Polymerization process of tetrafunctional long-chain branched polyolefin resin
The 'ladder branching' mechanism in polymer synthesis using multichain catalysts and dienes addresses the challenges of gel formation and reactor fouling, enabling high levels of long chain branching for improved polymer properties.
Patent Information
- Application Number
- JP2021515217
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-28
- Filing Date
- 2019-09-27
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2039-09-27
AI Technical Summary
Existing methods for synthesizing long chain branched polymers, such as polyethylene and polypropylene, face challenges in controlling the amount of branching, leading to issues like gel formation and reactor fouling, and traditional processes struggle to achieve high levels of long chain branching efficiently.
A process involving a multichain catalyst and diene comonomers is used to synthesize long chain branched polymers through a 'ladder branching' mechanism, where two polymer chains are connected during polymerization in a concerted manner, avoiding gel formation and reactor fouling.
The process achieves stable molecular weight distribution and high levels of long chain branching, resulting in polymers with improved mechanical and thermal properties, as well as enhanced processing characteristics.
Smart Images

Figure 0007587494000084 
Figure 0007587494000085 
Figure 0007587494000086
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 738,621, filed Sep. 28, 2018, the entire disclosure of which is incorporated herein by reference.
[0002] SUMMARY OF THE DISCLOSURE Embodiments of the present disclosure relate generally to polymer compositions having long chain branching and processes by which the polymer compositions are synthesized. [Background technology]
[0003] Olefin-based polymers, such as polyethylene and polypropylene, are produced through various catalyst systems. The selection of such catalyst system used in the polymerization process of an olefin-based polymer is an important factor that contributes to the characteristics and properties of such an olefin-based polymer.
[0004] Polyethylene and polypropylene are manufactured for a wide variety of products. The polyethylene and polypropylene polymerization process can be varied in several ways to produce a wide variety of resulting polyethylene resins with different physical properties that make the various resins suitable for use in different applications. The amount of short chain branching in a polyolefin affects the physical properties of that polyolefin. The effect of branching on the properties of polyethylene depends on the length and amount of branching. Short branching primarily affects the mechanical and thermal properties. At high frequencies of short chain branching, the polymer is unable to form lamellar crystals, resulting in reduced mechanical and thermal properties. Small amounts of long chain branching can significantly alter the processing properties of the polymer.
[0005] To form long chain branches, the vinyl or terminal double bonds of a polymer chain are incorporated into a new polymer chain. Reincorporation of vinyl terminated polymers and introduction of diene comonomers are two mechanisms by which vinyl groups of a polymer chain are incorporated into a second polymer chain. Furthermore, long chain branching is induced via radicals. It is difficult to control the amount of branching in all three mechanisms. Using radicals or dienes to initiate long chain branching can lead to too much branching, thereby causing gelation and fouling of the reactor. The reincorporation mechanism does not produce many branches, and branching can only occur after the polymer chains are generated, thereby further limiting the amount of branching that can occur. Summary of the Invention
[0006] An embodiment of the present disclosure includes a process for synthesizing a long chain branched copolymer. The process comprises the steps of: 2 -C 14 The method comprises contacting an alkene monomer, at least one diene or polyene, optionally a solvent, and a multi-chain catalyst with each other. The multi-chain catalyst comprises multiple polymerization sites and is C 2 -C 14 At least two polymer chains of alkene monomers are produced, with each polymer chain polymerizing at one of the polymerization sites. This process synthesizes long-chain branched polymers by connecting two polymer chains with a diene or polyene, and the joining of the two polymer chains occurs in a concerted manner during polymerization.
[0007] Various embodiments of the process occur in a solution polymerization reactor or a particle-forming polymerization reactor such as a slurry reactor or a gas phase reactor, the molecular or solid supported catalyst is delivered to or generated in the reaction medium, the reactor system is batch, continuous or hybrid such as semi-batch, and the reactor residence time distribution is narrow, such as in non-backmixed reactors, or broad, such as in backmixed reactors and series and recycle reactors. [Brief description of the drawings]
[0008] [Figure 1] 1 is a graphical representation of polymer molecular weight as the number of branched methines per 1000 carbons increases. [Diagram 2] 1 is a graphical model predicting the dependence of molecular weight distribution (MWD) curves on branching level. [Diagram 3] 1 is a graphical model predicting the dependence of relative peak molecular weight on branching level. [Figure 4] 1 is a graphical representation of the predicted dependence of molecular weight distribution (MWD) curves on trifunctional diene branching level. [Diagram 5] 1 is a graphical representation of the predicted dependence of relative peak molecular weight (MW) on trifunctional diene branching level. [Figure 6] FIG. 1 is a graphical representation of the model predicted effect of branching on peak molecular weight (Mp) for branches per polymer molecule for traditional diene branching (solid line) and "ladder branching" (dashed line). [Figure 7] FIG. 1 is a graphical representation of the model predicted effect of branching on weight average molecular weight (Mw) for branches per polymer molecule for traditional diene branching (solid line) and “ladder branching” (dashed line). [Figure 8] 1 is a graphical representation of the model predicted effect of branching on peak weight average molecular weight (Mp) (solid line) (vs. Bc) for branches per linear segment of conventional diene branching and Mp (dashed line) (vs. Rc) for "ladder branched" polymers. [Figure 9] FIG. 1 is a graphical representation of the model predicted effect of branch weight average molecular weight (Mw) on branches per linear segment for conventional diene branching (for Bc) (solid line) and for “ladder branched” polymers (dashed line) (for Rc). [Figure 10] Graphical representation of the MWD slope used to calculate the shape metrics G(79 / 29) and G(96 / 08), where S(X) is the slope at X% of the MWD height. G(A / B)=(S(A)-S(B)) / S(A). [Figure 11]FIG. 1 is a graphical representation of the model-predicted molecular weight distribution (MWD) shape metric G(79 / 29) comparing conventional branching and "ladder branching" as a function of branching level, expressed as relative peak MW (Mp / Mpo). [Figure 12] FIG. 1 is a graphical representation of the model-predicted MWD shape metric G(79 / 29) comparing conventional branching and "ladder branching" as a function of branching level expressed as relative weighted average MW (Mw / Mwo). [Figure 13] FIG. 1 is a graphical representation of the model-predicted MWD shape metric G(98 / 08) comparing conventional and "ladder bifurcation" as a function of branching level expressed as relative peak MW (Mp / Mpo). [Figure 14] FIG. 1 is a graphical representation of the model predicted MWD shape metric G(98 / 08) comparing conventional branching and "ladder branching" as a function of branching level expressed as relative weighted average MW (Mw / Mwo). [Figure 15] 1 is a graphical representation of a MWD curve showing how the point of maximum slope is used to define a high MWD tail area metric. [Figure 16] Figure 10: Model predicted MWD area metric AHIGH comparing conventional branching and "ladder branching" as a function of branching level expressed as relative weight average molecular weight (Mp / Mpo). [Figure 17] 1 is a model predicted MWD area metric AHIGH comparing conventional branching and "ladder branching" as a function of branching level expressed as relative peak molecular weight (Mw / Mwo). [Figure 18] A model predicted MWD area metric ATAIL comparing conventional branching and "ladder branching" as a function of branching level expressed as relative peak molecular weight (Mp / Mpo). [Figure 19] Figure 1 is a model predicted MWD area metric ATAIL comparing conventional branching and "ladder branching" as a function of branching level expressed as the conventional relative weight average molecular weight (Mw / Mwo). [Figure 20]1 is a graph of absolute molecular weight distribution (MWD) curves measured by GPC for Example Series 2.4 recorded in Table 2. [Figure 21] 1 is a conventional molecular weight distribution curve measured by conventional gel permeation chromatography (GPC). [Figure 22] This is an absolute molecular weight distribution curve measured by GPC triple light scattering detector (also called absolute GPC). [Diagram 23] 1 is a graph of extensional viscosity measured as a function of time in seconds for a "ladder branched" polymer resin. [Figure 24] 1 is a graph of melt strength (cN) as a function of speed (mm / s) for a "ladder branching" polymer resin. [Diagram 25] 1 is a conventional molecular weight distribution curve of an unbranched ethylene-based polymer and a "ladder-branched" polymer resin as measured by GPC. [Figure 26] 1 is a diagram showing absolute molecular weight distribution curves of unbranched ethylene-based polymers and "ladder-branched" polymer resins measured by GPC triple light scattering detector. [Figure 27] 1 is a graph of extensional viscosity measured as a function of time in seconds for a "ladder branched" polymer resin. [Figure 28] 1 is a graph of melt strength (cN) as a function of speed (mm / s) for a "ladder branching" polymer resin. [Figure 29] 1 is a GPC triple light scattering detector absolute molecular weight distribution curve for two comparative examples with no diene and four samples with varying amounts of diene. [Figure 30A] 1 is a graph of absolute molecular weight distributions of comparative conventional branched polymer samples having varying amounts of diene. [Figure 30B] 1 is a graph of conventional molecular weight distributions of comparative conventional branched polymer samples having varying amounts of diene. [Diagram 31] 1 is a graph of the rheological ratio as a function of average g' for various polymer resins and for a "ladder branched" polymer resin. [Diagram 32]1 is a graph of the rheological ratio as a function of polydispersity index (PDI) for various polymer resins and for a "ladder branched" polymer resin. [Diagram 33] FIG. 1 is a graph of melt strength (centinewtons, cN) as a function of melt index (LogI2) for polymers produced with single-chain and double-chain catalysts, with additional lines showing linear polyethylene, tubular low density polyethylene, and autoclaved low density polyethylene. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Next, the process for synthesizing the polymer of the present disclosure and the specific embodiment of the polymer synthesized by the process will be described.It should be understood that the process for synthesizing the polymer of the present disclosure may be embodied in different forms and should not be construed as being limited to the specific embodiment described in this disclosure.Rather, the embodiment is provided so that this disclosure will be thorough and complete, and will fully convey the scope of the subject matter to those skilled in the art.
[0010] definition The term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether the monomers are the same or different types. Thus, the generic term polymer encompasses the term "homopolymer," which is commonly used to refer to a polymer prepared from only one type of monomer, and "copolymer," which refers to a polymer prepared from two or more different monomers. As used herein, the term "interpolymer" refers to a polymer prepared by polymerization of at least two different types of monomers. Thus, the generic term interpolymer includes copolymers and polymers prepared from three or more different monomers, such as terpolymers.
[0011] "Polyethylene" or "ethylene-based polymer" is intended to mean a polymer containing more than 50% by weight of units derived from ethylene monomer. This includes polyethylene homopolymers or copolymers (meaning units derived from two or more comonomers). Common forms of polyethylene known in the art include low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (ULDPE), very low density polyethylene (VLDPE), single-site catalyzed linear low density polyethylene (m-LLDPE) containing both linear and substantially linear low density resins, medium density polyethylene (MDPE), and high density polyethylene (HDPE).
[0012] An embodiment of the present disclosure is 2 Monomer, optionally at least one C 3 -C 12 The process includes synthesizing a long-chain branched polymer by adding an alpha-olefin comonomer, at least one diene, a multi-chain catalyst, and optionally a solvent, where the multi-chain catalyst comprises a molecule with multiple polymerization sites to produce at least two copolymer chains, each copolymer chain copolymerizing at one of the polymerization sites, and synthesizing a long-chain branched polymer by connecting the two copolymer chains with a diene, where the connecting of the two copolymer chains is performed in a concerted manner with the copolymerization.
[0013] The synthesis process of polymers according to the present disclosure differs from traditional long chain branching. The term "long chain branching" refers to a branch having more than 100 carbon atoms. "Branch" refers to a portion of a polymer that extends from a tertiary or quaternary carbon atom. If a branch extends from a tertiary carbon atom, there are two other branches, which collectively may be the polymer chain from which the branch extends. Traditionally, long chain branching (LCB) can occur naturally in the polymerization process, as shown in Scheme 1. This can occur by vinyl terminating the polymer chain and reinserting the polymeric vinyl, creating a trifunctional long chain branch. Depending on the degree of branching, various methods can be used to determine LCB, such as nuclear magnetic resonance (NMR), or to distinguish the effect of LCB in a polymer. For example, the effect of LCB is observed in shear flow in van Gurp-Palmen analysis, and the increase in shear viscosity at low angular frequencies and the strength of shear thinning behavior can be attributed to LCB. In extensional flow, the effect of LCB is usually identified in the degree of hardening or strength of the melt and the maximum deformation achieved. Achieving high levels of natural LCB in the polymer is difficult because the concentration of vinyl-terminated polymers is limited (maximum one per polymer chain) and because high ethylene conversion must be carried out to ensure the formation of LCB. To ensure high conversion, the ethylene concentration in the reactor is low, so that a large amount of vinyl-terminated polymer can be reinserted into a second polymer chain. [ka]
[0014] In Scheme 1, "Cat" is the catalyst and "P" is the polymer chain.
[0015] There is minimal long chain branching formed through naturally occurring branching processes. One way to enhance LCB is to add α,ω-dienes to the polymerization system, whether it is a radical, heterogeneous, or homogeneous process. Generally, dienes are added to the polymer chain in a similar manner to α-olefins, but leave pendant vinyl groups that can once again insert into the polymer chain to produce LCB, as shown in Scheme 2. In general, the length of the diene is not important, only that it be able to link two polymer chains together. In principle, the concentration of the pendant vinyl can be controlled by the amount of diene added to the reactor. Thus, the degree of LCB can be controlled by the concentration of the pendant vinyl. [ka]
[0016] In Scheme 2, "Cat" is the catalyst, "P" is the polymer chain, and the diene in this example is 1,5-hexadiene.
[0017] Traditional processes incorporating dienes into polymer synthesis systems suffer from fundamental defects: gel formation or reactor fouling. Kinetic modeling, which will be described in the following paragraphs, may provide excellent predictive results that help to better understand gel formation. For example, longer polymer chains have more olefins inserted, and therefore more dienes inserted, and therefore more pendant vinyls, meaning that the longer polymer chains are more likely to reinsert into the catalyst to form LCBs. Thus, the longer polymer chains preferentially reinsert to form even larger polymer molecules, tetrafunctional branches, resulting in the gel problem. As shown in Scheme 2, the tetrafunctional LCBs have short segments (the number of carbons between the two double bonds of the diene) that bridge the two long chains on either side of the short segments. The weight average molecular weight (M) as a function of branching w ) and number average molecular weight (M n A simulation of the Mn As goes to infinity, M w increases only slightly. w If the .DELTA..times..times.200,000 grams per mole (g / mol), the polymer will gel, gelation will occur, or reactor fouling will occur.
[0018] The term "gel" or "gelation" refers to a solid that consists of at least two components, the first being a three-dimensional cross-linked polymer, and the second being a medium in which the polymer is not completely soluble. If the polymer gels and does not completely dissolve, the reactor can become contaminated with the polymer gel.
[0019] The term "ladder branched" polymer refers to a tetrafunctional long chain branched polymer as disclosed in this application, and this term or the term "ladder branching mechanism" refers to how the "ladder branched" polymer is formed.
[0020] In one or more embodiments of the present disclosure, the process of synthesizing long-chain branched polymers achieves long-chain branching and avoids gel formation or reactor fouling. Without intending to be bound by theory, it is believed that by reacting two alkenes of a diene in a concerted manner across two proximal polymer chains, reactor fouling is avoided. For example, as shown in Scheme 3, one alkene of a diene reacts before the second alkene, which reacts before the addition of excess ethylene molecules to the polymer chain, thereby removing the proximity that the second alkene has to reactive sites. The reaction of the first alkene of a diene to one polymer and the reaction of the second alkene of a diene to the adjacent polymer chain before many ethylene monomers are inserted is called the concerted addition of a diene to the proximal polymer chain. Scheme 3: Depiction of the incorporation of dienes in a concerted manner, also called the "ladder branching" mechanism (P is the polymer chain). [ka]
[0021] A polymer chain is a linear segment of a polymer, more specifically a copolymer, optionally joined at its end(s) by a branched junction. For example, as shown in Scheme 1, a tetrafunctional branched junction joins the ends of four polymer chains, as opposed to a trifunctional branched junction, which joins the ends of three polymer chains.
[0022] The combination of multichain catalysts and dienes affects the amount and type of branching. Embodiments of the present disclosure are directed to controlling polymer properties such as 1) the use of multiple diene species, 2) the use of multiple multichain catalyst species, or 3) a combination of polymerization environments including multiple reactor zones or zone gradients.
[0023] However, the use of multiple catalysts, including single chain catalysts, may allow for conventional branching. The use of multiple diene species also includes dienes that tend not to produce branches or result in "conventional" LCB. The synthesis process of polymers according to the present disclosure differs from conventional long chain branching. The term "long chain branch" refers to a branch having more than 100 carbon atoms. The term "branch" refers to a portion of a polymer that extends from a tertiary or quaternary carbon atom. If a branch extends from a tertiary carbon atom, there are two other branches, which collectively may be a polymer chain from which the branch extends. Long chain branching (LCB) may occur naturally in the polymerization process, as shown in Scheme 1. This may occur by the termination of the polymer chain and reinsertion of the polymeric vinyl to produce a trifunctional long chain branch.
[0024] In one or more embodiments, the process for polymerizing long-chain branched polymers includes a catalyst having at least two active sites in close proximity (multi-chain catalyst). Due to the close proximity of the two active sites, the two active sites can be less than 18.5 angstroms (Å) apart. In some embodiments, the two active sites include a distance of 2.5 angstroms (Å) to 18.5 Å, 9 Å to 14 Å, or about 11 Å. In various embodiments, the process for polymerizing long-chain branched polymers includes a multi-chain catalyst. In one or more embodiments, the multi-chain catalyst can include at least one metal center, with two active sites on the same metal center. In some embodiments, the multi-chain catalyst can include a metal-ligand complex with two active sites (two polymer chains) on the same metal center.
[0025] According to the X-ray crystal structure (ADBond, Chem. Comm. 2002, 1664), the distance between the terminal carbons of 1,9-decadiene is 10.8 Å. While there is data that 1,9-decadiene forms rungs between two polymer chains via a "ladder branching" mechanism, it is believed that α,ω-dienes with more than 10 carbon atoms may also form rungs via a "ladder branching" mechanism. Without intending to be bound by theory, the question of whether α,ω-dienes with more than 10 carbon atoms can form rungs may be determined by the distance between the two polymer chains. For example, if the two polymer chains are present on different metal atoms of the catalyst (e.g., bimetallic, heterogeneous), the α,ω-dienes may contain additional methylene units (same C-C bond length and angle) to extend this structure to 1,15-hexadecadiene. Without intending to be bound by theory, it is presumed that this 16-carbon analog may form rungs via a "ladder branching" mechanism. Thus, the dienes 1,11-dodecadiene (distance between terminal carbons is 13.3 Å), 1,13-tetradecadiene (distance between terminal carbons is 15.9 Å), and 1,15-hexadecadiene (distance between terminal carbons is 18.5 Å) can be considered. In some embodiments, the diene is 18.5 Å or less when the double-stranded catalyst of the "ladder branching" mechanism is a bimetallic catalyst.
[0026] It is well known that modern computational techniques can reproduce known experimental crystal structures with high accuracy as a way to estimate the distance between catalyst chains. In the case of heterogeneous systems, the surface concentration of the metal can be estimated, which is expressed as metal atoms per square nanometer (M / nm 2 ), which provides an estimate of the accessible metal on the surface that, if uniformly distributed, can be converted to MM distances, which reflect the distance between polymer chains. For extended surfaces, it is approximately 1 metal / nm 2 This leads to a distance between metal atoms of 10 Å, well within the desired cutoff range. At 18.5 Å, there are 0.3 metal atoms / nm 2 A coverage of 100% can be obtained.
[0027] Examples of catalysts having at least two active sites in close proximity include, but are not limited to, bimetallic transition metal catalysts, heterogeneous catalysts, dianionic activators having two associated active catalysts, ligated transition metal catalysts having multiple propagating polymer chains, Group IV olefin polymerization catalysts containing a monoanionic group, a bidentate monoanionic group, a tridentate monoanionic group, or a monodentate, bidentate, or tridentate monoanionic group with an external donor.
[0028] The catalysts in Table 1 are exemplary embodiments of the classes of catalysts described above and the specific catalysts contemplated. The examples in Table 1 are not intended to be limiting; rather, they are merely illustrative and specific examples of the classes of catalysts described above. [Table 1]
[0029] Without intending to be bound by theory, the mechanisms described in this section will explain how a double-chain catalyst can produce a unique cross-linked molecular structure when a diene comonomer is polymerized under the desired conditions. The term "diene" refers to a monomer or molecule having two alkenes. An illustration of the reaction kinetics is shown in Scheme 4, in which a catalyst center produces two polyolefin chains. Scheme 4 shows how a combination of diene cross-linking and chain transfer produces a diene "ladder-branched" polymer structure. The term diene "ladder-branched" polymer refers to long chain branching, in which a short chain or rung containing 1-12 carbon atoms links two long chains together. As shown, a metal-ligand catalyst with at least two polymer chain sites grows two separate polymer chains. One alkene of the diene is incorporated into one of the catalyst sites, and then, due to the proximity of the growing sites, a second alkene of the diene is rapidly incorporated into the second polymer chain, thereby forming a cross-link or rung. This successive addition of dienes is called "concerted" addition of dienes to distinguish them from catalysts where the addition of dienes results in a concentration of vinyl-containing polymer in the reactor and does not have two proximal chains to react later. The term "runge" refers to the diene after it has been incorporated into two separate polymer chains, thereby linking these polymer chains together. The first and second polymer chains continue to grow until the polymer is transferred to another catalyst, the polymer is released from the catalyst, the catalyst fails, or another diene is added.
[0030] Reaction kinetics Scheme 4. Illustration of the “ladder branch” reaction kinetics including the resulting molecular structures. Metal-ligand catalysts are + It is expressed collectively as: [ka]
[0031] Without intending to be bound by theory, it is believed that the molecular weight distributions associated with these proposed reaction kinetics are essentially stable at high branching levels when diene crosslinking reactions are the only source of branching. The molecular weight distribution (MWD) is determined by the number average molecular weight (M w / M n The inherent stability of MWD is defined by the weight average molecular weight divided by the weight average molecular weight (M w ) increases modestly even at high branching levels, which is in contrast to conventional diene comonomer branching techniques, where M w and M. w / M n goes to infinity at intermediate tetrafunctional branching levels.
[0032] A mathematical model is derived for the purpose of demonstrating how the process of synthesizing polyethylene produces long-chain branched polymers with diene "ladder branching" molecular architecture. The mathematical model is also used to establish the metrics and scope of the claims. The mathematical model of the branching structure described in this disclosure can be derived from a description of the reaction kinetics of the proposed branching mechanism. The model is based on several assumptions to facilitate mathematical simplification, but these assumptions are not intended to limit the scope of this disclosure. The assumptions follow the general industrial application of abiotic addition of copolymers, and the assumptions of addition specific to the hypothesized diene branching mechanism. The general assumptions made include: (1) propagation is much faster than chain transfer, so that the average chain length is much longer than that of one monomer; (2) only a single pure catalytic species is active; (3) the catalytic center creates many chains during its lifetime, so that the chain lifetime is a small fraction of the reaction or residence time; and (4) copolymerization can be approximated by a homopolymerization model when compositional drift is negligible.
[0033] Kinetics for the "ladder branching" theory of dienes. In addition to the four commonly made assumptions, there are four assumptions based on reaction kinetics for the diene "ladder branching" theory. The first assumption is that the catalytic center simultaneously produces two kinetic chains with the same reaction kinetics and statistics. Second, rungs are formed when a diene bridges two polymer chains that increase in length. Third, a branch point is formed whenever two unbridged chains are bridged by a diene. Finally, diene reactions that do not form bridges are ignored, since the MWD is not affected.
[0034] The kinetic description of the proposed diene "ladder branching" mechanism requires the development of a nomenclature system that describes how each reaction affects molecular structure. Some nomenclature elements below represent small molecules (M, A, D) while others represent molecular structures (P n,m , S n , D n ) Reaction kinetics describes how the named elements interact to form molecular structures.
[0035] Kinetic nomenclature M: monomer or comonomer; A: chain transfer agent species; D: diene branch species; n, m: indices reflecting the number of monomer repeat units of the subspecies; P n,m : A catalyst having two non-crosslinked propagating polymers having n and m monomer repeat units; D n : a dead polymer molecule having n monomer repeat units; S n : a catalyst that produces a crosslinked polymer molecule with n monomer repeat units; Kc: a kinetic chain is defined as a linear segment produced by chain transfer; Rg: a rung is defined as a crosslink between chain segments; Br: a crosslink is produced when two previously uncrosslinked molecules become crosslinked.
[0036] The branching kinetic equations are described below using the nomenclature and assumptions introduced above. Each reaction is briefly explained, and those skilled in the art of polymerization kinetics should be able to understand the kinetic scheme and kinetic rate laws. [Table 2]
[0037] Growth results in an incremental increase in chain size of only one repeat unit. Growth is described separately for each of the two molecules that increase in length from the catalytic center. For example, P n,m The first exponent is for the chain on the left side of the catalyst, and the second exponent is for the chain on the right side of the catalyst. The length of the bridging molecule (S n ), the rate doubles because there are now two strand positions, one to the left and one to the right, about each center that are equally available for reaction.
[0038] Chain transfer, like propagation, is described separately for positions to the left and right of the catalyst. n,m ) chain transfer occurs through the dead polymer molecule (D n Or D m ) and empty positions (P 0,m or P n,0 ) is generated. n ) participates in chain transfer, the non-bridged species (P n,0 or P 0,n ) is produced and no dead polymer is produced because all n repeat units are still attached to the catalyst. 0,m and P n,0 ) are assumed to very rapidly resume and participate in propagation. Because each diene has two polymerizable groups and each catalytic center has two positions (on the left and right) for incorporating a diene, the rate equation for the diene bridge contains a factor of four.
[0039] The diene bridge is uncrosslinked (P n,m Only when the ) species reacts productively with a diene does it result in the formation of tetrafunctional branches (br). Tetrafunctional branches refer to short segments from which four polymer chains emanate, two from each side of the short segment. With dienes, tetrafunctional branches are the type of LCB one would expect. Lang is a crosslinker (S n) molecule or non-crosslinked (P n,m ) molecule is generated when any catalytic center productively incorporates a diene (rg). Diene reactions that do not result in crosslinking, such as in-chain cyclization and pendant vinyl formation, are ignored and considered non-productive in these kinetics.
[0040] Developing a model from the reaction kinetics requires the derivation of a series of population balances for each type of polymer species involved. These population balances are derived as a function of chain length (n,m) and represent the kinetic rates of change of the various polymer subspecies. The population balances are shown below and are represented by the symbol P n,m , S n , and D. n The mass action rate law is assumed with the transport term Ω=k tra A+k trh H 2 +k b Only by expanding the definition of trh ) and beta hydride desorption (k b ) can be included.
number
[0041] In equations (1), (2), and (3), we have:
number
[0042] Other important population balances are on the left (L n ) and right side (R n ) can be derived from equations (1) to (8), such that the distribution of growing polymer subspecies for θ = θ ...
number
[0043] The rates of formation of molecular attributes such as chains (kc), branches (br), and rungs (rg) are expressed below using mass action rate laws derived from the kinetics scheme. The shorthand notation is 0,0 ) and the concentration of the catalyst with crosslinked polymer molecules (μ 0 ) is used to define the concentration of the catalyst with the total catalyst concentration being ξ 0,0 +μ 0 It is.
number
[0044] The first step in rendering a usable model is to determine the proportions of relevant polymer variants.
number
number
[0045] The "steady state assumption" is a simple branching metric (B c , B n , R cIn this particular case, the instantaneous characteristics are useful and relevant since they apply to a variety of reactors, such as a steady-state well-mixed reactor, or a batch reactor where temperature or composition deviations are negligible. The instantaneous bifurcation metric (B c , B n , R c ) is equivalent to the cumulative average value in the absence of spatial or temporal variations in the chain transfer (Ω) and diene bridge rate (Ψ) parameters.
number
[0046] Moments for forecasting MWD averages Models describing the moments of chain length distribution of polymer species can often be derived from population balances resulting from reaction kinetic schemes. Moment-based models are useful for predicting molecular weight averages and polydispersity indices, but generally do not account for small nuances in MWD such as bimodality, peak MW, tailing, etc. The moment method involves the definition of chain length distribution moments for various polymer subspecies, such as: Bulk polymer moments (λ i ) reflect bulk polymer properties, and the solution of the bulk moment model generally requires the solution of the various living polymer moments.
number
[0047] Any experienced polymer reaction engineer will understand the derivation of the moment models (equations (20) and (21)) from a series of population balances. The rate of change of the major bulk polymer moments (λ 0 , λ 1 , λ 2 ), is shown below, where negligible terms are removed after imposing the assumption that the kinetic chain is long, and hence that Φ>>Ω.
number
[0048] The evaluation of the rate of change of these bulk moments requires the moments of many living polymer subspecies. These live polymer moments are algebraic quantities due to the "steady state assumption" and are shown below. λ 3 If higher bulk moments are expected, such as
number
[0049] After algebraically simplifying the moment ratios, the instantaneous number and weight average chain lengths (DPn, DPw) are given below. Of course, the average molecular weight (M n , M w ) is equal to the average chain length multiplied by the apparent monomer repeat unit weight (g / mol).
number
[0050] The expression of this model is the average linear kinetic chain length DP, which is equal to Φ / Ω. no This model is further simplified by some substitutions such as c , B n , and R c For this model, the number of diene "ladder branches" (B c ) and branches per polymer molecule (B n ) is shown below. For this system, the number of branches per polymer molecule is proportional to the number of rungs per kinetic chain (B n =R c ) has previously been shown to be equal to
number
[0051] Number and weight average molecular weight (M n , M w ) is M no and M. wo After defining the number and weight average linear kinetic chain weight as c ) or branches per polymer molecule (B n ) can also be predicted.
number
[0052] An unexpected prediction arising from the moment model (Eqs. (20) and (21)) is that at high diene branching levels, the maximum polydispersity is approximately 4. Of course, this prediction is for an ideal copolymerization and a single symmetric catalyst system; nonideal ones can increase the polydispersity.
[0053] Complete MWD curve model Sometimes it is possible to solve the population balance of a molecular weight distribution curve. Explicit algebraic solutions are usually only available when there is no spatial or temporal variation in the reaction rate, as is assumed in this case. The solution starts with the specification of yet another distribution volume, Vn, derived from Pn,m. The population balance of Vn is derived by summing the population balances of Pn,m, using symmetry simplifications.
number
[0054] Because we assume long chains, it is possible to treat all subspecies distributions as if they were continuous functions rather than discrete. The population balance of a discrete steady-state polymer species can be closely approximated by a differential equation in a continuous variable n, if the difference terms are replaced by their derivatives. For example, the steady-state population balance of Sn contains the difference term Sn-Sn-1 replaced by its derivative as shown in equation (31).
number
[0055] Similar substitutions result in the following set of ordinary differential equations (ODEs), which can be integrated to yield the chain length distributions for the various predefined living subspecies distributions L(n), S(n), and V(n): The model is summarized below as an initial value problem, where the chain length distribution function is assumed to start at n=0. The n=0 lower limit on the distribution function is chosen solely for mathematical simplicity and ultimately does not significantly affect the predictions of the model when the polymer is formed.
number
[0056] The distribution of the instantaneous dead polymer chain lengths, as revealed by the species fraction, is n Proportional to
number
number
[0057] Complete MWD curve solution The distribution function for increasing polymer chain length can be solved either numerically or analytically by one familiar with the integration of ordinary differential equations. The analytical solution, although algebraically complex, is presented here because it is in perfect agreement with the moment model (equations (20) and (21)) and also predicts nuances in the MWD such as multimodality and tailing of peak positions.
[0058] A software package known as Mathematica™ was used to develop analytical solutions to a system of ordinary differential equations describing the growing polymer distribution functions L(n), S(n), and V(n). The analytical solution for L(n) was used to describe the instantaneous dead polymer distribution X(n) by normalizing L(n) by its integral.
number
[0059] An explicit analytical solution for X(n) can be obtained using Mathematica™. The analytical solution for X(n) is given by n and D.P. no The solution is given below as a function of R c Or B n With respect to the substitution R c =B n =B c / (1-B c )(36).
[0060] The chain length distribution function X(n) is evaluated as follows from the definition of RootSum given in Mathematica™. The following polynomial is 1 , x 2 and x 3 Two of the three roots of the polynomial are called B n is complex over the range of possible values of 0=1+B n +(3+5B n +2B n 2 )x+3(1+B n )x 2 +x 3 (37)
[0061] root x 1 , x 2 , and x 3 is used for the instantaneous dead chain length distribution function X(n).
number
[0062] Various moments of X(n) are evaluated to determine the instantaneous number and weight average chain length (DP n , D.P. w ) or molecular weight (M n , M w ) is obtained. The weights obtained from the average chain length and continuous distribution X(n) are equal to the moment model predictions given previously for the long chain polymerization and discrete distributions, and B c and B. n Both are shown below for R c =B n It is.
number
[0063] Those skilled in the art of polymer reaction engineering are familiar with the use of predicted bulk polymer MWD models to generate simulated size exclusion chromatography (SEC) curves. Such simulations are useful for correlating how reaction kinetics and recipes affect SEC measurements. The primary calibration result of an SEC measurement is a table or plot of dw / dLog(M) versus Log(M), where M is the molecular weight or size of the species, and dw / dLog(M) indicates the relative amount of polymer corresponding to M. The SEC results are expressed as n 2 It is generally accepted that one can simulate this with a table or plot of X(n) versus Log(M), where n 2 X(n) is expected to be proportional to dw / dLog(M).
[0064] Figure 2 shows the diene "ladder branch" (B c , B n , R c2 shows a series of simulated SEC curves with varying levels of . The independent variables in Figure 2 are scaled by linear molecular weight or chain length so that the plot is universal and independent of starting molecular weight. The zero-branching case in Figure 2 is the well-known "most probable" MWD (P. J. Flory, J. Am. Chem. Soc. 1936, 58, 1877), which is the expected MWD for linear additive copolymerization carried out under ideal homogeneous conditions.
[0065] A more detailed analysis of peak MW values was performed using a larger series of branching levels applied to the MWD model. Figure 3 shows a universal plot of relative peak MW as a function of branching level. Figure 3 shows the peak MW insensitive (0 <R c <0.15), as well as in the higher branching regime (R c ≥ 0.15), and the peak MW increases steadily with branching level.
[0066] Alternative trifunctional diene "ladder branching" mechanisms and models. There are alternative mechanisms that could explain the branching and MWD trends observed when the dual catalyst incorporates dienes under the desired conditions. n It is often observed that M increases with the addition of dienes, but for some catalyst-diene combinations, M w increased, and measurable M n There is little or no increase in M n One explanation for is that the elimination of a single beta hydride (or chain transfer to hydrogen) tends to occur immediately after the diene is inserted into both growing chains. In this scenario, the diene insertion produces trifunctional branches, which in the pure form are not cross-linked propagating species (S n ) is excluded from the reaction kinetics.
[0067] The kinetic scheme has been modified to take into account this alternative mechanism by replacing "diene bridge" with the following reaction: [Table 3]
[0068] Polymer reaction engineers skilled in the art of modeling and reaction kinetics can re-derive moment and MWD function models for these alternative reaction kinetics using the same set of assumptions as before. The resulting instantaneous dead chain length distribution function, X(n), is shown below for this trifunctional branching mechanism.
number
[0069] In formula (41), B c is defined as the branch points per kinetic chain, and DP no is defined as the average linear chain length not including dienes. The kinetic scheme assumes that the linear (kinetic) chain length actually decreases with diene incorporation due to diene-induced beta hydride elimination. Thus, a suitable surrogate for branching is B n which is defined as the number average branch points per polymer molecule, where B c =B n / (1+B n ) The function X(n) is B n can be easily rewritten in terms of
[0070] By integrating X(n), we obtain the instantaneous number and weight average chain length (DP n , D.P. w ) or molecular weight (M n , M w ) results. The average chain length and weight obtained from the continuous distribution X(n) are equal to the predictions of the moment model when long chain polymerization is assumed. By integrating X(n), we obtain the DP n and M. n is the level (B c Or B n) is confirmed to be constant with branching. The integral of X(n) shows how the polydispersity is expected to change with branching level if the diene is assumed to produce trifunctional branches.
number
[0071] Polydispersity (M w / M n The above relationship between ) and trifunctional branching level shows no instability or divergence at any branching level. Most surprising is that at higher branching levels, the polydispersity is predicted to plateau at 4. Of course, this prediction is for an ideal copolymerization and symmetric catalyst system with any non-idealities that would be expected to result in an increase in polydispersity.
[0072] The chain length distribution function can again be used to construct predicted MWD curves. c Or B n ) are varied. The independent variables in Figure 4 are scaled by linear molecular weight or chain length so that the plot is universal and independent of starting molecular weight. The zero branching case in Figure 4 is the well-known "most likely" MWD and is expected for linear addition copolymerizations conducted under ideal homogeneous conditions. Figure 5 is a plot of the relative peak MW of trifunctional diene branches, showing that the MWD peaks are roughly at 0.2 n <0.9 or 0.17 c It shows that it is most sensitive to branching level with intermediate branching levels in the range of <0.5.
[0073] Traditional branching model The purpose of this section is to compare various conventional diene branching and random polymer couplings with the "ladder branching" model. This comparison demonstrates the inherent instability of conventional diene branching and random polymer couplings, as opposed to "ladder branching." The molecular structures resulting from diene "ladder branching" are different from (a) the conventional diene continuous stirred tank reactor (CSTR) branching model, (b) the conventional diene semi-batch branching model, (c) the polymer-CSTR coupling model, and (d) the polymer-batch coupling model.
[0074] a) Conventional diene CSTR branching models Ver Strate-1980 (G. Ver Strate, C. Cozewith, W.W. Graessley, J. App. Polym. Sci. 1980, 25, 59), Guzman-2010 (J.D.Guzman, D.J.Arriola, T.Karjala, J.Gaubert, B.W.S.Kolthammer, AIChE 2010, 56, 1325):
number
[0075] b) Traditional diene semi-batch branching model, Cozewith-1979 (C. Cozewith, W.W. Graessley, G. Ver Strate, Chem. Eng. Sci. 1979, 34, 245), and d) Polymer batch coupling model, Cozewith-1979, Flory-1953 (P.J.Flory, Principles of Polymer Chemistry, Cornell University Press, 1953), Tobita-1995 (H.Tobita, J.Polym.Sci.B 1995, 33, 1191):
number
[0076] c) Polymer CSTR coupling model:
number
[0077] Characterization of tetrafunctional long-chain branched polyolefins Depending on the degree of branching, various methods can determine LCB, such as nuclear magnetic resonance (NMR), or distinguish the effect of LCB in a polymer. For example, the effect of LCB is observed in shear flows in van Gurp-Palmen analysis, and the increase in shear viscosity at low angular frequencies and the strength of shear thinning behavior can be attributed to LCB. In extensional flows, the effect of LCB is usually identified in the degree of stiffening or strength of the melt and the maximum deformation achieved. Other such methods include Mark-Houwink plots, spread molecular weight distribution (MWD), and g' vis Other plots such as the plot provide additional information regarding the LCB. Achieving high levels of native LCB in the polymer is difficult due to the limited concentration of vinyl terminated polymers (maximum one per polymer chain) and the need to run to high conversion to ensure the formation of LCB. To ensure high conversion, the ethylene concentration in the reactor is low, so that a large amount of vinyl terminated polymer can be reinserted into a second polymer chain.
[0078] Conventional processes incorporating dienes into polymer synthesis systems suffer from a fundamental flaw: gel formation or reactor fouling at high branching levels. The kinetic modeling described in the previous paragraph can provide excellent predictive results that allow for a better understanding of gel formation. For example, longer polymer chains have proportionally more pendant vinyls, and polymer chains containing more pendant vinyls are more likely to reinsert into the catalyst to form LCBs. Thus, larger polymer chains preferentially reinsert and form even larger polymer molecules, tetrafunctional branches, resulting in gel problems or instability when LCB levels reach a threshold. Conventional weight average molecular weight (M) as a function of tetrafunctional branching w ) and number average molecular weight (M nA simulation of M is shown in Figure 1 for an ethylene-based polymer in a constant pressure semi-batch reactor. n As goes to infinity, M w increases only slightly. In this example, M w When the molecular weight distribution (MWD) of a polymer becomes unstable and gels begin to form, the MWD is the weight average molecular weight M w The number average molecular weight M n Divided by (M w / M n )
[0079] Polymer gels are narrowly defined for the purposes of this disclosure as polymer moieties that are phase separated due to their high branching levels and / or high molecular weight. Polymer gels can be observed in solution or in the melt and tend to interfere with properties such as optical clarity and film and fiber performance. Polyethylene interpolymer gels can be measured by the degree of insolubility of the polymer in hot xylene. Gel content is often correlated with GPC polymer recovery and is therefore estimated. When polymer gels form, they can accumulate in the reactor and cause contamination.
[0080] Figures 7 and 8 show the difference in MWD curves expected from conventionally branched and "ladder branched" polymers. From the study of MWD data and comparison with MWD models, a set of metrics was developed to describe the characteristics of the MWD. Each of the MWD description metrics presented here is independent of the average MW and focuses on the high MW portion of the MWD. The MWD metrics are derived from the scaled MWD curve (dW / dlogM), where the primary or highest peak of the MWD is defined as having a value of 1. If multiple peaks are of the same height, the highest MW peak is the primary peak. The independent variable of the MWD curve is Log(M), which is the logarithm of M to the base 10. The metrics can be converted to branches per molecule or segment using Figures 6, 7, 8, and 9. w / M wo and M. p / M po Those skilled in the art of GPC data interpretation will understand these metrics and be able to calculate them from GPC data.
[0081] A family of GPC shape metrics, G(A / B), is calculated from the slopes at defined points on the right side of the MWD curve, where S(A) and S(B) are the first occurrences of these slopes to the right side of the primary peak at A% and B% of the height of the primary peak. Points A and B are selected as pairs that have approximately the same slope when the MWD is "most likely". A depiction of these points and their slopes is shown in the graph in Figure 10 for the most likely MWD. These slope pairs, S(A) and S(B), are used together to calculate a second derivative-like function, G(A / B), which is shown to be a useful metric for distinguishing "ladder branching" MWDs from conventional or random branching MWDs. The values of G(79 / 29) and G(96 / 08) represent the change in slope of the right side (RHS) of the MWD, defined below from the slope of the higher MW. G(79 / 29)=(S(79)-S(29)) / S(79) (48) G(96 / 08)=(S(96)-S(8)) / S(96) (49)
[0082] The shape metrics G(79 / 29) and G(96 / 08) were tested for tetrafunctional "ladder branching" and conventional diene branching in the MWD model, and the results are plotted in Figures 11, 12, 13, and 14. These figures show that conventional branching yields G(79 / 29) and G(96 / 08) values that steadily increase as the MW responds to branching. However, when applied to "ladder branching," these shape metrics tend to be more stable at low levels of branching (low M w / M wo ) and approaches zero at mid- to high-level branching. This is not surprising, since the high-MW portion of the "ladder branching" MWD resembles the most likely MWD.
[0083] Figures 11, 12, 13, and 14 show similar responses of the G(79 / 29) and G(96 / 08) metrics to branching, although the G(96 / 08) metric is expected to be more sensitive to the high MW tailing resulting from conventional diene branching. The term "high MW tailing" or "high molecular weight tail" refers to the high molecular weight portion exhibited by conventional and absolute GPC. Depending on the catalyst-diene pairing and experimental conditions, it is expected that there will be conventional branching in the "ladder branched" system, which will result in higher shape metric values than would be expected for pure "ladder branching".
[0084] MWD Area Metric Visual inspection of the "ladder branching" MWD shows that there is a lack of the high MW tail features typically seen in branched polymers. Figures 16 and 17 show how the model predicts the lack of tailing for "ladder branching" polymers. The "ladder branching" MWD data shows a lack of tail features in many experiments, but also indicates that tails can form depending on the polymerization conditions and diene / catalyst pairing.
[0085] Polydispersity index (M w / M n , M z / M w ) are known metrics for tailing, but are not preferred due to their sensitivity to low MWD artifacts. Therefore, a more focused version of the polydispersity index is used to develop a criterion where integration is only done in the high MW portion of the MWD. w / M n Metric and M z / M w The metric successfully distinguishes diene "ladder branches" from conventional branches and is highly sensitive to high MW baseline selection and baseline noise.
[0086] The area under the MWD curve is the MWD dispersibility index (M w / Mn , M z / M w It is relatively insensitive to baseline problems compared to the higher moments required for the calculation of the MWD, etc. It was therefore decided to develop a metric that involves an unweighted integral of the MWD. These MWD area metrics, A HIGH and A TAIL is calculated from the area of the GPC curve for a defined region to the right of the MWD curve. The MWD area metric (A HIGH and A TAIL ) is derived from the scaled MWD curve (dW / LogM), with the primary or highest peak of the MWD defined to have a value of 1. When multiple peaks are of the same height, the highest MW peak is the primary peak. The independent variable of the MWD curve is Log(M), which is the logarithm of M to the base 10. Both MWD area metrics depend on the point of maximum slope of the high MW portion of the MWD. The quantities and limitations required to evaluate the area metrics are listed below and shown in Figure 15 for the most likely MWDs. S max = First instance of maximum downward slope on the RHS (high MW side) of the primary peak (absolute value of slope) of the scaled MWD H smax = Scaled MWD height at the point of maximum slope pt1=S max LogM value of pt2=S max LogM value where the tangent line crosses the x-axis
[0087] The MWD area metric is defined below, and A HIGH is simply the area of the MWD region after the point of maximum slope. The second area metric A TAIL is the area of the small high MW shown in Figure 15, and A HIGH It is evaluated by subtracting the area of the triangle from
number
[0088] Area Metric A HIGH and A TAIL have been tested for the "ladder branched" and traditional diene branched MWD models, and the results are plotted in Figures 16, 17, 18, and 19. The plots show that A HIGH Or A TAIL It shows that the high-MW area, defined as the area of the nuclei that is the branching level of the nuclei, increases dramatically as the branching level of the nuclei increases. However, in the “ladder branching” model, the high-MW area metric (A HIGH Or A TAIL ) is largely unaffected by the "ladder branch" level. HIGH and A TAIL The values of A and B are approximately 0.07 and 0.015, respectively. The exemplary MWD data shows that the diene-free linear polymers have low A due to non-ideal aspects of the polymerization. HIGH and A TAIL The example data also shows that a variety of highly branched "ladder branched" polymers are essentially free of high MW tails beyond those expected from the most probable MWD. The high MW area metric also provides a measure of the slight level of high MW tail formation that "ladder branched" polymers may exhibit when accompanied by some degree of conventional branching. Metric A TAIL A HIGH Theoretically, however, A is less affected by the non-idealities of the linear MWD. HIGH Metric and A TAIL The metrics equally indicate high MW tail formation.
[0089] Tetrafunctional long chain branched polyolefin Polymers produced from "ladder branches," as depicted in Scheme 4, are included in the present disclosure.
[0090] In embodiments, the ethylene-based polymers of the present disclosure have a melt viscosity ratio or rheology ratio (V 0.1 / V 100 ), including V 0.1is the viscosity of the ethylene-based polymer at 190 °C at an angular frequency of 0.1 rad / s, and V 100 is the viscosity of the ethylene-based polymer at 190° C. at an angular frequency of 100 rad / sec. In one or more embodiments, the melt viscosity ratio is at least 14, at least 20, at least 25, or at least 30. In some embodiments, the melt viscosity ratio is greater than 50, at least greater than 60, or greater than 100. In some embodiments, the melt viscosity ratio is from 14 to 200.
[0091] "Rheology ratio" and "melt viscosity ratio" are V at 190°C. 0.1 / V 100 is defined by V 0.1 is the viscosity of the ethylene-based polymer at 190 °C at an angular frequency of 0.1 rad / s, and V 100 is the viscosity of the ethylene-based polymer at 190° C. at an angular frequency of 100 rad / sec.
[0092] In one or more embodiments, the ethylene-based polymers of the present disclosure have an average g' of less than 0.86, where the average g' is the intrinsic viscosity ratio determined by gel permeation chromatography using a triple detector. In some embodiments, the ethylene-based polymers of the present disclosure have an average g' of 0.64 to 0.86. All individual values and subranges within "0.64 to 0.86" are disclosed herein as separate embodiments, and for example, the average g' of the ethylene-based polymers can range from 0.64 to 0.75, 0.68 to 0.79, or 0.65 to 0.83. In one or more embodiments, the average g' is 0.65 to 0.84, 0.66 to 0.82, or 0.66 to 0.80.
[0093] In some embodiments, the ethylene-based polymers have a G(79 / 29) value of 0.035 or less, as determined from a gel permeation chromatography curve having a peak height, a slope M79 at 79% of the peak height, and a slope M29 at 29% of the peak height, where the G(79 / 29) value is equal to (M79-M29) / M79. All individual values and subranges falling within "0.035 or less" are disclosed herein as separate embodiments, for example, "0.035 or less" includes from 0.0 to 0.035, from 0.010 to 0.034, and includes negative values. In one or more embodiments, the ethylene-based polymers of the present disclosure may have a G(79 / 29) value of 0.030 or less, as determined from a gel permeation chromatography curve.
[0094] In one or more embodiments, the melt viscosity ratio of the ethylene-based polymers of this disclosure may be greater than 10 times the elastic modulus, and the melt viscosity ratio (V 0.1 / V 100 ) is the viscosity of ethylene-based polymers at 190°C with an angular frequency of 0.1 rad / s, V 0.1 , and V is the viscosity of the ethylene-based polymer at 190 °C with an angular frequency of 100 rad / s. 100 The elastic modulus m is determined by [((tan(δ 0.1 )-tan(δ 100 ))*1000) / (0.1-100))], and tan(δ 0.1 ) is the tangent of the phase angle in 0.1 radians / second, and tan(δ 100 ) is the tangent of the phase angle in 100 radians / second.
[0095] In one or more embodiments, the ethylene-based polymer may have an elastic modulus, m, at 190° C. that is 8 seconds / radian or less, where m is [((tan(δ 0.1 )-tan(δ 100 ))*1000) / (0.1-100)). In other embodiments, the ethylene-based polymer may have an elastic modulus, m, at 190° C. that is less than or equal to 4 seconds / radian.
[0096] In various embodiments, the melt strength of the ethylene-based polymers of the present disclosure may be greater than 6 cN (Rheotens device, 190° C., 2.4 mm / sec 2 , 120mm from die exit to wheel center, extrusion speed 38.2 seconds -1 , 30 mm long, 2 mm diameter, 180° inlet angle capillary die). In some embodiments, the melt strength of the ethylene-based polymer can be greater than 10 cN.
[0097] In an embodiment, the ethylene-based polymer has an MWD area metric A TAIL and a molecular weight tail quantified by A TAIL is less than or equal to 0.04. All individual values and subranges encompassed by "less than or equal to 0.04" are disclosed herein as separate embodiments. For example, in some embodiments, the A of the ethylene-based polymers of the present disclosure TAIL is greater than 0 and less than or equal to 0.03 as determined by gel permeation chromatography using a triple detector.
[0098] In an embodiment, the M of the ethylene-based polymer w In one or more embodiments, the M of the ethylene-based polymer may be less than or equal to 800,000 daltons as determined by gel permeation chromatography using a triple detector. w can be up to 400,000 daltons.
[0099] In various embodiments, the ethylene-based polymer has a M p / M p0 M p is the peak molecular weight of the ethylene-based polymer as determined by conventional gel permeation chromatography, and M p0 is the initial peak molecular weight of the ethylene-based polymer without the polyene comonomer.
[0100] In an embodiment, the ethylene-based polymer has a M w / M w0 M wis the weight average molecular weight of the ethylene-based polymer determined from the GPC curve of the ethylene-based polymer obtained by gel permeation chromatography. w0 is the initial weight average molecular weight of a comparative ethylene-based polymer by gel permeation chromatography. A comparative ethylene-based polymer is a polymer that is a mixture of all C monomers present in an ethylene-based polymer without ethylene monomer and, if present, at least one polyene comonomer, under defined polymerization reaction conditions. 3 ~C 14 It is the reaction product of polymerization with a comonomer.
[0101] Each M w0 and M. p0 is the metric of polymer resin without the addition of diene to the reactor during polymerization, as previously described. Each subsequent addition of diene produces a polymer resin, from which the metric M W or metric M p can be determined. The amount of diene incorporated into the reactor is small compared to the other reactants in the reactor, therefore the addition of diene does not affect the total amount of comonomer, ethylene, and solvent in the reactor.
[0102] In various embodiments, the ethylene-based polymer has a gpcBR branching index from 0.1 to 3.0. All individual values and subranges within "0.10 to 3.00" are disclosed herein as separate embodiments, for example, the ethylene-based polymer can have a gpcBR branching index from 0.10 to 2.00, 0.10 to 1.00, 0.15 to 0.65, 0.20 to 0.75, or 0.10 to 0.95.
[0103] The long chain branching polymerization process described in the previous paragraph is utilized for the polymerization of olefins, primarily ethylene and propylene. In some embodiments, only a single type of olefin or α-olefin is present in the polymerization scheme, producing what is essentially a homopolymer with a small amount of incorporated diene comonomer homopolymer. However, additional α-olefins may be incorporated into the polymerization procedure. The additional α-olefin comonomer typically has 20 or fewer carbon atoms. For example, the α-olefin comonomer may have 3 to 10 carbon atoms, or 3 to 8 carbon atoms. Exemplary α-olefin comonomers include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 4-methyl-1-pentene, and ethylidene norbornene. For example, the one or more α-olefin comonomers can be selected from the group consisting of propylene, 1-butene, 1-hexene, and 1-octene, or alternatively, from the group consisting of 1-hexene and 1-octene.
[0104] Long chain branched polymers, such as homopolymers and / or interpolymers (including copolymers) of ethylene and optional one or more comonomers, such as α-olefins, can contain at least 50 weight percent ethylene derived units. All individual values and subranges encompassed by "from at least 50 weight percent" are disclosed herein as separate embodiments, such as ethylene-based polymers, homopolymers and / or interpolymers (including copolymers) of ethylene, optional one or more comonomers, such as α-olefins, can contain at least 60 weight percent ethylene derived units, at least 70 weight percent ethylene derived units, at least 80 weight percent ethylene derived units, 50 to 100 weight percent ethylene derived units, or 80 to 100 weight percent ethylene derived units.
[0105] In some embodiments of the ethylene-based polymer, the ethylene-based polymer comprises an additional α-olefin. The amount of the additional α-olefin in the ethylene-based polymer is less than or equal to 50 mole percent (mol%), in other embodiments the amount of the additional α-olefin comprises at least 0.01 mol% to 25 mol%, and in further embodiments the amount of the additional α-olefin comprises at least 0.1 mol% to 10 mol%. In some embodiments, the additional α-olefin is 1-octene.
[0106] In some embodiments, the long chain branched polymer may comprise at least 50 mole percent of units derived from ethylene. All individual values and subranges from at least 90 mole percent are included herein and disclosed herein as separate embodiments. For example, the ethylene-based polymer may comprise at least 93 mole percent of units derived from ethylene, at least 96 mole percent of units derived from ethylene, at least 97 mole percent of units derived from ethylene, or alternatively, 90-100 mole percent of units derived from ethylene, 90-99.5 mole percent of units derived from ethylene, or 97-99.5 mole percent of units derived from ethylene.
[0107] In some embodiments of the long chain branched polymer, the amount of additional α-olefin is less than 50%, in other embodiments includes at least 1 mole percent (mol%) to 20 mol%, and in further embodiments includes at least 5 mol% to 10 mol%. In some embodiments, the additional α-olefin is 1-octene.
[0108] Any conventional polymerization process may be used to produce the long chain branched polymers, including, but not limited to, solution polymerization processes, gas phase polymerization processes, slurry phase polymerization processes, and any combination thereof, using one or more conventional reactors, such as loop reactors, isothermal reactors, fluidized bed gas phase reactors, stirred tank reactors, batch reactors, etc., in parallel, in series, or in any combination thereof.
[0109] In one embodiment, the ethylene-based polymer can be produced in a dual reactor system, for example a single loop reactor system, where ethylene and optionally one or more α-olefins are polymerized in the presence of the catalyst system described herein and herein and optionally one or more cocatalysts. In another embodiment, the ethylene-based polymer can be produced by solution polymerization in a dual reactor system, for example a dual loop reactor system, where ethylene and optionally one or more α-olefins are polymerized in the presence of the catalyst system described herein and herein and optionally one or more other catalysts. The catalyst system described herein can be used in the first reactor or the second reactor, optionally in combination with one or more other catalysts. In one embodiment, the ethylene-based polymer can be produced by solution polymerization in a dual reactor system, for example a dual loop reactor system, where ethylene and optionally one or more α-olefins are polymerized in both reactors in the presence of the catalyst system described herein.
[0110] In another embodiment, the long-chain branched polymers can be produced by solution polymerization in a single reactor system, such as a single loop reactor system, where ethylene and, optionally, one or more α-olefins are polymerized in the presence of a catalyst system as described in this disclosure, and, optionally, one or more cocatalysts as described in the previous paragraph. In some embodiments, the long-chain branching polymerization process to produce the long-chain branched polymers comprises polymerizing ethylene and at least one additional α-olefin in the presence of a catalyst system.
[0111] The long-chain branched polymer may further include one or more additives. Such additives include, but are not limited to, antistatic agents, color enhancers, dyes, lubricants, pigments, primary antioxidants, secondary antioxidants, processing aids, UV stabilizers, and combinations thereof. The ethylene-based polymer may contain any amount of additives. The ethylene-based polymer may be reduced by about 0 to about 10 percent by weight of the total of such additives, based on the weight of the ethylene-based polymer and the one or more additives. The ethylene-based polymer may further include a filler, which may include, but is not limited to, organic or inorganic fillers. The long-chain branched polymer may be reduced by about 0 to about 10 percent by weight of such additives, based on the weight of the ethylene-based polymer and all additives or fillers. 2 The ethylene-based polymer may contain from about 0 to about 20 weight percent of a filler such as. The ethylene-based polymer may be further compounded with one or more polymers to form a blend.
[0112] In some embodiments, a long chain polymerization process for producing a long chain branched polymer may include polymerizing ethylene and at least one additional α-olefin in the presence of a catalyst having two polymer forming sites. The long chain branched polymer obtained from such a catalyst having two polymer forming sites has a molecular weight of, for example, 0.850 g / cm according to ASTM D792, which is incorporated herein by reference in its entirety. 3 ~0.960g / cm 3 , 0.880g / cm 3 ~0.920g / cm 3 , 0.880g / cm 3 ~0.910g / cm 3 , or 0.880 g / cm 3 ~0.900g / cm 3 The density of the sintered body may be 0.01 to 0.01.
[0113] In another embodiment, the long chain branched polymer obtained from the long chain polymerization process has a melt flow ratio (I 10 / I 2 ), where the melt index I 2is measured according to ASTM D1238, which is incorporated herein by reference in its entirety, under 190° C. and a load of 2.16 kg; and the melt index I 10 is measured according to ASTM D1238 at 190° C. and a load of 10 kg. In another embodiment, the melt flow ratio (I 10 / I 2 ) is 5-50, in others the melt flow ratio is 5-25, and in others the melt flow ratio is 5-9.
[0114] In some embodiments, the long chain branched polymer obtained from the long chain polymerization process may have a molecular weight distribution (MWD) of 1 to 20, where MWD is M w / M n is defined as M w is the weight average molecular weight, and M n is the number average molecular weight. In another embodiment, the polymer resulting from the catalyst system has an MWD of 1 to 10. Another embodiment includes an MWD of 1 to 3, and another embodiment includes an MWD of 1.5 to 2.5.
[0115] Parallel Polymerization Reactor (PPR) An example of a small-scale solution polymerization is carried out in a 15 mL vial using 5 mL total liquid volume, a constant ethylene pressure of 150 psig, and a polymerization temperature of 120 °C. The 5 mL volume is composed of 0.84 mL of comonomer mixture containing 500 nmol MMAO-3A, catalyst and activator solution in toluene, with enough Isopar-E added to achieve a 5 mL liquid volume. Experiments for any given diene are carried out in the same H 2 As done at load, hydrogen (H 2 ) at 80°C and 20±3psig H 2to the reaction mixture by simultaneously prepressurizing an empty reaction vial with 100% CO. All liquid amounts were dispensed at room temperature and added volumetrically to a total volume of 5 mL. The catalyst was added last to the reaction mixture as a 5 mM solution in toluene, which was activated separately with 1.5 equivalents of cocatalyst A (methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)borate). The comonomer solution consisted of primarily 1-octene with small (0–6%) volume fractions of diene species. The polymerization was carried out for no more than approximately 30 min and quenched by CO addition followed by vial depressurization.
[0116] Gel Permeation Chromatography (GPC) (conventional GPC) The chromatography system consisted of a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5) and a four-capillary viscometer (DV) coupled to a Precision Detectors (now Agilent Technologies) two-angle laser light scattering (LS) detector model 2040. For all absolute light scattering measurements, a 15 degree angle is used for measurement purposes. The autosampler oven compartment was set at 160 degrees Celsius and the column compartment was set at 150 degrees Celsius. The columns used were four Agilent "Mixed A" 30 cm, 20 micron linear mixed bed columns. The chromatography solvent used was 1,2,4-trichlorobenzene containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was nitrogen injected. The injection volume used was 200 microliters and the flow rate was 1.0 milliliters / min.
[0117] The GPC column set was calibrated with at least 20 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 to 8,400,000, arranged in six "cocktail" mixtures with at least 10 intervals between each molecular weight. Standards were purchased from Agilent Technologies. Polystyrene standards were prepared at 0.025 grams in 50 milliliters of solvent for molecular weights 1,000,000 and above, and 0.05 grams in 50 milliliters of solvent for molecular weights below 1,000,000. The polystyrene standards were dissolved at 80 degrees Celsius for 30 minutes with gentle agitation. The polystyrene standard peak molecular weights were converted to polyethylene molecular weights using Equation 52 (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)). M ポリエチレン =A×(M ポリスチレン ) B (52) where M is the molecular weight, A has a value of 0.4315, and B is equal to 1.0.
[0118] A polynomial between the third and fifth order was used to fit each polyethylene equivalent calibration point. A small adjustment (approximately 0.415 to 0.44) was made to A to correct for column resolution and band broadening effects, such that the NIST standard NBS 1475 is obtained at 52,000 Mw.
[0119] Total plate counts of the GPC column set were performed using eicosane (prepared at 0.04 g in 50 milliliters of TCB and dissolved for 20 minutes with gentle agitation). Plate counts (Equation 53) and symmetry (Equation 54) were measured with a 200 microliter injection according to the following equations:
number
number
[0120] Samples were prepared semi-automatically using the PolymerChar "Instrument Control" software to target sample weights of 2 mg / ml and add solvent (containing 200 ppm BHT) via the PolymerChar high temperature autosampler to septa-capped vials that had been pre-sparged with nitrogen. Samples were dissolved at 160 degrees Celsius with "slow" shaking for 2 hours.
[0121] M n(GPC) , M w(GPC) , and M. z(GPC) The calculation of was based on GPC results obtained using the internal IR5 detector (measurement channel) of a PolymerChar GPC-IR chromatograph according to Equations 55-57 using PolymerChar GPCOne™ software, baseline-subtracted IR chromatograms at each equally spaced data collection point (i), and the polyethylene equivalent molecular weight obtained from a narrow standard calibration curve for point (i).
number
[0122] To monitor deviations over time, a flow marker (decane) was introduced into each sample via a micropump controlled by the PolymerChar GPC-IR system. This flow marker (FM) was used to linearly calibrate the pump flow rate (Flow (apparent)) of each sample by RV matching the respective decane peak in the sample (RV (FM sample)) with the decane peak in the narrow standard calibration (RV (FM calibrated)). Any change in time of the decane marker peak is thus assumed to be related to a linear shift in flow rate (Flow (effective)). To facilitate the highest accuracy of the RV measurement of the flow marker peak, a least squares fitting routine is used to fit the peaks of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation is then used to determine the true peak position. After calibrating the system based on the flow marker peaks, the effective flow rate (relative to the narrow standard calibration) is calculated as in Equation 58. Processing of the flow marker peaks was performed by PolymerChar GPCOne™ software. An acceptable flow correction is that the effective flow rate should be within + / - 2% of the apparent flow rate. Flow (effective) = Flow (apparent) * (RV(FM calibrated) / RV(FM sample)) (58)
[0123] Triple Detector GPC (TDGPC) (Absolute GPC) The chromatographic system, analytical conditions, column set, column calibration and calculation and distribution of conventional molecular weight moments were performed according to the methods described in Gel Permeation Chromatography (GPC).
[0124] With regard to the determination of the offsets of the viscometer and the light scattering detector from the IR5 detector, a systematic procedure for the determination of multi-detector offsets was performed in a manner consistent with that published by Balke, Mourey, et. al. (Mourey and Balke, Chromatography Polym. Chpt 12, (1992)) (Balke, Thitiratsakul, Lew, Cheung, Mourey, Chromatography Polym. Chpt 13, (1992)) using PolymerChar GPCOne™ software to measure the offsets of broad homopolymer polyethylene standards (M w / M n Optimize the triple detector log (MW and IV) results from the narrow standard column calibration from the narrow standard calibration curve.
[0125] Absolute molecular weight data are obtained using PolymerChar GPCOne™ software in a manner consistent with that published by Zimm (Zimm, BH, J. Chem. Phys., 16, 1099 (1948)) and Kratochvil (Kratochvil, P., Classical Light Scattering from Polymer Solutions, Elsevier, Oxford, NY (1987)). The overall injected concentration used in determining the molecular weight is obtained from the mass detector area and mass detector constant derived from a suitable linear polyethylene homopolymer or one of the polyethylene standards of known weight average molecular weight. The calculated molecular weight (using GPCOne™) is obtained using the light scattering constant and the refractive index concentration coefficient, dn / dc, of 0.104, derived from one or more of the polyethylene standards described below. Typically, the mass detector response (IR5) and light scattering constant (determined using GPCOne™) are determined from linear standards with molecular weights above about 50,000 g / mole. Viscometer calibration (determined using GPCOne™) can be accomplished using the method described by the manufacturer, or alternatively, by using published values of suitable linear standards, such as Standard Reference Material (SRM) 1475a (available from the National Institute of Standards and Technology (NIST)). A viscometer constant (obtained using GPCOne™) is calculated that relates the specific viscosity area (DV) and injected mass for the calibration standard to its intrinsic viscosity. The chromatographic concentration is assumed to be low enough to preclude addressing the second viral coefficient effect (concentration effect on molecular weight).
[0126] Absolute weight average molecular weight (M w(Abs) ) is obtained by dividing (using GPCOne™) the light scattering area (LS) integrated chromatogram (factored by the light scattering constant) by the mass recovered from the mass constant and mass detector (IR5) area. The molecular weight and intrinsic viscosity responses are linearly extrapolated (using GPCOne™) at the chromatographic ends where the signal-to-noise ratio is low. The other respective moments, Mn(Abs) and M. z(Abs) is calculated according to equations 59-60 as follows:
number
[0127] g' ave value g' is defined as the viscosity of the branched polymer divided by the viscosity of a linear polymer of the same MW.
number
[0128] g' ave Or the average g' is the weighted average value of g' (BH Zimm, WH Stockmayer, J. Chem. Phys. 1949, 17, 1301).
[0129] Dynamic Mechanical Spectroscopy (or Small Angle Oscillatory Shear) The complex viscosity (η*), elastic modulus (G', G"), tangent delta, and phase angle (δ) are obtained by dynamic oscillatory frequency sweep testing in the frequency range of 0.1-100 rad / s at 190 °C. The level of strain is set within the linear viscoelastic region identified by strain sweep testing at 100 rad / s at 190 °C. The tests are performed using stainless steel parallel plates of 25 mm diameter on a strain-controlled rheometer ARES-G2 manufactured by TA Instruments. The samples with a thickness of 3.3 mm are drawn and trimmed in two steps before the actual test. In the first step, the samples are melted for 2.5 min, drawn to a gap of 3 mm, and trimmed. After a further soak at 190 °C for 2.5 min, the samples are drawn to a gap of 2 mm and the excess material is trimmed. The method incorporates an additional delay of 5 min to allow the system to reach temperature equilibrium. The tests are performed under a nitrogen atmosphere.
[0130] gpcBR branching index by triple detector GPC (TDGPC) The gpcBR branching index was determined by first calibrating the light scattering, viscosity, and concentration detectors as described above. The baseline was then subtracted from the light scattering, viscometer, and concentration chromatograms. An integration window was then set to ensure integration of all of the low molecular weight retention volume range in the light scattering and viscometer chromatograms that indicate the presence of detectable polymer from the refractive index chromatogram. Linear polyethylene standards were then used to establish the Mark-Houwink constants for polyethylene and polystyrene. Once the constants were obtained, the two values were used to construct two linear reference conventional calibrations for polyethylene molecular weight and polyethylene intrinsic viscosity as a function of elution volume, as shown in Equations (62) and (63).
number
[0131] The gpcBR branching index is a robust method for characterizing long chain branching, as described in Yau, Wallace W., “Examples of Using 3D-GPC-TREF for Poly-olefin Characterization,” Macromol. Symp., 2007, 257, 29-45. This index avoids the traditionally used “slice-by-slice” TDGPC calculations in determining g′ values and calculating branching frequency in favor of the entire polymer detector area. From the TDGPC data, the peak area method was used to obtain the sample bulk absolute weight average molecular weight (M w, absolute) can be obtained. This method avoids the "slice-by-slice" ratio of light scattering detector signal to concentration detector signal required in traditional g' determination. Sample intrinsic viscosity was also obtained independently using TDGPC using Eq. (64). The area calculation in this case provides greater accuracy since it is less sensitive to detector noise and fluctuations caused by TDGPC settings to the baseline and integration limits as the overall sample area. More importantly, the peak area calculation was not affected by detector volume offsets. Similarly, highly accurate sample intrinsic viscosity (IV) was obtained by the area method in Eq. (64).
number
[0132] In equation (64), DPi represents the differential pressure signal monitored directly from the online viscometer. To determine the gpcBR branching index, the light scattering elution area of the sample polymer was used to determine the molecular weight of the sample. The viscosity detector elution area of the sample polymer was used to determine the intrinsic viscosity (IV or [η]) of the sample. First, the molecular weight and intrinsic viscosity of a linear polyethylene standard sample, such as SRM1475a or equivalent, were determined using conventional calibration ("cc") for both molecular weight and intrinsic viscosity as a function of elution volume.
number
number
[0133] All statistics with "cc or conventional" subscripts are determined using their respective elution volumes, corresponding conventional calibrations as described above, and concentrations (Ci). Values without subscripts are measurements based on mass detectors, LALLS, and viscometer areas. PE The values of are iteratively adjusted until the linear reference sample has a gpcBR measurement of zero. For example, in this particular case, the final values of α and log K for determining the gpcBR are 0.725 and -3.355, respectively, for polyethylene, and 0.722 and -3.993, respectively, for polystyrene. Once the K and α values have been determined using the procedures described above.
[0134] Previously, this procedure was repeated using the branched sample. The branched sample was analyzed using the final Mark-Houck constant as the best "cc" calibration value.
[0135] The interpretation of gpcBR is straightforward. For linear polymers, the values measured by LS and viscometer are close to the traditional calibration standards, so gpcBR is close to zero. For branched polymers, the measured polymer molecular weight is calculated as M w,cc higher than the calculated IV ccis higher than the measured polymer IV, so that gpcBR becomes greater than zero, especially at high levels of long chain branching. In fact, the gpcBR value represents the fractional IV change due to the molecular size shrinkage effect as a result of polymer branching. A gpcBR value of 0.5 or 2.0 means a molecular size shrinkage effect of IV at a level of 50% and 200%, respectively, for an equivalent weight of linear polymer molecules. In these particular examples, the advantage of using gpcBR compared to traditional "g' index" and branching frequency calculations is due to the higher accuracy of gpcBR. All parameters used in gpcBR index determination are obtained with good accuracy and are not adversely affected by the low TDGPC detector response at high molecular weights from the concentration detector. Errors in the alignment of the detector volume also do not affect the accuracy of the gpcBR index determination.
[0136] Batch Reactor Polymerization Procedure The batch reactor polymerization reaction is carried out in a 2L Parr™ batch reactor. The reactor is heated by an electric heating mantle and cooled by an internal serpentine cooling coil containing cooling water. Both the reactor and the heating / cooling system are controlled and monitored by a Camile™ TG process computer. The bottom of the reactor is fitted with a dump valve that transfers the reactor contents to a stainless steel dump pot. The dump pot is pre-filled with a catalyst deactivation solution (typically 5 mL of an Irgafos / Irganox / toluene mixture). Both the pot and the tank are purged with nitrogen and the dump pot is vented to a 30 gallon blowdown tank. All solvents used for polymerization or catalyst make-up are passed through a solvent purification column to remove any impurities that may affect the polymerization. The 1-octene and IsoparE are passed through two columns, the first containing A2 alumina and the second containing Q5. Ethylene is passed through two columns, the first containing a204 alumina and the second containing Q5. 2 is passed through a single column containing A204 alumina, 4 Å molecular sieves and Q5.
[0137] The reactor is first charged from a shot tank which may contain IsoparE solvent and / or 1-octene depending on the reactor load. The shot tank is filled to the load set point using a lab scale attached to the shot tank. After the liquid feed is added, the reactor is heated to the polymerization temperature set point. If ethylene is used, it is added to the reactor at the reaction temperature to maintain the reaction pressure set point. The amount of ethylene added is monitored with a micromotion flow meter. In some experiments, standard conditions at 150°C are 13g ethylene, 15g 1-octene, and 240 psi hydrogen in 585g IsoparE, and standard conditions at 150°C are 15g ethylene, 45g 1-octene, and 200 psi hydrogen in 555g IsoparE.
[0138] The procatalyst and activator are mixed with an appropriate amount of purified toluene to obtain a solution of the desired molar concentration. The procatalyst and activator are handled in an inert glove box, drawn into a syringe, and pressure transferred into the catalyst shot tank. The syringe is rinsed three times with 5 mL of toluene. Immediately after the catalyst is added, a run timer is started. If ethylene is used, it is added by Camille to maintain the reaction pressure set point in the reactor. The polymerization reaction is run for 10 minutes, then the agitator is stopped and the bottom dump valve is opened to transfer the reactor contents to a dump pot. The dump pot contents are poured into a tray and placed in a lab hood where the solvent is allowed to evaporate overnight. The tray containing the remaining polymer is transferred to a vacuum oven and heated to 140° C. under vacuum to remove any remaining solvent. After the tray is cooled to ambient temperature, the polymer yield is measured to measure efficiency and subjected to polymer testing. EXAMPLES
[0139] Tetrafunctional branching in the presence of various multichain catalysts and various dienes The results of the small scale polymerizations are summarized in Tables 3-7 (the experiments are carried out in a parallel polymerization reactor, PPR). The polymer results recorded in Tables 3-7 were produced by polymerizing ethylene, octene, and diene species in the presence of multichain catalysts and single chain catalyst controls. The polymer results in each table of Tables 3-7 were the products of various catalysts and diene species. The results in Table 3 are based on the polymer products of 3-methyl-1,4-pentadiene, ethylene, and octene in the presence of Comparative Catalyst C1 ("Comp. Cat. C1"), Catalyst 1 ("Cat. 1"), and Catalyst 2 ("Cat. 2"). The results in Table 4 are based on the polymer products of 1,4-pentadiene, ethylene, and octene in the presence of Cat. 2 and Catalyst 4 ("Cat. 4"). The results in Table 5 are based on the polymer production of 1,5-hexadiene, ethylene, and octene in the presence of Comp. Cat. C1, Catalyst 3 ("Cat. 3"), Catalyst 5 ("Cat. 5"), and Catalyst 6 ("Cat. 6"). The results in Table 6 are based on the polymer production of 1,7-octadiene, ethylene, and octene in the presence of Comp. Cat. C1, Cat. 6, Cat. 2, and Cat. 4. The results in Table 7 are based on the polymer products of 1,9-decadiene, ethylene, and octene in the presence of Cat. 3, Cat. 5, Cat. 6, and Cat. 2 (Figueroa, R., Froese, RD, He, Y., Klosin, J., Theriault, CN, Abboud, KAOrganometallics 2011, 30, 1695-1709, Froese, RD, Jazdzewski, BA; Klosin, J., Kuhlman, RL, Theriault, CN, Welsh, DM, Abboud, KAOrganometallics 2011, 30, 251-262). [Table 4-1] [Table 4-2]
[0140] The single chain catalyst of Series 3.C (Comp.Cat.C1) incorporated increased amounts of α-olefins as indicated by more than twice the higher octene levels in the polymer when compared to the other catalysts. When using the single chain catalyst in Series 3.C (Comp.Cat.C1), the various levels of diene added did not significantly affect the polymer MWD. However, adding dienes to the dual chain catalysts in Tables 3-7 increased the MWD as the diene level increased. w and M. p This resulted in higher values of , and in many cases there was no evidence of high molecular weight tails forming.
[0141] In each example containing a diene, the amount of diene incorporated into the reactor was small compared to the other reactants in the reactor, and therefore the addition of the diene did not affect the amount of comonomer, ethylene, and solvent added to the reactor. Example 1 - Tetrafunctional branching with 3-methyl-1,4-pentadiene [Table 5] Example 2 - Tetrafunctional branching with 1,4-pentadiene [Table 6-1] [Table 6-2]
[0142] Figure 20 shows the shift in peak weight average molecular weight as the amount of diene increases. In Figure 20, the P2.4.1-P2.4.4 series recorded in Table 4 are plotted as dWdLogM as a function of LogM, which is a GPC plot. As the volume fraction of diene increased, the peak in the GPC plot shifted to the right. Example 3 - Tetrafunctional branching with 1,5-hexadiene [Table 7] Example 4 - Tetrafunctional branching with 1,7-octadiene [Table 8] Example 5 - Tetrafunctional branching with 1,9-decadiene [Table 9]
[0143] Branched examples from batch reactors The molecular weight distribution (MWD) curves and DSC of the two branched examples were examined and compared to the linear sample.
[0144] Batch Reactor Example 1 In Tables 8-12, the polymer properties of the comparative linear polymer sample (1C) are compared to the branched polymer from a batch reactor. The polymerization reaction was carried out at a temperature of 150° C., 555 g of ISOPAR-E™, and 200 psi hydrogen pressure (ΔH 2 The ethylene pressure was kept constant at 150 psi in the presence of 0.3 micromoles of catalyst 8, 0.36 micromoles of cocatalyst A (methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)borate), and 10 micromoles of MMAO-3A. [Table 10-1] [Table 10-2]
[0145] Figure 21 shows conventional molecular weight distribution curves of polymers of series 8.C (linear) and 8.1 (branched) as determined by GPC. The shape of the curve for the branched polymer, series 8.1, is altered compared to the linear polymer. In addition, the peak of the molecular weight curve is shifted to the right.
[0146] FIG. 22 is the absolute molecular weight distribution curves of polymers of series 8.C (linear) and 8.1 (branched) as determined by GPC.
[0147] FIG. 23 is an extensional viscosity fixture of the branched sample, series 8.1. [Table 11]
[0148] Dynamic mechanical spectra of the branched Example 8.1 were measured and the results are recorded in Table 9. The viscosity at 0.1 rad / sec was calculated to be 27,457 Pa s, the viscosity at 100 rad / sec was measured to be 974 Pa s, and the rheological ratio (V 0.1 / V 100 ) was 28.2.
[0149] The elastic modulus m is [((tan(δ 0.1 )-tan(δ 100 ))*1000) / (0.1-100)). tan(δ 0.1 ) is the tangent of the phase angle at 0.1 rad / s, and tan(δ 100 ) is the tangent of the phase angle at 100 rad / s. 0.1 ) is 1.6, and tan(δ 100 ) was 0.8 resulting in an elastic modulus of 7.9 at 190°C. [Table 12]
[0150] The dynamic mechanical spectrum of Comparative 8.C was measured and the results are recorded in Table 10. The shear viscosity at 0.1 rad / sec was calculated to be 892 Pa s, the shear viscosity at 100 rad / sec was measured to be 526 Pa s, and the rheological ratio (V 0.1 / V 100 ) was 1.7. The tan(δ 0.1 ), 8.C is 53.3, and tan(δ 100) was 2.0 resulting in an elastic modulus of 513.4 at 190℃.
[0151] The rheology ratio of the linear comparative polymer resin was very low (1.7) when compared to that of the branched Example, Series 8.1. The increased rheology ratio and low elastic modulus of the branched Example 1, Series 8.1, are indicative of non-linear polymer behavior. Strong shear thinning and elastic behavior are often indicative of entangled long chain branched polymers.
[0152] FIG. 24 is the melt strength obtained with the branched Example 1, Series 8.1 Rheotens device.
[0153] Branched Example 2 In Table 11, a branched polyethylene was synthesized in which the diene was 1,9-decadiene. The branched polymer was prepared by polymerization of 555 g of IsoparE at a temperature of 150° C. and 200 psi of hydrogen pressure (ΔH 2 The ethylene pressure was kept constant at 150 psi in the presence of 0.3 micromoles of catalyst 7, 0.36 micromoles of cocatalyst A, and 10 micromoles of MMAO-3A. [Table 13]
[0154] Figure 25 is a conventional molecular weight distribution curve of the branched Example 2 polymers of series 11.C (linear) and 11.1 (branched) as determined by GPC. Figure 26 is an absolute molecular weight distribution curve of the polymers of series 11.C (linear) and 11.1 (branched) as determined by light scattering triple photodetector. The shape of the curve for the branched polymer, series 11.1, is altered compared to the linear polymer.
[0155] FIG. 27 shows the extensional viscosity obtained with the branched Example 2 extensional viscosity fixture of Series 11.1. [Table 14]
[0156] The comparative dynamic mechanical spectra were measured and the results are recorded in Table 12. The shear viscosity at 0.1 rad / sec was calculated to be 17,643 Pa s, and the shear viscosity at 100 rad / sec was measured to be 857 Pa s, giving a rheological ratio (V 0.1 / V 100 ) was obtained. The tan(δ) of the branched polymer series 11.1 in Example 2 was 0.1 ) is 2.0, and tan(δ 100 ) was 1.0 resulting in an elastic modulus of 10.4 at 190°C.
[0157] FIG. 28 is the melt strength obtained with the branched Example 2, Series 11.1 Rheotens device.
[0158] Branching studies under various conditions Tetrafunctional "ladder branching" was studied under a variety of conditions, including increasing ethylene pressure, increasing octene monomer, increasing starting molecular weight, decreasing starting molecular weight, various dienes, increasing or decreasing amounts of diene, and various multi-chain catalysts.
[0159] Example 1: Various dienes and amounts of dienes The examples in Tables 13-22 were prepared under identical conditions and polymerized in the presence of catalyst 7 at a temperature of 150° C. Conditions included: 585 g Isopar E, 15 g 1-octene, 240 psi hydrogen pressure, 150 psi ethylene pressure, 0.3 micromoles of catalyst 7, 0.36 micromoles of cocatalyst A, and 10 micromoles of MMAO-3A. [Table 15-1] [Table 15-2] [Table 15-3]
[0160] The results in Table 13 show that when dienes are present in the polymerization reaction, molecular weight increases without a high molecular weight tail. Example 2: Conditions that result in high molecular weight [Table 16]
[0161] Utilizing these polymerization conditions to produce high molecular weight polymers resulted in tetrafunctional "ladder branches" that arise when dienes are incorporated into the polymerization reaction. The polymerization reaction resulted in a polymer resin with high molecular weight and tetrafunctional "ladder branches." Example 3: Conditions that lead to branched homopolymers [Table 17]
[0162] Incorporating a diene into the polymerization reaction used to make the homopolymer (with a small amount of diene) increased the molecular weight (tetrafunctional "ladder branching"). The data recorded in Table 15 shows that for the example ethylene-only resin, the molecular weight increased when two different dienes were incorporated into the polymerization reaction. [Table 18]
[0163] The results in Table 16 showed that branching occurred with different catalysts and at different densities. The resins in Table 16 showed sufficient branching with catalyst 8 and 7 mol % octene in the polymer. [Table 19]
[0164] Based on the results in Table 17, the molecular weight increased with the addition of dienes that exhibited tetrafunctional "ladder branching." These examples had higher linear molecular weights. In Examples 5.1 and 5.2, catalyst 8 produced higher molecular weight polymer resins when decadiene or pentadiene was present in the polymerization reaction. [Table 20]
[0165] The results in Table 18 show that an increase in molecular weight (tetrafunctional "ladder branching") occurred when different α-olefin comonomers were used. The polymer resins in Table 18 were produced with two different catalysts and two different hexene loadings. [Table 21]
[0166] Based on the results in Table 19, diene-induced molecular weight increase (tetrafunctional "ladder branching") occurred at various levels of octene. The examples in Table 19 show that tetrafunctional "ladder branching" occurred even with 7 mol% octene in the polymer. [Table 22]
[0167] As shown in Table 20, tetrafunctional "ladder branches" occurred at various levels of octene and higher starting molecular weights. Examples 8.1 and 8.2 were prepared using 7 mol % octene and a starting M of approximately 83,000 g / mol. w It has been shown that polymer resins having both decadiene and pentadiene branching are obtained. [Table 23]
[0168] The results in Table 21 show that there was a much lower density (higher levels of octene in the polymer) and increased molecular weight (tetrafunctional "ladder branching") at a lower starting molecular weight. In Example 9.1, the polymer resin contained more than 9 mol % octene and the starting M w was approximately 43,000 g / mol. When dienes were incorporated into the polymerization reaction, the molecular weight increased ("ladder branching" occurred). [Table 24]
[0169] The results in Table 22 show the molecular weights cased with dienes with different levels of incorporated octene (tetrafunctional "ladder branching") at lower starting molecular weights. In Example 22.1, the starting molecular weight of the polymer resin was about 51,000 g / mol, but when dienes were incorporated into the polymerization reaction, the molecular weight increased to 70,000 g / mol (tetrafunctional "ladder branching" occurred). [Table 25]
[0170] According to the data in Tables 23 and 24, increasing the ethylene pressure and the amount of octene in the reactor increased the molecular weight (tetrafunctional "ladder branching" occurred). [Table 26] Example 4: Decadiene homopolymer catalyzed by catalyst 7 [Table 27-1] [Table 27-2]
[0171] The results summarized in Table 25 show that tetrafunctional "ladder branching" occurs when octene is not present in the reactor. The molecular weight of each example in Table 25 increased as the amount of decadiene in the polymerization reaction increased. [Table 28]
[0172] Example 26.C.1 is the result of a polymerization reaction containing 0.2 octene. FIG. 29 is a graph of Log(MW) for Examples 26.C.1, 26.C.2, and 26.1-26.4. As the amount of decadiene increases, the molecular weight peak shifts to the right. Tables 27-32 summarize the results of the dynamic mechanical spectroscopy for Examples 26.C.1, 26.C.2, and 26.1-26.4. The results in each of Tables 27-32 show that the elastic modulus m decreases as the amount of tetrafunctional "ladder branch" increases. Additionally, the results in each of Tables 27-32 show that the rheology ratio increases as the amount of tetrafunctional "ladder branch" increases.
[0173] FIG. 29 is a conventional molecular weight distribution of curves in series 26.C.1, 26.C.2, and 26.1-26.4. [Table 29]
[0174] The comparative dynamic mechanical spectra were measured and the results are recorded in Table 27. The shear viscosity at 0.1 rad / sec was calculated to be 762 Pa s, the shear viscosity at 100 rad / sec was measured to be 552 Pa s, and the rheological ratio (V 0.1 / V 100 The tan(δ) of the branched polymer in Example 26.C.1 was 1.4. 0.1 ) is 192.8, and tan(δ 100 ) was 2.8 resulting in an elastic modulus of 1901.6 at 190°C. [Table 30]
[0175] The dynamic mechanical spectrum of Comparative Example 26.C.1 was measured and the results are recorded in Table 28. The shear viscosity at 0.1 rad / sec was calculated to be 662 Pa s, the shear viscosity at 100 rad / sec was measured to be 501 Pa s, and the rheological ratio (V 0.1 / V 100 The tan(δ) of the linear polymer of Example 26.C.1 was 1.3. 0.1 ) is 401.3, and tan(δ 100 ) was 3.1 resulting in an elastic modulus of 3986.2 at 190°C. [Table 31]
[0176] The dynamic mechanical spectrum of Example 26.1 was measured and the results are recorded in Table 29. The shear viscosity at 0.1 rad / sec was calculated to be 7,410 Pa s, the shear viscosity at 100 rad / sec was measured to be 883 Pa s, and the rheological ratio (V 0.1 / V 100 The tan(δ) of the branched polymer of Example 13.1 was 8.4. 0.1 ) is 4.3, and tan(δ 100 ) was 1.3 resulting in an elastic modulus of 29.8 at 190℃. [Table 32]
[0177] The dynamic mechanical spectrum of Example 26.2 was measured and the results are recorded in Table 30. The shear viscosity at 0.1 rad / sec was calculated to be 56,549 Pa s, the shear viscosity at 100 rad / sec was measured to be 1,236 Pa s, and the rheological ratio (V 0.1 / V 100 The tan(δ) of the branched polymer of Example 26.2 was 45.8. 0.1 ) is 1.2, and tan(δ 100 ) was 0.8 resulting in an elastic modulus of 4.2 at 190℃. [Table 33]
[0178] The dynamic mechanical spectrum of Example 26.3 was measured and the results are recorded in Table 31. The shear viscosity at 0.1 rad / sec was calculated to be 56,549 Pa s, the shear viscosity at 100 rad / sec was measured to be 1,236 Pa s, and the rheological ratio (V 0.1 / V 100 The tan(δ) of the branched polymer of Example 26.3 was 117.8. 0.1 ) is 1.2, and tan(δ 100 ) was 0.8 resulting in an elastic modulus of 1.5 at 190℃. [Table 34]
[0179] The dynamic mechanical spectrum of Example 26.4 was measured and the results are recorded in Table 32. The shear viscosity at 0.1 rad / sec was calculated to be 909,000 Pa s, the shear viscosity at 100 rad / sec was measured to be 3,054 Pa s, and the rheological ratio (V 0.1 / V 100 The tan(δ) of the branched polymer of Example 26.4 was 297.6. 0.1 ) is 0.3, and tan(δ 100 ) was 0.3 resulting in an elastic modulus of 0.4 at 190℃.
[0180] Guzman-2010 demonstrated and analyzed the MWD and physical properties resulting from conventional diene branching in a steady-state CSTR. A constrained geometry catalyst (CGC) was used to copolymerize ethylene, 1-octene, and 1,9-decadiene in a very well-mixed one-gallon reactor system. The specific CGC catalyst used by Guzman is described in detail in U.S. Pat. No. 5,965,756 (Structure IX) and U.S. Pat. No. 7,553,917 (Example 3). The Guzman-2010 catalyst was designed to grow a single chain from the catalyst center. Guzman's data was collected at steady state while the CSTR was operated at a pressure of 525 psig and a temperature of 155° C. over a range of diene feed concentrations. The various steady-state polymer samples collected by Guzman did not contain measurable levels of gel or insoluble material. However, at the highest level of diene feed, some internal reactor fouling was observed and higher levels of diene feed were expected to result in gel formation or reactor MWD instability.
[0181] A selected set of data from Guzman is summarized in Table 33 for reactor conditions fixed across a spectrum of diene feed levels. Throughout the series, ethylene and 1-octene feed concentrations were set at 13.8 wt% and 3.6 wt%, respectively. The catalyst feed rate was continuously adjusted to maintain a constant ethylene conversion of 79% throughout the series, resulting in a fixed polymer production rate of 2.2 kg / hr. Polymer density, a measure of copolymer composition, remained constant at approximately 0.922 g / cc. [Table 35]
[0182] According to the data in Table 33, I 2 and I 10The effect of conventional diene branching on molecular weight is shown in Table 33 for both absolute and conventional MWD measurement techniques. Absolute MWD measurement is the preferred method for branched polymers, but is not always available. Therefore, Table 33 also includes molecular weights measured by the conventional technique using a refractive index detector. The results in Table 33 show that for both measurement techniques, increasing the diene feed rate from zero to 923 ppm significantly increases the weight average molecular weight (M w ) shows a significant increase.
[0183] Although not reported in Guzman, the associated MWD curves were found in Table 33 and are plotted in Figures 30A and 30B for the absolute and conventional GPC measurement techniques, respectively. The MWD curve data in Figures 30A and 30B show the expected high M w The lack of significant movement of the peak MW with increasing diene branching is also evident from the MWD curves, indicating that tail formation has occurred.
[0184] The molecular weight distribution data in Figures 30A and 30B have been simplified into simple metrics that describe the evolution of the position and shape of the MWD curve as more diene monomer is fed to the CSTR. The data in Table 34 show these MWD metrics for both absolute and conventional MWD measurements of Guzman polymer samples. The absolute MWD measurement data in Table 34 show that as 1,9-decadiene feed amounts range from 0 to 923 ppm, molecular weight increases by up to 87%. The peak molecular weight change is p As shown in Table 34, neither means of molecular weight measurement changed significantly, which is not consistent with the results for the "ladder branched" polymers. The shape factors are summarized in Table 34 and are a function of diene feed level and M w As increases, G 79 / 29 and A TAILSince both values of , and , increase, their shape factors are not consistent with "ladder bifurcations." [Table 36]
[0185] Some important parameters for the commercial resins are given in Table 35. Some of the basic parameters of the materials were made in solution, gas phase, and high pressure reactors. [Table 37]
[0186] The data summarized in Table 35 are plotted in the graphs of Figures 31 and 32. The data show the differences in "ladder-branched" polymers compared to LDPE, LLDPE, ULDPE, and ethylene resins containing diene monomers. In Figures 31 and 32, the "ladder-branched" polymers of the present disclosure (Ladder-PE in the graph legend) are clustered together, thus showing that "ladder-branched" polymers have unique polymer properties compared to other ethylene-based resins. As shown in the graph of Figure 31, the "ladder-branched" polymers have at least 10 rheological ratios and an average g' of less than 0.86. In Figure 31, the plotted LDPE resins have an average g' of less than 0.65, and the prior art ethylene-diene resins (listed as Prior Art ET-Diene in the legend) do not cluster together.
[0187] In Figure 33, melt strength (centinewtons, cN) is plotted against melt index (Log I 2) was measured as a function of . The polymers produced from the dual-chain catalyst were compared to the polymers produced from the single-chain catalyst as well as literature-based curves for autoclave LDPE, tubular LDPE, and linear polyethylene, as indicated by the triangles and circles. The melt strengths of the polymers produced from the dual-chain catalyst were less than those of the autoclave LDPE, tubular LDPE, and single-chain catalyst, but significantly greater than the linear polyethylene. This indicates that the polymers produced from the dual-chain catalyst have intertwined long chain branches. 。
[0188] It will be apparent to those skilled in the art that various modifications can be made to the described embodiments without departing from the spirit and scope of the claimed subject matter. Thus, it is intended that this specification cover modifications and variations of the described embodiments provided such modifications and variations come within the scope of the appended claims and their equivalents. The present application also relates to the following aspects: (1) A process for synthesizing a long-chain branched copolymer, comprising the steps of: Contacting one or more C2-C14 alkene monomers, at least one diene or polyene, optionally a solvent, and a multi-chain catalyst together, wherein the multi-chain catalyst comprises: contacting a polymerizable compound comprising a plurality of polymerization sites; producing at least two polymer chains of said C2-C14 alkene monomer, each polymer chain polymerizing at one of said polymerization sites; and synthesizing the long chain branched polymer by connecting the two polymer chains with the diene or polyene, wherein the joining of the two polymer chains occurs in a concerted manner during the polymerization. (2) The process of (1) above, wherein ethylene is added to such an extent that the resulting copolymer has an ethylene content of greater than 50 mole percent. (3) The process of (1) or (2) above, wherein the diene and polyene comonomers are incorporated at a level to achieve at least one crosslink junction per 100 copolymer chains. (4) The process according to any one of (1) to (3) above, wherein the diene is non-conjugated or the polyene has at least two non-conjugated bonds per molecule. (5) The process according to any one of (1) to (4), wherein the multi-chain catalyst is a heterogeneous catalyst having a surface concentration of metal atoms of 0.3 metal atoms per square nanometer (metal / nm2) or more. (6) The process according to any one of (1) to (5), wherein the multi-chain catalyst has two linked transition metals linked by a dianionic activator, and the distance between the atoms of the metals is 18.5 Å or less. (7) The process according to any one of (1) to (6), wherein the multi-chain catalyst is composed of two or more covalently linked transition metals, and the distance between the metal atoms is 18.5 Å or less. (8) The process according to any one of (1) to (7), wherein the multi-chain catalyst has two or more polymer chains on the same metal. (9) The process according to any one of (1) to (8), wherein the multi-chain catalyst has a monoanionic ligand, is a Group IV metal (Ti, Zr, Hf), and has two polymer chains on the same metal. Process. (10) The process according to any one of (1) to (9) above, wherein the Mw of the long chain branching copolymer is at least 20% greater than the Mw of a polymer synthesized without the diene or polyene, or the Mp of the long chain branching copolymer is at least 20% greater than the Mp of a polymer synthesized without the diene or polyene. (11) The process according to any one of (1) to (10), wherein the polydisperse long-chain branched polymer has from 0.01 to 0.5 diene junctions per number average copolymer chain, or from 0.02 to 1.0 diene junctions per weight average copolymer chain. (12) The process according to any one of (1) to (11), wherein the polymerization occurs in a solution polymerization reactor or a particle-forming polymerization reactor such as a slurry reactor or a gas-phase reactor, a molecular or solid supported catalyst is delivered to the reaction medium or generated in the reaction medium, the reactor system is batch, continuous, or a hybrid such as semi-batch, and the reactor residence time distribution is narrow, such as in a non-backmixed reactor, or broad, such as in a backmixed reactor and in series and recycle reactors.
Claims
1. 1. A process for synthesizing a long chain branched copolymer, comprising: One or more C 2 -C 14 contacting an alkene monomer, at least one diene, optionally a solvent, and a double-stranded catalyst with each other; the double-stranded catalyst comprises two polymerization sites; the double-stranded catalyst has a monoanionic ligand, is a Group IV metal, has two polymer strands on the same metal, and the diene is selected from 2-methyl-1,4-pentadiene, 3-methyl-1,4-pentadiene, 1,3-divinylcyclopentane, 2-methyl-1,5-hexadiene, 1,4-pentadiene, 1,5-hexadiene, 1,7-octadiene, 1,8-nonadiene, 1,9-decadiene, 1,11-dodecadiene, and 1,15-hexadecadiene; Said C 2 -C 14 forming at least two polymer chains of an alkene monomer, each polymer chain polymerizing at one of said polymerization sites; synthesizing a long chain branched polymer by connecting said two polymer chains with said diene, wherein said connecting of said two polymer chains occurs in a concerted manner during said polymerization.
2. 10. The process of claim 1, wherein ethylene is added to an extent such that the resulting copolymer has a content of greater than 50 mole percent ethylene.
3. 3. The process of claim 1 or 2, wherein the diene comonomer is incorporated at a level to achieve at least one crosslink junction per 100 copolymer chains.
4. The double-stranded catalyst has a density of 0.3 metal atoms per square nanometer (metal / nm 2 4. The process according to claim 1, wherein the catalyst is a heterogeneous catalyst having a surface concentration of metal atoms of at least 10000000000.
5. 5. The process of any one of claims 1 to 4, wherein the double-stranded catalyst has two linked transition metals linked by a dianionic activator, the distance between the metal atoms being 18.5 Å or less.
6. 6. The process of any one of claims 1 to 5, wherein the double-stranded catalyst consists of two or more covalently linked transition metals, the distance between the metal atoms being 18.5 Å or less.
7. The process of any one of claims 1 to 6, wherein the double-stranded catalyst has two or more polymer chains on the same metal.
8. The process of any one of claims 1 to 7, wherein the double-stranded catalyst has a monoanionic ligand and is Ti, Zr, or Hf, and has two polymer chains on the same metal.
9. 9. The process of any one of claims 1 to 8, wherein the Mw of the long chain branched copolymer is at least 20% greater than the Mw of a polymer synthesized without the diene, or the Mp of the long chain branched copolymer is at least 20% greater than the Mp of a polymer synthesized without the diene.
10. The process of any one of claims 1 to 9, wherein the polydisperse long chain branched polymer has from 0.01 to 0.5 diene junctions per number average copolymer chain, or from 0.02 to 1.0 diene junctions per weight average copolymer chain.
11. 11. The process of any one of claims 1 to 10, wherein the polymerization occurs in a solution polymerization reactor, or a slurry reactor or a particle formation polymerization reactor, a molecular or solid supported catalyst is delivered to or generated in the reaction medium, the reactor system is batch, continuous or hybrid, and the reactor residence time distribution is narrow as in non-backmixed reactors or broad as in backmixed reactors and series and recycle reactors.
Citation Information
Patent Citations
Catalyst for production of olefin polymer
JP2002513443A
Imino-amide catalyst compounds for olefin polymerization
JP2005511867A
Modified polyethylene composition
JP2014530272A
Bimetallic complex comprising cyclopentadienyl and amidine ligands
US20160122370A1
Metal complex, metal catalyst composition comprising same metal complex, and method for preparing copolymer containing ethylene, alpha-olefin and diene using same metal catalyst composition
WO2018155982A1