Steel wire and wire mesh
A steel wire with a specific composition and metal structure addresses the low tensile strength and energy absorption issues of existing nets, providing effective rockfall protection with minimal overhang and improved workability.
Patent Information
- Application Number
- JP2020118789
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-09
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-07-09
AI Technical Summary
Existing steel wires used in rockfall protection nets have low tensile strength and energy absorption capacity, leading to potential overhang and obstruction of traffic, and their manufacturing methods are complex and costly.
A steel wire composition with specific elements (C: 0.30-1.20%, Si: 0.10-1.50%, Mn: 0.10-1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0200% or less, O: 0.0070% or less, with a metal structure containing at least ferrite and cementite, and a fractal dimension of grain boundaries, achieving a tensile strength of 500-1200 MPa and absorbed energy of 1550 J/cm².
The steel wire exhibits high energy absorption performance with minimal overhang, ensuring effective rockfall protection and improved workability, while suppressing wire mesh extension when hit by falling rocks.
Smart Images

Figure 0007587106000008 
Figure 0007587106000009 
Figure 0007587106000010
Abstract
Description
[Technical field]
[0001] The present disclosure relates to steel wire and wire mesh. [Background technology]
[0002] For example, in mountainous areas, rockfall protection works are installed to prevent disasters caused by falling rocks on roads. Examples of rockfall protection works include waiting-type rockfall protection nets and rockfall protection fences that secure natural slopes. These rockfall protection works include wire mesh, and the material used for this wire mesh is generally Zn-plated steel wire, which is made by drawing, annealing, and plating a steel wire with a steel composition that contains almost no C. The material required for this wire mesh is high energy absorption performance to absorb the falling energy of falling rocks. In addition, when the protection works are installed in a position close to the road, even if the wire mesh does not break and the rock does not fly out when it catches a falling rock, if the wire mesh overhangs too far, it will hinder traffic. For this reason, it is desirable for the wire mesh of rockfall protection nets to also have the ability to absorb high energy with little elongation.
[0003] Generally, the energy absorption capacity is greatly affected by tensile strength and elongation. For steel wires, a technology has been proposed to control the structure and mechanical properties by combining wire drawing and heat treatment. For example, Patent Document 1 shows that hot-rolled wire rod is drawn and then spheroidized under specified conditions in a short period of time, thereby making it possible to spheroidize carbides to a degree comparable to that achieved by conventional methods. In addition, Patent Document 2 describes a method for reducing the absorbed energy to 1,300 J / cm by controlling the grain size of ferrite in the cross section to 9 μm or less and the amount of retained austenite to 8% or more in terms of area ratio. 2 The above steel wire is disclosed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 59-116330 [Patent Document 2] JP 2017-190515 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, although the steel wire disclosed in Patent Document 1 has the same ductility as that measured by the reduction in area compared to conventional methods, it has low tensile strength, and even if it is applied to wire mesh, it is thought that the absorbed energy of the wire mesh will be small. The steel wire disclosed in Patent Document 2 requires the area ratio of retained austenite to be 8% or more and ferrite to be refined to 9 μm or less, and therefore the manufacturing method is presumed to be complicated and costly. In addition, in the area where bending was performed during net manufacturing, the retained austenite may change structure, which may reduce its function as a rockfall protection structure.
[0006] The present disclosure aims to provide a steel wire and wire mesh that have high energy absorption performance and, when used, for example, as material for wire mesh in rockfall protection work, can suppress the protrusion of the wire mesh due to falling rocks. [Means for solving the problem]
[0007] The above object can be achieved by the following means. <1> The steel composition is, in mass%, C: 0.30-1.20%, Si: 0.10-1.50%, Mn: 0.10-1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0200% or less, and O: 0.0070% or less with the remainder being Fe and impurities; A steel wire having a metal structure including at least ferrite and cementite, in which in a cross section perpendicular to the longitudinal direction of the steel wire, the total area ratio of the ferrite, the cementite, and pearlite is 95.0% or more, and the grain boundaries of the ferrite grains have a fractal dimension of 1.20 to 1.95. <2> Instead of a part of the Fe, in mass%, Cr: 1.50% or less, B: 0.0050% or less, Ti: 0.040% or less, Mo: 0.40% or less V: 0.30% or less, Cu: 0.50% or less, Al: 0.080% or less, Ni: 0.50% or less, and Nb: 0.10% or less, Contains one or more selected from the group consisting of <1> The steel wire according to claim 1. <3> Instead of a part of the Fe, in mass%, Mg: 0.010% or less, Zr: 0.010% or less, Sb: 0.015% or less, W: 0.010% or less, REM (elements with atomic numbers 57 to 71): 0.005% or less Hf: 0.005% or less, Ta: 0.050% or less, Ca: 0.005% or less, Sn: 0.050% or less, Bi: 0.050% or less, Te: 0.050% or less, Zn: 0.050% or less, and Co:0.10% or less Contains one or more selected from the group consisting of <1> or <2> The steel wire according to claim 1. <4> The tensile strength in the tensile test is 500 to 1200 MPa, and the absorbed energy per unit cross-sectional area is 1600 J / cm 2 That's all. <1> ~ <3> 2. The steel wire according to claim 1 . <5> In the metal structure, when the radius of the steel wire is R, in a central region within a distance of 0.4 × R from the central axis of the cross section, the total area ratio of spherical cementite having an aspect ratio of 1.0 to 2.5, ferrite in which the spherical cementite is dispersed, and pearlite having a lamellar spacing of 0.3 μm or more is 70% or more. <1> ~ <4> 2. The steel wire according to claim 1 . <6> In the metal structure, when the radius of the steel wire is R, in a central region within a distance of 0.4×R from the central axis of the cross section, the total area ratio of pearlite and bainite having a lamellar spacing of less than 0.3 μm is 30.0% or less. <1> ~ <5> 2. The steel wire according to claim 1 . <7> In the metal structure, in a central region within a distance of 0.4×R from the central axis of the cross section, the area ratio of the spheroidal cementite having an aspect ratio of 1.0 to 2.5 and a major axis of 0.1 to 0.5 μm is 90.0% or more with respect to the spheroidal cementite having an aspect ratio of 1.0 to 2.5, where R is the radius of the steel wire. <1> ~ <6> 2. The steel wire according to claim 1 . <8> The breaking elongation in the tensile test is 10.0 to 30.0%, and the number of twists until breaking without longitudinal cracking in the torsion test is 25 or more. <1> ~ <7> 2. The steel wire according to claim 1 . <9> The yield ratio in the tensile test is 50.0 to 80.0%, and the reduction in area is 55.0% or more. <1> ~ <8> 2. The steel wire according to claim 1 . <10> Has a zinc-based plating layer on the surface <1> ~ <9> 2. The steel wire according to claim 1 . <11> For wire mesh <1> ~ <10> 2. The steel wire according to claim 1 . <12> <1> ~ <11> 1. A wire mesh manufactured using the steel wire according to any one of the preceding claims. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a steel wire and wire mesh that have high energy absorption performance and, for example, when used as a material for wire mesh in rockfall protection work, can suppress the protrusion of the wire mesh due to falling rocks. [Brief description of the drawings]
[0009] [Figure 1] This figure is an explanatory diagram for explaining how to calculate the fractal dimension, and shows the results of counting the number of sections (N) through which the grain boundary passes when the number of divisions (1 / L) is 3, 4, 6, and 8, for two cases in which the grain boundary has a simple shape and one in which it has a complex shape. [Diagram 2] FIG. 3 is an explanatory diagram for explaining how to determine the fractal dimension, and shows a method for counting the number of sections (N) through which the grain boundary passes when the number of divisions (1 / L) = 12 and 16 for two cases, one with a simple grain boundary shape and one with a complex grain boundary shape, and calculating the fractal dimension from the slope of the relationship between logL (number of divisions) and logN (number of sections through which the grain boundary passes) together with the counting results shown in FIG. [Diagram 3] FIG. 2 is a schematic diagram showing a central region for observing the metal structure in a cross section of a steel wire according to the present disclosure. [Figure 4] 1 is a SEM image showing an example of spheroidal cementite observed in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment that is an example of the present disclosure will be described in detail. In this specification, the "%" designation for the content of each element in a chemical composition means "mass %." The content of each element in a chemical composition is sometimes expressed as "amount." For example, the carbon content is sometimes expressed as the carbon amount. A numerical range expressed using "~" means a range that includes the numbers before and after "~" as the lower and upper limits. However, when the numbers before and after "~" are followed by "more than" or "less than," the numerical range does not include these numbers as the lower or upper limits. In the present specification, the upper limit of a certain numerical range may be replaced by the upper limit of another numerical range, and the lower limit of a certain numerical range may be replaced by the lower limit of another numerical range. The upper limit or lower limit may also be replaced by a value shown in the examples. The term "central axis" refers to an imaginary line that passes through the center point of a cross section (transverse cross section) perpendicular to the axial direction (longitudinal direction) of a steel wire and extends in the axial direction. The term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0011] The present inventors have carried out investigations to create a steel wire suitable as a component of a wire mesh for effectively absorbing the impact of falling rocks and the like. The carbon content of iron wire used in rockfall protection mesh is normally 0.1% or less, and it is generally annealed after drawing before use. However, this is done to soften the iron wire, whose bending workability has been reduced by the drawing, in preparation for the subsequent process of making mesh, and is not done to increase energy absorption capacity. On the other hand, in the field of high carbon steel wire, where high tensile strength is generally obtained by cold drawing, there is little need to go to the trouble of annealing high carbon steel wire, which has already achieved high tensile strength, to the trouble of spheroidizing annealing at the expense of annealing. Examples of steel products with a carbon content of 0.30% or more that include spheroidizing annealing in the manufacturing process include steel for bolts and steel for bearings. However, in both cases, this is done to ensure workability in subsequent forming processes such as cold forging, and is not intended to improve the energy absorption capacity of rockfall protection structures, etc. Therefore, the inventors of the present invention have conducted extensive research and found that a steel wire with high energy absorption capacity and capable of being used for wire mesh production can be obtained by controlling the steel components and metal structure, such as by including a C content equal to or greater than that of medium carbon steel. They also found that a diamond-shaped wire mesh can be obtained by using this steel wire to produce a diamond-shaped wire mesh that can reduce the overhang distance when absorbing falling rocks and effectively absorb impact energy, leading to the completion of the present disclosure.
[0012] Hereinafter, the steel wire according to the present disclosure will be described in detail. The steel wire according to the present disclosure comprises: The steel composition is, in mass%, C: 0.30-1.20%, Si: 0.10-1.50%, Mn: 0.10-1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0200% or less, and O: 0.0070% or less with the remainder being Fe and impurities; The metal structure includes at least the ferrite and the cementite, and in a cross section perpendicular to the longitudinal direction of the steel wire, the total area ratio of the ferrite, the cementite, and the pearlite is 95.0% or more, and the grain boundaries of the ferrite grains have a fractal dimension of 1.20 to 1.95.
[0013] [Steel composition] The steel composition of the steel wire according to the present disclosure will be described.
[0014] (C:0.30%~1.20%) C (carbon) is an essential element for imparting the necessary strength to steel materials. If the C content is less than 0.30%, the amount of cementite is small, making it difficult to obtain the metal structure specified in the present disclosure. In addition, this leads to a decrease in the tensile strength of the steel wire, and the energy absorption capacity decreases. Therefore, the C content is set to 0.30% or more. On the other hand, if the C content exceeds 1.20%, the tensile strength of the steel wire becomes excessively high, the net-making property decreases, and the breaking elongation decreases, resulting in a decrease in the energy absorption capacity when catching falling rocks. Therefore, the upper limit of the C content is set to 1.20%. The C content is preferably 0.60% or more and 1.15% or less, more preferably 0.80% or more and 1.10% or less, and even more preferably 0.90% or more and 1.08% or less.
[0015] (Si: 0.10 to 1.50%) Silicon (Si) is an element effective in deoxidizing steel, and also has the effect of suppressing the formation of pro-eutectoid cementite and strengthening ferrite. In order to effectively exert these effects, it is necessary to contain 0.10% or more of Si. However, if Si is contained in excess, these effects become saturated, so the upper limit of the Si content is set at 1.50%. The Si content is preferably 0.15% or more and 1.00% or less.
[0016] (Mn: 0.10-1.00%) Mn (manganese) is useful for deoxidization and desulfurization, and has the effect of delaying the transformation of proeutectoid cementite and grain boundary ferrite from austenite, and is a useful element for making the structure of wire rod mainly pearlite. In order to effectively exert such an effect, the Mn content needs to be 0.10% or more, preferably 0.20% or more, and more preferably 0.40% or more. On the other hand, even if Mn is contained excessively, the above effect is saturated and there is a possibility that workability is reduced due to segregation. Therefore, the upper limit of the Mn content is 1.00%, preferably 0.80% or less, and more preferably 0.60% or less.
[0017] (P:0.030% or less) Since P (phosphorus) is an impurity element that segregates at grain boundaries and embrittles steel, the upper limit of the P content is limited to 0.030%, preferably 0.020% or less, and more preferably 0.010% or less. Although the smaller the P content, the more preferable, from the viewpoint of reducing the dephosphorization cost, the lower limit of the P content may be 0.003% or may be 0.005%.
[0018] (S:0.030% or less) Since S (sulfur) is an impurity element that segregates at grain boundaries and embrittles steel, the upper limit of the S content is limited to 0.030%, preferably 0.020% or less, and more preferably 0.010% or less. Although the smaller the S content, the more preferable, from the viewpoint of reducing the desulfurization cost, the lower limit of the S content may be 0.003% or may be 0.005%.
[0019] (N:0.0200% or less) N (nitrogen) is an impurity element that dissolves in the ferritic matrix and embrittles the steel, and the upper limit is set to 0.0200%. The N content is preferably 0.0050% or less, and more preferably 0.0040% or less. Although there is no lower limit for the N content, from the viewpoint of reducing the denitrification cost, the lower limit for the N content may be 0.0010% or 0.0020%.
[0020] (O:0.0070% or less) O (oxygen) is an impurity element that affects the amount of oxide-based inclusions in steel wire. By making the O content 0.0070% or less, it is possible to suppress the decrease in absorbed energy caused by coarse oxides. It is preferably 0.0050% or less, and more preferably 0.0040% or less. Although there is no lower limit for the O content, from the viewpoint of reducing the de-O cost, the lower limit for the O content may be 0.0005% or 0.0010%.
[0021] The steel wire according to the present disclosure has the above elements as the basic components of the steel, and the balance is mainly Fe (iron). Here, "mainly Fe" means that the balance other than the basic components of the steel is Fe and impurities, or Fe, impurities, and optional components. That is, the steel composition of the steel wire according to the present disclosure may be composed of the above basic components, Fe, and impurities, or may actively contain one or more of the following optional elements (optional elements) in place of a portion of Fe, for the purpose of further improving strength, mesh-making properties, etc. However, the following optional elements are not essential, and the effect of the steel wire according to the present disclosure can be obtained even if they are not contained (i.e., even if the content is 0%). The impurities refer to substances that are mixed in from raw materials such as ore, scrap, or the manufacturing environment when industrially manufacturing a steel wire, and are acceptable within a range that does not adversely affect the steel wire according to the present disclosure (i.e., does not hinder the effects).
[0022] (Al: 0.080% or less) Although Al (aluminum) is not an essential component, it may be contained since it is useful as a deoxidizing element during steelmaking. When Al is contained, it has the effect of precipitating AlN and refining the ferrite matrix. However, when Al is contained in excess of 0.080%, coarse Al inclusions are generated, which may reduce ductility. Therefore, the upper limit when Al is contained is set to 0.080%. More preferably, it is 0.050% or less, and further preferably, it is 0.030% or less. The lower limit of the Al content is not particularly limited, but when Al is actively used as a deoxidizing element, it is preferably 0.005% or more, and more preferably, it is 0.010% or more. When Al is not utilized as a deoxidizing element, Al is contained within the range as an impurity, and the upper limit of the Al content may be less than 0.010%.
[0023] (Cr:1.50% or less) Cr (chromium) has the effect of delaying the transformation of proeutectoid cementite and grain boundary ferrite from austenite, similar to Mn, and is a useful element for obtaining a pearlite-based structure in the rolled wire rod before wire drawing to obtain the steel wire according to the present disclosure. In addition, Cr stabilizes cementite, and is expected to have the effect of moderately assisting spheroidization during annealing. However, if the Cr content exceeds 1.50%, these effects are saturated, and the hardenability is increased, and supercooled structures such as bainite and martensite are likely to occur during the cooling process during hot rolling, and the time until the transformation is completed is long, leading to a decrease in productivity and an increase in equipment costs. The Cr content is preferably 0.05% or more and 0.30% or less, and more preferably 0.10% or more and 0.25% or less.
[0024] (B:0.0050% or less) B (boron) strengthens the grain boundary strength and suppresses the precipitation of grain boundary ferrite when added in small amounts. However, if the B content exceeds 0.0050%, the Fe 23B forms carbides such as (CB)6, which becomes a factor of inhibiting grain boundary bonding. Therefore, when B is contained, the B content is preferably 0.0050% or less. The B content is more preferably 0.0005 to 0.0030%, and further preferably 0.0008 to 0.0020%.
[0025] (Ti:0.040% or less) Ti (titanium) forms TiN in steel, fixes N, and has the effect of preventing strain aging. However, if Ti is contained in excess of 0.040%, coarse TiN may be formed in the steel, adversely affecting the material quality. Therefore, it is effective to contain Ti at 0.040% or less. The Ti content is more preferably 0.005 to 0.030%, and further preferably 0.008 to 0.020%.
[0026] (Mo: 0.40% or less) An appropriate content of Mo (molybdenum) improves hardenability, reduces the ferrite fraction, and promotes the grain boundary strengthening by B. However, if the Mo content exceeds 0.40%, the hardenability of the steel becomes too high, and an undercooled structure such as martensite is formed in the steel during the cooling process during hot rolling, adversely affecting wire drawability. Therefore, it is effective to include Mo at 0.40% or less. The Mo content is more preferably 0.05 to 0.20%, and further preferably 0.07 to 0.10%.
[0027] (V:0.30% or less) Vanadium (V) has the effect of increasing the strength of ferrite, but if the content exceeds 0.30%, it becomes embrittled. Therefore, when V is contained, it is effective to set the upper limit of the V content to 0.30%. The V content is more preferably 0.05 to 0.30%, and further preferably 0.07 to 0.15%.
[0028] (Cu:0.50% or less) Although Cu (copper) has the effect of dissolving in ferrite to strengthen steel, if it is contained in an amount exceeding 0.50%, it will concentrate at the grain boundaries during heating of the slab, embrittling the steel. Therefore, when Cu is contained, it is effective to set the upper limit of the Cu content to 0.50%. The Cu content is more preferably 0.02 to 0.30%, and further preferably 0.03 to 0.20%.
[0029] (Ni:0.50% or less) Ni (nickel) has a solid solution strengthening effect, but the effect tends to saturate at 0.50%. Therefore, when Ni is contained, it is effective to set the upper limit to 0.50%. The Ni content is more preferably 0.01 to 0.30%, and further preferably 0.03 to 0.20%.
[0030] (Nb:0.10% or less) Nb (niobium) precipitates in steel as fine carbides and has the effect of strengthening ferrite, but if the content exceeds 0.10%, it embrittles the steel. Therefore, it is effective to set the upper limit of the N content to 0.10%. The Nb content is more preferably 0.02 to 0.07%, and further preferably 0.03 to 0.05%.
[0031] The steel wire according to the present disclosure is composed of the above-mentioned basic components and optional elements, but may further contain the following elements: The effects of the present disclosure can be obtained even if one or more of the following elements are contained: Mg 0.010% or less, Zr 0.010% or less, Sb 0.015% or less, W 0.010% or less, REM (elements with atomic numbers 57 to 71) 0.005% or less, Hf 0.005% or less, Ta 0.050% or less, Ca 0.005% or less, Sn 0.050% or less, Bi 0.050% or less, Te 0.050% or less, Zn 0.050% or less, and Co 0.10% or less.
[0032] [Metal structure] Next, the metal structure of the steel wire according to the present disclosure will be described. The present inventors manufactured various steel wires by changing the amount of cold drawing and annealing conditions using the above-mentioned steel material having a C content of 0.30% or more, and conducted a detailed study on the relationship between the structure and mechanical properties of the steel wires, and obtained the following findings. In order to obtain a steel wire that has the ability to be formed into wire mesh and also has excellent energy absorption capabilities when catching falling rocks, it is appropriate to use steel with the above-mentioned components, and the desired performance can be obtained by controlling the shape of the ferrite grain size and the morphology of the carbides.
[0033] The metal structure of the steel wire according to the present disclosure includes at least ferrite and cementite, and may further include pearlite and / or bainite. The above "ferrite" excludes the ferrite phase contained in pearlite or bainite, but does not matter whether or not cementite is present within the grains. For example, when the cementite phase precipitated as part of pearlite or bainite is spheroidized by annealing and the spheroidized cementite is dispersed in the ferrite matrix, the ferrite matrix is included in the above ferrite. The above-mentioned "cementite" refers to cementite other than the cementite phase precipitated as part of pearlite or bainite, and the shape is not limited, and refers to cementite of various shapes such as spherical, plate-like, etc. For example, there are spheroidal cementite in which the cementite phase contained in pearlite, the cementite phase contained in bainite, or pro-eutectoid cementite is spheroidized by annealing, and plate-like cementite that is not in a lamellar state and is austenitized during annealing and then generated in the cooling process. In the steel wire according to the present disclosure, the total area ratio of ferrite, cementite, and pearlite in a cross section perpendicular to the longitudinal direction is 95.0% or more. If the total area ratio of such structures is less than 95.0%, the elongation of the steel wire decreases, and the energy absorption capacity decreases.
[0034] (Fractal dimension of grain boundaries of ferrite grains) Next, the reason for specifying the boundaries of the ferrite grain boundaries will be described. In the steel wire of the present disclosure, the boundaries of the ferrite grain boundaries have a fractal dimension of 1.20 to 1.95. In the steel wire of the present disclosure, the shape of the boundary line of the ferrite grain boundary has an important meaning. The ferrite grain boundary plays an important role in balancing plastic deformability (ductility) and strength at a high level. When the degree of unevenness of the ferrite grain boundary becomes complex, it has the effect of ensuring ductility without reducing the strength of the steel material, and in the present disclosure, the degree of complexity of the grain boundary is expressed by the fractal dimension. If the fractal dimension of the ferrite grain boundary is 1.20 to 1.95, the energy absorption capacity per unit cross-sectional area is 1550 J / cm. 2 As a result, the properties required for a diamond-shaped wire mesh are satisfied. The fractal dimension of the ferrite grain boundary is more preferably in the range of 1.40 to 1.80.
[0035] In addition to the above-mentioned structure, by controlling the morphology of the carbide (cementite), it is possible to obtain a steel wire that has the ability to be formed into wire mesh and also has excellent energy absorption capacity when catching falling rocks. (a) The balance between the strength, ductility, and absorbed energy of a steel wire depends on the morphology and quantitative ratio of carbides in a portion near the center on a cross section perpendicular to the longitudinal direction of the steel wire. (b) The spheroidal cementite in the above-mentioned portion effectively increases the fracture elongation and reduction in area when the aspect ratio is small. In particular, when the spheroidal cementite is fine, the effect is remarkable. (c) When the pearlite in the above-mentioned region is divided into those having lamellar spacings of 0.3 μm or more and those having lamellar spacings of less than 0.3 μm, if the ratio of the cementite in the pearlite having lamellar spacings of 0.3 μm or more to the total cementite is large, the fracture elongation and reduction in area become large, and as a result, the absorbed energy also becomes large. A preferred metal structure for obtaining a steel wire having both mesh-making properties and excellent energy absorption capacity when catching falling rocks will be described below.
[0036] FIG. 3 is a schematic diagram showing a central region M for observing the metal structure of the steel wire 10 according to the present disclosure. The steel wire according to the present disclosure is manufactured by using a rolled wire material and going through a process of wire drawing-annealing or wire drawing-annealing-plating. In either case, when the radius of the steel wire is R, the steel wire according to the present disclosure is preferably configured such that the metal structure of the central region M within a distance of 0.4×R from the central axis in a cross section perpendicular to the longitudinal direction (axial direction) of the steel wire 10 is composed of spheroidal cementite and ferrite, and may further include pearlite and / or bainite. The spheroidal cementite may be any one of pearlite, pro-eutectoid cementite, and bainite in structure before spheroidization. In the present disclosure, "pearlite" refers to a layered structure (lamellar structure) of cementite and ferrite. "Spherical cementite" refers to cementite in which cementite is dispersed in a granular form in a ferrite matrix, and typically has an aspect ratio in the range of 1.0 to 2.5, but also includes cementite with an aspect ratio exceeding 2.5. In the measurement method described later, when two or more pieces of spheroidal cementite are connected, the cementite is divided at the constricted portion to measure the aspect ratio. Regarding the presence or absence of a constricted portion, if the thickness of the cementite is thin except at both ends and is less than half the thickness of the nearby maximum thickness, it is determined that a constricted portion is present and multiple pieces of spheroidal cementite are connected, and the cementite is divided at the constricted portion to measure the aspect ratio of each piece of spheroidal cementite. Bainite is a mixed structure of ferrite and cementite that contains more dislocations than normal ferrite, and does not belong to either lamellar pearlite or a structure in which spheroidal cementite is dispersed in a ferrite matrix.
[0037] Hereinafter, a preferred metal structure observed in a central region within a distance of 0.4×R from the central axis in a cross section perpendicular to the longitudinal direction of the steel wire, where R is the radius of the steel wire, will be described.
[0038] (Spherical cementite with an aspect ratio of 1.0 to 2.5, ferrite with the spherical cementite dispersed therein, and pearlite with lamellar spacing of 0.30 μm or more) In the central region of the steel wire according to the present disclosure, the cementite is mainly spheroidal cementite having an aspect ratio of 1.0 to 2.5 obtained by spheroidizing pearlite, pro-eutectoid cementite, or bainite, and all of the spheroidal cementite may be spheroidal cementite having an aspect ratio of 1.0 to 2.5. The aspect ratio of the spheroidal cementite means the value obtained by dividing the major axis by the minor axis (i.e., major axis / minor axis). Here, the major axis of the spheroidal cementite means the maximum length of the spheroidal cementite, and the minor axis of the spheroidal cementite means the maximum length in the direction perpendicular to the major axis direction. The total area ratio of the spherical cementite having an aspect ratio of 1.0 to 2.5, the ferrite in which the spherical cementite is dispersed, and the pearlite having a lamellar spacing of 0.30 μm or more is preferably 70.0% or more. If the total area ratio of the spherical cementite having an aspect ratio of 1.0 to 2.5, the ferrite in which the spherical cementite is dispersed, and the pearlite having a lamellar spacing of 0.30 μm or more is 80.0% or more, the strength is reduced and the elongation is increased, so that the absorbed energy ability is improved, which is more preferable. The total area ratio is more preferably 83.0% or more, and particularly preferably 85.0% or more.
[0039] (The ratio of spheroidal cementite with a major axis of 0.1 to 0.5 μm among spheroidal cementite with an aspect ratio of 1.0 to 2.5) In addition, the spherical cementite having an aspect ratio of 1.0 to 2.5 preferably has a major axis in the range of 0.1 to 0.5 μm, and the area ratio of the spherical cementite having a major axis of 0.1 to 0.5 μm is preferably 90.0% or more, more preferably 92.0% or more, relative to the total spherical cementite having an aspect ratio of 1.0 to 2.5. If there is a small amount of spherical cementite having a major axis of less than 0.1 μm, the increase in strength and yield ratio is suppressed, and elongation and workability tend to be improved. On the other hand, if there is a small amount of spherical cementite having a major axis of more than 0.5 μm, while the tensile strength and absorbed energy are high, the elongation is small, and the overhang distance when a wire mesh made of the steel wire according to the present disclosure receives a falling rock tends to be small.
[0040] (Total area ratio of pearlite and bainite with lamellar spacing less than 0.30 μm) The total area of pearlite and bainite with lamellar spacing of less than 0.30 μm is preferably 30.0% or less of the total area of the observation field. When the total area ratio of pearlite and bainite with lamellar spacing of less than 0.30 μm is 30.0% or less, the tensile strength decreases, but the elongation improves and the energy absorption capacity also improves. The total area ratio of pearlite and bainite with lamellar spacing of less than 0.30 μm is more preferably 25% or less, and particularly preferably 20% or less. The area ratio of pearlite having a lamellar spacing of less than 0.30 μm is preferably 20.0% or less, and more preferably 10.0% or less.
[0041] (Method of measuring metal structure) Observation of the metal structure of the steel wire and measurement of the area ratio of the structure can be performed as follows. In order to be able to observe the cross section perpendicular to the longitudinal direction of the steel wire, the steel wire is cut, embedded in resin, polished with polishing paper or alumina abrasive grains, and mirror-finished to prepare a specimen. This mirror-finished part is corroded for 5 seconds in a 3% picral solution at room temperature, and then immediately washed with alcohol to prepare an observation specimen. If the boundary between the ferrite and carbide (cementite) is unclear after the corrosion, an additional 5 seconds of corrosion may be performed. The corroded portion of the specimen is observed and photographed using a field emission scanning electron microscope (FE-SEM). Photographs are taken at 2000x magnification for a total of eight visual fields, two of which are centered on the line passing through the center of the steel wire, at 0.1×R, 0.2×R, 0.3×R, and 0.4×R (R is the radius of the steel wire) from the center. The total observation area is 2400 μm 2 Using the photograph taken above, draw five straight lines vertically and horizontally at 10 μm intervals, dividing the area into 25 intersection points.
[0042] -Method to distinguish between cementite-containing structures and ferrite- Based on the cementite present at each intersection (spheroidal cementite, lamellar cementite, or cementite other than spherical cementite and lamellar cementite), the intersection is judged to be a structure containing cementite. When no cementite is present at the intersection, the intersection is judged to be a structure containing cementite based on the cementite closest to the intersection. Examples of the "structure containing cementite" include pearlite and bainite, as well as a structure in which the above-mentioned spherical cementite is dispersed in a ferrite matrix, and plate-like cementite that is not in a lamellar state. When no cementite is present at the intersection and no cementite is present within a 10 μm square drawn vertically and horizontally from the intersection, the intersection is judged to be a structure such as ferrite, martensite, etc., based on the structure present therein. The total area of the "ferrite structure" and the structures other than bainite among the "structures containing cementite" is defined as the "total area of ferrite, cementite, and pearlite."
[0043] (A) Measurement of the area ratio of a structure containing spheroidal cementite having an aspect ratio of 1.0 to 2.5 and ferrite in which the spheroidal cementite is dispersed, and the area ratio of pearlite having a lamellar spacing of 0.3 μm or more The number of intersections where the cementite present at or closest to the intersections is spheroidal cementite with an aspect ratio of 1.0 to 2.5, and the number of intersections where the cementite is coarse lamellar cementite with a lamellar spacing of 0.3 μm or more are counted. On the other hand, if the cementite present at or closest to each intersection is spheroidal cementite with an aspect ratio of more than 2.5, lamellar cementite with a lamellar spacing of less than 0.3 μm, or cementite other than spheroidal cementite and lamellar cementite, it is not included in the above count. The ratio of the number of measured intersections where the cementite present at each intersection or closest to each intersection is spheroidal cementite with an aspect ratio of 1.0 to 2.5 out of the total number of measurement points (200 points) is defined as the area ratio of a structure containing spheroidal cementite with an aspect ratio of 1.0 to 2.5 and ferrite in which the spheroidal cementite is dispersed, and the ratio of the number of measured intersections where the cementite present at each intersection or closest to each intersection is coarse lamellar cementite with a lamellar spacing of 0.3 μm or more is defined as the area ratio of pearlite structure with a lamellar spacing of 0.3 μm or more (sometimes referred to as "coarse lamellar pearlite" in this disclosure).
[0044] (B) Measurement of the area ratio of pearlite and bainite with lamellar spacing less than 0.3 μm Observation and measurement are performed in the same manner as above, and the ratio of the number of intersections of lamellar cementite with a lamellar spacing of less than 0.3 μm to all measured points is defined as the area ratio to the total observed area of pearlite structure with a lamellar spacing of less than 0.3 μm, and the ratio of the number of intersections of bainite cementite to all measured points is defined as the area ratio to the total observed area of bainite structure.
[0045] (C) Measurement of area ratio of other tissues The ratio of the number of intersections of cementite other than (A) and (B) and intersections not containing cementite within a 10 μm square centered on the intersections is defined as the area ratio to the total observation area of other structures. Examples of other structures include ferrite with dispersed cementite having an aspect ratio of more than 2.5, and ferrite and martensite with no dispersed cementite.
[0046] (D) Measurement of the area ratio of spheroidal cementite having an aspect ratio of 1.0 to 2.5 and a major axis of 0.1 to 0.5 μm to spheroidal cementite having an aspect ratio of 1.0 to 2.5 The captured SEM images can be binarized using image analysis software to measure the carbide shape and area. The measurement items are a) the total area of spheroidal cementite with an aspect ratio of 1.0 to 2.5, and b) the total area of spheroidal cementite with an aspect ratio of 1.0 to 2.5 and a major axis of 0.1 to 0.5 μm. b / a is defined as the area ratio of spheroidal cementite having an aspect ratio of 1.0 to 2.5 and a major axis of 0.1 to 0.5 μm to the spheroidal cementite having an aspect ratio of 1.0 to 2.5.
[0047] (Method of measuring fractal dimension of ferrite grains) Fractal dimension is geometrically quantified by calculation using the method shown in Figures 1 and 2, and always takes a value in the range of 1.00 to 2.00. A larger fractal dimension value indicates that the boundaries of the ferrite grain boundaries are more intricate and complex. First, a diagram tracing ferrite grain boundaries in the metal structure of the steel wire is obtained. A backscatter diffraction (EBSD) device is used to observe the ferrite grain boundaries. The cross section of the obtained steel wire is embedded in resin, polished with alumina and colloidal silica to remove distortion, and then used for measurement. Note that polishing can also be done by electrolytic polishing. The measurement locations were within an area of D / 8 to 3D / 8 depth from the surface (outer periphery) on the cross section of the steel wire. In order to suppress the variation in structure due to location, images were taken at five locations within the above-mentioned area. The measurements were taken at a magnification of 1000x, and a ferrite crystal orientation data map was collected from the photographed area at 0.2μm / step. Ferrite grains were defined as those with a crystal orientation difference of 15° or less and connected by 15 pixels or more, and the grain boundaries were determined. The measurement area (area) at each location for evaluating the fractal dimension was 10,800μm per field of view at a magnification of 1000x. 2 (90μm vertical × 120μm horizontal), 2 horizontal × 2 vertical fields (total of 4 fields) connected together (measurement field area: 43200μm 2 ) which corresponds to a 500x magnification in the field of view of a normal optical microscope. In order to evaluate the fractal dimension, the minimum magnification of the photograph required to obtain sufficient resolution of the grain boundary lines is approximately 500x. Note that there are no limitations on the structure in which the ferrite grains to be measured exist, and ferrite grains existing in any structure, such as ferrite, pearlite, or bainite, may be used. Next, each point is superimposed on the area divided into grids, and the number of divisions (1 / L) is made finer, such as 3, 4, 6, 8, 12, 16, etc., as shown in Figures 1 and 2. Then, the number of grids (rectangles) (N) through which the line diagram representing the grain boundary passes is counted. Finally, as shown in the graph in Figure 2(G), the common logarithm of the inverse of the number of divisions is plotted on the horizontal axis and the common logarithm of the number of grids through which the grain boundary passes on the vertical axis, and the slope of the line connecting the plotted points is found using the least squares method. The absolute value of the slope of this line is the fractal dimension. The fractal dimension is measured at each point, and a total of five fractal dimension values are obtained, and their average value is taken as the fractal dimension of the entire structure.
[0048] [Mechanical properties] The mechanical properties of the steel wire according to the present disclosure are preferably a tensile strength of 500 to 1200 MPa and an absorbed energy per unit cross-sectional area of 1550 J / cm 2 More preferably, 1600 J / cm 2 By having such mechanical properties, the material has particularly high energy absorption performance and excellent workability, and when used in wire mesh, it is possible to suppress overhang when hit by falling rocks. Moreover, the mechanical properties of the steel wire according to the present disclosure are preferably such that the breaking elongation in a tensile test is 10.0 to 30.0%, and the number of twists until breaking in a torsion test is 25 or more without the occurrence of longitudinal cracks. Furthermore, the mechanical properties of the steel wire according to the present disclosure are preferably such that in a tensile test, the yield ratio is 50.0 to 80.0% and the reduction in area is 55.0% or more. Each mechanical property and its measurement method will be described below.
[0049] (Tensile strength) The steel wire according to the present disclosure preferably has a tensile strength of 500 to 1200 MPa. If the tensile strength is 500 MPa or more, the strength is high, so that the absorbed energy is high and the overhang distance can be kept short when using a wire net to protect against falling rocks. On the other hand, if the tensile strength is 1200 MPa or less, the elongation becomes large, and the energy absorption capacity of the plated wire or wire mesh improves. When the C content (mass %) of the steel wire according to the present disclosure is defined as the "C amount", the tensile strength TS (MPa) is preferably in the range of the following formula (1). More preferably, it is in the range of the following formula (2). 275 × C amount + 450 < TS < 600 × C amount + 470 ··· Formula (1) 300 × C amount + 450 < TS < 550 × C amount + 470 ··· Formula (2)
[0050] (Absorbed energy) The absorbed energy per unit area in the tensile test of the steel wire according to the present disclosure is not limited, but is preferably 1550 J / cm 2 or more, more preferably 1600 J / cm 2 or more. When the absorbed energy is 1550 J / cm 2 or more, the overhang when a falling rock hits the wire mesh made using the steel wire according to the present disclosure can be more effectively suppressed. The absorbed energy per unit area of the steel wire according to the present disclosure is more preferably 1700 J / cm 2 or more, and even more preferably 1800 J / cm 2 or more.
[0051] (Elongation at break) The elongation at break in the tensile test of the steel wire according to the present disclosure is preferably 10.0 to 30.0%. If the elongation at break is 10.0% or more, the absorbed energy capacity of the plated steel wire increases, and the absorbed energy in the wire mesh also improves. On the other hand, by setting the elongation at break to 30.0% or less, the overhang distance becomes smaller when protecting against falling rocks with the wire mesh. The elongation at break is determined from the length between the chucks before the test and the length between the chucks at the time of break in the tensile test described below. The elongation at break is preferably 13.0% or more, and even more preferably 15.0% or more.
[0052] (Number of torsions) In the torsion test, the steel wire according to the present disclosure is preferably twisted 25 times or more without longitudinal cracks until breakage. If the number of twists until breakage without longitudinal cracks is 25 times or more, the decrease in absorbed energy during wire mesh formation can be effectively suppressed. In the torsion test, the number of twists until breakage without longitudinal cracks is preferably 28 times or more, and more preferably 30 times or more. On the other hand, there is no upper limit to the number of twists until breakage, but the upper limit is thought to be about 60 times.
[0053] (yield ratio) The steel wire according to the present disclosure preferably has a yield ratio of 50.0 to 80.0% in a tensile test. If the yield ratio is 50.0% or more, the wire is less likely to deform under a small load and elongation is suppressed, so that the overhang distance of a wire mesh made from the steel wire according to the present disclosure when it receives a falling rock is small. On the other hand, if the yield ratio is 80.0% or less, the work hardening rate is high, and the energy absorption capacity is high, as well as the workability during mesh making is high. The yield ratio is more preferably 60.0% to 75.0%.
[0054] (Aperture) The steel wire according to the present disclosure preferably has a reduction in area of 55.0% or more in a tensile test. If the reduction in area is 55.0% or more, the wire is less likely to deform under a small load and elongation is suppressed, so that the overhang distance when a wire mesh made from the steel wire according to the present disclosure receives a falling rock is reduced. The reduction in area is more preferably 58.0% or more, and further preferably 60.0% or more.
[0055] (Tensile test method) In measuring the above mechanical properties of the steel wire according to the present disclosure, a tensile test is carried out in the following manner. A 200mm long sample is taken from the steel wire to be measured, excluding the non-steady-state portion, and used for the tensile test. The tensile test is performed with a chuck distance of 100mm and a strain rate of 10 / s. The same test is performed three times, and the average is taken as each measured value. If the fracture occurs in the chuck portion during the tensile test, the test result is not included and the measurement is performed again. The absorbed energy per unit area is evaluated by calculating the area enclosed by the strain-stress curve up to break during the tensile test (the value obtained by integrating the change in load as the crosshead moves up to break by the amount of crosshead movement) and dividing this by the cross-sectional area of the steel wire before the test. The tensile strength, yield ratio, elongation at break, and reduction in area are also determined by the above tensile test.
[0056] (Torsion test method) In the measurement of the mechanical properties of the steel wire according to the present disclosure, the torsion test is performed according to the method described in JIS G 3548:2011. Specifically, a sample having a length that allows a gripping interval of 100 times the diameter of the steel wire is taken from the steel wire to be measured, excluding the non-steady portion, and used for the test. The sample is straightened using a roll or the like so as not to scratch the surface, and then both ends of the sample are gripped at an interval of 100 times the diameter of the steel wire, a load of 1% of the tensile strength is applied to the sample, and the sample is rotated in the same direction while being tensioned until one side breaks. The number of rotations at the time of breakage is the number of twisting rotations until breakage. The presence or absence of vertical cracks is judged by observing the fracture surface after breakage and the presence or absence of cracks perpendicular to the wire axis on the fracture surface. If multiple fractures occur, all fracture surfaces are observed, and if there is at least one fracture surface without vertical cracks, it is judged to be "fractured without vertical cracks."
[0057] [Steel wire diameter] The diameter (wire diameter) of the steel wire according to the present disclosure is not particularly limited, but if the wire diameter of the steel wire is too thick, there are problems such as difficulty in net making and increased weight, while if the wire diameter of the steel wire is too thin, the energy absorption capacity decreases. Therefore, the diameter of the steel wire according to the present disclosure is preferably in the range of 2.0 to 6.0 mm, and more preferably in the range of 3.0 to 5.0 mm.
[0058] [Steel wire manufacturing method] Next, a method for producing the steel wire according to the present disclosure will be described. Note that the production method described below is an example, and is not limited to the following procedure and method, and any method may be adopted as long as it can realize the configuration of the steel wire according to the present disclosure. The steel wire according to the present disclosure can be obtained by forming a steel billet, the composition of which has been adjusted to the above-mentioned steel composition, into a wire rod by hot rolling or the like, and then performing wire drawing, annealing, and, if necessary, zinc (Zn)-based plating.
[0059] The wire rod may be produced under normal hot rolling conditions. For example, the steel having the above-mentioned composition is cast, and the cast piece is bloomed to produce a steel piece having a size suitable for wire rod rolling (a steel piece before wire rod rolling, generally called a billet), which is then subjected to hot rolling. When rolling the wire rod, the steel slab is heated to 950 to 1150° C., and the finish rolling start temperature is controlled to 800° C. or more and 950° C. or less. The rolling temperature of the wire rod is measured by a radiation thermometer, and means the surface temperature of the steel material.
[0060] It is desirable that the structure of the wire rod is mainly composed of pearlite in the wire rod having a C content equal to or greater than that of eutectoid steel, and that the structure of the wire rod is mainly composed of ferrite-pearlite in the wire rod having a C content less than that of eutectoid steel. A high area ratio of pearlite is desirable, and in wire rods having a C content less than that of eutectoid steel, the area ratio of pearlite is desirably (C content: mass %+0.1)×100% or more. In wire rods having a C content equal to or greater than that of eutectoid steel, the area ratio of pearlite is desirably 90% or more, and the total area ratio of grain boundary ferrite, pro-eutectoid cementite, bainite, and martensite is desirably 10% or less. To obtain these structures, the coiling temperature of the rolled material is set to 800°C or higher, and the average cooling rate from coiling to 620°C is set to 5.0°C / s or higher. Thereafter, the cooling rate from 620 to 550°C is set to 10.0°C / s or lower. On the other hand, if the cooling rate is too slow, the cementite will be broken up and spheroidized, so the cooling rate is preferably 0.5°C / s or higher.
[0061] The wire rod is drawn to a predetermined wire diameter by dry wire drawing. At that time, the area reduction rate in one pass is preferably 30% or less, and the total amount of strain is preferably in the range of 0.4 to 2.0 in true strain. If the area reduction rate in one pass exceeds 30%, the possibility of wire breakage during drawing increases. This tendency is particularly strong when the C content is high, so the area reduction rate in one pass is preferably 25% or less. Furthermore, if the total true strain in the wire drawing process is less than 0.4, it is difficult to obtain favorable microstructure and mechanical properties during the subsequent annealing, and the elongation and energy absorption capacity are reduced. On the other hand, the total true strain in the wire drawing process may be more than 2.0, but the effect of introducing strain to spheroidize cementite after wire drawing is saturated, and considering the handling of the steel wire and the load of the wire drawing work due to wire drawing strain, the strain should be about 2.0 or less. The true strain can be calculated from the formula -2 x ln (wire diameter of drawn wire material / wire diameter of wire material). "ln" is the natural logarithm.
[0062] Annealing is carried out by a normal industrial method. Annealing is preferably carried out in an atmosphere furnace or a fluidized bed furnace in which the atmosphere is controlled. Annealing is carried out by heating to a heating temperature T point (650 to 800°C) within 60 s (s: seconds). Annealing varies depending on the amount of C and the holding temperature, and is preferably carried out under conditions that satisfy the following (A). 5700≦(T+273)×(log(s / 3600)+8-0.6×C)≦6200 …(A) Here, T is the holding temperature (°C), s is the holding time at temperature T (seconds), and C is the amount of C (%). However, the method is not limited to the above, and for example, annealing at 1000°C in an atmospheric furnace can also be used as long as the steel wire specified in the present disclosure can be obtained.
[0063] [Zinc-plated steel wire] The steel wire according to the present disclosure may be zinc-based plated. That is, the zinc-based plated steel wire according to the present disclosure has a zinc-based plating layer that coats the surface of the steel wire. The zinc-based plating may be either hot-dip plating or electroplating. The thickness of the zinc-based plating layer is not particularly limited, but if the thickness of the plating layer is less than 3 μm, the sacrificial anticorrosive effect may be insufficient, so a layer thickness of 3 μm or more is preferable. On the other hand, even if the thickness of the zinc-based plating layer is made thicker than 70 μm, the effect is substantially saturated and it becomes uneconomical, so a layer thickness of 70 μm or less is preferable. Therefore, the thickness of the zinc-based plating layer is preferably in the range of 3 μm to 70 μm. The zinc-based plating is a plating mainly composed of Zn, and may be an alloy plating containing other components. The other components are, for example, Al and Mg. The preferred range of the Al content in the zinc-based plating layer is 0 to 25 mass %, and the preferred range of the Mg content is 0 to 3 mass %.
[0064] By using the steel composition of the present disclosure and adjusting the production conditions as described above, the metal structure of the steel wire can be within the range of the present disclosure.
[0065] [Application] The steel wire according to the present disclosure can be used for any purpose, including as a material for wire mesh, bridge wire, concrete reinforcing wire, guard wire used to prevent highways and bridge girders from falling, and is particularly suitable for manufacturing wire mesh for rockfall protection nets. That is, if a wire mesh manufactured using the steel wire or zinc-plated steel wire according to the present disclosure is used as a wire mesh for rockfall protection nets, it will have low elongation and high energy absorption performance when a falling rock is received, and the wire mesh will be prevented from protruding toward the road. EXAMPLES
[0066] Hereinafter, the steel wire according to the present disclosure will be described in more detail with reference to examples of the steel wire according to the present disclosure. However, the present disclosure is not limited to the following examples, and may be modified within the scope of the purpose described above and below, and all such modifications are included in the technical scope of the present disclosure. Tables 1A and 1B show the steel composition, Tables 2A and 2B show the hot rolling conditions, wire rod structure evaluation, wire drawing and heat treatment conditions, and Tables 3A and 3B show the steel wire structure evaluation, tensile test evaluation and absorbed energy properties. The cooling rate A1, the cooling rate A2 and the formula (A) shown in Tables 2A and 2B are defined as follows. Cooling rate A1: Average cooling rate up to 620℃ after coiling Cooling rate A2: Average cooling rate from 620℃ to 570℃ Formula (A): (T+273)×(log(s / 3600)+8-0.6×C) The symbols in formula (A) have the following meanings. T: Furnace atmosphere temperature (℃) s: Time in the furnace (seconds) C: C content in steel composition (mass%)
[0067] [Table 1A]
[0068] [Table 1B]
[0069] [Table 2A]
[0070] [Table 2B]
[0071] [Table 3A]
[0072] [Table 3B]
[0073] In the steel compositions in Tables 1A and 1B, "-" indicates that the component is not included or is less than the analytical lower limit. Steel types with an Al content of less than 0.010% contain Al as an impurity, and all steel types contain P, S, N, and O as impurities. In each table, values outside the range of the steel wire according to the present disclosure (desirable range for manufacturing conditions) are underlined.
[0074] Levels A1 to A43 are examples of the present disclosure. Levels B1 to B9 are comparative examples in which either the steel composition or the metal structure is outside the appropriate range of the present disclosure, and the absorbed energy of the steel wire is insufficient.
[0075] (Wire rod manufacturing) In both the examples and comparative examples of the present disclosure, hot rolling was performed by first heating a billet to 1000 to 1100°C, and then rolling and coiling it into a ring shape at the coiling temperature, the cooling rate after coiling to 620°C (cooling rate A1), and the cooling rate from 620°C to 570°C (cooling rate A2) shown in Tables 2A and 2B. The diameters of the hot-rolled wire rods are shown in Tables 2A and 2B. The structure, pro-eutectoid cementite area ratio, grain boundary ferrite and bainite area ratio, and pearlite area ratio of the hot-rolled wire rod were evaluated according to the same methods as those for observing the metal structure of the steel wire and measuring the area ratios. The results are shown in Tables 2A and 2B. The field emission scanning electron microscope used was JSM7100F manufactured by JEOL Ltd. The image analysis software used was Image-J from the National Institutes of Health.
[0076] (Steel wire manufacturing) The wire obtained as described above was subjected to wire drawing (dry wire drawing) and heat treatment under the conditions shown in Tables 2A and 2B to obtain steel wires. Note that, in the dry wire drawing, as pretreatment, scale removal was performed by pickling or bending, and lime coating treatment was performed, followed by wire drawing at an area reduction rate of 12 to 30% per pass. The wire diameters of the steel wires are shown in Tables 2A and 2B. Annealing after wire drawing was performed using a fluidized bed furnace. The fluidized bed conditions (holding temperature and holding time) are shown in Tables 2A and 2B. Thereafter, for some of the steel wires, the oxide scale formed on the surface was dissolved and removed with 17% hydrochloric acid at 60°C, and then the steel wires were passed through an ammonium zinc chloride solution as a flux, and then passed through molten zinc adjusted to about 450°C to 460°C, and pulled up to produce hot-dip galvanized steel wires. Note that it is optional whether or not to perform plating.
[0077] The steel wire thus obtained was subjected to a structural evaluation and a tensile test. The microstructure evaluation was carried out based on the fractal dimension of the ferrite grain boundary, the total area ratio of spheroidal cementite with an aspect ratio of 1.0 to 2.5, ferrite in which the spheroidal cementite is dispersed, and pearlite with a lamellar spacing of 0.3 μm or more (represented as "(A) Total area ratio of spheroidal cementite with an aspect ratio of 2.5 or less, ferrite in which the spheroidal cementite is dispersed, and coarse lamellar pearlite" in Tables 3A and 3B), and the total area ratio of spheroidal cementite with an aspect ratio of 1.0 to 2.5. The evaluation was performed based on the area ratio of spherical cementite having an aspect ratio of 1.0 to 2.5 and a major axis of 0.1 to 0.5 μm relative to the spherical cementite having an aspect ratio of 2.5 or less (represented as "the ratio of major axis of 0.1 to 0.5 μm in spherical cementite having an aspect ratio of 2.5 or less" in Tables 3A and 3B), (B) the total area ratio of pearlite structure and bainite having a lamellar spacing of less than 0.3 μm, and (C) the total area ratio of other structures. Note that (C) other structures are other than the above (A) and (B), that is, ferrite in which cementite having an aspect ratio of more than 2.5 is dispersed or ferrite in which cementite is not dispersed. The evaluation method was performed according to the above-mentioned method. FIG. 4 is an SEM image showing an example of spherical cementite observed in the central region of the steel wire of the example. In addition, in the case where two or more spheroidal cementite particles were connected to form the aforementioned constricted portion, each of the constricted portions was separated and measured.
[0078] [Tensile test] The tensile test was performed using the Shimadzu Autograph AG-250K and analysis software TRPEZIUMX, as described above. The absorbed energy was calculated using the software from the load and strain until breakage, and then divided by the evaluation volume (cross-sectional area x chuck length). Absorbed energy: 1550 J / cm 2 The above was judged to be good.
[0079] Levels A1 to A28 are all examples of the present disclosure, and all of the steel wires have a tensile strength of 500 to 1200 MPa and an absorbed energy of 1550 J / cm 2 The above excellent characteristics were observed. B1 is the steel composition currently used in ordinary galvanized wires. It has a low carbon content and low tensile strength, resulting in low absorbed energy and a large breaking elongation. Therefore, when a rockfall is received by the wire mesh, it is expected that the overhang will be large. B2 is an example in which the amount of C was excessive, so that the breaking elongation was reduced, vertical cracks occurred in the torsion test, and the absorbed energy was reduced. B3 is an example in which the Mn content was excessive, so that supercooled structures such as martensite and bainite were formed during hot rolling, causing cracks during wire drawing. B4 is an example in which the ferrite area ratio of the rolled material was low and the heat treatment did not satisfy formula (A), so that recrystallization progressed and the fractal dimension of the ferrite grain boundary became low, resulting in a decrease in absorbed energy. B5 is an example in which sufficient tensile strength and absorbed energy were not obtained because the holding time at high temperature during heat treatment was long and the spheroidization of cementite progressed excessively. B6 is an example in which the tensile strength of the steel wire is high, and the heat treatment temperature is low and the holding time is short, so that the spheroidal cementite does not coarsen and the recovery of ferrite grains is small, resulting in a small fractal dimension and reduced absorbed energy. In the case of B7, the holding time during heat treatment was short, so the spheroidal cementite did not coarsen and the recovery of ferrite grains was small, so the fracture elongation and reduction in area were reduced, resulting in a decrease in absorbed energy. B8 is an example of a material that experienced high temperatures during heat treatment, which led to recrystallization and austenitization, lowering the fractal dimension of the ferrite grain boundaries, increasing the area ratio of bainite, lowering the fracture elongation, and causing vertical cracks in the torsion test, resulting in a decrease in absorbed energy. B9 is an example in which the wire drawing strain was small, so that the spheroidization of cementite and the recrystallization of ferrite grains did not progress, the fractal dimension decreased, and the absorbed energy decreased.
[0080] (Manufacturing and evaluation of wire mesh) Among the above examples, A2, A6, A7, A9, A13, A15, A16, A19, and A24, as well as B1, B5, and B6 as comparative examples, were plated with Zn-based coating, and then made into diamond-shaped wire meshes, and the absorbed energy characteristics of the wire meshes were evaluated. The components and coating weight of the coating, and the absorbed energy of the wire meshes are shown in Table 4.
[0081] [Table 4]
[0082] The Zn-based plating method is hot-dip plating, where the steel wire is passed through a plating bath of molten Zn and then pulled up. When plating with elements other than Zn, such as Al, is performed, the wire is immersed in a plating bath containing a mixture of Zn and Al after Zn plating, and then pulled up.
[0083] Next, the method for evaluating the energy absorption capacity of wire mesh will be described. First, the above-mentioned hot-dip galvanized wire was formed into a diamond-shaped wire mesh having a size of 3 m x 3 m and a mesh size of 50 mm x 50 mm. The wire mesh thus produced was fixed with bolts on both opposing sides and rope on the remaining side, after which a spherical weight with a diameter of 0.7 m and a weight of 1.6 t was dropped from various heights. The maximum height at which the weight did not penetrate the wire mesh was used to calculate the energy (kJ) that the wire mesh could absorb, and this energy was divided by the cross-sectional area of the plated wire used in the wire mesh to determine the absorbed energy (kJ / mm 2) was evaluated. The criterion for judging high energy absorption wire mesh is the absorbed energy (kJ / mm 2 ) is 4.5kJ / mm 2 That's all. As shown in Table 4, the wire mesh produced using the steel wires of the examples exhibited excellent absorbed energy at all levels.
Claims
1. The steel composition is, in mass%, C: 0.30-1.20%, Si: 0.10 to 1.50%, Mn: 0.10-1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0200% or less, and O: 0.0070% or less with the balance being Fe and impurities; the metal structure includes at least ferrite and cementite, in a cross section perpendicular to the longitudinal direction of the steel wire, the total area ratio of the ferrite, the cementite, and the pearlite is 95.0% or more, and the grain boundaries of the ferrite grains have a fractal dimension of 1.20 to 1.95; A steel wire having a wire diameter of 2.0 to 6.0 mm.
2. Instead of a part of the Fe, Cr: 1.50% or less, B: 0.0050% or less, Ti: 0.040% or less, Mo: 0.40% or less, V: 0.30% or less, Cu: 0.50% or less, Al: 0.080% or less, Ni: 0.50% or less, and Nb: 0.10% or less, The steel wire according to claim 1, comprising one or more selected from the group consisting of:
3. Instead of a part of the Fe, Mg: 0.010% or less, Zr: 0.010% or less, Sb: 0.015% or less, W: 0.010% or less, REM (elements with atomic numbers 57 to 71): 0.005% or less, Hf: 0.005% or less, Ta: 0.050% or less, Ca: 0.005% or less, Sn: 0.050% or less, Bi: 0.050% or less, Te: 0.050% or less, Zn: 0.050% or less, and Co: 0.10% or less The steel wire according to claim 1 or 2, comprising one or more selected from the group consisting of:
4. The tensile strength in the tensile test is 500 to 1200 MPa, and the absorbed energy per unit cross-sectional area is 1600 J / cm 2 The steel wire according to any one of claims 1 to 3.
5. The steel wire according to any one of claims 1 to 4, wherein, in the metal structure, when a radius of the steel wire is R, in a central region at a distance of 0.4 × R or less from a central axis of the cross section, a total area ratio of spherical cementite having an aspect ratio of 1.0 to 2.5, ferrite in which the spherical cementite is dispersed, and pearlite having a lamellar spacing of 0.3 µm or more is 70% or more.
6. The steel wire according to any one of claims 1 to 5, wherein, in the metal structure, in a central region at a distance of 0.4 × R or less from a central axis of the cross section, a total area ratio of pearlite and bainite having a lamellar spacing of less than 0.3 µm is 30.0% or less, when a radius of the steel wire is R.
7. The steel wire according to any one of claims 1 to 6, wherein, in the metal structure, in a central region within a distance of 0.4 × R from a central axis of the cross section, an area ratio of the spheroidal cementite having an aspect ratio of 1.0 to 2.5 and a major axis of 0.1 to 0.5 μm is 90.0% or more relative to the spheroidal cementite having an aspect ratio of 1.0 to 2.5, where R is a radius of the steel wire.
8. 8. The steel wire according to claim 1, wherein the breaking elongation in a tensile test is 10.0 to 30.0%, and the number of twists until breaking without longitudinal cracking in a torsion test is 25 or more.
9. The steel wire according to any one of claims 1 to 8, which has a yield ratio in a tensile test of 50.0 to 80.0% and a reduction in area of 55.0% or more.
10. The steel wire according to any one of claims 1 to 9, which has a zinc-based plating layer on a surface thereof.
11. The steel wire according to any one of claims 1 to 10, which is for wire mesh.
12. A wire mesh produced using the steel wire according to any one of claims 1 to 11.
Citation Information
Patent Citations
Continuous spheroidizing treatment of steel wire
JP1984116330A
Hot rolled wire rod-bar steel for machine structure and production thereof
JP2000336456A
Wire or rod steel suppressed arising of deformation resistance at room temperature and in area of working heat generation
JP2001342544A
Steel excellent in cold forgeability, and method of manufacturing the same
JP2012140674A
High carbon steel wire rod and method for producing high carbon steel wire rod
JP2012233254A