Polyamide resin composition for sliding parts, and sliding parts
A polyamide resin composition with finely dispersed reactive components addresses moldability, heat resistance, and sliding properties challenges, enhancing toughness and wear resistance for complex molded products.
Patent Information
- Application Number
- JP2021548804
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-27
- Filing Date
- 2020-09-11
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-09-11
AI Technical Summary
Existing polyamide resin compositions for sliding parts face challenges in achieving excellent moldability, heat resistance stability, toughness, and sliding properties, with solid lubricants compromising toughness and liquid lubricants causing surface contamination, while recent trends towards lighter and more complex molded products require higher-level properties.
A polyamide resin composition comprising a crystalline polyamide resin, modified polyolefin resin with reactive functional groups, thermoplastic elastomer, antioxidant, mold release agent, and solid lubricant, where these components are finely dispersed in domains of 5 μm or less, enhancing compatibility and maintaining toughness while improving sliding properties.
The composition achieves improved moldability, heat-resistant stability, and toughness with reduced wear and friction, offering both low abrasion and low friction, suitable for sliding parts requiring excellent wear resistance and stability.
Smart Images

Figure 0007587209000003 
Figure 0007587209000004 
Figure 0007587209000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide resin composition, and more particularly to a polyamide resin composition that is suitably used for molding sliding parts. [Background technology]
[0002] Polyamide resin is a molding material with excellent sliding properties due to its crystallinity. In order to obtain even better sliding properties, it is known to compound it with solid lubricants such as molybdenum disulfide, graphite and fluororesin, various lubricating oils, or liquid lubricants such as silicone oil.
[0003] Among these sliding improvers, solid lubricants have the drawback of needing to be blended in large amounts, which significantly reduces the toughness of the base polyamide resin.Liquid lubricants can provide effective sliding properties with a relatively small amount, but in many cases they are poorly compatible with the base polyamide resin, and the surface of the molded product is easily contaminated by the liquid lubricant, which limits their use.
[0004] As methods for improving the drawbacks caused by the blending of such various lubricants, a method of blending a modified styrene-based polymer with a modified high-density polyethylene having a specific range of molecular weight (Patent Document 1) and a method of using a high-viscosity crystalline polyamide resin and blending it with a modified polyolefin resin have been proposed (Patent Document 2).
[0005] Such polyamide resin compositions have made it possible to provide molded articles that are free from the above-mentioned drawbacks and have excellent sliding properties. However, due to recent trends such as weight reduction and more complex shapes of molded articles, there is a demand for higher levels of properties such as improved moldability, improved heat resistance stability, and improved sliding properties. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-157714 [Patent Document 2] WO2008 / 075699 publication Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a polyamide resin composition which is suitable for use in molding sliding parts which are required to have excellent moldability, heat stability, and toughness as well as excellent abrasion resistance and sliding stability. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted extensive research to achieve the above object, and have discovered that an antioxidant and a mold release agent, which are added to improve moldability and heat resistance, improve the sliding properties, and that the sliding properties are further improved by adding a solid lubricant to a polyamide resin composition to maintain toughness, thereby arriving at the present invention.
[0009] That is, the present invention comprises the following configuration. [1] The composition comprises a crystalline polyamide resin (A), a modified polyolefin resin (B) having a reactive functional group capable of reacting with an end group and / or a main chain amide group of the polyamide resin (A), and / or a thermoplastic elastomer (C) having a reactive functional group capable of reacting with an end group and / or a main chain amide group of the polyamide resin (A), an antioxidant (D), a mold release agent (E), and a solid lubricant (F), The polyamide resin composition for sliding parts, wherein the modified polyolefin resin (B) and / or the thermoplastic elastomer (C) are dispersed in a matrix of the polyamide resin (A) in the form of domains having a particle size of 5 μm or less. [2] The polyamide resin composition for sliding parts according to [1], wherein the antioxidant (D) and the release agent (E) are compounds that suppress deactivation of the reactive functional groups possessed by the modified polyolefin resin (B) and the thermoplastic elastomer (C). [3] The polyamide resin composition according to [1] or [2], wherein the reactive functional group is an acid anhydride group. [4] The polyamide resin composition for sliding parts according to any one of [1] to [3], wherein the antioxidant (D) is a hindered phenol-based antioxidant. [5] The polyamide resin composition for sliding parts according to any one of [1] to [4], wherein the release agent (E) is a higher fatty acid ester compound. [6] The polyamide resin composition for sliding parts according to any one of [1] to [5], wherein the thermoplastic elastomer (C) is a styrene-based and / or olefin-based thermoplastic elastomer. [7] The polyamide resin composition for sliding parts according to any one of [1] to [6], wherein the solid lubricant (F) is a fluorine-based lubricant and / or an acrylic-modified polyorganosiloxane. [8] A sliding part obtained from the polyamide resin composition for sliding parts according to any one of [1] to [7]. Effect of the Invention
[0010] The polyamide resin composition of the present invention is not only excellent in moldability, heat resistance, and toughness, but also shows further improvement in sliding properties such as improved wear resistance and small change in friction coefficient, etc. Furthermore, the polyamide resin composition of the present invention can achieve both low wear and low friction. [Brief description of the drawings]
[0011] [Figure 1] 1 is an image of a cross section of an evaluation sample prepared in Example 2 observed with a differential interference contrast microscope. [Diagram 2] 1 is an image of a cross section of an evaluation sample prepared in Comparative Example 10, observed with a differential interference microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be specifically described below. The polyamide resin composition for sliding parts of the present invention contains a crystalline polyamide resin (A), a modified polyolefin resin (B) having a reactive functional group capable of reacting with an end group and / or a main chain amide group of the polyamide resin (A) (hereinafter also referred to as modified polyolefin resin (B)) and / or a thermoplastic elastomer (C) having a reactive functional group capable of reacting with an end group and / or a main chain amide group of the polyamide resin (A) (hereinafter also referred to as thermoplastic elastomer (C)), an antioxidant (D), a mold release agent (E), and a solid lubricant (F).
[0013] The amount of each component is expressed in parts by mass when the total amount of all resin components, crystalline polyamide resin (A), modified polyolefin resin (B), thermoplastic elastomer (C), and solid lubricant (F), is taken as 100 parts by mass. In the polyamide resin composition of the present invention, the amount of each component is the content in the polyamide resin composition.
[0014] The crystalline polyamide resin (A) is not particularly limited as long as it is a crystalline polymer having an amide bond (-NHCO-) in the main chain, and examples thereof include polyamide 6 (NY6), polyamide 66 (NY66), polyamide 46 (NY46), polyamide 11 (NY11), polyamide 12 (NY12), polyamide 610 (NY610), polyamide 612 (NY612), polymetaxylylene adipamide (MXD6), hexamethylenediamine-terephthalic acid polymer (6T), hexamethylenediamine-terephthalic acid, and and adipic acid polymer (66T), hexamethylenediamine-terephthalic acid and ε-caprolactam copolymer (6T / 6), trimethylhexamethylenediamine-terephthalic acid polymer (TMD-T), metaxylylenediamine, adipic acid and isophthalic acid copolymer (MXD-6 / I), trihexamethylenediamine, terephthalic acid and ε-caprolactam copolymer (TMD-T / 6), diaminodicyclohexylenemethane (CA), isophthalic acid and lauryllactam copolymer, etc. These may be used alone or in combination of two or more. Of these, it is preferable to use polyamide 6 (NY6) and polyamide 66 (NY66).
[0015] The relative viscosity of the crystalline polyamide resin (A) is not particularly limited, but is preferably 2.0 to 5.0, more preferably 2.0 to 3.5, as measured in a 96% sulfuric acid solution (polyamide resin concentration 1 g / dl, temperature 25° C.).
[0016] The modified polyolefin resin (B) is a modified polyolefin resin. Examples of polyolefin resins include high-density polyethylene, low-density polyethylene, ultra-high molecular weight polyethylene, linear low-density polyethylene, polypropylene, poly(1-butene), poly(4-methylpentene), etc. These may be used alone or in a blend of two or more. Of these, it is preferable to use high-density polyethylene.
[0017] In order to improve compatibility with the crystalline polyamide resin (A), the modified polyolefin resin (B) has a reactive functional group capable of reacting with the terminal group (amino group or carboxy group) and / or main chain amide group of the polyamide resin (A). Examples of the reactive functional group include a carboxy group, an acid anhydride group, an epoxy group, an oxazoline group, an amino group, an isocyanate group, etc. Among these, an acid anhydride group is preferred from the viewpoint of high reactivity with the polyamide resin (A).
[0018] The content of the reactive functional group in the modified polyolefin resin (B) is preferably 0.05 to 8 mass%, more preferably 0.1 to 5 mass%. The method for producing the modified polyolefin resin (B) having the reactive functional group is not particularly limited, and examples thereof include a method in which a compound having the reactive functional group is reacted in a process for producing a polyolefin resin, and a method in which pellets of a polyolefin resin and a compound having the reactive functional group are mixed and kneaded in an extruder or the like to cause the reaction.
[0019] The amount of modified polyolefin resin (B) is not particularly limited as long as it is an amount that allows the modified polyolefin resin (B) to be dispersed in the matrix of the polyamide resin (A) in domains having a particle size of 5 μm or less, but is usually 0.5 to 10 mass %, preferably 1 to 8 mass %, and more preferably 2 to 6 mass %, relative to 100 mass % of the total resin components.
[0020] The thermoplastic elastomer (C) is not particularly limited, and examples thereof include styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, etc. These may be used alone or in a blend of two or more.
[0021] The styrene-based thermoplastic elastomer is not particularly limited, and examples thereof include styrene / butadiene / styrene block copolymer (SBS), its hydrogenated product styrene / ethylene-butylene / styrene block copolymer (SEBS), styrene / butadiene copolymer (SBR), its hydrogenated product styrene / ethylene / butylene copolymer (HSBR), styrene / isoprene / styrene block copolymer (SIS), its hydrogenated product styrene / ethylene-propylene / styrene block copolymer (SEPS), and the like.
[0022] The olefin-based thermoplastic elastomer is not particularly limited, and examples thereof include rubbers such as ethylene / propylene / diene rubber (EPDM), ethylene / propylene rubber (EPR), and butyl rubber (IIR), dynamically crosslinked olefin-based thermoplastic elastomers, and flexible ethylene-based copolymers.
[0023] The polyamide-based thermoplastic elastomer is not particularly limited, and examples thereof include polyether ester amides and polyester amides, which have a crystalline polyamide with a high melting temperature as a hard segment and a polyether or polyester with a low glass transition temperature as a soft segment.
[0024] The polyester-based thermoplastic elastomer is not particularly limited, and examples thereof include block copolymers of polyether polyester and polyester polyester, in which a crystalline polyester having a high melting temperature is used as a hard segment and a polyether or polyester having a low glass transition temperature is used as a soft segment.
[0025] The polyurethane-based thermoplastic elastomer is not particularly limited, and examples thereof include polyether polyurethane and polyester polyurethane, which have crystalline polyester with a high melting temperature as a hard segment and polyether or polyester with a low glass transition temperature as a soft segment.
[0026] Among these thermoplastic elastomers, from the viewpoint of the balance between the toughness improving effect and the elastic modulus, styrene-based and / or olefin-based thermoplastic elastomers are preferred, styrene-based thermoplastic elastomers are more preferred, and SEBS is even more preferred.
[0027] In order to improve compatibility with the crystalline polyamide resin (A), the thermoplastic elastomer (C) has a reactive functional group capable of reacting with the terminal group (amino group or carboxy group) and / or main chain amide group of the polyamide resin (A). Examples of the reactive functional group include a carboxy group, an acid anhydride group, an epoxy group, an oxazoline group, an amino group, an isocyanate group, etc. Among these, an acid anhydride group is preferred from the viewpoint of high reactivity with the polyamide resin (A).
[0028] The content of the reactive functional group in the thermoplastic elastomer (C) is preferably 0.05 to 8 mass%, more preferably 0.1 to 5 mass%. The method for producing the thermoplastic elastomer (C) having the reactive functional group is not particularly limited, and examples thereof include a method in which a compound having the reactive functional group is reacted in a step for producing a thermoplastic elastomer, and a method in which pellets of a thermoplastic elastomer and a compound having the reactive functional group are mixed and kneaded in an extruder or the like to cause the reaction.
[0029] The amount of the thermoplastic elastomer (C) is not particularly limited as long as the thermoplastic elastomer (C) can be dispersed in the matrix of the polyamide resin (A) in domains having a particle size of 5 μm or less. The amount is usually 0.1 to 10 mass %, and preferably 1 to 7 mass %, relative to 100 mass % of the total resin components.
[0030] The antioxidant (D) is preferably a compound that suppresses the deactivation of the reactive functional groups contained in the modified polyolefin resin (B) and the thermoplastic elastomer (C). "Suppressing the deactivation of the reactive functional groups" means "not reacting with the reactive functional groups". In other words, the antioxidant (D) is a compound that does not inhibit the fine dispersion of the modified polyolefin resin (B) and the thermoplastic elastomer (C) in the matrix of the polyamide resin (A).
[0031] The antioxidant (D) is not particularly limited, and for example, when the reactive functional group of the modified polyolefin resin (B) and the thermoplastic elastomer (C) is an acid anhydride group, examples of the antioxidant include organic antioxidants such as hindered phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants that do not have a functional group that reacts with the acid anhydride group, and heat stabilizers, and the like, and is preferably a hindered phenol-based antioxidant. These may be used alone or in a blend of two or more. Examples of functional groups that react with the acid anhydride group include amino groups and hydroxyl groups. The phenolic hydroxyl group of the hindered phenol structure does not fall under the category of functional groups that react with the acid anhydride group. Amine-based antioxidants are not preferred because they react with the reactive functional group and deactivate it.
[0032] The blending amount of the antioxidant (D) is preferably 0.01 to 1 part by mass, more preferably 0.1 to 0.5 parts by mass, based on 100 parts by mass of the total resin components. If the blending amount of the antioxidant (D) is within the above range, it not only contributes to improving the sliding property and toughness of the polyamide resin composition, but also prevents oxidative deterioration over time as an appropriate formulation amount according to the amount of the polyamide resin composition.
[0033] The release agent (E) is preferably a compound that suppresses the deactivation of the reactive functional groups contained in the modified polyolefin resin (B) and the thermoplastic elastomer (C). "Suppressing the deactivation of the reactive functional groups" means "not reacting with the reactive functional groups". In other words, the release agent (E) is a compound that does not inhibit the fine dispersion of the modified polyolefin resin (B) and the thermoplastic elastomer (C) in the matrix of the polyamide resin (A).
[0034] The release agent (E) is not particularly limited, and examples thereof include higher fatty acid ester compounds, amide compounds, polyethylene wax, silicone, and polyethylene oxide. These may be used alone or in a blend of two or more. When the reactive functional groups possessed by the modified polyolefin resin (B) and the thermoplastic elastomer (C) are acid anhydride groups, the release agent (E) is preferably a higher fatty acid ester compound. The higher fatty acid is a fatty acid having more than 10 carbon atoms, preferably a fatty acid having 11 to 30 carbon atoms. Metal salt compounds are not preferred because they react with the reactive functional groups and deactivate them.
[0035] The amount of the release agent (E) is preferably 0.05 to 1 part by mass, more preferably 0.1 to 0.8 parts by mass, based on 100 parts by mass of the total resin components. If the amount of the release agent (E) is within the above range, it not only contributes to improving the sliding property and toughness of the polyamide resin composition, but also ensures appropriate release property.
[0036] The antioxidant (D) and the release agent (E) do not inhibit the modified polyolefin resin (B) and the thermoplastic elastomer (C) from being finely dispersed in the matrix of the polyamide resin (A). Therefore, the modified polyolefin resin (B) and the thermoplastic elastomer (C) react efficiently with the polyamide resin (A) and are finely dispersed in the matrix of the polyamide resin (A) in domains having a particle size of 5 μm or less. As a result, the sliding property improving effect of the modified polyolefin resin (B) and the toughness improving effect of the thermoplastic elastomer (C) are effectively acted, and it is considered that the unique effect of the present invention is expressed. The particle size is preferably 4 μm or less, more preferably 3.5 μm or less. The lower limit of the particle size is not particularly limited, but from the viewpoint of flowability, it is preferably 1 μm or more, more preferably 2 μm or more.
[0037] The solid lubricant (F) contributes to improving the surface friction characteristics and has the effect of suppressing a decrease in toughness. It is believed that the addition of the solid lubricant (F) to the polyamide resin composition brings about the effects unique to the present invention.
[0038] The solid lubricant (F) is not particularly limited, but fluorine-based lubricants and acrylic-modified polyorganosiloxanes are preferred. These may be used alone or in combination of two or more.
[0039] Examples of the fluorine-based lubricant include polytetrafluoroethylene resin (PTFE), perfluoroalkoxy resin (PFA), polytetrafluoroethylene-hexafluoropropylene copolymer resin (FEP), polytetrafluoroethylene-ethylene copolymer resin (ETFE), polyvinylidene fluoride resin (PVDF), polychlorotrifluoroethylene resin (PCTFE), etc. Among these, PTFE is preferred from the viewpoints of heat resistance, sliding properties, etc.
[0040] The average particle size of the fluorine-based lubricant is preferably 1 to 200 μm, more preferably 7 to 100 μm, and even more preferably 10 to 50 μm. If the average particle size exceeds 200 μm, the dispersibility of the fluorine-based lubricant in the matrix of the polyamide resin (A) becomes poor, and the mechanical strength of the molded body tends to decrease. On the other hand, if the average particle size is less than 1 μm, the particles of the fluorine-based lubricant tend to cause secondary aggregation, making it difficult to mix uniformly, and the mechanical strength of the molded body tends to decrease.
[0041] The acrylic modified polyorganosiloxane may be, for example, a polyorganosiloxane graft-copolymerized with at least a (meth)acrylic acid ester. In particular, a polyorganosiloxane graft-copolymerized with a mixture of 70% by mass or more of a (meth)acrylic acid ester and 30% by mass or less of other copolymerizable monomers in a mass ratio of 5 / 95 to 95 / 5 is preferred.
[0042] Examples of the (meth)acrylic acid ester include acrylic acid esters such as methyl acrylate, ethyl acrylate, isopropyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, n-octyl acrylate, 2-hydroxyethyl acrylate, and 2-methoxyethyl acrylate; and methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-ethoxyethyl methacrylate. These may be used alone or in a blend of two or more. Of these, it is preferable to use methyl methacrylate as at least one component.
[0043] Examples of the other copolymerizable monomers include styrene-based compounds such as styrene, vinyl toluene, and α-methyl styrene; unsaturated nitriles such as acrylonitrile and methacrylonitrile; halogenated olefins such as vinyl chloride and vinylidene chloride; vinyl esters such as vinyl acetate and vinyl propionate; unsaturated amides such as acrylamide, methacrylamide, and N-methylolacrylamide; monomers having one double bond such as unsaturated carboxylic acids such as acrylic acid, methacrylic acid, and maleic anhydride; and polyunsaturated monomers such as ethylene glycol dimethacrylate, propylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, allyl methacrylate, triallyl cyanurate, and triallyl isocyanurate. These may be used alone or in a blend of two or more.
[0044] The average particle size of the acrylic modified polyorganosiloxane is preferably 1 to 500 μm, more preferably 10 to 400 μm, and even more preferably 30 to 350 μm. If the average particle size exceeds 500 μm, the dispersibility of the acrylic modified polyorganosiloxane in the matrix of the polyamide resin (A) becomes poor, and the mechanical strength of the molded product tends to decrease. On the other hand, if the average particle size is less than 1 μm, the particles of the acrylic modified polyorganosiloxane tend to cause secondary aggregation, making it difficult to mix uniformly, and the mechanical strength of the molded product tends to decrease.
[0045] The amount of the solid lubricant (F) is preferably 0.1 to 20 mass% and more preferably 0.5 to 10 mass% based on 100 mass% of the total resin components. If it is 0.1 mass% or more, the wear resistance, sliding stability, and surface lubricity are effectively improved. On the other hand, if it is 20 mass% or less, the mechanical properties, particularly the toughness, of the polyamide resin composition are effectively improved.
[0046] In the polyamide resin composition of the present invention, in addition to the above-mentioned components (A) to (F), additives such as carbon black, which is a weather resistance improver, copper oxide, alkali metal halide, light or heat stabilizer, crystal nucleating agent, antistatic agent, pigment, dye, coupling agent, etc., which are added to conventional polyamide resin compositions, may be added as long as they do not inhibit the fine dispersion of the modified polyolefin resin (B) and the thermoplastic elastomer (C) in the matrix of the polyamide resin (A). Furthermore, by adding a filler to the extent that the toughness of the polyamide resin composition is not impaired, the strength and rigidity of the molded product can be significantly improved. Examples of fillers include glass fiber, carbon fiber, metal fiber, aramid fiber, asbestos, potassium titanate whisker, wollastonite, glass flakes, glass beads, talc, mica, clay, calcium carbonate, barium sulfate, titanium oxide, aluminum oxide, etc. The polyamide resin composition of the present invention preferably contains the above-mentioned components (A) to (F) in total at 70 mass % or more, more preferably at 80 mass % or more, and even more preferably at 90 mass % or more.
[0047] The polyamide resin composition of the present invention is produced, for example, by kneading each component using a kneading device such as a single screw extruder, a twin screw extruder, or a pressure kneader. The kneading device is preferably a twin screw extruder. In one embodiment, the components (A) to (F) and, depending on the application, a pigment or the like are mixed and charged into a twin screw extruder. By uniformly kneading with the twin screw extruder, a polyamide resin composition having excellent sliding properties can be produced. The kneading temperature of the twin screw extruder is preferably 220 to 300°C, and the kneading time is preferably about 2 to 15 minutes.
[0048] The polyamide resin composition of the present invention can be widely used as a raw material for sliding parts that require slidability, such as electric and electronic parts, automobile parts, building parts, and industrial parts. Specific examples of sliding parts include bearings, gears, door checkers, and chain guide parts. EXAMPLES
[0049] The present invention will be described in detail below using examples, but the present invention is not limited to these examples. The physical properties of the polyamide resin molded products obtained in each of the following examples were measured based on the following test methods.
[0050] The raw materials used in the examples and comparative examples are as follows. As the crystalline polyamide resin (A), (A1) to (A3) were used. (A1) Polyamide 66 (RV=3.4): EPR34W (manufactured by Shanghai Shenma Plastic Technology Co., Ltd.), melting point 265℃ (A2) Polyamide 66 (RV=2.8): Vydyne 21FSR (manufactured by Ascend), melting point 265°C (A3) Polyamide 66 (RV=2.4): EPR24 (manufactured by Shanghai Shenma Plastic Technology Co., Ltd.), melting point 265℃
[0051] As the modified polyolefin resin (B), (B1) and (B2) were used. (B1) Maleic anhydride modified polyethylene: Modic DH0200 (manufactured by Mitsubishi Chemical Corporation) (B2) Unmodified polyethylene: Hi-Zex 6203B (manufactured by Prime Polymer Co., Ltd.)
[0052] As the thermoplastic elastomer (C), (C1) and (C2) were used. (C1) Maleic anhydride modified SEBS: Tuftec M-1943 (manufactured by Asahi Kasei Corporation) (C2) Unmodified SEBS: Tuftec H-1221 (manufactured by Asahi Kasei Corporation)
[0053] As the antioxidant (D), (D1) and (D2) were used. (D1) Hindered phenol-based antioxidant: triethylene glycol-bis-3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate (SONGWON, SONGNOX2450) (D2) Amine-based antioxidant: Nonflex DCD (Seiko Chemical Co., Ltd.)
[0054] As the release agent (E), (E1) to (E3) were used. (E1) Aliphatic ester: Lycorb WE-40 (manufactured by Clariant Japan Co., Ltd.) (E2) Magnesium stearate: NP1500-S (manufactured by Tannan Chemical Industry Co., Ltd.) (E3) Calcium montanate: Licomont Cav102 (manufactured by Clariant Japan Co., Ltd.)
[0055] As the solid lubricant (F), (F1) to (F3) were used. (F1) PTFE: KT-300M (Kitamura Co., Ltd.), average particle size 15 μm (F2) Acrylic modified polyorganosiloxane: Chaline R-170S (manufactured by Nissin Chemical Industry Co., Ltd.), average particle size 30 μm (F3) Silicone powder: KMP-590 (manufactured by Shin-Etsu Silicone Co., Ltd.), average particle size 2 μm The average particle size was measured as follows: Each solid lubricant was observed and photographed using a differential interference microscope. Ten particles were randomly selected from the particles in the micrographs, and the major axis of the selected particles was measured, and the average value was taken as the average particle size.
[0056] [Examples 1 to 13, Comparative Examples 1 to 15] The evaluation samples were produced by weighing out the raw materials in the blending ratio of the polyamide resin composition shown in Tables 1 and 2, mixing them in a tumbler, and then feeding them into a twin-screw extruder. The temperature of the twin-screw extruder was set to 250°C to 300°C, and the kneading time was 5 to 10 minutes. Using the obtained pellets, various evaluation samples were molded in an injection molding machine. The cylinder temperature of the injection molding machine was set to 250°C to 290°C, and the mold temperature was 80°C.
[0057] The various evaluation and measurement methods are as follows. The evaluation and measurement results are shown in Tables 1 and 2. 1. Relative Viscosity of Polyamide Resin (96% Sulfuric Acid Solution Method) The viscosity was measured using an Ubbelohde viscosity tube at 25° C. in a 96% by weight sulfuric acid solution with a polyamide resin concentration of 1 g / dL.
[0058] 2. Melting point of polyamide resin The endothermic peak temperature was determined by measuring at a temperature rise rate of 20° C. / min using a differential scanning calorimeter (Seiko Instruments Inc., EXSTAR 6000).
[0059] 3. Tensile strength, tensile modulus, tensile elongation Measured in accordance with ISO178.
[0060] 4. Shock resistance Measurements were performed in accordance with ISO179-1.
[0061] 5. Sliding properties Using a thrust type abrasion tester, a certain amount of dust made by mixing grease containing molybdenum disulfide, silica sand, and volcanic ash in a mass ratio of 1:1:1 was evenly applied to the surface of a polyamide resin plate and a cylindrical molded product made of polyoxymethylene (POM). The plate was then placed in contact with the plate and subjected to a load of 30 kgf / cm for 30 minutes. 2 The friction coefficient was calculated from the difference in weight before and after abrasion and the converged abrasion load value during the friction test.
[0062] 6.Particle size The molded evaluation sample was cut out, and a cross section was prepared using a microtome equipped with a glass knife. The prepared cross section was observed with a differential interference microscope and photographed. In the micrograph, 10 domains with the largest dispersion diameter were arbitrarily selected from the domains of the modified polyolefin resin (B) and the thermoplastic elastomer (C), and the major axis of the selected domains was measured, and the average value was taken as the particle diameter.
[0063] [Table 1]
[0064] [Table 2]
[0065] In Examples 1 to 13, the Charpy impact strength was 6 kJ / m 2 The above results show that the polyamide resin composition has low wear amount and dynamic friction coefficient, and has both toughness and sliding properties. In addition, the tensile modulus and tensile elongation are not significantly impaired. In Comparative Examples 1 to 3, the brittle surface destruction during sliding cannot be suppressed only by the polyolefin resin alloy due to insufficient toughness, and the wear amount is large. In Comparative Examples 4 to 7, although the toughness is sufficient, the tensile modulus is insufficient, and the dust is embedded in the material surface, so that it is easy to wear, and the sliding improvement effect of the polyolefin resin is difficult to work. Comparative Examples 8 and 12 are not suitable because they are formulated with unmodified polyolefin resin or unmodified thermoplastic elastomer, and therefore it is difficult to form a finely dispersed domain, and the particle size is difficult to express excellent physical properties. Comparative Examples 9 to 11 use an amine-based antioxidant or a fatty acid metal salt, respectively, and therefore react with the reactive functional group of the polyolefin resin or thermoplastic elastomer, and the reactive functional group is deactivated, so that a finely dispersed domain cannot be formed. Comparative Example 13 contains a solid lubricant, but is a simple silicone powder, so aggregates are easily formed in the polyamide resin composition, which makes brittle fracture more likely to occur at the interface between the silicone powder and the polyamide resin, resulting in a large amount of wear. Comparative Examples 14 and 15 contain a solid lubricant, but do not contain a polyolefin resin or a thermoplastic elastomer, so although the dynamic friction coefficient is low, brittle fracture cannot be suppressed and the amount of wear cannot be reduced.
[0066] FIG. 1 is an image of the cross section of Example 2 observed with a differential interference microscope. It can be seen that the polyolefin resin and the thermoplastic elastomer are uniformly dispersed in the polyamide resin matrix in domains with a particle size of 5 μm or less. On the other hand, FIG. 2 is an image of the cross section of Comparative Example 10 observed with a differential interference microscope. The above two modifiers are unevenly dispersed in the polyamide resin matrix, and are not finely dispersed. In addition, they exist in coarse domains, which may concentrate stress during wear and become the starting point of wear. [Industrial Applicability]
[0067] The polyamide resin composition of the present invention is a molding material that has both excellent toughness and sliding properties. It is particularly suitable for sliding parts that require excellent wear resistance and sliding stability, and is expected to make a great contribution to the industrial world as an engineering plastic that can be used in a wide range of fields.
Claims
1. The present invention comprises a crystalline polyamide resin (A), a modified polyolefin resin (B) having a reactive functional group capable of reacting with an end group and / or a main chain amide group of the polyamide resin (A) and / or a thermoplastic elastomer (C) having a reactive functional group capable of reacting with an end group and / or a main chain amide group of the polyamide resin (A), an antioxidant (D), a mold release agent (E), and a solid lubricant (F), The solid lubricant (F) is a fluorine-based lubricant and / or an acrylic-modified polyorganosiloxane, The polyamide resin composition for sliding parts, wherein the modified polyolefin resin (B) and / or the thermoplastic elastomer (C) are dispersed in a matrix of the polyamide resin (A) in the form of domains having a particle size of 5 μm or less.
2. 2. The polyamide resin composition for sliding parts according to claim 1, wherein the antioxidant (D) and the release agent (E) are compounds that suppress deactivation of the reactive functional groups possessed by the modified polyolefin resin (B) and the thermoplastic elastomer (C).
3. 3. The polyamide resin composition for sliding parts according to claim 1, wherein the reactive functional group is an acid anhydride group.
4. 4. The polyamide resin composition for sliding parts according to claim 1, wherein the antioxidant (D) is a hindered phenol-based antioxidant.
5. 5. The polyamide resin composition for sliding parts according to claim 1, wherein the release agent (E) is a higher fatty acid ester compound.
6. 6. The polyamide resin composition for sliding parts according to claim 1, wherein the thermoplastic elastomer (C) is a styrene-based and / or olefin-based thermoplastic elastomer.
7. A sliding part obtained from the polyamide resin composition for sliding parts according to any one of claims 1 to 6.
Citation Information
Patent Citations
Polyamide resin molding
JP1996157714A
Polyamide resin composition excellent in rigidity and molded article therefrom
JP2007297581A
Polyamide resin composition
JP2014218574A
Crystalline polyamide based resin composition
WO2008075699A1
Sliding member
WO2019098210A1