an isocyanate moiety; Providing an isocyanate-reactive composition according to any one of claims 1 to 4; Optionally providing a catalyst, a surfactant, a blowing agent or a combination thereof; mixing the isocyanate compound, the isocyanate-reactive composition and the optional catalyst, surfactant, blowing agent or combination thereof to form the reaction mixture, the reaction mixture having a molar ratio of the isocyanate moieties to the isocyanate-reactive moieties of from 1.2:1 to 7:1; The process includes:

Citation Information

Patent Citations

  • Composition for low-smoking flame-retardant polyisocyanurate foam and low-smoking flame-retardantfoam prepared therefrom

    JP1999140150A

  • Flame-retardant polyamide resin composition for ionizing radiation irradiation

    JP2010163472A

  • Use of trialkyl phosphate as a smoke suppressant in polyurethane foams

    JP2014532098A

  • Oxazolidone ring-containing epoxy resin and method for producing the same, epoxy resin composition, and cured product

    JP2016169314A

  • Foamable urethane resin composition and polyurethane foam

    JP2020172603A