Composite and its uses

A graft polymer with specific solubility parameters improves compatibility between aliphatic polycarbonate and cellulose resin, enhancing transparency and mechanical strength in composite materials.

JP7587504B2Active Publication Date: 2024-11-20MURATA MFG CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021539256
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-09
Filing Date
2020-08-07
Publication Date
2024-11-20
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

Aliphatic polycarbonate and cellulose resin have poor compatibility, leading to issues such as decreased transparency and easy peeling at the interface when attempting to form composites.

Method used

A composite is formed using a graft polymer with a cellulose resin backbone and a branch polymer having a solubility parameter of 17-24 MPa, which enhances compatibility with aliphatic polycarbonate.

Benefits of technology

The composite exhibits high compatibility, resulting in improved transparency and reduced peeling, with uniform distribution and strong bonding between components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587504000001
    Figure 0007587504000001
  • Figure 0007587504000002
    Figure 0007587504000002
  • Figure 0007587504000003
    Figure 0007587504000003
Patent Text Reader

Abstract

Provided are a composite body wherein the compatibility between a cellulose-based resin and an aliphatic polycarbonate is excellent, and an application therefor. This composite body comprises a graft polymer and an aliphatic polycarbonate. The graft polymer comprises a backbone polymer and a branching polymer bonded to the backbone polymer. The backbone polymer contains a cellulose-based resin. The branching polymer is a polymer having a solubility parameter according to Fedors' method of 17 to 24 MPa0.5.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite and uses thereof. [Background technology]

[0002] In recent years, various environmentally friendly functional resins have been developed due to concerns about environmental pollution caused by plastics. In this regard, since aliphatic polycarbonate is a biodegradable resin, the development of resins using aliphatic polycarbonate or blending technology of aliphatic polycarbonate with other biodegradable resins has been attracting attention. Among aliphatic polycarbonates, the use of aliphatic polycarbonate made from carbon dioxide as a raw material can be said to be an environmentally friendly material in that carbon dioxide can be fixed.

[0003] For example, Patent Document 1 proposes a composite material containing a cellulose material and an aliphatic polycarbonate. It is disclosed that such a composite material improves the physical properties of the aliphatic polycarbonate, such as the mechanical strength. Patent Document 2 proposes a composite material containing cellulose and an aliphatic polycarbonate having a specific structure. Such a composite material allows the biodegradation rate to be controlled, forming a biodegradable material that can be used for a long period of time even in the natural environment. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-001263 A [Patent Document 2] JP 2006-036954 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, since aliphatic polycarbonate and cellulose-based resin are not very compatible with each other, even if attempts are made to combine the two materials, it is difficult to obtain the desired composite. For example, the composite of aliphatic polycarbonate and cellulose-based resin has problems such as reduced transparency or easy peeling at the interface between the aliphatic polycarbonate and the cellulose-based resin.

[0006] The present invention has been made in view of the above, and an object of the present invention is to provide a composite in which a cellulose-based resin and an aliphatic polycarbonate have good compatibility, and uses thereof. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object, and as a result have found that the above object can be achieved by using a graft polymer in which the branch polymer has a specific solubility parameter, thereby completing the present invention.

[0008] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 A composite comprising a graft polymer and an aliphatic polycarbonate, The graft polymer has a trunk polymer and a branch polymer bonded to the trunk polymer, the trunk polymer containing a cellulose-based resin, The branched polymer has a solubility parameter of 17 to 24 MPa as determined by the Fedors method. 0.5 The complex is a polymer B. Section 2 Item 2. The composite according to item 1, wherein the proportion of the polymer relative to the cellulose-based resin is 10% by mass or more and 400% by mass or less. Section 3 Item 3. The complex according to item 1 or 2, wherein the polymer B is at least one selected from the group consisting of polycaprolactone, polylactic acid, poly(3-hydroxybutyric acid), polybutylene succinate, polyethylene carbonate, polypropylene carbonate, polytrimethylene carbonate, polyethylene glycol, polypropylene glycol, and polymethyl methacrylate. Section 4 4. The composite according to any one of items 1 to 3, wherein the cellulose-based resin is at least one selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, and cellulose ester. Section 5 Item 5. The composite according to any one of items 1 to 4, wherein the graft polymer has a mass average molecular weight of 50,000 or more and 1,000,000 or less. Section 6 Item 6. A film comprising the composite according to any one of items 1 to 5. Section 6-1 Item 6. Use of the composite according to any one of items 1 to 5 in a film. Section 7 Item 6. A sheet comprising the composite according to any one of items 1 to 5. Section 7-1 Item 6. Use of the composite according to any one of items 1 to 5 in a sheet. Section 8 A particle comprising the complex according to any one of items 1 to 5. Section 8-1 Item 6. Use of the complex according to any one of items 1 to 5 in particles. Section 9 Item 6. A fiber comprising the composite according to any one of items 1 to 5. Section 9-1 Item 6. Use of the composite according to any one of items 1 to 5 in fibers. Effect of the Invention

[0009] The composite according to the present invention has excellent physical properties due to the high compatibility between the cellulose-based resin and the aliphatic polycarbonate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present invention will be described in detail. In this specification, the expressions "contain" and "include" include the concepts of "contain", "include", "consist essentially of" and "consist only of". In addition, in this specification, a numerical value connected with "~" means a numerical range including the numerical values ​​before and after "~" as the lower and upper limits.

[0011] The composite of the present invention includes a graft polymer and an aliphatic polycarbonate. In particular, the graft polymer has a trunk polymer and a branch polymer bonded to the trunk polymer, the trunk polymer includes a cellulose-based resin, and the branch polymer has a solubility parameter of 17 to 24 MPa as determined by the Fedors method. 0.5 Polymer B is:

[0012] According to the composite of the present invention, the cellulose-based resin and the aliphatic polycarbonate have high compatibility, and therefore have excellent physical properties. Specifically, the cellulose-based resin in the graft polymer has a polymer having a predetermined solubility parameter as a branch polymer as a graft chain, and therefore has high affinity for aliphatic polycarbonate, and is therefore easily compatible with aliphatic polycarbonate. Therefore, for example, when the composite is a film or sheet, the transparency is high. Also, when the composite is a multilayer film or multilayer sheet having a layer containing a graft polymer and a layer containing an aliphatic polycarbonate, peeling at the interface is unlikely to occur. Also, when the composite is a particle containing a graft polymer and an aliphatic polycarbonate, both can be uniformly distributed in the particle, or core-shell particles can be easily formed. Also, when the composite is a fiber containing a graft polymer and an aliphatic polycarbonate, both can be uniformly distributed, or a core-sheath structure can be easily formed.

[0013] (Graft polymer) In the graft polymer, the type of cellulose resin constituting the trunk polymer is not particularly limited, and for example, known cellulose resins can be widely applied. Specific examples of cellulose resins include alkyl celluloses such as methyl cellulose, ethyl cellulose, methylethyl cellulose, n-propyl cellulose, isopropyl cellulose, n-butyl cellulose, tert-butyl cellulose, and n-hexyl cellulose; hydroxyalkyl celluloses such as hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and hydroxybutyl cellulose; cellulose esters such as cellulose acetate, cellulose diacetate, cellulose triacetate, cellulose acetate propionate, and cellulose acetate butyrate; carboxyalkyl celluloses such as carboxymethyl cellulose, carboxyethyl cellulose, and carboxypropyl cellulose; and cellulose derivatives such as nitrocellulose, aldehyde cellulose, dialdehyde cellulose, and sulfonated cellulose, and cellulose. The type of cellulose resin constituting the trunk polymer can be one or more types.

[0014] Among them, from the viewpoint of easy production of the graft polymer and easy improvement of compatibility with the aliphatic polycarbonate, the cellulose-based resin is preferably one or more selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, and cellulose ester. Among them, ethyl cellulose, hydroxypropyl cellulose, and cellulose acetate butyrate are more preferable, and ethyl cellulose is particularly preferable.

[0015] In the graft polymer, the degree of substitution of the cellulose-based resin is not particularly limited and may be various values ​​as long as the effects of the present invention are not impaired. For example, the degree of substitution of the cellulose-based resin is 2 or more and 3 or less, and is generally 3.

[0016] In this specification, the degree of substitution of a cellulose-based resin refers to the total number of hydroxyl groups substituted with groups other than hydroxyl groups, including those of branch polymers, out of all hydroxyl groups in the structural units of the cellulose-based resin.

[0017] The trunk polymer may contain structural units other than the cellulose-based resin, or may be formed only from the cellulose-based resin. When the trunk polymer contains structural units other than the cellulose-based resin, the content of such units may be 30% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 1% by mass or less, based on the total structural units of the trunk polymer.

[0018] In the graft polymer, the branch polymer has a solubility parameter of 17-24MPa as determined by the Fedors method. 0.5 The polymer B is represented by the formula: The solubility parameter determined by the Fedors method is a calculation method that is widely used to determine the solubility parameter (SP value) of various organic compounds and polymeric compounds, and the solubility parameter can be easily calculated based on the molecular structure (Fedors: Polym. Eng. Sci., 14[2], 147-154(1974)).

[0019] In the graft polymer, the branch polymer is usually present by being bonded to the cellulose resin trunk polymer via a chemical bond (particularly a covalent bond). In one embodiment, the graft polymer of the present invention has a hydroxyl group or a hydrogen atom of the hydroxyl group in the structural unit of the cellulose resin substituted with a branch polymer. In another embodiment, the graft polymer of the present invention has a hydrogen atom on a carbon atom in the structural unit of the cellulose resin substituted with a branch polymer. In another embodiment, the branch polymer is bonded to a carbon atom or an oxygen atom at the cleavage site of the glucose ring.

[0020] In the composite of the present invention, the branch polymer constituting the graft polymer has a viscosity of 17 to 24 MPa. 0.5 As long as the polymer B is a branch polymer of the graft polymer, various polymers can be used as the branch polymer of the graft polymer.

[0021] Examples of such polymer B include polycaprolactone (20.9), polyglycolic acid (19.9), polylactic acid (21.6), poly(3-hydroxypropionic acid) (23.6), poly(3-hydroxybutyric acid) (21.6), poly(3-hydroxyvaleric acid) (21.6), poly(4-hydroxybutyric acid) (22.3), polyethylene succinate (23.6), polyethylene adipate (22.3), polybutylene succinate (22.3), polybutylene adipate (21.4), poly(p-dioxanone) (22.8), polyethylene carbonate (22.6), polypropylene carbonate (19.5), polybutylene carbonate (19.2), polycyclohexene carbonate (19.6), polytrimethylene carbonate. (21.5), poly(2,2-dimethyltrimethylene carbonate) (18.4), polyethylene glycol (19.2), polypropylene glycol (17.7), polytrimethylene glycol (18.7), polytetramethylene glycol (18.4), polyethyleneimine (22.3), poly(N-methylethyleneimine) (17.3), poly(N-ethylethyleneimine) (18.1), polyvinyl acetate (20.5), polymethyl acrylate (20.9), polyethyl acrylate (20.4), polyhydroxyethyl acrylate (21.6), polymethyl methacrylate (19.4), polyethyl methacrylate (19.2), polyhydroxyethyl methacrylate (19.6), and polystyrene (20.7). The polymer may have only one of them, or two or more of them. The numbers in parentheses indicate the solubility parameters determined by the Fedors method.

[0022] Polymer B is preferably at least one of polyethylene carbonate, polypropylene carbonate, polycaprolactone, and polylactic acid, although it depends on the type of aliphatic polycarbonate to be composited.

[0023] In the graft polymer, the content ratio of the cellulose resin constituting the trunk polymer and the polymer B constituting the branch polymer is not particularly limited as long as the effects of the present invention are not impaired. From the viewpoint of making the compatibility between the graft polymer and the aliphatic polycarbonate easier to increase, the graft polymer preferably has a ratio of the polymer B of 10% by mass or more and 400% by mass or less relative to the cellulose resin. In particular, the ratio of the polymer to the cellulose resin is preferably 50% by mass or more and 250% by mass or less.

[0024] The ratio of the polymer to the cellulose-based resin can be determined by nuclear magnetic resonance spectroscopy (NMR analysis). In a graft polymer, the ratio of the polymer to the cellulose-based resin is also called the "graft ratio."

[0025] The mass average molecular weight of the graft polymer is not particularly limited, and can be, for example, 50,000 to 1,000,000. In this case, the graft polymer can have better mechanical properties such as strength, elongation, and fracture toughness, and also has excellent moldability. It is more preferable that the mass average molecular weight of the graft polymer is 100,000 to 600,000.

[0026] The method for producing the graft polymer is not particularly limited, and for example, a method similar to a method for producing a known graft polymer can be adopted.

[0027] Specifically, the graft polymer can be produced by a production method including a step of ring-opening polymerization of a cyclic compound in the presence of a cellulose-based resin. Hereinafter, this method is referred to as "Production Method A of a Graft Polymer."

[0028] In the method A for producing a graft polymer, ring-opening polymerization of a cyclic compound is carried out in the presence of a cellulose-based resin. The cellulose-based resin used in the method A for producing a graft polymer is a raw material for forming a trunk polymer of the graft polymer. In the method A for producing a graft polymer, the polymer formed by the ring-opening polymerization of the cyclic compound has a solubility parameter of 17 to 24 MPa as determined by the Fedors method.0.5 In other words, the cyclic compound used in the method for producing a graft polymer A is a raw material for forming a branch polymer of the graft polymer.

[0029] The type of cellulose resin used in the method for producing a graft polymer A is not particularly limited, and for example, known cellulose resins can be widely applied. Specific examples of cellulose resins include alkyl celluloses such as methyl cellulose, ethyl cellulose, methylethyl cellulose, n-propyl cellulose, isopropyl cellulose, n-butyl cellulose, tert-butyl cellulose, and n-hexyl cellulose; hydroxyalkyl celluloses such as hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and hydroxybutyl cellulose; cellulose esters such as cellulose acetate, cellulose diacetate, cellulose triacetate, cellulose acetate propionate, and cellulose acetate butyrate; carboxyalkyl celluloses such as carboxymethyl cellulose, carboxyethyl cellulose, and carboxypropyl cellulose; and cellulose derivatives or celluloses such as nitrocellulose, aldehyde cellulose, dialdehyde cellulose, and sulfonated cellulose. The cellulose resin used in the method for producing a graft polymer A can be one or more types.

[0030] Among them, the cellulose-based resin is preferably one or more selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, and cellulose ester, more preferably ethyl cellulose, hydroxypropyl cellulose, and cellulose acetate butyrate, and more preferably ethyl cellulose and hydroxypropyl cellulose, and particularly preferably ethyl cellulose.

[0031] The mass average molecular weight of the cellulose-based resin used in the graft polymer production method A is not particularly limited. For example, the mass average molecular weight of the cellulose-based resin is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 100,000 or more. In addition, the mass average molecular weight of the cellulose-based resin is preferably 1,000,000 or less, more preferably 750,000 or less, and even more preferably 500,000 or less.

[0032] The cyclic compound used in the graft polymer manufacturing method A has a solubility parameter of 17 to 24 MPa as determined by the Fedors method. 0.5 The type of the cyclic compound is not particularly limited as long as it can form a polymer B having the formula: ##STR00011## Specific examples of the cyclic compound include ε-caprolactone, glycolide, L-lactide, D-lactide, meso-lactide, β-propiolactone, β-butyrolactone, γ-butyrolactone, δ-valerolactone, p-dioxanone, ethylene carbonate, propylene carbonate, butylene carbonate, cyclohexene carbonate, trimethylene carbonate, 2,2-dimethyltrimethylene carbonate, ethylene oxide, propylene oxide, trimethylene oxide (oxetane), tetrahydrofuran, aziridine, N-methylaziridine, and N-ethylaziridine.

[0033] When the cyclic compound is ε-caprolactone, the branch polymer of the graft polymer is polycaprolactone. When the cyclic compound is L-lactide, the branch polymer of the graft polymer is polylactic acid in the L configuration. When the cyclic compound is D-lactide, the branch polymer of the graft polymer is polylactic acid in the D configuration. When the cyclic compound is meso-lactide, the branch polymer of the graft polymer is polylactic acid in the syndiotactic configuration. When the cyclic compound is β-propiolactone, the branch polymer of the graft polymer is poly(3-hydroxypropionic acid). When the cyclic compound is β-butyrolactone, the branch polymer of the graft polymer is poly(3-hydroxybutyric acid). When the cyclic compound is γ-butyrolactone, the branch polymer of the graft polymer is poly(4-hydroxybutyric acid). When the cyclic compound is δ-valerolactone, the branch polymer of the graft polymer is poly(3-hydroxyvaleric acid). When the cyclic compound is p-dioxanone, the branch polymer of the graft polymer is poly(p-dioxanone). When the cyclic compound is ethylene carbonate, the branch polymer of the graft polymer is polyethylene carbonate. When the cyclic compound is propylene carbonate, the branch polymer of the graft polymer is polypropylene carbonate. When the cyclic compound is butylene carbonate, the branch polymer of the graft polymer is polybutylene carbonate. When the cyclic compound is cyclohexene carbonate, the branch polymer of the graft polymer is polycyclohexene carbonate. When the cyclic compound is trimethylene carbonate, the branch polymer of the graft polymer is polytrimethylene carbonate. When the cyclic compound is 2,2-dimethyltrimethylene carbonate, the branch polymer of the graft polymer is poly(2,2-dimethyltrimethylene carbonate). When the cyclic compound is ethylene oxide, the branch polymer of the graft polymer is polyethylene glycol. When the cyclic compound is propylene oxide, the branch polymer of the graft polymer is polypropylene glycol. When the cyclic compound is trimethylene oxide (oxetane), the branch polymer of the graft polymer is polytrimethylene glycol.When the cyclic compound is tetrahydrofuran, the branch polymer of the graft polymer is polytetramethylene glycol. When the cyclic compound is aziridine, the branch polymer of the graft polymer is polyethyleneimine. When the cyclic compound is N-methylaziridine, the branch polymer of the graft polymer is poly(N-methylaziridine). When the cyclic compound is N-ethylaziridine, the branch polymer of the graft polymer is poly(N-ethylaziridine).

[0034] In the method for producing a graft polymer A, the method for ring-opening polymerization of a cyclic compound is not particularly limited, and known ring-opening polymerization conditions can be widely adopted. For example, the ring-opening polymerization of a cyclic compound can be carried out in the presence of a catalyst. Examples of the catalyst include metal catalysts such as sodium, potassium, sodium hydroxide, potassium hydroxide, triethylaluminum, aluminum triisopropoxide, n-butyllithium, titanium tetraisopropoxide, titanium tetrachloride, zirconium tetraisopropoxide, tin tetrachloride, sodium stannate, tin octanoate, dibutyltin dilaurate, and diethylzinc; base catalysts such as pyridine, 4-dimethylaminopyridine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD), and 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU); acid catalysts such as hydrochloric acid, acetic acid, methanesulfonic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, diphenyl phosphoric acid, and phenol; and N-heterocyclic carbenes such as 1,3-bis(2-propyl)-4,5-dimethylimidazol-2-ylidene and 1,3-di-i-propylimidazol-2-ylidene. The catalyst used in the ring-opening polymerization may be one type alone or two or more types.

[0035] The ring-opening polymerization of cyclic carbonates can also be carried out using a cocatalyst, such as N-cyclohexyl-N'-phenylthiourea, N,N'-bis[3,5-bis(trifluoromethyl)phenyl]thiourea, N-[3,5-bis(trifluoromethyl)phenyl]-N'-cyclohexylthiourea, (-)-sparteine, etc.

[0036] The amount of catalyst (co-catalyst if necessary) used in the ring-opening polymerization of cyclic compounds can be the same as the ring-opening polymerization conditions of known cyclic compounds. From the viewpoint of promoting the progress of the polymerization reaction, it is preferably 0.001 mol or more, more preferably 0.005 mol or more, per 1 mol of cyclic compounds. In addition, the amount of catalyst (co-catalyst if necessary) used in the polymerization reaction is preferably 0.2 mol or less, more preferably 0.1 mol or less, per 1 mol of cyclic compounds, from the viewpoint of obtaining an effect commensurate with the amount used.

[0037] In the ring-opening polymerization of a cyclic compound, a reaction solvent may be used as necessary. The reaction solvent is not particularly limited, and various organic solvents can be used. Examples of the organic solvent include aliphatic hydrocarbon solvents such as pentane, hexane, octane, decane, and cyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, and xylene; halogenated hydrocarbon solvents such as methylene chloride, chloroform, 1,1-dichloroethane, 1,2-dichloroethane, chlorobenzene, and bromobenzene; ether solvents such as ethylene glycol dimethyl ether (monoglyme), diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and anisole; ester solvents such as ethyl acetate, n-propyl acetate, and isopropyl acetate; amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and carbonate solvents such as dimethyl carbonate, diethyl carbonate, and propylene carbonate.

[0038] The amount of the reaction solvent used is preferably 100 to 10,000 parts by mass per 100 parts by mass of the cyclic compound, from the viewpoint of smoothly proceeding with the ring-opening polymerization.

[0039] The ring-opening polymerization can be carried out, for example, by charging a cellulose-based resin, a cyclic compound, a catalyst, and optionally a co-catalyst, a reaction solvent, and the like into a glass flask, mixing them, and allowing them to react.

[0040] The reaction temperature for the ring-opening polymerization cannot be determined in general because it differs depending on the type of cyclic compound, but is preferably -80°C or higher, more preferably -40°C or higher, and even more preferably 0°C or higher, and from the viewpoint of suppressing side reactions and improving the yield, is preferably 250°C or lower, more preferably 200°C or lower, and even more preferably 150°C or lower.

[0041] The reaction time varies depending on the polymerization reaction conditions and cannot be generally determined, but it is usually preferably about 1 to 40 hours.

[0042] In the method A for producing a graft polymer, the ratio of the cellulose resin to the cyclic compound is not particularly limited and can be appropriately set depending on the desired graft ratio and the degree of substitution of the cellulose resin. From the viewpoint of high affinity of the resulting graft polymer to the aliphatic polycarbonate and easy compatibility with the aliphatic polycarbonate, the amount of the cyclic compound used per 100 parts by mass of the cellulose resin is preferably 10 parts by mass or more and 1000 parts by mass or less, more preferably 50 parts by mass or more and 500 parts by mass or less.

[0043] As described above, in the method A for producing a graft polymer, the ring-opening polymerization of a cyclic compound is carried out in the presence of a cellulose-based resin, whereby the cyclic compound undergoes ring-opening polymerization to produce polymer B, and the hydroxyl groups in the structural units of the cellulose-based resin also react with the cyclic compound. As a result, a graft polymer having a structure in which the hydroxyl groups in the structural units of the cellulose-based resin or the hydrogen atoms of the hydroxyl groups are substituted with polymer B formed by ring-opening polymerization is obtained.

[0044] In the method A for producing the graft polymer, after the polymerization reaction, the obtained graft polymer can be purified by an appropriate method as required.

[0045] On the other hand, the graft polymer can also be produced by a method other than the above-mentioned Production Method A. Specifically, the graft polymer can be produced by a production method including a step of copolymerizing a cyclic ether with carbon dioxide in the presence of a cellulose-based resin. Hereinafter, this method is referred to as "Production Method B of a Graft Polymer."

[0046] In the method for producing a graft polymer B, a cyclic ether and carbon dioxide are copolymerized in the presence of a cellulose-based resin. The cellulose-based resin used in the method for producing a graft polymer B is a raw material for forming the trunk polymer of the graft polymer. In addition, the polymer formed by the copolymerization of a cyclic ether and carbon dioxide has a solubility parameter of 17 to 24 MPa as determined by the Fedors method. 0.5 That is, the cyclic ether and carbon dioxide used in the graft polymer production method B are raw materials for forming the branch polymer of the graft polymer.

[0047] The type of cellulose-based resin used in the graft polymer production method B is not particularly limited, and may be the same as the cellulose-based resin used in the graft polymer production method A. Therefore, the cellulose-based resin used in the graft polymer production method B is preferably one or more selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, and cellulose ester, and is particularly preferably ethyl cellulose.

[0048] Examples of the cyclic ether used in the graft polymer production method B include ethylene oxide, propylene oxide, trimethylene oxide (oxetane), 3,3-dimethyltrimethylene oxide (3,3-dimethyloxetane), 1,2-butylene oxide, 2,3-butylene oxide, isobutylene oxide, 1-pentene oxide, 2-pentene oxide, 1-hexene oxide, 1-octene oxide, 1-dodecene oxide, cyclopentene oxide, cyclohexene oxide, styrene oxide, vinylcyclohexane oxide, 3-phenylpropylene oxide, 3,3,3-trifluoropropylene oxide, 3-naphthylpropylene oxide, 2-phenoxypropylene oxide, 3-naphthoxypropylene oxide, butadiene monoxide, 3-vinyloxypropylene oxide, and 3-trimethylsilyloxypropylene oxide. Among these, from the viewpoint of high affinity of the resulting polymer to aliphatic polycarbonate and easy compatibility with aliphatic polycarbonate, ethylene oxide, propylene oxide, trimethylene oxide and 1,2-butylene oxide are preferred, and ethylene oxide, propylene oxide and trimethylene oxide are more preferred. When the cyclic ether contains ethylene oxide, the resulting polycarbonate is polyethylene carbonate, when the cyclic ether contains propylene oxide, the resulting polycarbonate is polypropylene carbonate, and when the cyclic ether contains trimethylene oxide, the resulting polycarbonate is polytrimethylene carbonate.

[0049] The polymerization reaction for copolymerizing the cyclic ether and carbon dioxide can also be carried out in the presence of a metal catalyst. Examples of the metal catalyst include zinc-based catalysts, aluminum-based catalysts, chromium-based catalysts, and cobalt-based catalysts. Among these, zinc-based catalysts and cobalt-based catalysts are preferred because they have high polymerization activity in the polymerization reaction of the cyclic ether and carbon dioxide.

[0050] Examples of zinc-based catalysts include diethylzinc-water catalyst, diethylzinc-pyrogallol catalyst, bis((2,6-diphenyl)phenoxy)zinc, N-(2,6-diisopropylphenyl)-3,5-di-tert-butylsalicylaldiminatozinc, 2-((2,6-diisopropylphenyl)amido)-4-((2,6-diisopropylphenyl)imino)-2-pentenezinc acetate, zinc adipate, and zinc glutarate.

[0051] Cobalt-based catalysts include cobalt acetate-acetic acid catalysts, N,N'-bis(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt acetate, N,N'-bis(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt pentafluorobenzoate, N,N'-bis(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt chloride, and N,N'-bis(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt nitride. tetraphenylporphyrin cobalt chloride, tetraphenylporphyrin cobalt acetate, N,N'-bis[2-(ethoxycarbonyl)-3-oxobutylidene]-1,2-cyclohexanediaminatocobalt chloride, and N,N'-bis[2-(ethoxycarbonyl)-3-oxobutylidene]-1,2-cyclohexanediaminatocobalt pentafluorobenzoate.

[0052] When using a cobalt catalyst, it is preferable to use a cocatalyst, such as pyridine, N,N-4-dimethylaminopyridine, N-methylimidazole, tetrabutylammonium chloride, tetrabutylammonium acetate, triphenylphosphine, bis(triphenylphosphoranylidene)ammonium chloride, and bis(triphenylphosphoranylidene)ammonium acetate.

[0053] The amount of the metal catalyst (co-catalyst if necessary) used in the polymerization reaction can be the same as the known copolymerization conditions of cyclic ether and carbon dioxide, and is preferably 0.001 mol or more, more preferably 0.005 mol or more, per 1 mol of cyclic ether, from the viewpoint of promoting the progress of the polymerization reaction. In addition, the amount of the metal catalyst (co-catalyst if necessary) used in the polymerization reaction is preferably 0.2 mol or less, more preferably 0.1 mol or less, per 1 mol of cyclic ether, from the viewpoint of obtaining an effect commensurate with the amount used.

[0054] A reaction solvent may be used in the polymerization reaction as necessary. The reaction solvent is not particularly limited, and various organic solvents can be used. Examples of the organic solvent include aliphatic hydrocarbon solvents such as pentane, hexane, octane, decane, and cyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, and xylene; halogenated hydrocarbon solvents such as methylene chloride, chloroform, 1,1-dichloroethane, 1,2-dichloroethane, chlorobenzene, and bromobenzene; ether solvents such as dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and anisole; ester solvents such as ethyl acetate, n-propyl acetate, and isopropyl acetate; amide solvents such as N,N-dimethylformamide and N,N-dimethylacetamide; and carbonate solvents such as dimethyl carbonate, diethyl carbonate, and propylene carbonate.

[0055] The amount of the reaction solvent used is preferably 100 to 10,000 parts by mass per 100 parts by mass of the cyclic ether, from the viewpoint of smoothly proceeding with the reaction.

[0056] The method for polymerizing an epoxide and carbon dioxide in the presence of a metal catalyst is not particularly limited, but examples thereof include a method in which a cellulose-based resin, a cyclic ether, a catalyst, and optionally a co-catalyst, a reaction solvent, and the like are charged into an autoclave, mixed, and then carbon dioxide is injected to cause the reaction.

[0057] The amount of carbon dioxide used in the polymerization reaction is preferably 0.5 to 10 mol, more preferably 0.6 to 5 mol, and further preferably 0.7 to 3 mol, per mol of the cyclic ether.

[0058] In the polymerization reaction, the pressure of carbon dioxide is not particularly limited, but from the viewpoint of smoothly progressing the reaction, it is preferably 0.1 MPa or more, more preferably 0.2 MPa or more, and even more preferably 0.5 MPa or more, and from the viewpoint of obtaining an effect commensurate with the pressure used, it is preferably 20 MPa or less, more preferably 10 MPa or less, and even more preferably 5 MPa or less.

[0059] The polymerization reaction temperature in the polymerization reaction is not particularly limited, but from the viewpoint of shortening the reaction time, it is preferably 0° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher, and from the viewpoint of suppressing side reactions and improving the yield, it is preferably 100° C. or lower, more preferably 80° C. or lower, and even more preferably 60° C. or lower.

[0060] The reaction time varies depending on the polymerization reaction conditions and cannot be generally determined, but it is usually preferably about 1 to 40 hours.

[0061] In the method for producing a graft polymer B, the ratio of the cellulose resin to the cyclic ether is not particularly limited and can be appropriately set depending on the desired graft ratio and the degree of substitution of the cellulose resin. From the viewpoint that the obtained graft polymer is likely to exhibit high affinity for the aliphatic polycarbonate, the amount of the cyclic ether used is preferably 100 parts by mass or more and 10,000 parts by mass or less, and more preferably 250 parts by mass or more and 5,000 parts by mass or less, per 100 parts by mass of the cellulose resin.

[0062] As described above, by copolymerizing a cyclic ether with carbon dioxide in the presence of a cellulose-based resin, the cyclic ether and carbon dioxide are copolymerized to produce a polycarbonate, and the hydroxyl groups in the structural units of the cellulose-based resin also react with the cyclic ether, resulting in a graft polymer having a structure in which the hydroxyl groups in the structural units of the cellulose-based resin or the hydrogen atoms of the hydroxyl groups are substituted with polycarbonate.

[0063] In the method B for producing a graft polymer, after the polymerization reaction, the obtained graft polymer can be purified by an appropriate method as necessary.

[0064] The graft polymer can be produced by a method other than the above-mentioned production method A and production method B. For example, when the branch polymer of the graft polymer is polyethylene succinate, polyethylene adipate, polybutylene succinate, or polybutylene adipate, it is produced in the presence of the above-mentioned cellulose-based resin by copolymerizing ethylene glycol with succinic acid, copolymerizing ethylene glycol with adipic acid, copolymerizing 1,4-butanediol with succinic acid, or copolymerizing 1,4-butanediol with adipic acid, respectively. In any of the copolymerizations, for example, polymerization conditions similar to known polymerization conditions can be adopted.

[0065] When the branch polymer of the graft polymer is a vinyl polymer such as polyacrylic acid ester, polymethacrylic acid ester, or polystyrene, it is produced by radical polymerization of a vinyl monomer in the presence of the cellulose resin. In this case, the radical polymerization can be carried out under the same conditions as those of known radical polymerization.

[0066] (Aliphatic polycarbonate) In the composite of the present invention, the type of aliphatic polycarbonate is not particularly limited, and for example, known aliphatic polycarbonates can be widely used. Examples of aliphatic polycarbonates include polyethylene carbonate, polypropylene carbonate, polytrimethylene carbonate, polybutylene carbonate, polycyclohexene carbonate, polyhexamethylene carbonate, poly(1,4-cyclohexanedimethylene) carbonate, and polyisosorbide carbonate.

[0067] The mass average molecular weight, molecular weight distribution, etc. of the aliphatic polycarbonate are not particularly limited. For example, from the viewpoint of ease of handling of the composite, the mass average molecular weight of the aliphatic polycarbonate is preferably 10,000 or more, more preferably 50,000 or more, and even more preferably 100,000 or more. In addition, the mass average molecular weight of the aliphatic polycarbonate is preferably 1,000,000 or less, more preferably 750,000 or less, and even more preferably 500,000 or less. From the viewpoint of ease of molding and processing, the molecular weight distribution of the aliphatic polycarbonate is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more. In addition, the molecular weight distribution of the aliphatic polycarbonate is preferably 20 or less, more preferably 15 or less, and even more preferably 10 or less.

[0068] The method for producing the aliphatic polycarbonate is not particularly limited, and for example, the aliphatic polycarbonate can be obtained by a known method for producing an aliphatic polycarbonate. Alternatively, the aliphatic polycarbonate can be obtained from a commercial product or the like.

[0069] (Complex) The composite of the present invention contains the above-mentioned graft polymer and an aliphatic polycarbonate, and is formed, for example, by contacting the graft polymer with an aliphatic polycarbonate. The shape, structure, etc. of the composite are not particularly limited as long as it contains the above-mentioned graft polymer and an aliphatic polycarbonate.

[0070] For example, the composite of the present invention can be formed into various shapes such as a film, sheet, plate, block, pellet, strand, fiber, powder, and the like.

[0071] For example, when the composite is in the form of a film, sheet, plate, etc., the composite may have a single-layer structure (for example, a single-layer film) or a laminated structure (for example, a laminated film). When the composite has a single-layer structure, the composite becomes a mixed layer in which both the graft polymer and the aliphatic polycarbonate are present in the single layer. In this mixed layer, the state of existence of both is not particularly limited, and for example, both can be mixed uniformly, or one can be dispersed in the matrix of either one. In particular, since the graft polymer is formed with a specific trunk polymer and branch polymer, it has high compatibility with aliphatic polycarbonate, so that both are easily mixed uniformly, or one is easily dispersed in the other (for example, the graft polymer is uniformly dispersed in the aliphatic polycarbonate matrix). Therefore, the composite containing the mixed layer is a material in which the functions of both the graft polymer and the aliphatic polycarbonate are easily exerted effectively and also has high transparency.

[0072] When the composite has a laminated structure, the composite may be formed into a two-layer structure, or may be formed into a multi-layer structure of three or more layers. For example, when the composite is formed into a two-layer structure, one layer can be a layer of a graft polymer, and the other layer can be a layer of an aliphatic polycarbonate. Alternatively, when the composite is formed into a two-layer structure, one or both layers may have the same configuration as the above-mentioned mixed layer. When the composite is formed into a multi-layer structure of three or more layers, one or more layers of the multi-layer structure can be a layer of a graft polymer, and the other one or two or more layers can be a layer of an aliphatic polycarbonate. Moreover, even in such a multi-layer structure, at least one layer may have the same configuration as the above-mentioned mixed layer.

[0073] In the case where the composite has a laminated structure, when a layer of a graft polymer and a layer of an aliphatic polycarbonate are in contact with each other, the layer of the graft polymer and the layer of the aliphatic polycarbonate have high compatibility with each other, and therefore can be firmly bonded to each other, so that the films or sheets are less likely to slip or peel off from each other.

[0074] In addition, whether the composite has a single-layer structure or a laminate structure, the high compatibility between the graft polymer and the aliphatic polycarbonate makes it possible to produce a material with high transparency. Moreover, the high compatibility between the graft polymer layer and the aliphatic polycarbonate improves the mechanical strength compared to a case where the compatibility between the graft polymer layer and the aliphatic polycarbonate is not taken into consideration.

[0075] When the composite has a single layer structure, the thickness is not particularly limited and can be appropriately set according to the intended use. For example, when the composite is a single layer film, the thickness can be 10 to 250 μm. When the composite has a laminated structure, the thickness and the thickness of each layer are not particularly limited and can be appropriately set according to the intended use. For example, when the composite is a laminated film, the thickness can be 20 to 250 μm. In this case, the thickness of each layer is not particularly limited, and for example, the thickness of the graft polymer layer can be 10 to 100 μm, the thickness of the aliphatic polycarbonate layer can be 10 to 100 μm, and the thickness of the mixed layer can be 10 to 100 μm.

[0076] When the composite of the present invention is in the form of, for example, pellets or powder, the composite may be, for example, particulate, flaky, thin, or irregular. When the composite is particulate, the particles may be, for example, spherical, elliptical, or irregular. When the composite is particulate, the graft polymer and the aliphatic polycarbonate may be uniformly mixed, or a so-called core-shell structure may be formed. In the core-shell structure, for example, the core may be an aliphatic polycarbonate and the shell may be a graft polymer, or vice versa.

[0077] When the complex of the present invention is in the form of particles, the average particle size is not particularly limited, and for example, the median particle size measured by a laser diffraction / scattering method can be 0.1 to 500 μm.

[0078] When the composite of the present invention is fibrous, the fiber can be a monofilament or a multifilament. When the composite is a multifilament, the composite can be a monofilament in which the graft polymer and the aliphatic polycarbonate are uniformly mixed and spun, or the composite can be a monofilament in which the graft polymer and the aliphatic polycarbonate are spun and mixed and spun, or a so-called core-sheath structure can be formed. In the core-sheath structure, for example, the core can be an aliphatic polycarbonate and the sheath can be a graft polymer, or vice versa. When the composite of the present invention is fibrous, the diameter of the fiber is not particularly limited, and can be, for example, 1 to 1000 μm in diameter.

[0079] In the composite of the present invention, the content ratio of the graft polymer and the aliphatic polycarbonate is not particularly limited and can be appropriately adjusted to the extent that the effects of the present invention are not impaired. For example, the content ratio of the graft polymer can be 1 to 99 mass%, preferably 5 to 95 mass%, more preferably 10 to 90 mass%, further preferably 20 to 80 mass%, and particularly preferably 30 to 70 mass%, based on the total mass of the graft polymer and the aliphatic polycarbonate.

[0080] The composite of the present invention may contain additives as long as the effects of the present invention are not impaired. The type of additive is not particularly limited, and examples thereof include light stabilizers, antioxidants, preservatives, surfactants, fillers, flame retardants, pigments, colorants, antifungal agents, lubricants, etc. When the composite contains additives, the content thereof may be 20% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 1% by mass or less, based on the total mass of the composite.

[0081] In addition, when the composite has the above-mentioned laminated structure, the graft polymer layer may contain the additive to an extent that the effects of the present invention are not impaired, and the aliphatic polycarbonate layer may also contain the additive to an extent that the effects of the present invention are not impaired.

[0082] (Method of Manufacturing the Composite) The method for producing the composite is not particularly limited. For example, the composite can be formed by a known method using a graft polymer and an aliphatic polycarbonate.

[0083] For example, when the composite is a single-layer film, sheet, etc., a film, sheet, etc. can be produced by molding the graft polymer and aliphatic polycarbonate as raw materials using a known method. The molding method and molding conditions are not particularly limited, and for example, known molding methods and molding conditions can be widely adopted. Specifically, the composite of the graft polymer and the aliphatic polycarbonate can be molded into a film or sheet by an inflation method, a T-die method, a calendar method, a solution casting method, etc. In addition, the obtained film or sheet may be stretched uniaxially or biaxially by a roll stretching method, a tenter stretching method, a tubular stretching method, etc.

[0084] In addition, even when the composite is a film, sheet, etc. having a laminated structure, the manufacturing method is not particularly limited, and for example, a method for manufacturing a known laminate can be widely adopted. Specifically, a composite having a laminated structure can be manufactured by laminating a layer containing a graft polymer and a layer containing an aliphatic polycarbonate on each other. The lamination method and lamination conditions are not particularly limited, and for example, a known molding method and molding conditions can be widely adopted. Specifically, molding can be performed by a co-extrusion inflation method, a co-extrusion T-die method, etc. Alternatively, molding can be performed by an extrusion lamination method, a thermal lamination method, a dry lamination method, etc., or a single-layer film obtained by the above molding method can be laminated and pressed by heating to form a laminate. In addition, the obtained film or sheet having a laminated structure can be stretched uniaxially or biaxially by a roll stretching method, a tenter stretching method, a tubular stretching method, etc. and used.

[0085] In addition, when the composite is a particle, the method of manufacturing the composite is not particularly limited, and for example, a known method of manufacturing a particle can be widely adopted. For example, the method of mechanically pulverizing the composite of the graft polymer and the aliphatic polycarbonate, the method of dissolving or dispersing the composite of the graft polymer and the aliphatic polycarbonate in an organic solvent and spray drying, the method of dissolving the composite of the graft polymer and the aliphatic polycarbonate in an organic solvent, adding a solvent that is not miscible with the organic solvent, emulsifying by high-speed stirring, and then removing the solvent such as the organic solvent, the method of emulsifying the composite of the graft polymer and the aliphatic polycarbonate in a solvent that does not dissolve the composite of the graft polymer and the aliphatic polycarbonate by high-speed stirring while heating to a melting temperature or higher, and then quenching to form particles, or the method of quenching the organic solvent in which the graft polymer and the aliphatic polycarbonate are dissolved or dispersed to form particles can be mentioned. Examples of the organic solvent include solvents capable of dissolving or dispersing the graft polymer, such as aromatic compounds, such as xylene, toluene, and benzene; aliphatic hydrocarbons, such as hexane and heptane; alicyclic hydrocarbons, such as cyclohexane; chlorinated hydrocarbons, such as chloroform and 1,2-dichloroethane; esters, such as ethyl acetate and propyl acetate; ketones, such as acetone, methyl ethyl ketone, and cyclohexanone; and alcohols, such as methanol, ethanol, isopropyl alcohol, and tert-butanol.

[0086] For example, when particles are formed by quenching an organic solvent in which the graft polymer and the aliphatic polycarbonate are dissolved or dispersed, the organic solvent containing the graft polymer and the aliphatic polycarbonate can be heated before quenching. The heating temperature can be 60 to 200°C. The quenching can be performed after the heating. In the quenching, the organic solvent containing the graft polymer and the aliphatic polycarbonate can be cooled to 20°C or less.

[0087] The above rapid cooling makes it possible to obtain a suspension containing the graft polymer and the aliphatic polycarbonate, and the target particulate composite can then be obtained by a process such as filtration. The composite thus obtained is formed, for example, into a core-shell structure. Whether the core and shell are the graft polymer or the aliphatic polycarbonate depends on the type of organic solvent used, etc. For example, when the organic solvent is a good solvent for the graft polymer and a poor solvent for the aliphatic polycarbonate, a core-shell structure is formed in which the aliphatic polycarbonate is the core and the graft polymer is the shell. When the organic solvent is a poor solvent for the graft polymer and a good solvent for the aliphatic polycarbonate, the opposite structure is obtained.

[0088] Furthermore, when the composite is a fiber, the manufacturing method thereof is not particularly limited, and for example, a wide variety of known fiber manufacturing methods can be adopted. For example, a method of melt spinning, dry spinning, or wet spinning of a composite of a graft polymer and an aliphatic polycarbonate can be used. The fiber formed by the spinning may be further subjected to a process such as drawing or spinning. Furthermore, when a fiber having a core-sheath structure is to be formed, a co-extrusion melt spinning method, or a method of immersing a monofilament of a graft polymer or an aliphatic polycarbonate in a solution in which the other polymer is dissolved in an organic solvent and then drying the solvent can be used.

[0089] (Use of the complex) As described above, the composite of the present invention can be formed into a film, sheet, etc., and can be formed into a laminated structure, and therefore can be used, for example, for various multilayer film applications. Since this multilayer film contains the composite of the present invention, it has high transparency and excellent mechanical strength, and since the layer of the graft polymer and the layer of the aliphatic polycarbonate in the multilayer film have high compatibility, displacement or peeling between the films is unlikely to occur. Therefore, by using the composite in a multilayer film, various functions can be expressed.

[0090] The composite of the present invention is also suitable for use in optical films, agricultural films, or packaging films. In particular, the composite of the present invention has high compatibility between the graft polymer and the aliphatic polycarbonate, and therefore has high transparency in both a single-layer structure and a laminate structure, and also has excellent mechanical strength, making it suitable for use in optical films or agricultural films.

[0091] When the composite of the present invention is applied to a multilayer film, an optical film, or an agricultural film, the other configurations are not particularly limited as long as the composite is included. For example, the composite can have the same configuration as a known multilayer film, an optical film, or an agricultural film, except that the composite is included.

[0092] The composite of the present invention can form not only films and the like, but also particles or fibers as described above, and therefore can be suitably used as various additives such as fillers, light diffusing agents, weight reducing agents, lubricants, and antiblocking agents. EXAMPLES

[0093] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0094] The mass average molecular weight (Mw) of the graft polymer obtained in each of the Examples and Comparative Examples was measured by the following method.

[0095] [Mass average molecular weight (Mw) of graft polymer] A tetrahydrofuran solution with a graft polymer concentration of 0.2% by mass was prepared, and the mass average molecular weight (Mw) of the graft polymer was measured using a high performance liquid chromatograph (HPLC). The measured value was compared with that of polystyrene with a known mass average molecular weight measured under the same conditions, and the mass average molecular weight Mw of the graft polymer was calculated. The measurement conditions were as follows: Column: GPC column (Shodex OHPac SB-804, SB-805, product name of Showa Denko K.K.) Column temperature: 40℃ Eluent: Tetrahydrofuran ·Flow rate: 1.0mL / min

[0096] (Production Example 1) In a separable flask equipped with a cooling tube, a thermometer and a stirrer, 30 parts by mass of ethyl cellulose (Mw = 180,000, ethoxylation rate 48.0%), 100 parts by mass of propylene carbonate, 0.5 parts by mass of tin octanoate, 0.5 parts by mass of 1,5,7-triazabicyclo[4.4.0]dec-5-ene and 250 parts by mass of diglyme were charged. Then, the temperature was raised to 150 ° C under a nitrogen atmosphere, and the mixture was reacted by stirring at the same temperature for 24 hours. A solid was precipitated by dropping the reaction solution into 1000 parts by mass of a 50% by mass aqueous methanol solution. The precipitated solid was collected by filtration, washed with 500 parts by mass of a 50% by mass aqueous methanol solution, and then dried at 70 ° C for 8 hours to obtain a graft polymer. The obtained graft polymer had a branch polymer of polypropylene carbonate (SP value 19.5), a graft rate of 53% by mass, and an Mw of 220,000.

[0097] (Production Example 2) Except for using ethylene carbonate instead of propylene carbonate, a graft polymer was obtained in the same manner as in Production Example 1. The obtained graft polymer had a branch polymer of polyethylene carbonate (SP value 22.6), a graft rate of 90 mass%, and Mw of 300,000.

[0098] (Production Example 3) In a separable flask equipped with a cooling tube, a thermometer, and a stirrer, 30 parts by mass of hydroxypropyl cellulose (Mw = 180,000), 40 parts by mass of ε-caprolactone, 1 part by mass of tin octanoate, and 250 parts by mass of diglyme were charged. Then, the temperature was raised to 150 ° C under a nitrogen atmosphere, and the mixture was reacted by stirring at the same temperature for 6 hours. A solid was precipitated by dropping the reaction solution into 1000 parts by mass of a 50% by mass aqueous methanol solution. The precipitated solid was collected by filtration, washed with 500 parts by mass of a 50% by mass aqueous methanol solution, and then dried at 70 ° C for 8 hours to obtain a graft polymer. The obtained graft polymer had a branch polymer of polycaprolactone (SP value 20.9), a graft ratio of 130% by mass, and an Mw of 320,000.

[0099] (Production Example 4) A graft polymer was obtained in the same manner as in Production Example 3, except that 40 parts by mass of ε-caprolactone was replaced with 100 parts by mass of L-lactide. The branch polymer of the obtained graft polymer was polylactic acid (SP value 21.6), the graft ratio was 230% by mass, and Mw was 530,000.

[0100] Example 1 The graft polymer obtained in Production Example 1 was pressed at 150°C and a pressure of 5 MPa·G for 5 minutes using a press molding machine (40 ton heated press manufactured by Gonno Hydraulic Machinery Co., Ltd.) to form a 100 μm thick film, and a 100 μm thick film obtained by molding aliphatic polycarbonate (polypropylene carbonate manufactured by Sumitomo Seika Chemicals) (Mw=340,000) in the same manner was laminated, and the two were pressed together at 100°C and 0.3 MPa for 1 minute using the same press molding machine to obtain a two-layer film. This two-layer film was used as a composite containing the graft polymer and aliphatic polycarbonate.

[0101] Example 2 A two-layer film was obtained in the same manner as in Example 1, except that the graft polymer obtained in Production Example 1 was changed to the graft polymer obtained in Production Example 2. This two-layer film was used as a composite containing the graft polymer and an aliphatic polycarbonate.

[0102] Example 3 A two-layer film was obtained in the same manner as in Example 1, except that the graft polymer obtained in Production Example 1 was changed to the graft polymer obtained in Production Example 3. This two-layer film was used as a composite containing the graft polymer and an aliphatic polycarbonate.

[0103] Example 4 A two-layer film was obtained in the same manner as in Example 1, except that the graft polymer obtained in Production Example 1 was changed to the graft polymer obtained in Production Example 4.

[0104] Comparative Example 1 A bilayer film was obtained in the same manner as in Example 1, except that the graft polymer obtained in Production Example 1 was changed to ethyl cellulose (Mw=180,000, ethoxylation rate 48.0%). This bilayer film was used as a comparative film for the composite.

[0105] Example 5 A 50 μm thick film was prepared by molding the graft polymer obtained in Production Example 1 in the same manner as in Example 1, and two 50 μm thick films were prepared by molding aliphatic polycarbonate (polypropylene carbonate manufactured by Sumitomo Seika Chemicals) (Mw=340,000) in the same manner as in Example 1. Both sides of the 50 μm thick film formed using the graft polymer were sandwiched between aliphatic polycarbonate films, and the films were pressed at 100° C. and 0.3 MPa for 1 minute to obtain a three-layer film. This three-layer film was used as a composite containing the graft polymer and the aliphatic polycarbonate.

[0106] Example 6 A mixed solution was prepared by dissolving 100 parts by mass of the graft polymer obtained in Production Example 3 and 100 parts by mass of aliphatic polycarbonate (polypropylene carbonate manufactured by Sumitomo Seika Chemicals) (Mw=340,000) in 500 parts by mass of acetone. The mixed solution obtained was spread on a glass petri dish and dried to obtain a mixed film (single layer) of the graft body and aliphatic polycarbonate having a thickness of 250 μm. This mixed film was used as a composite containing the graft polymer and the aliphatic polycarbonate.

[0107] Comparative Example 2 A mixed film was obtained in the same manner as in Example 6, except that the graft polymer obtained in Production Example 3 was changed to hydroxypropyl cellulose (Mw = 180,000). This mixed film was used as a comparative film for the composite.

[0108] Example 7 A solution was prepared by dissolving 10 parts by mass of the graft polymer obtained in Production Example 4 in 240 parts by mass of xylene, and 5 parts by mass of aliphatic polycarbonate (polyethylene carbonate manufactured by Sumitomo Seika Chemicals) (Mw = 200,000) was added to this solution, and the mixture was stirred at 140 ° C. and 800 rpm to melt and disperse the aliphatic polycarbonate. Then, the mixture was rapidly cooled to 10 ° C. to obtain a suspension. The suspension obtained was filtered through a 0.45 μm filter, and the obtained filtrate was washed with 200 parts by mass of n-hexane cooled to 10 ° C. and dried to obtain a powder. The obtained powder had a median particle diameter of 440 μm, and infrared spectroscopy analysis of the powder revealed that ester groups were observed on the surface and carbonate groups were not observed, and that carbonate groups were observed inside and ester groups were not observed, so that the particles were core-shell particles having an aliphatic polycarbonate as a core layer and a graft polymer as a shell layer. The core-shell particles were made into a composite containing a graft polymer and an aliphatic polycarbonate.

[0109] (Evaluation example 1) The bilayer films obtained in Examples 1 to 4 and Comparative Example 1 were subjected to a delamination test in accordance with JIS Z0238:1998 using a universal testing machine (Shimadzu Corporation's AGS-J) at a test speed of 50 mm / min, and the performance of each film was evaluated based on the following criteria. A: The layer was bonded until it broke. B: None of the layers were broken, but the adhesive surface was significantly deformed when peeled off. C: None of the layers were deformed or broken, and they peeled off with almost no resistance.

[0110] [Table 1]

[0111] Table 1 shows the evaluation results of Evaluation Example 1 (interlayer peeling test). From these results, it was found that the two-layer film (multilayer film) obtained in the example was less susceptible to interlayer slippage and peeling. Since the compatibility of the graft polymer in the two-layer film obtained in the example with the aliphatic polycarbonate is greater than that of the cellulose-based resin, it is considered that the adhesion between the graft polymer layer and the aliphatic polycarbonate layer is improved.

[0112] (Evaluation example 2) The total light transmittance of each of the films obtained in Examples 1 to 6 and Comparative Examples 1 and 2 was measured using a haze meter (NDH300A, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0113] [Table 2]

[0114] Table 2 shows the evaluation results of Evaluation Example 2 (total light transmittance). From these results, it was found that the films obtained in each Example had excellent transparency. In particular, the films obtained in each Example had improved transparency compared to the film obtained by simply blending hydroxypropyl cellulose and aliphatic polycarbonate as in Comparative Example 2. From this, it is found that a composite containing a graft polymer having a specific structure and an aliphatic polycarbonate can be suitably used as an optical film.

[0115] (Evaluation example 3) The mechanical strength of the films obtained in Example 6 and Comparative Example 2 was measured by a universal testing machine (AGS-J, manufactured by Shimadzu Corporation) at 25° C. and a tensile speed of 50 mm / min to determine the breaking strength and breaking strain.

[0116] [Table 3]

[0117] Table 3 shows the evaluation results of Evaluation Example 3 (mechanical strength). It was found that the mixed film obtained in Example 6 had better mechanical strength than the mixed film obtained in Comparative Example 2. In the mixed film of Comparative Example 2, the aliphatic polycarbonate and the cellulose-based resin were not mixed uniformly, so the film was easily broken. In contrast, in the mixed film of Example 6, the aliphatic polycarbonate and the graft polymer are highly compatible with each other, so the two are mixed uniformly, and it is believed that the mixed film obtained in Example 6 has excellent mechanical strength.

Claims

1. A composite comprising a graft polymer and an aliphatic polycarbonate, The graft polymer has a trunk polymer and a branch polymer bonded to the trunk polymer, the trunk polymer containing a cellulose-based resin, The cellulose-based resin is at least one selected from the group consisting of alkyl cellulose and hydroxyalkyl cellulose, The branched polymer has a solubility parameter of 17 to 24 MPa as determined by the Fedors method. 0.5 The complex is a polymer B,

2. The composite according to claim 1 , wherein a ratio of the polymer B to the cellulose-based resin is 10% by mass or more and 400% by mass or less.

3. 3. The composite according to claim 1, wherein the polymer B is at least one selected from the group consisting of polycaprolactone, polylactic acid, poly(3-hydroxybutyric acid), polybutylene succinate, polyethylene carbonate, polypropylene carbonate, polytrimethylene carbonate, polyethylene glycol, polypropylene glycol, and polymethyl methacrylate.

4. The composite according to any one of claims 1 to 3, wherein the mass average molecular weight of the graft polymer is 50,000 or more and 1,000,000 or less.

5. A film comprising the composite of any one of claims 1 to 4.

6. A sheet comprising the composite material according to any one of claims 1 to 4.

7. A particle comprising the complex according to any one of claims 1 to 4.

8. A fiber comprising the composite material according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • JP1971043996B

  • Production of new graft polymer

    JP1984086621A

  • Polycarbonate composition and method for producing the same

    JP2006036954A

  • Modified cellulose acylate resin composition

    JP2007231050A

  • Heat resistance improver, thermoplastic resin composition and molded product

    JP2009155626A