Epoxy resin composition, prepreg, and fiber-reinforced plastic using the same

A bifunctional epoxy resin composition with controlled ratios of phenol compound and catalyst improves adhesion to reinforcing fibers, addressing low bending strength issues in thermoplastic epoxy resins, resulting in enhanced mechanical properties for fiber-reinforced plastics.

JP7587683B2Active Publication Date: 2024-11-20NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023510801
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-30
Filing Date
2022-03-10
Publication Date
2024-11-20
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

Existing thermoplastic epoxy resins used in fiber-reinforced plastics (FRP) face challenges in achieving high adhesion to reinforcing fibers, leading to low bending strength in the 90-degree direction, and require complex surface modification methods that compromise productivity.

Method used

A specific epoxy resin composition containing a bifunctional phenol compound, bifunctional epoxy resin, and a polymerization catalyst, with controlled raw material ratios, achieves improved adhesion by forming a thermoplastic epoxy resin with a high epoxy group concentration, resulting in a polymer with a bending strength of 70 MPa or more.

Benefits of technology

The solution enhances the adhesion between reinforcing fibers and resin, thereby improving the bending strength of the composite material, offering a simple and productive method for enhancing mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587683000001
    Figure 0007587683000001
  • Figure 0007587683000002
    Figure 0007587683000002
  • Figure 0007587683000003
    Figure 0007587683000003
Patent Text Reader

Abstract

Provided is an epoxy resin composition that improves adhesion of a thermoplastic epoxy resin to reinforcing fibers. This epoxy resin composition contains a difunctional phenol compound, a difunctional epoxy resin and a polymerization catalyst, and is characterized by containing 50 wt% or more of an epoxy resin (a) represented by formula (1) as the difunctional epoxy resin, and in that the difunctional epoxy resin / difunctional phenol compound molar ratio is 1.01-1.05, and a polymer obtained from this epoxy resin composition has an epoxy equivalent weight of 5000-20,000 g / eq., a bending strength of 70 MPa or more, and a tetrahydrofuran-insolubles content of 10 wt% or less. (A is represented by formula (2), X is a single bond, an alkylene group, an arylene group, O, CO, or the like, and Y1 is an alkyl group or an aryl group.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an epoxy resin composition, a reinforcing fiber-containing epoxy resin composition, a prepreg, and a fiber-reinforced plastic using the same. [Background technology]

[0002] Fiber-reinforced plastics (FRP) have excellent physical properties such as light weight and high strength, and are used in many fields. Among them, those using carbon fiber as the reinforcing fiber (CFRP) are known to have particularly excellent mechanical strength.

[0003] Epoxy resin is mainly used as the base resin for FRP because it has an excellent balance between price and physical properties. Epoxy resin also forms a good adhesive surface with reinforcing fibers due to its secondary hydroxyl group, so it is known to exhibit good mechanical properties as a base resin for CFRP.

[0004] On the other hand, those that use thermoplastic resin as the base resin are called FRTP, and their development is progressing due to their excellent mass production, moldability, and recyclability. Nylon, polypropylene, polycarbonate, etc. are mainly used as the base resin for FRTP.

[0005] One of the issues with FRTP is that the 90-degree bending strength of unidirectional materials (UD materials) is low due to the low adhesion between the reinforcing fibers and the resin. In order to improve the adhesion between the reinforcing fibers and the resin, various methods have been considered for modifying the reinforcing fiber surface, such as cleaning the sizing agent attached to the fibers and oxidizing the fiber surface with ozone or acid, but all of these methods require additional steps and are not simple (Non-Patent Document 1).

[0006] In-situ polymerization type thermoplastic epoxy resin has been proposed as a thermoplastic resin with improved adhesion to reinforcing fibers. In-situ polymerization type thermoplastic epoxy resin has good impregnation properties because it is impregnated into fibers in a low viscosity state before polymerization, and it is possible to increase the proportion of reinforcing fibers. In addition, the presence of secondary hydroxyl groups in the epoxy resin is expected to provide good adhesion to reinforcing fibers.

[0007] Previous reports on the adhesion between thermoplastic epoxy resins and carbon fibers have shown that increasing the molecular weight of the thermoplastic epoxy improves the interfacial shear strength between the carbon fiber and the matrix (Non-Patent Document 2). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2006-321897 A [Non-patent literature]

[0009] [Non-Patent Document 1] Improvement of Bending Strength of Carbon Fiber / Thermoplastic Epoxy Composites (Open Journal of Composite Materials, 2017, 7, 207-217) [Non-Patent Document 2] Journal of the Adhesion Society of Japan VOL.53 No.11(2017)375-380 Summary of the Invention

[0010] However, according to the study by the present inventors, in order to sufficiently increase the molecular weight of the thermoplastic epoxy resin in the reinforcing fiber, it is necessary to allow a sufficient time for polymerization. In addition, if the skeleton of the thermoplastic epoxy resin is made bulky in order to increase the heat resistance, the steric hindrance of the reaction becomes large, so that the curing time for polymerization becomes longer and the productivity is poor. For this reason, a method for improving the adhesion of the thermoplastic epoxy resin to the reinforcing fiber and improving the bending strength in the 90 degree direction by a simple method with excellent productivity has been required.

[0011] The present inventors conducted extensive research aimed at developing adhesive properties for thermoplastic epoxy resins to reinforcing fibers, and discovered that the use of a specific epoxy resin composition can improve adhesion to reinforcing fibers and increase bending strength in the 90 degree direction.

[0012] That is, the present invention provides an epoxy resin composition comprising, as essential components, a bifunctional phenol compound, a bifunctional epoxy resin, and a polymerization catalyst, The difunctional epoxy resin contains 50% by weight or more of a difunctional epoxy resin (a) represented by the following formula (1): The amount of the difunctional epoxy resin is 1.01 to 1.05 moles per mole of the difunctional phenol compound, The epoxy resin composition is characterized in that the polymer obtained from the epoxy resin composition is a thermoplastic epoxy resin, has an epoxy equivalent of 5,000 g / eq. or more and 20,000 g / eq. or less, has a bending strength of 70 MPa or more, and contains 10% by weight or less of components that become insoluble when dissolved in tetrahydrofuran.

[0013] [ka] In the formula (1), A is represented by the formula (2), n is the number of repetitions, the average value of which is 0 to 5, X is a single bond, a hydrocarbon group having 1 to 13 carbon atoms, -O-, -CO-, -COO-, -S-, or -SO2-, and Y 1 is independently an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 10 carbon atoms; Y2 and Y 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an aryl group having 6 to 10 carbon atoms.

[0014] The present invention also relates to a reinforcing fiber-containing epoxy resin composition or prepreg obtained by mixing the above-mentioned epoxy resin composition with reinforcing fibers.

[0015] The reinforcing fibers are preferably PAN-based carbon fibers, and are preferably contained in the resin composition or prepreg in a proportion of 50% by weight or more and 80% by weight or less.

[0016] The present invention also relates to a fiber-reinforced plastic using the above-mentioned reinforcing fiber-containing epoxy resin composition or the above-mentioned prepreg.

[0017] According to the present invention, a thermoplastic epoxy resin composition having excellent adhesion to reinforcing fibers can be provided.

[0018] The reason why the adhesion between the reinforcing fibers and the resin was demonstrated is thought to be that by controlling the raw material composition ratio, an epoxy resin with a low epoxy equivalent and a high epoxy group concentration can be obtained, which forms good adhesion with the functional groups on the surface of the reinforcing fibers and the sizing agent. In addition, when the polymerization is not sufficiently advanced, the bending strength of the polymer is 70 MPa or more, so that the composite material can exhibit sufficient strength. Conventionally, the adhesiveness of epoxy resins is believed to be due to secondary hydroxyl groups, and there have been no reports that mention the effect of the epoxy group concentration of the polymer. According to the present invention, the adhesiveness to reinforcing fibers can be exhibited by a simple method of adjusting the feed ratio of the raw materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will be described in detail below based on preferred embodiments thereof. The epoxy resin composition of the present invention is a composition that contains a bifunctional phenol compound, a bifunctional epoxy resin, and a polymerization catalyst as essential components and can be polymerized by heating. This composition may also contain additives such as an organic solvent, a filler, and a flame retardant.

[0020] The bifunctional epoxy resin contains the epoxy resin (a) represented by the formula (1) as an essential component in an amount of 50% by weight or more, preferably 66% by weight or more, more preferably 75% by weight or more, and even more preferably 80% by weight or more. The epoxy resin (a) constitutes a part of the bifunctional epoxy resin. The epoxy equivalent of the difunctional epoxy resin is preferably 150 to 350 g / eq.

[0021] In formula (1), A is a divalent group represented by the above formula (2), and n is the number of repetitions, the average value of which is 0 to 5, and preferably 0 to 1.

[0022] In formula (2), X is any one of a single bond, a hydrocarbon group having 1 to 13 carbon atoms, -O-, -CO-, -COO-, -S-, and -SO2-. The hydrocarbon group having 1 to 13 carbon atoms is preferably an alkylene group having 1 to 9 carbon atoms or an arylene group having 6 to 13 carbon atoms, and examples thereof include -CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -CHPh-, -C(CH3)Ph-, 1,1-cyclopropylene group, 1,1-cyclobutylene group, 1,1-cyclopentylene group, 1,1-cyclohexylene group, 4-methyl-1,1-cyclohexylene group, 3,3,5-trimethyl-1,1-cyclohexylene group, 1,1-cyclooctylene group, 1,1-cyclononylene group, 1,2-ethylene group, a 1,2-cyclopropylene group, a 1,2-cyclobutylene group, a 1,2-cyclopentylene group, a 1,2-cyclohexylene group, a 1,2-phenylene group, a 1,3-propylene group, a 1,3-cyclobutylene group, a 1,3-cyclopentylene group, a 1,3-cyclohexylene group, a 1,3-phenylene group, a 1,4-butylene group, a 1,4-cyclohexylene group, a 1,4-phenylene group, a 1,1-fluorene group, a 1,2-xylylene group, a 1,4-xylylene group, a tetrahydrodicyclopentadienylene group, and a tetrahydrotricyclopentadienylene group. Among these, a single bond, -O-, -CO-, -COO-, -S-, -SO2-, -CH2-, -CH(CH3)-, -C(CH3)2-, -CHPh-, -C(CH3)Ph-, a 1,1-cyclohexylene group, a 4-methyl-1,1-cyclohexylene group, a 3,3,5-trimethyl-1,1-cyclohexylene group, a 1,4-cyclohexylene group, a 1,4-phenylene group, and a 1,1-fluorene group are preferred, and a single bond, -O-, -CO-, -COO-, -S-, -SO2-, -CH2-, -CH(CH3)-, -C(CH3)2-, -C(CH3)Ph-, a 1,1-cyclohexylene group, a 3,3,5-trimethyl-1,1-cyclohexylene group, and a 1,1-fluorene group are more preferred. In addition, Ph represents a phenyl group. The alkylene group is meant to include an alkylidene group.

[0023] Y 1 are independently either an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 10 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, a sec-butyl group, an iso-butyl group, and a t-butyl group. Examples of the aryl group having 6 to 10 carbon atoms include a phenyl group, a tolyl group, an ethylphenyl group, a xylyl group, an n-propylphenyl group, an isopropylphenyl group, a mesityl group, and a naphthyl group. Of these, a methyl group, an ethyl group, an n-propyl group, an n-butyl group, a t-butyl group, a phenyl group, a tolyl group, a xylyl group, or a naphthyl group is preferred, and a methyl group, an ethyl group, an n-propyl group, an n-butyl group, a t-butyl group, a phenyl group, or a tolyl group is more preferred.

[0024] Y 2 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an aryl group having 6 to 10 carbon atoms, and a group other than a hydrogen atom is preferable. Examples of the alkyl group and aryl group include the above-mentioned Y 1 The preferred Y 2 is Y 1 is the same as: Y 3 are independently any one of a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, and an aryl group having 6 to 10 carbon atoms. Examples of the alkyl group and the aryl group include Y 1 The preferred Y 3 is a hydrogen atom or Y 1 is the same as the groups exemplified above.

[0025] Examples of the bifunctional epoxy resin (a) include tetramethylbisphenol F type epoxy resins (e.g., YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.)), tetramethylbiphenol type epoxy resins (e.g., YX-4000 (manufactured by Mitsubishi Chemical Corporation)), and biscresolfluorene type epoxy resins (e.g., OGSOL CG-500 (manufactured by Osaka Gas Chemicals Co., Ltd.)).

[0026] In addition, epoxy resins other than the epoxy resin (a) can be used in combination as long as they are bifunctional epoxy resins, and the purity is preferably 95% or more. If the purity as a bifunctional epoxy resin is high, positional isomers and oligomers may be included. Examples of epoxy resins that can be used in combination with the epoxy resin (a) include, but are not limited to, bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol acetophenone type epoxy resins, diphenyl sulfide type epoxy resins, diphenyl ether type epoxy resins, and bisphenol fluorene type epoxy resins, biphenol type epoxy resins, diphenyl dicyclopentadiene type epoxy resins, alkylene glycol type epoxy resins, dihydroxy naphthalene type epoxy resins, and dihydroxy benzene type epoxy resins. The bifunctional epoxy resin that can be used in combination with the epoxy resin (a) is preferably less than 50% by weight, and more preferably less than 30% by weight, of the total epoxy resin. If it exceeds 50% by weight, it may gel and produce components that are difficult to dissolve in solvents, which may deteriorate the reshapeability.

[0027] If monofunctional impurities are contained in a bifunctional epoxy resin, the molecular weight after polymerization will not increase, and the mechanical properties of the resulting thermoplastic resin product may deteriorate. Therefore, it is preferable that the monofunctional impurities are 2% by weight or less relative to the bifunctional epoxy resin. When trifunctional or higher impurities are contained, the impurities tend to form crosslinked structures starting from the impurities, which may lead to increased dispersion of the polymer and gelation, resulting in loss of thermoplasticity. Therefore, it is preferable that the amount of trifunctional or higher impurities is 1% by weight or less relative to the bifunctional epoxy resin. In addition, impurity components that do not have active groups that react with either epoxy resins or phenolic hydroxyl groups and that do not inhibit the polymerization reaction by themselves may cause the molecular weight after polymerization to decrease if their amount is large. Therefore, it is preferable that the amount of such impurity components is 2% by weight or less relative to the bifunctional epoxy resin.

[0028] The bifunctional phenol compound used in the epoxy resin composition of the present invention is a compound having two phenolic hydroxyl groups in one molecule, and its purity is preferably 95% by weight or more. If the purity of the bifunctional phenol compound is high, positional isomers may be included. If monofunctional impurities are contained, the molecular weight after polymerization will not increase, and the mechanical properties of the produced thermoplastic resin may deteriorate. Therefore, it is preferable that the monofunctional impurities are 2% by weight or less relative to the bifunctional phenol compound. When trifunctional or higher impurities are contained, the impurities tend to form crosslinked structures as starting points, which may lead to increased dispersion of the polymer and gelation, resulting in loss of thermoplasticity. Therefore, it is preferable that the trifunctional or higher impurities are 1% by weight or less relative to the bifunctional phenol compound. In addition, impurity components that do not have active groups that react with either epoxy resins or phenolic hydroxyl groups and that do not inhibit the polymerization reaction by themselves may cause the molecular weight after polymerization to decrease if their amount is large. Therefore, it is preferable that the amount of such impurity components is 2% by weight or less relative to the bifunctional phenol compound.

[0029] The bifunctional phenol compound is preferably a bisphenol compound or a biphenol compound. Examples of the bisphenol compound include bisphenol A, bisphenol F (all manufactured by Nippon Steel Chemical & Material Co., Ltd.), bisphenol fluorene (manufactured by Osaka Gas Chemical Co., Ltd.), Bis-E, Bis-Z, BisOC-FL, BisP-AP, BisP-CDE, BisP-HTG, BisP-MIBK, BisP-3MZ, S-BOC (all manufactured by Honshu Chemical Industry Co., Ltd.), and bisphenol S. Examples of the biphenol compound include biphenol, dimethylbiphenol, and tetramethylbiphenol. Examples of other bifunctional phenol compounds include benzenediols such as hydroquinone, methylhydroquinone, dibutylhydroquinone, resorcin, methylresorcin, catechol, and methylcatechol, and naphthalenediols such as naphthalenediol. Among these, bisphenol compounds or biphenol compounds are preferred.

[0030] The ratio of the bifunctional epoxy resin contained in the epoxy resin composition of the present invention is 1.01 to 1.05 mol, preferably 1.02 to 1.03 mol, per mol of the bifunctional phenolic compound. In the thermoplastic epoxy resin, the epoxy resin and the phenolic compound react successively to form a linear structure, thereby exhibiting thermoplasticity. If the epoxy resin is in excess, the epoxy group ends, and if the phenolic compound is in excess, the phenolic group ends, and the reaction ends. If the ratio of the epoxy resin is less than 1.01 mol, the polymer is likely to have phenolic group terminals, and there is a risk that adhesion to the reinforcing fibers will not be exhibited. If the ratio of the epoxy resin exceeds 1.05 mol, unreacted epoxy resin components will remain in the resin even after the polymerization reaction is completed, which may adversely affect the strength of the resin.

[0031] In an epoxy resin composition, if a phenolic compound is present in a crystalline state in the epoxy resin, the molar ratio will deviate from the design when viewed microscopically. If the reaction is started in this state, the polymerization may not proceed sufficiently. In order to allow the polymerization to proceed sufficiently, an epoxy resin composition in which the phenolic compound and the epoxy resin are uniformly dissolved (compatible) with each other is preferred. In addition, it is desirable that the epoxy resin composition before blending with reinforcing fibers, etc., is completely dissolved or in a uniform liquid state, but for example, when the molten mixture is poured into a glass petri dish to a thickness of 2 mm without any air bubbles and the haze value in the thickness direction is measured, if the haze value in the thickness direction is less than 30%, it is judged that the composition has dissolved to a level that does not affect the polymerization reaction or has become a uniform liquid state. The haze value is more preferably less than 20%, and even more preferably less than 10%.

[0032] The polymerization catalyst used in the epoxy resin composition is not limited, but any known catalyst can be used.Specific examples include phosphorus-based polymerization catalysts such as triphenylphosphine, tris(paratoluyl)phosphine, tris(orthotoluyl)phosphine, and tris(paramethoxyphenyl)phosphine.Other polymerization catalysts include imidazole compounds such as 1B2MZ, 1B2PZ, and TBZ (manufactured by Shikoku Chemical Industry Co., Ltd.).

[0033] The polymerization catalyst is preferably 0.05% by weight or more and 5% by weight or less based on the total amount of the resin composition consisting of a bifunctional epoxy resin and a bifunctional phenolic compound. If it is less than 0.05% by weight, the in-situ polymerization takes too long, which may reduce productivity, and it may be deactivated for some reason before the target molecular weight is reached. If it exceeds 5% by weight, the polymerization reaction proceeds quickly, but storage stability may be impaired, which may cause problems with process compatibility, and since it is a component that participates in the reaction but is not incorporated into the skeleton, there is a risk of impairing the physical properties after polymerization, and it is simply expensive, which is economically disadvantageous.

[0034] The epoxy resin composition may contain an organic solvent as a solvent for the polymerization catalyst or to adjust the viscosity. The organic solvent to be used is not particularly limited as long as it does not inhibit the reaction between the epoxy resin and the phenolic compound, but hydrocarbons, ketones, and ethers are preferred because of their ease of availability. Specific examples include toluene, xylene, acetone, methyl ethyl ketone, isobutyl ketone, cyclopentanone, cyclohexanone, and diethylene glycol dimethyl ether. However, if a large amount of organic solvent is present during the reaction, it inhibits the polymerization reaction. In addition, if the organic solvent remains in the polymer, it deteriorates the mechanical properties and heat resistance. For this reason, the proportion of the organic solvent is preferably 5% by weight or less based on the total weight of the epoxy resin composition.

[0035] The progress of polymerization of the epoxy resin composition can be judged from the change in the epoxy equivalent of the polymer. If the heating is performed for less than one hour, the epoxy equivalent tends to increase, and it is possible that the polymerization has not progressed sufficiently. If the heating is performed for more than one hour, the epoxy equivalent hardly increases from the value at the one-hour mark, and it can be judged that the polymerization has progressed sufficiently. Therefore, the polymerization conditions for obtaining a polymer from the epoxy resin composition were set to heating at 160°C for one hour. In the present invention, the polymer for measuring the tetrahydrofuran (THF) insoluble content refers to the polymerized product polymerized under these conditions.

[0036] The progress of polymerization of the reinforcing fiber-containing epoxy resin composition and the prepreg was also judged by the change in epoxy equivalent, in the same way as the progress of the polymerization. When heated for less than 4 hours, the epoxy equivalent tends to increase, and it is possible that polymerization has not progressed sufficiently. When heated for more than 4 hours, the epoxy equivalent hardly increases from the value at the 4-hour point, and it was judged that polymerization has progressed sufficiently. In the epoxy resin composition in which fibers are compounded, the epoxy equivalent is almost the same when the heating time is four times that of the epoxy resin composition alone. This is thought to be because the reaction is suppressed in the fiber. Therefore, the curing conditions for obtaining fiber-reinforced plastic from the reinforcing fiber-containing epoxy resin composition or prepreg were set to heating at 160°C for 4 hours.

[0037] It is important that the bending strength of the polymer obtained by polymerizing the epoxy resin composition of the present invention without containing fillers such as reinforcing fibers or additives is 70 MPa or more. If the bending strength of the polymer is below the lower limit of the range, it cannot fully exhibit mechanical strength as a fiber reinforced plastic. The higher this strength is, the better the mechanical strength of the fiber reinforced plastic is, so there is no need to specify an upper limit.

[0038] The epoxy equivalent of the polymer obtained by polymerizing the epoxy resin composition of the present invention is 5000 g / eq. or more and 20000 g / eq. or less. If the epoxy equivalent of the polymer is below the lower limit of the range, the polymer contains a large amount of epoxy resin that has not been sufficiently polymerized, and there is a risk of the mechanical strength being deteriorated. If the epoxy equivalent of the polymer is above the upper limit of the range, the terminal group becomes a phenol group, and there is a risk of the adhesion of the reinforcing fiber being deteriorated.

[0039] The epoxy resin composition of the present invention may contain additives. Examples of additives include fillers such as fumed silica, flame retardants such as aluminum hydroxide and red phosphorus, and modifiers such as core-shell rubber. From the viewpoint of stabilizing the polymerization reaction, it is desirable to mix additives different from those in the resin phase, but plasticizers and compatible flame retardants may be included within the range that does not affect the reaction.

[0040] The epoxy resin composition of the present invention can be polymerized to form a thermoplastic epoxy resin, which is excellent as a resin component for fiber-reinforced plastics. The reinforcing fiber-containing epoxy resin composition of the present invention can be obtained by mixing or impregnating the above-mentioned epoxy resin composition with reinforcing fibers. The prepreg can be obtained as follows.

[0041] The epoxy resin composition of the present invention is applied to a release-treated paper or plastic film, and a release-treated cover film is applied as necessary to obtain an epoxy resin composition film. The release paper, release plastic film, and cover film can be any known one, and are not particularly limited. The thickness of the epoxy resin composition film is determined by the design thickness and resin ratio of the prepreg, and is usually 1 μm or more and 300 μm or less. If the thickness is less than 1 μm, there is a problem that the opening of the fiber becomes noticeable unless the reinforcing fiber is defibrated cleanly, and if the thickness exceeds 300 μm, it is difficult to uniformly impregnate the reinforcing fiber. The thickness is preferably 5 μm or more and 150 μm or less, and more preferably 10 μm or more and 100 μm or less.

[0042] The reinforcing fibers used in the present invention are intended to reinforce plastics, such as carbon fibers, aramid fibers, and cellulose fibers, and are not particularly limited. The form of the fibers is also not particularly limited, and includes UD sheets, woven fabrics, tows, chopped fibers, nonwoven fabrics, paper, and the like, in which the fibers are aligned. However, from the viewpoint of impregnation, the thickness of each fiber bundle is 1 mm or less, preferably 0.5 mm or less, and more preferably 0.2 mm or less.

[0043] The reinforcing fiber-containing epoxy resin composition or prepreg of the present invention is obtained from the above-mentioned epoxy resin composition and / or epoxy resin composition film and reinforcing fibers. The ratio by weight of the reinforcing fibers to the epoxy resin composition is preferably 5:5 to 8:2. If the ratio of the reinforcing fibers is too small, the strength required for the fiber-reinforced material may not be fully satisfied, and if the ratio of the reinforcing fibers is too large, defects such as voids may occur. EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. Unless otherwise specified, "parts" refers to parts by weight, and "%" refers to % by weight.

[0045] The raw materials, catalysts, solvents, and reinforcing fibers used in the examples are as follows.

[0046] [Epoxy resin] A1: Tetramethylbiphenol type epoxy resin (Mitsubishi Chemical Corporation, YX-4000, epoxy equivalent 188) A2: Bisphenol A type epoxy resin (manufactured by Nippon Steel Chemical & Material Co., Ltd., YD-8125, epoxy equivalent 173)

[0047] [Phenol compounds] B1: Bisphenol A (manufactured by Nippon Steel Chemical & Material Co., Ltd., hydroxyl equivalent: 114) B2: 4,4'-bis(3,3,5-trimethylcyclohexylidene)bisphenol (Honshu Chemical Industry Co., Ltd., BisP-HTG, hydroxyl equivalent 155)

[0048] [Polymerization catalyst] C1: Tris(paramethoxyphenyl)phosphine (TPAP, manufactured by Hokko Chemical Industry Co., Ltd.) C2: 2,3-dihydro-1H-pyrrolo-[1,2-a]benzimidazole (manufactured by Shikoku Chemical Industry Co., Ltd., TBZ)

[0049] [solvent] D1: Cyclohexanone

[0050] [Reinforced fiber] E: PAN-based carbon fiber (Toray Industries, Inc., T700-12K-50C)

[0051] The evaluation methods used in the examples are as follows.

[0052] Epoxy equivalent weight: The measurements were carried out in accordance with the Japanese Industrial Standard JIS K7236 and expressed in units of "g / eq." The polymer was measured as it was, and the resin component of the fiber-reinforced plastic was extracted by the following procedure, and the obtained resin component was used for the measurement. Approximately 4 g of sample was weighed into a 110 mL vial, 100 mL of tetrahydrofuran (THF) was added, and ultrasonic diffusion was performed at room temperature for 1 hour, followed by leaving it to stand at room temperature for more than 23 hours to dissolve. The resulting THF solution was filtered under reduced pressure using a 5 μm filter paper, and the filtrate was collected. The collected filtrate was dried in a silicon vat at 20°C for more than 24 hours, and then dried in an oven set at 110°C for more than 5 hours to obtain a film-formed resin component.

[0053] Hydroxyl equivalent: The measurement was carried out in accordance with JIS K0070 standard, and the unit was expressed as "g / eq." Unless otherwise specified, the hydroxyl equivalent of the phenolic resin means the phenolic hydroxyl equivalent.

[0054] uniformity; The haze value was used to determine whether the phenol compound was uniformly dissolved in the epoxy resin. The epoxy resin composition was placed in a colorless, transparent glass petri dish to a thickness of 2 mm, and the haze value was evaluated using a haze standard plate manufactured by Murakami Color Research Laboratory as a reference, with a 5-level scale of "less than 5% (<5)", "less than 10% (<10)", "less than 20% (<20)", "less than 30% (<30)", and "30% or more (30≦)". If the haze value was less than 30%, it was determined that the phenol compound was uniformly dissolved in the epoxy resin, and was marked with "◯", and if it was 30% or more, it was determined that the phenol compound was not uniformly dissolved, and was marked with "X".

[0055] Gel fraction; Approximately 1 g of the sample was weighed out in a 100 mL vial, 50 mL of tetrahydrofuran was added, ultrasonic diffusion was performed at room temperature for 1 hour, and the sample was dissolved by leaving it at room temperature for more than 23 hours. A 325 mesh wire mesh was dried in an oven at 100 °C for 1 hour and its weight was measured. The wire mesh was folded into a funnel shape, and the entire sample solution was poured onto the funnel. The vial was washed with tetrahydrofuran until no insoluble matter of the sample remained, and then poured into the funnel. The insoluble matter on the wire mesh was further washed with tetrahydrofuran and dried in an oven at 100 °C for more than 4 hours. The gel fraction was evaluated by subtracting the dry weight of the wire mesh from the weight of the dried sample and wire mesh, and dividing this by the weight of the sample. The gel fraction is equal to the weight % of the THF insoluble matter.

[0056] Bending test; The bending strength of the polymer was measured according to JIS K 7171. The test machine used was an autograph AGS-X manufactured by Shimadzu Science Co., Ltd. The sample dimensions were 4 mm thick, 100 mm long, and 15 mm wide, the bending span was 70 mm, and the test was performed at a test speed of 1 mm / min. The 90 degree bending strength of unidirectional fiber reinforced plastics was measured in accordance with JIS K 7074. The test machine used was an Autograph AGS-X manufactured by Shimadzu Science Co., Ltd. The sample dimensions were 2 mm thick, 100 mm long, and 15 mm wide, the bending span was 70 mm, and the test was performed at a test speed of 1 mm / min.

[0057] Resin Adhesion: The cross section of the fiber reinforced plastic after bending test was observed with a SEM (JSM-7900F, manufactured by JEOL Ltd.) to confirm the amount of resin attached to the fiber. If the adhesion between the fiber and resin is good, it can be confirmed that the resin is well attached to the fiber surface at the fracture surface. Ten fibers were observed with SEM and the number of fibers with resin attached to 80% or more of the fiber surface was used for evaluation. 9 or more: 〇, 8 or less: ×

[0058] Example 1 2913 parts of A1, 1000 parts of B1, and 1000 parts of B2 were weighed out and pulverized and mixed using a Henschel mixer. Then, melt mixing was performed using an S1KRC kneader (manufactured by Kurimoto Iron Works, Ltd.) whose barrel temperature was preheated to 170°C, and the entire amount was collected in a metal can and cooled while stirring to obtain a precursor mixture (F1) of an epoxy resin composition.

[0059] 5 parts of C1 (polymerization catalyst) was dissolved in 5 parts of D1 (organic solvent) in advance. The precursor mixture (F1) was placed in a planetary mixer set at 60°C, and the polymerization catalyst solution was added and mixed. After mixing, the mixture was quickly removed and immediately cooled to 40°C or less to obtain an epoxy resin composition (G1).

[0060] The obtained epoxy resin composition (G1) was heated to about 70°C and stirred, poured into a chrome-plated iron mold container with a clearance of 4 mm set in advance, and thermally polymerized at 160°C for 60 minutes in a hot air circulating oven to obtain a polymerized product.

[0061] The epoxy equivalent of the resulting polymer was measured and found to be 9900 g / eq. The bending strength of the resulting polymer was measured and found to be 87 MPa. The gel fraction of the resulting polymer was measured and found to be 1%.

[0062] Examples 2 to 3, Comparative Examples 1 to 4 An epoxy resin composition and a polymer were obtained in the same manner as in Example 1 under the conditions shown in Table 1. The epoxy equivalent, bending strength and gel fraction of the obtained polymer were measured in the same manner as in Example 1, and the evaluation results are shown in Table 1.

[0063] However, in Comparative Examples 3 and 4, instead of pulverization and mixing using a Henschel mixer, stirring and mixing were performed in a planetary mixer set at 60°C. In Comparative Example 3, the barrel temperature during melt mixing was set to 80° C. At this time, the haze value of the obtained epoxy resin composition was 30% or more, and the molten state of the phenol compound was judged to be ×. In addition, in Comparative Example 4, the gel fraction of the heavy product was 95%, and the polymer could not be dissolved in a solvent, so that the epoxy equivalent was not measured.

[0064] [Table 1]

[0065] Example 4 A release-treated release paper was fixed on a hot plate preheated to 70°C with the release side facing up, and the epoxy resin composition (G1) obtained in Example 1 was placed on the release paper. Then, a bar coater preheated to 70°C was used to coat the epoxy resin composition (G1) on the release paper until the area weight of the resin was 79 g / m. 2 Immediately after coating, the sheet was removed from the hot plate and cooled in air to obtain an epoxy resin composition sheet. Next, a fiber sheet having an area weight of 153 g / m was applied onto the obtained epoxy resin composition sheet. 2 Carbon fibers (E) were laminated together so that the surface pressure was 0.5 MPa, and a hot press preheated to 90° C. was used to apply pressure. After 1 minute, the material was removed and air-cooled to obtain a prepreg with Rc=34%. Thirteen of the prepregs were then laminated together with the fibers oriented in the same direction, sandwiched between release films, and vacuum pressed to obtain a unidirectional fiber-reinforced plastic. The vacuum pressing conditions were 160°C, 0.1 MPa, and 240 minutes.

[0066] The 90 degree bending strength of the obtained unidirectional fiber reinforced plastic was measured and found to be 86 MPa. The epoxy equivalent of the resin component of the obtained unidirectional fiber reinforced plastic was measured and found to be 9800 g / eq.

[0067] For Examples 5 to 6 and Comparative Examples 5 to 8, unidirectional fiber-reinforced plastics were obtained in the same manner as in Example 4. Note that for Comparative Example 8, a large amount of insoluble matter was generated during epoxy equivalent measurement, so that the epoxy equivalent was not measured.

[0068] [Table 2]

[0069] From Tables 1 and 2, it can be seen that if the epoxy equivalent of the polymer is between 5,000 g / eq. and 20,000 g / eq. and the resin strength is 70 MPa or more, the 90 degree bending strength of the reinforced fiber plastic will be 80 MPa or more. From Comparative Example 5 (Comparative Example 1), it can be confirmed that when the epoxy equivalent of the polymer is high, the adhesion between the fiber and the resin is weak, and the 90 degree bending strength is not sufficiently exhibited. From Comparative Examples 6 and 7 (Comparative Examples 2 and 3), it can be confirmed that if the resin strength of the polymer is not sufficiently high, the 90 degree bending strength is not sufficiently exhibited. From Comparative Example 8 (Comparative Example 4), it can be confirmed that if there are many insoluble components in the polymer, the 90 degree bending strength is not sufficiently expressed. Resins containing many gel components tend to have a high minimum melt viscosity during the polymerization reaction, which is thought to make it easier for voids to remain in the CFRP molded product, adversely affecting the 90 degree bending strength.

Claims

1. An epoxy resin composition containing a reinforcing fiber and an epoxy resin composition containing a difunctional phenol compound, a difunctional epoxy resin, and a polymerization catalyst as essential components, the epoxy resin composition comprising a reinforcing fiber, The difunctional epoxy resin contains 50% by weight or more of a difunctional epoxy resin (a) represented by the following formula (1): The compounding ratio of the bifunctional phenol compound to the bifunctional epoxy resin is 1.01 to 1.05 moles of the bifunctional epoxy resin per mole of the bifunctional phenol compound, A polymer obtained by heating the epoxy resin composition at 160°C for 1 hour is a thermoplastic epoxy resin, the polymer having an epoxy equivalent of 5000 g / eq. or more and 20000 g / eq. or less, a bending strength of 70 MPa or more, and a content of a component that is insoluble when dissolved in tetrahydrofuran of 10% by weight or less. Here, the bending strength of the polymer and the component that becomes insoluble when dissolved in tetrahydrofuran (gel fraction) are values ​​measured by the methods described in paragraphs 0056 and 0055 of the specification. 【Chemistry 1】 Here, A is a divalent group represented by formula (2), n is the number of repetitions, the average value of which is 0 to 5, and X is a single bond, a hydrocarbon group having 1 to 13 carbon atoms, -O-, -CO-, -COO-, -S-, or -SO 2 - and Y 1 are independently an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 10 carbon atoms; Y 2 and Y 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an aryl group having 6 to 10 carbon atoms.

2. 2. The reinforcing fiber-containing epoxy resin composition according to claim 1, comprising PAN-based carbon fibers as reinforcing fibers in an amount of 50% by weight or more and 80% by weight or less.

3. A prepreg comprising a mixture containing a reinforcing fiber and an epoxy resin composition containing a bifunctional phenol compound, a bifunctional epoxy resin, and a polymerization catalyst as essential components, The difunctional epoxy resin contains 50% by weight or more of a difunctional epoxy resin (a) represented by the following formula (1): The compounding ratio of the bifunctional phenol compound to the bifunctional epoxy resin is 1.01 to 1.05 moles of the bifunctional epoxy resin per mole of the bifunctional phenol compound, A prepreg characterized in that a polymer obtained by heating the epoxy resin composition at 160°C for 1 hour is a thermoplastic epoxy resin, the polymer having an epoxy equivalent of 5000 g / eq. or more and 20000 g / eq. or less, a bending strength of 70 MPa or more, and a content of a component that becomes insoluble when dissolved in tetrahydrofuran of 10% by weight or less. Here, the bending strength of the polymer and the component that becomes insoluble when dissolved in tetrahydrofuran (gel fraction) are values ​​measured by the methods described in paragraphs 0056 and 0055 of the specification. 【Chemistry 2】 Here, A is a divalent group represented by formula (2), n is the number of repetitions and its average value is 0 to 5. X is a single bond, a hydrocarbon group having 1 to 13 carbon atoms, -O-, -CO-, -COO-, -S-, or -SO 2 -, Y 1 is independently an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 10 carbon atoms, and Y 2 and Y 3 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an aryl group having 6 to 10 carbon atoms.

4. 4. The prepreg according to claim 3, containing PAN-based carbon fibers as reinforcing fibers in a ratio of 50% by weight or more and 80% by weight or less.

5. A fiber reinforced plastic using the prepreg according to claim 3.

6. A fiber-reinforced plastic using the reinforcing fiber-containing epoxy resin composition according to claim 1.

Citation Information

Patent Citations

  • Method for molding fiber-reinforced thermoplastic resin

    JP2006321897A

  • Sulfo group-containing polyhydroxypolyether resin, resin composition containing the resin, curable resin composition containing the resin, and film obtained from them

    JP2011144319A

  • High molecular weight epoxy resin, resin composition and cured product using the same

    JP2014005345A

  • Epoxy resin, epoxy resin composition, epoxy resin cured product and composite material

    JP2020143191A

  • Curable resin composition and cured product thereof

    JP2020176188A