Manufacturing method of highly heat-resistant transparent polyethylene terephthalate (PET) copolyester

The production of PET copolyester using a talcum powder and side group ester compound addresses the slow crystallization and high haze issues, resulting in a product with enhanced transparency and heat resistance for faster molding and broader applications.

JP7586950B2Active Publication Date: 2024-11-19NANYA PLASTICS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023044795
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-12-15
Filing Date
2023-03-20
Publication Date
2024-11-19
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

Polyethylene terephthalate (PET) resin has a slow crystallization rate, requiring high molding temperatures and long cooling times, limiting its application in engineering plastics and exhibiting high haze due to its rigid structure.

Method used

A method involving a dispersion slurry containing talcum powder and a side group ester compound is used to produce a PET copolyester through transesterification and polymerization reactions, enhancing nucleation and improving transparency and heat resistance.

Benefits of technology

The resulting PET copolyester exhibits a fast crystallization rate, high crystallinity, reduced haze, and improved heat resistance, thereby shortening injection molding time and expanding its applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586950000001
    Figure 0007586950000001
Patent Text Reader

Abstract

PURPOSE: To provide a high heat resistant and transparent polyethylene terephthalate (PET) copolyester and a manufacturing method thereof.SOLUTION: A manufacturing method for a polyethylene terephthalate (PET) copolyester includes the following steps. A dispersion slurry including a talcum powder is formulated. Terephthalic acid and ethylene glycol are mixed, and the dispersion slurry and a side-group ester compound are introduced to perform a transesterification reaction, forming bis-2-hydroxyethyl terephthalate. Then, a prepolymerization reaction and a polycondensation reaction are carried out to form a polyethylene terephthalate copolyester.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyethylene terephthalate (PET) copolyester and a method for producing the same, and more particularly to a highly heat-resistant and transparent polyethylene terephthalate (PET) copolyester and a method for producing the same. [Background technology]

[0002] In general, the crystallization rate of polyethylene terephthalate (PET) resin is slower than that of polybutylene terephthalate (PBT) resin, so a relatively high molding temperature and a relatively long cooling time are required when injection processing PET resin. This limits the application of PET resin to engineering plastics. In addition, polyethylene terephthalate (PET) resin has a high melting point due to its rigid structure, which results in high haze in the product.

[0003] Therefore, it has become an important task in the industry to develop a transparent PET resin with a fast crystallization rate and low haze, thereby shortening the injection molding time, improving transparency and heat resistance, and expanding product applications. Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention provides a polyethylene terephthalate (PET) copolyester, which has the advantages of fast crystallization rate and high crystallinity of PET polymer, and can effectively shorten the injection molding time and improve the transparency and heat resistance, and a method for producing the same. [Means for solving the problem]

[0005] The present invention provides a method for preparing polyethylene terephthalate (PET) copolyester, which includes the following steps: Prepare a dispersion slurry containing talcum powder; Mix terephthalic acid and ethylene glycol to introduce the dispersion slurry and a side group ester compound, and carry out an ester exchange reaction to form bis-2-hydroxyethyl terephthalate; Then, carry out a prepolymerization reaction and a condensation polymerization reaction to form a polyethylene terephthalate copolyester.

[0006] In one embodiment of the present invention, the talcum powder has an average particle size of 1.0 μm to 5.0 μm and a viscosity of 20 μm. 2 / g~12m 2 / g average specific surface area.

[0007] In one embodiment of the invention, the pendant ester compound comprises 2,6-naphthalene dicarboxylate.

[0008] In one embodiment of the present invention, the content of the talcum powder is in the range of 1 wt % to 8 wt % based on the total weight of the dispersion slurry.

[0009] In one embodiment of the present invention, the dispersion slurry further contains a dispersant and ethylene glycol, and the content of the dispersant is in the range of 99 wt % to 1 wt % with respect to the total weight of the dispersion slurry.

[0010] In one embodiment of the present invention, the amount of the dispersion slurry added is in the range of 1 wt % to 6 wt % based on the total weight of bis-2-hydroxyethyl terephthalate.

[0011] In one embodiment of the present invention, during the transesterification reaction, the equivalent ratio of terephthalic acid to ethylene glycol is in the range of 1:1.2 to 1:1.8, the reaction temperature is in the range of 200°C to 230°C, and the reaction time is in the range of 2 hours to 4 hours.

[0012] In one embodiment of the present invention, the amount of the side group ester compound added is in the range of 1 wt % to 5 wt % based on the total weight of bis-2-hydroxyethyl terephthalate.

[0013] In one embodiment of the present invention, during the prepolymerization reaction, the reactants include bis-2-hydroxyethyl terephthalate and polyethylene glycol, and the content of polyethylene glycol is in the range of 0.5 wt% to 4 wt% based on the total weight of bis-2-hydroxyethyl terephthalate, the reaction temperature is in the range of 230°C to 270°C, the degree of vacuum is in the range of 760 mmHg to 10 mmHg, and the reaction time is in the range of 1 hour to 2 hours.

[0014] In one embodiment of the present invention, a condensation polymerization reaction is carried out after the preliminary polymerization reaction, and during the condensation polymerization reaction, the reaction temperature is in the range of 260°C to 280°C, the degree of vacuum is in the range of 1 mmHg to 3 mmHg, and the reaction time is in the range of 2 hours to 4 hours.

[0015] The present invention provides a polyethylene terephthalate (PET) copolyester produced by the above-mentioned production method. Effect of the Invention

[0016] As described above, the present invention introduces a talc-containing dispersion slurry and a side group ester compound into the reaction process for producing PET copolyester. The talcum powder, which has a small particle size and a large specific surface area, is useful for inducing PET nucleation, so that the crystallization rate can be improved. In addition, the side group ester compound can increase the transparency and heat resistance and reduce the haze. The PET copolyester produced by the above method has fast crystallization and high crystallinity, so that the processing time of injection molding can be effectively reduced and its application can be expanded. In addition, the above production method can produce a PET copolyester with high transparency, low haze and excellent heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, embodiments of the present invention will be described in detail. However, these embodiments are merely illustrative and do not limit the present invention.

[0018] Here, ranges expressed as "one value to another value" are a summary method to avoid listing every value in the range in the specification. Thus, the description of a particular numerical range includes any value in that numerical range and smaller numerical ranges defined by any value in that numerical range, and is the same as if the any value and the smaller numerical range were specified in the specification.

[0019] The present invention provides a polyethylene terephthalate (PET) copolyester, which includes the following steps: Prepare a dispersion slurry containing talcum powder; Mix terephthalic acid and ethylene glycol to introduce the dispersion slurry and a side group ester compound, and carry out an ester exchange reaction to form bis-2-hydroxyethyl terephthalate; Then, carry out a prepolymerization reaction and a condensation polymerization reaction to form a polyethylene terephthalate copolyester. Each step will be described in detail below.

[0020] Preparation of dispersion slurry

[0021] In this embodiment, a dispersion slurry is prepared, and the dispersion slurry includes talcum powder, and further includes a dispersant and ethylene glycol (EG), but the present invention is not limited thereto. Here, the method of preparing the dispersion slurry includes, for example, mixing talcum powder, a dispersant, and ethylene glycol, and mixing the mixture at room temperature for 1 hour while applying ultrasonic vibration, but the present invention is not limited thereto.

[0022] Specifically, the talcum powder may be an ultrafine talcum powder and may be used as a nucleating agent. In some embodiments, the shape of the talcum powder may have an irregular or round granular structure, the average particle size may be in the range of 1 μm to 5 μm, and the average specific surface area may be less than 20 m 2 / g~12m 2 In some preferred embodiments, the average particle size of the talcum powder may be in the range of 1 μm to 2 μm, and the average specific surface area may be in the range of 20 m 2 / g~16m 2 / g range. Due to its small particle size and high specific surface area, talcum powder can accelerate the nucleation of PET, thereby increasing the crystallization rate of PET.

[0023] In some embodiments, the content of the talcum powder may be in the range of 1 wt% to 8 wt% based on the total weight of the dispersion slurry. In some preferred embodiments, the content of the talcum powder may be in the range of 1 wt% to 6 wt%. In some more preferred embodiments, the content of the talcum powder may be in the range of 1 wt% to 5 wt%. When the content of the talcum powder in the dispersion slurry is more than 8 wt%, the excess talcum powder is likely to cause talc accumulation. When the content of the talcum powder in the dispersion slurry is less than 1 wt%, the talcum powder content is too low, making it difficult to crystallize PET. When the content of the talcum powder is between 1 wt% and 5 wt%, the crystallization rate of PET can be significantly improved.

[0024] The dispersant may include a coupling agent containing a hydroxyl functional group for dispersing the components in the dispersion liquid (i.e., the dispersion slurry), such as a chelate titanium coupling agent such as hexyltrimethoxysilane or bis(octyl pyrophosphate)glycolic acid titanate. In some embodiments, the content of the dispersant may be in the range of 0.2 wt% to 2 wt% based on the total weight of the dispersion slurry. In some preferred embodiments, the content of the dispersant may be in the range of 0.3 wt% to 1.5 wt%. In some more preferred embodiments, the content of the dispersant may be in the range of 0.5 wt% to 1.0 wt%. When the content of the dispersant in the dispersion slurry is more than 2 wt%, the dispersion uniformity is poor and the reactivity of the condensation polymerization reaction of the copolymerized polyester is reduced. When the content of the dispersant in the dispersion slurry is less than 0.2 wt%, the content of the dispersant is so small that the components in the solution are not effectively dispersed, resulting in the phenomenon of accumulation. When the content of the dispersant is between 0.5wt% and 1.0wt%, an excellent dispersion effect can be achieved.

[0025] Transesterification

[0026] In this embodiment, terephthalic acid (PTA) and ethylene glycol (EG) are mixed, and the dispersion slurry and the side group ester compound are introduced to carry out an ester exchange reaction to form bis-2-hydroxylethyl terephthalate (BHET). The main reactants of the ester exchange reaction (i.e., the raw materials for synthesizing bis-2-hydroxyethyl terephthalate) include terephthalic acid and ethylene glycol, and the equivalent ratio of terephthalic acid to ethylene glycol may be in the range of 1:1.2 to 1:1.8, the reaction temperature may be in the range of 200°C to 230°C, and the reaction time may be in the range of 2 hours to 4 hours. When the reaction conditions are set as above, the esterification rate is about 90% to 96%, but the present invention is not limited thereto. The side group ester compound includes 2,6-naphthalene dicarboxylate. The side group ester compound can improve transparency and heat resistance and reduce haze, making it possible to produce a PET copolyester having high transparency, low haze and excellent heat resistance.

[0027] Specifically, in this step, the dispersion slurry and the side group ester compound can be further added to aid the nucleation and crystallization stages when forming PET. The amount of dispersion slurry added may be in the range of 2 wt% to 20 wt% based on the total weight of bis-2-hydroxyethyl terephthalate (BHET). That is, the amount of talcum powder added may be in the range of 0.1 wt% to 1 wt%, preferably in the range of 0.2 wt% to 0.8 wt%, and more preferably in the range of 0.3 wt% to 0.6 wt%. When the amount of talcum powder added is less than 0.1 wt%, the amount added is too small, so the talcum powder has no effect. When the amount of talcum powder added is more than 1.0 wt%, the nucleation rate is not significantly improved, and the excess talcum powder affects the reaction rate. When the amount of talcum powder (or dispersion slurry) added is within the above range, the crystallization time of PET can be effectively shortened and the crystallization rate can be increased.

[0028] In this embodiment, the amount of the side group ester compound added may be in the range of 1 wt% to 5 wt% based on the total weight of bis-2-hydroxyethyl terephthalate (BHET). When the amount of the side group ester compound added is less than 1 wt%, the injection appearance of the finished product becomes cloudy, and the improvement in heat resistance is unclear. When the amount of the side group ester compound added is more than 5 wt%, the heat distortion temperature of the modified polyester decreases. When the amount of the side group ester compound added is within the above range, the transparency and heat resistance can be improved and the haze can be reduced, so that a PET copolyester having high transparency, low haze, and excellent heat resistance can be produced.

[0029] Prepolymerization and Condensation Polymerization

[0030] Specifically, during the prepolymerization reaction, the reactants may include bis-2-hydroxyethyl terephthalate (BHET) and polyethylene glycol (PEG). The content of polyethylene glycol (PEG) may be in the range of 0.5wt%-4wt% (preferably 1wt%-4wt%) based on the total weight of bis-2-hydroxyethyl terephthalate (BHET), the reaction temperature may be in the range of 230°C-270°C, the degree of vacuum may be slowly lowered to 20Torr-10Torr (i.e. mmHg), and the reaction time may be in the range of 1 hour-2 hours.

[0031] After the preliminary polymerization reaction, a condensation polymerization reaction is carried out. In this embodiment, during the condensation polymerization reaction, the reaction temperature may be in the range of 260°C to 280°C, the vacuum degree may be in the range of 1 Torr to 3 Torr, and the reaction time may be in the range of 2 hours to 4 hours. More specifically, the reaction is completed when the stirring efficiency increases from 80 watts (w) to 110 watts. In this way, the production of the PET copolyester is completed.

[0032] Generally, the conventional PET injection processing has the following problems: (1) terephthalic acid and ethylene glycol are used as raw materials, but short-chain ethylene glycol does not have flexibility, so the crystallization power of PET is inhibited; (2) PET has a rigid structure with a high melting point, so high temperature is required during injection molding processing, and the product has high haze. Therefore, the application field of the conventional PET is limited. In the embodiment of the present invention, talc-containing dispersion slurry is added during polymerization, so that the small particle size and high specific surface area of ​​talcum powder are helpful in causing PET nucleation, thereby improving the crystallization rate. In addition, a side group ester compound is further added during polymerization, so that the transparency and heat resistance can be improved and the haze can be reduced, so that a PET copolyester with high transparency, low haze and excellent heat resistance can be produced. The PET copolyester produced by the above optimized process has the advantages of fast crystallization, shortened half-crystallization time, high crystallinity, high transparency, low haze, better heat resistance, and shortened injection molding processing time.

[0033] The PET copolyester of the present invention and its production method will be described in detail below using experimental examples, but the following experimental examples are not intended to limit the present invention.

[0034] Experimental Example

[0035] [Table 1]

[0036] As shown in Table 1, the Comparative Example does not use the naphthalene diacid ester and ultrafine talcum powder of the present invention, and therefore has a lower crystallization rate and transparency and a higher haze than Examples 1 to 5, which use the naphthalene diacid ester and ultrafine talcum powder of the present invention.

[0037] As described above, the present invention introduces a talc-containing dispersion slurry and a side group ester compound into the reaction process for producing a PET copolyester, and the talcum powder with a large specific surface area and small particle size can cause PET nucleation and improve the crystallization rate. In addition, the side group ester compound can increase transparency and heat resistance and reduce haze. The PET copolyester produced by the above method has fast crystallization and high crystallinity, which can effectively reduce the processing time of injection molding and expand its application. Meanwhile, the above production method can produce a PET copolyester with high transparency, low haze and excellent heat resistance.

[0038] As described above, the present invention has been disclosed by the embodiments, but the present invention is not intended to be limited thereto. As can be easily understood by those skilled in the art, appropriate changes and modifications can be made without departing from the spirit and scope of the present invention, and therefore the scope of patent protection should be determined based on the scope of the claims. [Industrial Applicability]

[0039] The present invention provides a polyethylene terephthalate (PET) copolyester, which has the advantages of fast crystallization rate and high crystallinity of PET polymer, and can effectively shorten the injection molding time and improve the transparency and heat resistance, and a method for producing the same.

Claims

1. preparing a dispersion slurry including talcum powder; Mixing terephthalic acid and ethylene glycol, introducing the dispersion slurry and an ester compound, and carrying out an ester exchange reaction to form bis-2-hydroxyethyl terephthalate; carrying out a prepolymerization reaction and a condensation polymerization reaction of the bis-2-hydroxyethyl terephthalate to form a polyethylene terephthalate (PET) copolyester; Including, the ester compound comprises 2,6-naphthalenedicarboxylate, The amount of the ester compound added is in the range of 1 wt % to 5 wt % based on the total weight of the bis-2-hydroxyethyl terephthalate, The method for producing a polyethylene terephthalate copolyester, wherein the talcum powder has an average particle size of 1.0 μm to 5.0 μm and an average specific surface area of ​​20 m 2 / g to 12 m 2 / g.

2. 2. The method according to claim 1, wherein the content of the talcum powder is in the range of 1 wt % to 8 wt % based on the total weight of the dispersion slurry.

3. 2. The manufacturing method according to claim 1, wherein the dispersion slurry further contains a dispersant and ethylene glycol, and the content of the dispersant is in the range of 99 wt % to 1 wt % based on the total weight of the dispersion slurry.

4. 2. The method according to claim 1, wherein the amount of the dispersion slurry added is in the range of 1 wt % to 6 wt % based on the total weight of the bis-2-hydroxyethyl terephthalate.

5. 2. The process according to claim 1, wherein during the transesterification reaction, the equivalent ratio of the terephthalic acid to the ethylene glycol is in the range of 1:1.2 to 1:1.8, the reaction temperature is in the range of 200° C. to 230° C., and the reaction time is in the range of 2 hours to 4 hours.

6. The method according to claim 1, wherein during the prepolymerization reaction, reactants include the bis-2-hydroxyethyl terephthalate and polyethylene glycol, the content of the polyethylene glycol is in the range of 0.5 wt % to 4 wt % based on the total weight of the bis-2-hydroxyethyl terephthalate, the reaction temperature is in the range of 230° C. to 270° C., the degree of vacuum is in the range of 760 mmHg to 10 mmHg, and the reaction time is in the range of 1 hour to 2 hours.

7. The method according to claim 1, wherein the condensation polymerization reaction is carried out after the preliminary polymerization reaction, and during the condensation polymerization reaction, the reaction temperature is in the range of 260°C to 280°C, the degree of vacuum is in the range of 1 mmHg to 3 mmHg, and the reaction time is in the range of 2 hours to 4 hours.

Citation Information

Patent Citations

  • Method for producing copolyester containing ethylene naphthalate unit

    JP2002226567A

  • Polyester resin composition for binder fiber and nonwoven fabric using the same

    JP2006169653A

  • Copolyester and polyester filling container produced therefrom

    JP2007314591A

  • Polyester direct blow molded article

    JP2009179654A