Polyurethane modified epoxy resin and resin composition

The novel polyurethane-modified epoxy resin composition addresses limitations in urethane concentration and property balance by using specific molecular weight polyols and polyisocyanates, improving strength, toughness, and glass transition temperature for diverse applications.

JP7587386B2Active Publication Date: 2024-11-20NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020165690
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-11-20
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing polyurethane-modified epoxy resins have limitations in design freedom due to low urethane concentration and inadequate balance of strength, fracture toughness, and glass transition temperature, making them unsuitable for various applications.

Method used

A novel polyurethane-modified epoxy resin composition using a bisphenol-based epoxy resin with specific molecular weights and a combination of medium-high and low molecular weight polyols, along with a polyisocyanate compound, to enhance urethane concentration and achieve a balanced properties.

Benefits of technology

The composition improves elastic modulus, strength, and fracture toughness while maintaining high glass transition temperature, suitable for adhesives, coatings, and composite materials, enhancing design flexibility and application suitability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587386000001
    Figure 0007587386000001
  • Figure 0007587386000002
    Figure 0007587386000002
  • Figure 0007587386000003
    Figure 0007587386000003
Patent Text Reader

Abstract

To provide a polyurethane-modified epoxy resin composition which can achieve both high elasticity and high toughness.SOLUTION: A polyurethane-modified epoxy resin is obtained by modifying a bisphenol-based epoxy resin (a) having an epoxy equivalent of 150-300 g / eq and a hydroxy group equivalent of 800-2,000 g / eq with a polyol compound (b) of a middle to high molecular weight having a number average molecular weight of 500 or more, a polyisocyanate compound (c) and a polyol compound (d) of a low molecular weight of having a number average molecular weight of less than 500, in which 50-75 wt.% of the epoxy resin (a) is used with respect to the total amount of the components (a), (b), (c) and (d), and 5-10 wt.% of the component (d) is used with respect to the total amount of the components (b) and (d).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyurethane-modified epoxy resin and a composition thereof. [Background technology]

[0002] Epoxy resins have excellent processability and a variety of cured product properties, including high heat resistance, high insulation reliability, high rigidity, high adhesion, and high corrosion resistance, and are therefore used in large quantities for a variety of applications, including electrical insulating materials (casting, impregnation, laminates, and sealing materials), matrix resins for composite materials such as CFRP, structural adhesives, and heavy-duty corrosion-resistant paints.

[0003] On the other hand, epoxy resin cured products have low elongation at break, low fracture toughness, and low peel strength. Therefore, in applications such as matrix resins for composite materials and structural adhesives where these properties are required, the above properties have been improved by various modifications such as rubber modification and polyurethane modification.

[0004] As a method for modifying polyurethane, for example, Patent Documents 1 and 2 disclose an epoxy resin / polyurethane mixture (B) which contains a diglycidyl ether of a bisphenol A-alkylene oxide adduct (A), an epoxy resin, and a polyurethane dispersed in the epoxy resin, and in which the polyurethane is a polyurethane obtained by reacting, in the epoxy resin, a polyisocyanate compound with a curing agent capable of reacting with the polyisocyanate compound. Patent Document 3 discloses a resin composition containing a compound having an epoxy group and a polyurethane containing a structural unit represented by general formula (II) in the molecule. Patent Document 4 discloses a polyurethane-modified epoxy resin obtained by modifying a bisphenol-based epoxy resin (a) with a medium- to high-molecular-weight polyol compound (b), a polyisocyanate compound (c), and a low-molecular-weight polyol compound (d) as a chain extender, using a predetermined amount of epoxy resin (a) and reacting the medium- to high-molecular-weight polyol compound (b) and the polyisocyanate compound (c) in predetermined amounts, and then adding a predetermined amount of the low-molecular-weight polyol compound (d). Patent Document 5 discloses a polycarbonate-modified epoxy resin in which a hydroxyl group-containing epoxy resin (A), a polyisocyanate compound (B) and a polycarbonate polyol (C) are essential reaction raw materials, and the polycarbonate polyol (C) is contained in a predetermined amount. Patent Document 6 discloses an epoxy resin composition for fiber-reinforced composite materials obtained by blending an epoxy resin (A), a urethane prepolymer (B) having a structure derived from a polyether polyol and having an isocyanate group or a hydroxyl group at both ends of the molecular chain, and a curing agent (C), in which (A) and (B) are compatible with each other before the curing reaction, and after the curing reaction, (A) forms a sea structure and (B) forms an island structure, and the resulting cured product of the epoxy resin composition has a sea-island phase-separated structure. The present invention proposes polyurethane-modified epoxy resins which satisfy the physical properties required for various applications and are excellent in heat resistance (Tg), fracture toughness (KIC) and tensile properties, by using a method different from the urethane modification methods disclosed in the prior patent documents 1 to 6.

[0005] In addition, when modifying epoxy resins with polyurethane, bisphenol-type epoxy resins with a hydroxyl equivalent of 2000 to 4000 g / eq are generally used as the raw material epoxy resin. Due to the large hydroxyl equivalent, a large amount of bisphenol-type epoxy resin is used, which poses the problem that the urethane concentration cannot be increased. Therefore, in epoxy compositions containing polyurethane-modified epoxy resins, there is a drawback in that the degree of freedom in design is limited and they cannot be applied to the properties required for various applications. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2007-284467 A [Patent Document 2] JP 2007-284474 A [Patent Document 3] JP 2007-224144 A [Patent Document 4] JP 2016-11409 A [Patent Document 5] JP 2017-226717 A [Patent Document 6] JP 2017-82128 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention aims to provide a novel polyurethane-modified epoxy resin composition and a cured product thereof which are used in, for example, casting materials, composite materials, structural adhesives, etc., and which do not experience a decrease in glass transition temperature and have an excellent balance between strength and fracture toughness of the cured product. [Means for solving the problem]

[0008] The present invention relates to a polyurethane-modified epoxy resin, which is prepared by modifying a bisphenol-based epoxy resin (a) represented by the following formula (1) having an epoxy equivalent of 150 to 300 g / eq and a hydroxyl equivalent of 800 to 2000 g / eq with a medium to high molecular weight polyol compound (b) having a number average molecular weight of 500 or more, a polyisocyanate compound (c) and a low molecular weight polyol compound (d) having a number average molecular weight of less than 500, wherein the epoxy resin (a) is used in an amount of 50 to 75% by weight based on the total amount of the components (a), (b), (c) and (d) and the component (d) is used in an amount of 5 to 10% by weight based on the total amount of the components (b) and (d). [ka] Here, R, R 1 are H or a methyl group, and a is a number from 0 to 10.

[0009] In the polyurethane-modified epoxy resin of the present invention, the medium- to high-molecular-weight polyol compound (b) preferably contains a polyester polyol compound (b-1) having an ester structure in the molecule and a non-polyester polyol compound (b-2), and the weight ratio of component (b-1) to component (b-2) is preferably 1:5 to 5:1.

[0010] The present invention relates to an epoxy resin composition comprising the polyurethane-modified epoxy resin. The epoxy resin composition of the present invention comprises, as essential components, a polyurethane-modified epoxy resin (A), a polyurethane-unmodified liquid epoxy resin (B) that is liquid at 30°C, and a curing agent (C), and it is preferable that the polyurethane-modified epoxy resin (A) is contained in an amount of 10 to 60% by weight based on the total weight (solid content) of the composition. The present invention relates to a resin molded product obtained by molding the above-mentioned epoxy resin composition. Effect of the Invention

[0011] By using an optimal amount of the polyurethane-modified epoxy resin of the present invention, the elastic modulus, strength, and fracture toughness of the cured product can be improved, and the glass transition temperature can be maintained high, making the resin composition and cured product suitable for use as adhesives, coating materials, electric and electronic materials, matrix resins for composite materials, etc. It becomes possible to increase the urethane concentration of the polyurethane-modified epoxy resin, expanding the degree of freedom in designing the composition and enabling it to be adapted to the required characteristics of various applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The polyurethane-modified epoxy resin of the present invention uses, as essential components, a specific bisphenol-based epoxy resin (a), a medium- to high-molecular-weight polyol compound (b) having a molecular weight of 500 or more, a polyisocyanate compound (c), and a low-molecular-weight polyol compound (d) having a molecular weight of less than 500. Preferably, the polyol compound (b) having a molecular weight of 500 or more includes a polyester polyol compound (b-1) and a non-polyester type polyol compound (b-2). Here, the non-polyester type polyol compound (b-2) refers to a polyol compound that does not have an ester structure in the molecule, unlike the polyester polyol compound (b-1). Each component will be described below.

[0013] The epoxy resin (a) to be polyurethane-modified is a bisphenol-based epoxy resin which is liquid at room temperature and is represented by the following general formula. [ka] In the formula, R 1 are each independently H or an alkyl group, and a is a number from 0 to 10. 1 When is an alkyl group, it preferably has 1 to 3 carbon atoms, and more preferably has 1 carbon atom. In particular, it is a bisphenol A type epoxy resin represented by formula (2) or a bisphenol F type epoxy resin represented by formula (3). [ka] In the formula, a1 and a2 are numbers from 0 to 10.

[0014] In the present invention, the epoxy resin (a) is characterized in that it is a secondary hydroxyl group-containing bisphenol-based epoxy resin that is liquid at room temperature and has an epoxy equivalent of 150 to 300 g / eq and a hydroxyl group equivalent of 800 to 2000 g / eq. Because the hydroxyl group equivalent is small, the urethane concentration of the resulting modified epoxy resin can be increased by using a small amount of the bisphenol-type epoxy resin. More preferably, the epoxy equivalent is 150 to 280 g / eq, and the hydroxyl equivalent is 800 to 1,600.

[0015] The medium- to high-molecular-weight polyol compound (b) preferably contains a polyester polyol (b-1) having an ester structure in the molecule and a non-polyester polyol compound (b-2), and the weight ratio of component (b-1) to component (b-2) is preferably 1:5 to 5:1.

[0016] As the polyester polyol compound (b-1), compounds having an aromatic, aliphatic, alicyclic or other structure can be used so long as they are polyols having an ester bond in the molecule. For example, those obtained by reacting an aliphatic diol compound with a dibasic acid component can be used, and specific examples of the diol compound include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,12-dodecanediol, diethylene glycol, 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,2-dimethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-ethyl-1,3-hexanediol, 2,4-diethyl-1,5-pentanediol, 1,4-cyclohexanedimethanol, 1,4-benzenedimethanol, polyethylene glycol 200, and polyethylene glycol 400. These diol compounds can be used alone or in combination of two or more. When using two or more in combination, it is preferable that the weight average molecular weight of each diol compound is 570 or less, preferably 550 or less. Among these, 3-methyl-1,5-pentanediol is particularly preferable in terms of physical properties. Examples of dibasic components include aliphatic dibasic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, acelic acid, sepacic acid, dodecanedioic acid, brassylic acid, and dimer acid, alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, and aromatic dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid. Among them, taking into consideration availability, it is preferable to use adipic acid, azelaic acid, sebacic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid. These dibasic acids may be used alone or in combination of two or more. Commercially available products include RX-4800, OD-X-2523, and OD-X-2547 manufactured by DIC Corporation, and P2010, P2011, P2020, P2050, and P5010 manufactured by Kuraray Co., Ltd.

[0017] The polyester polyol compound (b-1) has a molecular weight of 500 or more, and in consideration of flexibility and compatibility with other resins, it is particularly preferable that the number average molecular weight (Mn) is about 1000 to 4000.

[0018] Specific examples of the polyester polyol compound (b-1) include compounds represented by the following formula (4) or (5). [ka] Here, n is a number from 1 to 50.

[0019] As the non-polyester type polyol compound (b-2), one having a number average molecular weight (Mn) of 500 or more and other than the polyester polyol compound (b-1) is used.

[0020] In the polyol compounds (b) and (d), the OH groups may be secondary hydroxyl groups, but when they are primary hydroxyl groups, the reactivity is excellent.

[0021] The non-polyester polyol compound (b-2) is preferably a compound represented by any one of the following formulas (6) to (8), and may be used alone or in combination of two or more kinds. [ka] Here, R 2 is H or a methyl group, b1, b2, and b3 are independently numbers from 1 to 50, and c is a number of 0 or 1.

[0022] [ka] Here, q1, q2, q3, and q4 are independently numbers from 1 to 20. [ka] Here, r, s, and t are independently numbers from 1 to 20, and n is a number from 1 to 50.

[0023] The non-polyester polyol compound (b-2) preferably has a number average molecular weight (Mn) of 500 or more, a molecular structure of any one of the above formulas (6) to (8), and excellent compatibility with the epoxy resin (a). For example, polyethylene glycols and polypropylene glycols obtained by ring-opening polyaddition of ethylene oxide or propylene oxide to a polyhydric alcohol such as ethylene glycol or glycerin can be exemplified. In formula (6), c is 0, R 2 Polypropylene glycol represented by formula (9) in which is a methyl group is preferred from the viewpoints of availability and a good balance between price and properties. The number of OH groups in the polyol compound (b) may be 2 or more, and is preferably 2. [ka] Here, b1 and b2 are independently numbers from 1 to 50.

[0024] As the polypropylene glycol, a polypropylene glycol having a number average molecular weight (Mn) of 1500 to 5000, preferably 2000 to 4000, is preferred from the viewpoints of not thickening or semi-solidifying the polyurethane-modified epoxy resin composition and ensuring good tackiness, conformability to the bonding surface, castability, and good impregnation of carbon fibers and glass fibers of the composition.

[0025] The polyisocyanate compound (c) is represented by the formula (10), 4 is preferably a divalent group selected from the formulae (10a) to (10f). Among these, those having excellent compatibility with the epoxy resin (a) are preferred. Specific examples include toluene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI), hydrogenated xylylene diisocyanate (HXDI), isophorone diisocyanate (IPDI), naphthalene diisocyanate, etc., and MDI represented by formula (11) is preferred from the viewpoints of low molecular weight, no thickening, low cost, safety, etc. The number of NCO groups in the polyisocyanate compound (c) may be 2 or more, and is preferably 2. [ka] Here, R 4 is a divalent group selected from formulas 10a to 10f. [ka] [ka]

[0026] The low molecular weight polyol compound (d) is a polyol compound having a number average molecular weight of less than 500, more preferably less than 200. This is used as a chain extender. It is preferably a diol compound represented by formula (12) having two primary hydroxyl groups. [ka] Here, R 5 is an alkylene group represented by formula 12a, and g is a number from 1 to 10.

[0027] Specific examples of the low molecular weight polyol compound (d) include polyhydric alcohols such as 1,4-butanediol, 1,6-pentanediol, etc. In particular, 1,4-butanediol is more preferred in terms of availability and a good balance between price and properties.

[0028] Next, polyurethane-modified epoxy resins using each of the components (a), (b-1), (b-2), (c) and (d) will be explained along with the reaction mechanism. Each component can be used alone or in combination of two or more.

[0029] The OH groups in the epoxy resin (a) are mainly secondary OH groups. On the other hand, the OH groups in the polyester polyol compound (b-1) and the polyol compound (b-2) are mainly primary OH groups. Therefore, when the epoxy resin (a), the polyester polyol compound (b-1), the non-polyester polyol compound (b-2) and the polyisocyanate compound (c) are charged and reacted, the primary OH groups of the polyester polyol compound (b-1) and the non-polyester polyol compound (b-2) react preferentially with the NCO group of the polyisocyanate compound (c).

[0030] Typically, the primary OH groups in the polyester polyol compound (b-1) and polyol compound (b-2) react with the NCO groups in the polyisocyanate compound (c) first to produce the NCO-terminated urethane prepolymer (P1).Then, the secondary OH groups in the epoxy resin (a) react with some of the terminal NCO groups of the urethane prepolymer (P1) to form urethane bonds, which is thought to result in the urethane prepolymer (P2) with the epoxy resin (a) added to both ends or one end of the urethane prepolymer.

[0031] In other words, the urethane prepolymer (P) is thought to be a mixture of NCO-terminated urethane prepolymer (P1) and urethane prepolymer (P2) in which epoxy resin (a) has been added to both ends or one end of P1; however, because the molar ratio of NCO groups is large and a large excess of epoxy resin is used, it is thought that mainly urethane prepolymer (P2) in which epoxy resin has been added to both ends is produced.

[0032] The epoxy resin (a) to be urethane-modified is preferably used in an amount of 50 to 75% by weight based on the total amount of the components (a), (b-1), (b-2), (c) and (d). In other words, the urethane modification rate of the epoxy resin (a) or the urethane concentration of the resulting polyurethane-modified epoxy resin can be increased to 25 to 50% by weight. It is also possible to increase it to 35% by weight or more, and even 40% by weight or more.

[0033] As the charging ratio of epoxy resin (a) is increased, both ends or one end is blocked with epoxy resin (a), the terminal NCO groups are consumed, the amount of urethane prepolymer (P2) which does not react with the chain extender low molecular weight polyol compound (d) increases, the ratio of the original urethane prepolymer (P1) having NCO groups at the ends decreases, and the amount of polyurethane produced by the reaction between the terminal NCO groups of P1 and the OH groups of the chain extender low molecular weight polyol compound (d) decreases, so that the molecular weight distribution of the polyurethane modified epoxy resin also shifts to the lower molecular weight side.

[0034] Conversely, if the ratio of epoxy resin (a) is reduced, the amount of urethane prepolymer (P2) with both or one end blocked with epoxy resin (a) decreases, and the ratio of the original urethane prepolymer (P1) with NCO groups at the ends increases. Therefore, the amount of polyurethane produced by the reaction between the terminal NCO groups of P1 and the OH groups of the low molecular weight polyol compound (d), which is a chain extender, increases, and the molecular weight distribution of the polyurethane-modified epoxy resin is also thought to shift to the higher molecular weight side.

[0035] Epoxy resin (a) is often a mixture of a monomer with a repeat number a of 0 and a polymer with a repeat number a of 1 or more, but in the case of the polymer, it has a secondary OH group generated by ring-opening of the epoxy group. This OH group is reactive with the NCO group of the polyisocyanate compound (c) or the terminal NCO group of the urethane prepolymer (P), so the a=1 or more form in the epoxy resin (a) reacts with it. Note that the a=0 form, which does not have an OH group, does not participate in this reaction.

[0036] In the present invention, the epoxy resin (a) has an epoxy equivalent of 150 to 300 g / eq and a hydroxyl equivalent of 800 to 2000 g / eq, and is characterized by using a resin having a high proportion of polymers with a repeat number a, a1, or a2 of 1 or more. The average value (number average) of the repeat number a, a1, or a2 is Less than 1 The range is. Therefore , compared to general-purpose bisphenol-based epoxy resins Since there is little a=0 that is not involved in the reaction, the proportions of the other components (b), (c), and (d) are relatively high. This makes it possible to synthesize polyurethane-modified epoxy resins with a high urethane concentration.

[0037] The reason why epoxy resin compositions using polyurethane-modified epoxy resins exhibit high toughness is because the urethane-modified epoxy resin portion undergoes phase separation in the epoxy resin composition to form a sea-island structure. It is believed that in response to external stress, the phase-separated islands (polyurethane-modified epoxy resin portion) undergo plastic deformation to absorb energy, or absorb energy by interfacial peeling between the islands and the sea portion. For this reason, it becomes necessary to control the size and number of the islands, their adhesion to the sea portion, etc.

[0038] The size of the island part that undergoes phase separation is governed not only by the molecular weight of the polyurethane-modified epoxy resin, but also by its compatibility with the sea part. If the compatibility is low, phase separation between the sea part and the island part becomes prominent when the epoxy resin composition is cured, and the island part becomes larger and the number of islands decreases. Therefore, in order to form islands of a desired size and number, the polyurethane-modified epoxy resin of the island part needs a certain degree of compatibility (affinity) with the epoxy resin of the sea part. The compatibility is governed by the polar functional group in the polyurethane-modified epoxy resin structure. Until now, a non-polyester type polyol compound (b-2) with a molecular weight of 500 or more and a polyol compound (d) with a molecular weight of less than 500 formed a urethane bond with a polyisocyanate compound (c) to form a polar functional group, but if one tries to increase the polarity, the polyol compound (d) with a molecular weight of less than 500 is increased, and a polyurethane-modified epoxy resin with a small molecular weight is formed. Although the molecular weight is small, it is highly elastic, but it is difficult to impart toughness because the island part is small. Furthermore, when the amount of polyol compound (d) having a molecular weight of less than 500 is reduced, the amount of non-polyester polyol compound (b-2) having a molecular weight of 500 or more is increased relatively, resulting in an increase in the molecular weight and a decrease in the compatibility with the epoxy resin in the sea portion, resulting in an increase in the size of the islands and a decrease in their number, and similarly making it difficult to impart sufficient toughness. Therefore, in the present invention, by using the polyester polyol compound (b-1), it is possible to appropriately increase the compatibility with the sea part while maintaining the molecular weight of the island part without excessively increasing the amount of the component (d), and it is believed that this makes it possible to express high toughness. It is also believed that the introduction of a rigid structure into the polyester polyol compound makes it possible to achieve high elasticity.

[0039] As a result of considering the optimization of such a composition, it is found that the amount of polyol compound (d) having a molecular weight of less than 500 is preferably 5 to 10% by weight based on the total amount of all polyols forming urethane bonds, i.e., the total amount of components (b-1), (b-2) and (d), and more preferably 8% by weight or less.

[0040] The polyester polyol compound (b-1) is preferably contained in a ratio of 1:5 to 5:1 relative to the non-polyester type polyol compound (b-2). If the ratio is less than 1:5, the effect of high elasticity due to the rigid structure of the component (b-1) is reduced, and if the ratio is more than 5:1, the effect of high elasticity of the component (b-1) is expressed, but the effect of high toughness of the component (b-2) is reduced. A ratio of 1:2 to 2:1 is particularly preferred. The amount of polyester polyol compound (b-1) used is preferably 15 to 80% by weight, more preferably 20 to 70% by weight, and even more preferably 30 to 65% by weight, based on the total amount of all polyols forming urethane bonds, i.e., the total amount of components (b-1), (b-2), and (d).

[0041] The weight average molecular weight (Mw) of the polyurethane-modified epoxy resin is preferably 3,000 or more and 30,000 or less, and more preferably 5,000 or more.

[0042] As a method for producing the polyurethane-modified epoxy resin used in the present invention, for example, the epoxy resin (a) is used in an amount of 50 to 75% by weight based on the total amount of the polyester polyol compound (b-1), the non-polyester type polyol compound (b-2), the polyisocyanate compound (c) and the polyol compound (d), and the polyester polyol compound (b-1), the non-polyester type polyol compound (b-2) and the polyisocyanate compound (c) are reacted in the presence of the epoxy resin (a) (reaction 1). In this reaction 1, the reaction of the polyester polyol compound (b-1) and the polyol compound (b-2) with the polyisocyanate compound (c) occurs preferentially, and the urethane prepolymer (P1) is generated. After that, a part of the urethane prepolymer (P1) reacts with the epoxy resin (a), and the urethane prepolymer (P2) with both ends epoxidized is mainly generated, and it is preferable that the mixture is formed with the urethane prepolymer (P2) with one end epoxidized and the urethane prepolymer (P1) with both ends remaining NCO, which is generated in a small amount.

[0043] In the reaction of the urethane prepolymer (P1) with the epoxy resin (a), it is necessary to react the low-reactive secondary OH groups in the epoxy resin (a) with NCO groups to produce urethane bonds, so the reaction temperature is preferably in the range of 80 to 150°C and the reaction time is preferably in the range of 1 to 5 hours.

[0044] Then, a low molecular weight polyol compound (d) is added so that the molar ratio (P):(d) of the NCO group in the urethane prepolymer (P) to the OH group in the low molecular weight polyol compound (d) is in the range of 0.9:1 to 1:0.9, and a polyurethane reaction is carried out (reaction 2). Note that the epoxy group of the epoxy resin and the OH group of the polyol compound (d) do not react with each other because they are alcoholic OH groups.

[0045] The reaction temperature of Reaction 2 is preferably in the range of 80 to 150°C, and the reaction time is preferably in the range of 1 to 5 hours. However, since Reaction 2 is a reaction between the NCO group and the OH group in the low-molecular-weight polyol compound (d), milder conditions than Reaction 1 may be used.

[0046] A catalyst can be used as necessary in the course of the reactions (Reactions 1 and 2). The catalyst is used for the purpose of sufficiently completing the formation of the urethane bond, and examples of the catalyst include amine compounds such as ethylenediamine, tin compounds, and zinc compounds.

[0047] In reaction 2, the small amount of urethane prepolymer (P1) having NCO at both or just one end reacts with the low molecular weight polyol compound (d) to extend the chain length and form polyurethane, while the urethane prepolymer (P2) having both ends an adduct of epoxy resin (a) remains unreacted. Therefore, the polyurethane-modified epoxy resin obtained by reactions 1 and 2 is a mixture of mainly a resin component in which epoxy resin (a) is attached to both ends of the urethane prepolymer (P), a minor component being a resin component in which epoxy resin (a) is attached to one end of the urethane prepolymer (P) and the other end is an NCO group, a resin component in which both ends of the urethane prepolymer (P) are NCO groups, and unmodified epoxy resin (a).

[0048] The epoxy resin composition of the present invention is characterized in that it contains, as essential components, a polyurethane-modified epoxy resin (A), a polyurethane-unmodified liquid epoxy resin (B) serving as an adjuster for the polyurethane concentration, and an amine-based curing agent (C), and contains 10 to 60% by weight of the polyurethane-modified epoxy resin (A) relative to the total weight (solid content) of the epoxy resin composition.

[0049] If necessary, the resin composition of the present invention may contain other epoxy resins (D) for fine adjustment of viscosity and Tg, curing accelerators (E), and inorganic fillers such as calcium carbonate, talc, and titanium dioxide as extenders and reinforcing materials.

[0050] The polyurethane-unmodified liquid epoxy resin (B) is not particularly limited as long as it is an epoxy resin that is not polyurethane-modified and is liquid at 30°C. However, bisphenol A type epoxy resin or bisphenol F type epoxy resin is preferred from the viewpoints of availability and a good balance between price and properties.

[0051] The polyurethane concentration in the epoxy resin composition can be increased or decreased by increasing or decreasing the amount of the liquid epoxy resin (B). The polyurethane concentration in the epoxy resin composition is calculated by the following formula: Polyurethane concentration = {(b-1) + (b-2) + (c) + (d)} x 100 / {(a) + (b-1) + (b-2) + (c) + (d) + (B) + (C)} Here, (a) to (d), (B), and (C) are the weights of the corresponding essential components. When other components, such as other epoxy resins (D) and curing accelerators (E), are added to the essential components, the amounts of these other components are added to the denominator.

[0052] As the polyurethane concentration in the cured product increases, the properties of the cured product, such as bending strain, impact strength, and glass transition temperature, change. In general, as the polyurethane concentration increases, the bending strain and impact strength of the cured product tend to increase.

[0053] When a liquid bisphenol A type epoxy resin or a liquid bisphenol F type epoxy resin is used as the polyurethane-unmodified liquid epoxy resin (B), the polyurethane modification rate (=polyurethane concentration) in the cured product is preferably in the range of 7 to 15 wt %.

[0054] As the amine-based curing agent (C), dicyandiamide (DICY) or its derivatives are used because they can be made into a one-component solution with excellent storage stability and are easily available.

[0055] When the curing agent is DICY, the amount of the amine curing agent (C) is set so that the ratio of the number of moles of epoxy groups in the total epoxy resin including the polyurethane-modified epoxy resin and the polyurethane-unmodified epoxy resin (B) to the number of moles of active hydrogen groups in DICY is in the range of 1:0.3 to 1:1.2, preferably 1:0.9 to 1:1.1, from the viewpoint of the properties of the cured product.

[0056] In the epoxy resin composition of the present invention, a multifunctional epoxy resin having three or more functionalities can be used as the other epoxy resin (D) in order to finely adjust the viscosity or increase Tg. When a multifunctional epoxy resin is used, the crosslink density increases, the phase separation state changes, or the fracture toughness is lost, so it is preferable to use 0.1 to 10% by weight based on the total composition weight. Examples of multifunctional epoxy resins having three or more functionalities include phenol novolac type epoxy resins, cresol novolac type epoxy resins, glycidylamine type epoxy resins such as tetraglycidyldiaminodiphenylmethane, glycidylphenyl ether type epoxy resins such as tetrakis(glycidyloxyphenyl)ethane and tris(glycidyloxyphenyl)methane, and glycidylamine type and glycidylphenyl ether type epoxy resins such as triglycidylaminophenol. Furthermore, epoxy resins obtained by modifying these epoxy resins, and brominated epoxy resins obtained by brominating these epoxy resins can be used.

[0057] The epoxy resin composition of the present invention may further contain a curing accelerator (E). As the curing accelerator (E), a crystalline imidazole compound such as 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid addition salt (2MA-OK) or a urea compound such as 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU) may be used. The amount of the curing accelerator (E) is preferably in the range of 0.1 to 5 wt% based on the total amount of the epoxy resin including the polyurethane-modified epoxy resin and the polyurethane-unmodified liquid epoxy resin (B) and the curing agent (D).

[0058] The epoxy resin composition of the present invention does not impair processability such as tackiness, conformability to a bonding surface, castability into a mold, and impregnation into carbon fiber, glass fiber, and fabrics made of these.

[0059] A cured product of the epoxy resin composition of the present invention can be obtained by casting the epoxy resin composition into a mold, or applying it as an adhesive to an adherend and laminating it, or applying it as a paint to an object to be coated, or impregnating carbon fiber, glass fiber, or woven fabrics thereof with the composition, and then heating it to a temperature of 80°C to 200°C and maintaining it for several hours.

[0060] The cured product of the epoxy resin composition of the present invention has a glass transition temperature (Tg) of 120°C or higher, a tensile elasticity of 2.8 GPa or higher, a tensile strength of 80 MPa or higher, a tensile elongation of 6.5% or higher, and a fracture toughness of 1.7 MPa m 1 / 2 It can be more than that. EXAMPLES

[0061] The present invention will now be described in detail with reference to examples. The present invention is not limited to these examples, and various modifications and alterations are possible without departing from the gist of the present invention. The physical properties were evaluated as follows.

[0062] (1) Determination of the presence or absence of residual NCO groups by IR: 0.05 g of the obtained polyurethane-modified epoxy resin was dissolved in 10 ml of tetrahydrofuran, and then applied to a KBr plate using a Micro Spatula flat plate. The plate was dried at room temperature for 15 minutes to evaporate the tetrahydrofuran and prepare a sample for IR measurement. This was set in a PerkinElmer FT-IR Spectrum-One device and the characteristic absorption band of the NCO group, 2270 cm -1 When the stretching vibration absorption spectrum of the compound disappeared, it was determined that no remaining NCO groups existed. (2) Epoxy equivalent: Quantified according to JIS K 7236. (3) Hydroxyl equivalent: 25 ml of dimethylformamide is placed in a 200 ml glass-stoppered Erlenmeyer flask, and a sample containing 11 mg / equivalent or less of hydroxyl is added and dissolved. 20 ml of 1 mol / L-phenylisocyanate toluene solution and 1 ml of dibutyltin maleate catalyst solution are added with a pipette, shaken well to mix, and then sealed and allowed to react for 30 to 60 minutes. After the reaction is complete, 20 ml of 2 mol / L-dibutylamine toluene solution is added, shaken well to mix, and left for 15 minutes to react with the excess phenylisocyanate. Next, 30 ml of methyl cellosolve and 0.5 ml of bromocresol green indicator are added, and the excess amine is titrated with a standardized methyl cellosolve perchlorate solution. The indicator changes from blue to green and then to yellow, so the first point at which it turns yellow is taken as the end point, and the hydroxyl equivalent is calculated using the following formulas I and II. Hydroxyl group equivalent (g / eq)=(1000×W) / C(SB) (i) C: Concentration of methyl perchlorate cellosolve solution (mol / L) W: sample weight (g) S: Titration volume of methyl perchlorate cellosolve solution (ml) B: The amount of methyl perchlorate cellosolve solution required for the blank test during titration (ml) C=(1000×W) / {121×(sb)}···(ii) w: Amount of tris-(hydroxymethyl)-aminomethane weighed for standardization (g) s: Amount of methyl perchlorate cellosolve solution required for the titration of tris-(hydroxymethyl)-aminomethane (ml) b: Titration volume (ml) of methyl perchlorate cellosolve solution required for blank test during standardization

[0063] (4) Glass transition temperature (Tg): Using a differential scanning calorimeter (DSC) at a heating rate of 10° C. / min, the intersection of the tangent line at the baseline and the inflection point was determined as the glass transition temperature (Tg). (5) Tensile test: The cured material was molded into a shape according to JIS K 7161 by casting into a mold to prepare a test piece. A tensile test was carried out at room temperature of 23°C using a universal testing machine to measure the tensile strength, tensile elongation, and tensile modulus of elasticity. (6) Fracture toughness (KIC): Test pieces were prepared by casting the cured material into the shape specified in JIS K 6911, and tested using a universal testing machine at a room temperature of 23°C and a crosshead speed of 0.5 mm / min. Before testing, notches were made in the test pieces by placing a razor blade on the test piece and impacting the razor blade with a hammer.

[0064] The raw materials used are as follows: Ingredient A Epoxy resin (a): Nippon Steel Chemical & Material Epotohto YDF-170, bisphenol F type epoxy resin, epoxy equivalent 170g / eq, hydroxyl equivalent 2600g / eq Nippon Steel Chemical & Material Co., Ltd. Epotohto YD-128, bisphenol A type epoxy resin, epoxy equivalent 187g / eq, hydroxyl equivalent 3000g / eq Developed product 1: Bisphenol F type epoxy resin, epoxy equivalent 192g / eq, hydroxyl equivalent 1500g / eq Developed product 2: Bisphenol A type epoxy resin, epoxy equivalent 262g / eq, hydroxyl equivalent 915g / eq Medium to high molecular weight polyester polyol (b-1): Kuraray P2020, polyester diol, number average molecular weight 2000, hydroxyl equivalent 1020g / eq Medium to high molecular weight non-polyester polyol (b-2): ADEKA ADEKA Polyether P-2000, polypropylene glycol, number average molecular weight 2000, hydroxyl equivalent 1020g / eq Polyisocyanates (c): Mitsui Chemicals Cosmonate PH, 4,4'-diphenylmethane diisocyanate Low molecular weight polyol (d): 1,4-Butanediol (reagent), molecular weight 90 Component B Liquid epoxy resin (B): Epotohto YD-128 made by Nippon Steel Chemical & Material, bisphenol A type epoxy resin, epoxy equivalent 187g / eq, hydroxyl equivalent 3000g / eq Component C Hardener: EVONIK DICYANEX 1400F, dicyandiamide Component E Crystalline imidazole manufactured by Shikoku Chemical Industry Co., Ltd., Curesol 2MA-OK, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct salt

[0065] Synthesis Example 1 Bisphenol F epoxy resin (Development Product 1) as epoxy resin (a), Kuraray P2020 as polyester polyol (b-1), and Adeka Polyether P-2000 as non-polyester polyol (b-2) were charged in a 1000 ml four-neck separable flask equipped with a nitrogen inlet tube, stirrer, and temperature controller in the weights shown in Table 1, and mixed at room temperature for 15 minutes. Next, Cosmonate PH was charged in the same flask as polyisocyanate (c) in the weight shown in Table 1, and reacted at 120 °C for 2 hours. Thereafter, 1,4-butanediol was charged as a chain extender, low molecular weight polyol (d), in the weight shown in Table 1, into the same flask, and the mixture was reacted at 120°C for 2 hours to obtain a polyurethane-modified bisphenol F type epoxy resin (resin 1). Here, the epoxy resin (a) was charged at 70% by weight relative to 100% by weight of the product of reaction 2. Compound (d) was charged at 7% by weight relative to the total amount of compounds (b-1), (b-2), and (d). Compounds (b-1) and (b-2) were charged at a weight ratio of 1:1. The completion of the reaction was confirmed by the disappearance of the absorption spectrum of the NCO group by IR measurement. The epoxy equivalent of the obtained polyurethane-modified bisphenol F type epoxy resin (resin 1) was 275 g / eq and Mw was 5500.

[0066] Synthesis Examples 2-11 Except for using the raw material compositions as shown in Tables 1 and 2, the reaction was carried out in the same manner as in Synthesis Example 1 to obtain polyurethane-modified bisphenol-type epoxy resins (resins 2 to 11).

[0067] [Table 1]

[0068] [Table 2]

[0069] Next, examples of epoxy resin compositions and cured epoxy resin products using the polyurethane-modified epoxy resins (resins 1 to 11) obtained in the above-mentioned Synthesis Examples 1 to 11 will be shown. The results are also summarized in Tables 3 and 4.

[0070] Example 1 The polyurethane-modified bisphenol F epoxy resin (resin 1) obtained in Synthesis Example 1 as the polyurethane-modified epoxy resin (A), Epotohto YD-128 as the polyurethane-unmodified liquid epoxy resin (B), dicyandiamide as the curing agent (C), and 2MAOK as the curing accelerator (E) were charged in a 300 ml dedicated disposable cup in the proportions shown in Table 2, and the mixture was stirred and mixed while vacuum degassing for 5 minutes using a vacuum planetary mixer for rotation and revolution laboratory to obtain a liquid resin composition. Here, the molar ratio of epoxy groups to dicyandiamide was 1:0.5, and 140 g of a polyurethane-modified bisphenol F epoxy resin composition was prepared with a polyurethane concentration of 12 wt% in the cured product. This liquid resin composition was then poured into a metal mold having the shape specified in JIS K7161. The metal mold into which the resin had been poured was then placed in a hot air oven and heat cured at 120°C for 50 minutes and then at 150°C for 50 minutes to prepare a cured epoxy resin test piece. The test results using this test piece are shown in Table 2.

[0071] Examples 2 to 7, Reference Examples 1 and 2, Comparative Examples 1 and 2 Polyurethane-modified bisphenol F-type epoxy resin compositions with different polyurethane concentrations in the cured products were prepared in the same manner as in Example 1, except that the polyurethane-modified epoxy resin (A), unmodified liquid epoxy resin (B), curing agent (C) and curing accelerator (E) were mixed in the compositions shown in Tables 3 and 4. Next, the liquid resin composition was poured into a mold and heat-cured to prepare a test piece for property evaluation in the same manner as in Example 1. The physical properties and test results of the obtained composition are shown in Tables 3 and 4. In each table, the blend amount is shown in grams.

[0072] It was confirmed that the compositions containing the urethane-modified epoxy resin using the bisphenol-based epoxy resin having a hydroxyl equivalent of 800 to 2000 g / eq in Examples 1 to 7 were excellent in heat resistance (Tg), fracture toughness (KIC) and tensile properties, and had both high elasticity and high toughness. In addition, by using an epoxy resin with a small hydroxyl equivalent as the raw material for urethane modification, it is possible to increase the urethane concentration of the polyurethane-modified epoxy resin, thereby expanding the design freedom of the composition and enabling it to be adapted to the required properties of various applications.

[0073] [Table 3]

[0074] [Table 4]

Claims

1. A polyurethane-modified epoxy resin, which is obtained by modifying a bisphenol-based epoxy resin (a) represented by the following formula (1) having an epoxy equivalent of 150 to 300 g / eq and a hydroxyl equivalent of 800 to 2000 g / eq with a medium- to high-molecular-weight polyol compound (b) having a number average molecular weight of 500 or more, a polyisocyanate compound (c) and a low-molecular-weight polyol compound (d) having a number average molecular weight of less than 500, wherein the epoxy resin (a) is used in an amount of 50 to 75% by weight based on the total amount of components (a), (b), (c) and (d), and component (d) is used in an amount of 5 to 10% by weight based on the total amount of components (b) and (d), the medium- to high-molecular-weight polyol compound (b) contains a polyester polyol compound (b-1) having an ester structure in the molecule and a non-polyester polyol compound (b-2), and the weight ratio of component (b-1) to component (b-2) is 1:5 to 5:

1. 【Chemistry 1】 Here, R, R 1 are H or a methyl group. a is the number of repetitions, and the average value of a is less than 1.

2. An epoxy resin composition comprising the polyurethane-modified epoxy resin according to claim 1.

3. 3. The epoxy resin composition according to claim 2, comprising as essential components a polyurethane-modified epoxy resin (A), a polyurethane-unmodified liquid epoxy resin (B) that is liquid at 30°C, and a curing agent (C), wherein the polyurethane-modified epoxy resin (A) is contained in an amount of 10 to 60% by weight based on the total weight (solid content) of the composition.

4. A resin molded product obtained by molding the epoxy resin composition according to claim 2.

Citation Information

Patent Citations

  • New urethane polymer alloy containing reactive epoxy-functional group

    JP1991119020A

  • Resin composition

    JP2007224144A

  • Epoxy resin composition

    JP2007284467A

  • Epoxy resin composition

    JP2007284474A

  • Polyurethane modified epoxy resin, manufacturing method therefor, epoxy resin composition and cured article

    JP2016011409A