Method for producing expandable styrene resin particles

The method addresses the challenge of residual styrene and benzene in expandable styrenic resin particles by using specific organic peroxides and a brominated styrene-butadiene copolymer in suspension polymerization, achieving low residual content and high flame retardancy for automotive applications.

JP7588511B2Active Publication Date: 2024-11-22JSP CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020215484
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-11-22
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

Existing methods for producing expandable styrenic resin particles with flame retardants face challenges in reducing residual styrene and benzene content while maintaining flame retardancy, and often require the use of special polymerization initiators that affect productivity.

Method used

A method involving suspension polymerization of styrene monomers with a dissolved flame retardant, using specific aliphatic peroxyester and peroxyketal organic peroxides as initiators, and a brominated styrene-butadiene copolymer as the flame retardant, to achieve styrene and benzene contents of 25 mass ppm or less and 1.5 mass ppm or less, respectively, while ensuring high flame retardancy.

Benefits of technology

The method produces expandable styrenic resin particles with low styrene and benzene content, enabling the production of foam molded articles with excellent flame retardancy and improved mechanical properties, suitable for automotive interior materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588511000001
    Figure 0007588511000001
  • Figure 0007588511000002
    Figure 0007588511000002
  • Figure 0007588511000003
    Figure 0007588511000003
Patent Text Reader

Abstract

To provide a method for producing foamable styrenic resin particles which enables easy production of a styrenic resin foam particle molding that has excellent flame retardancy and has small contents of styrene and benzene.SOLUTION: There is provided a method for producing formable styrenic resin particles containing a flame retardant and a foaming agent by a polymerization step. The polymerization step adds a styrenic monomer in which a flame retardant is dissolved in an aqueous medium, and performs suspension polymerization. The polymerization step uses an aliphatic peroxy ester type and / or an aliphatic peroxy ketal type first organic peroxide having a 10 hr half-life temperature of 65°C or higher and 90°C or lower, and a second organic peroxide having a 10 hr half-life temperature of higher than 90°C and 110°C or lower, as polymerization initiators. The flame retardant is a bromide of a styrene-butadiene-based copolymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing expandable styrene-based resin particles containing a flame retardant by suspension polymerization of a styrene-based monomer. [Background technology]

[0002] A styrene resin expanded bead molded product (hereinafter, appropriately referred to as "expanded molded product") obtained from expandable styrene resin particles has excellent heat insulating performance and is therefore used for residential heat insulating materials, cold storage boxes, etc. In addition, since the expanded molded product is also lightweight and has excellent shock-absorbing performance, it is also used as an automobile interior material such as a shock-absorbing material or a floor raising material. In such applications, a flame-retardant expanded molded product containing a flame retardant is used. In addition, it is desired to reduce the content of volatile organic compounds (i.e., VOCs) such as unreacted styrene monomer (hereinafter, appropriately referred to as "residual styrene") in the expanded molded product.

[0003] In particular, for interior materials for vehicles such as automobiles, foamed molded articles with low emission of volatile organic compounds are required more than for residential insulation materials. However, when suspension polymerization of styrene-based monomers is carried out in the presence of a flame retardant in order to obtain foamed molded articles with excellent flame retardancy, polymerization inhibition occurs, making it difficult to sufficiently reduce the amount of residual styrene in the expandable styrene-based resin particles.

[0004] In response to this, for example, Patent Documents 1 and 2 disclose a method for producing expandable styrene-based resin particles that exhibit excellent flame retardancy and have a low content of styrene-based monomers by performing suspension polymerization in the presence of a flame retardant made of a brominated styrene-butadiene copolymer. Patent Document 3 discloses a method for producing expandable styrene-based resin particles that use a specific polymerization initiator and that can provide an expanded molded article that has flame retardancy, a low content of styrene-based monomers, and reduced unpleasant odors. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-71669 A [Patent Document 2] JP 2020-147668 A [Patent Document 3] JP 2016-37573 A Summary of the Invention [Problem to be solved by the invention]

[0006] The manufacturing method of Patent Document 1 has difficulty in sufficiently reducing the amount of residual styrene in the expandable styrene-based resin particles, and also leaves a problem in the flame retardancy of the resulting foamed molded article. The manufacturing method of Patent Document 2 leaves a problem in the flame retardancy of the resulting foamed molded article. In addition, the manufacturing method of Patent Document 2 requires the use of an organic peroxide having a special structure as a polymerization initiator, and is also poor in productivity. The manufacturing method of Patent Document 3 can sufficiently reduce the amount of residual styrene in the expandable styrene-based resin particles, and also has excellent flame retardancy of the resulting foamed molded article. However, the expandable styrene-based resin particles obtained by the manufacturing method of Patent Document 3 may have benzene detected in the particles, and there is room for improvement depending on the application.

[0007] The present invention has been made in view of the above background, and aims to provide a method for producing expandable styrene-based resin beads, which enables easy production of expanded styrene-based resin bead moldings having excellent flame retardancy and low styrene and benzene contents. [Means for solving the problem]

[0008] One aspect of the present invention is a method for producing expandable styrene-based resin particles containing a flame retardant and a blowing agent, comprising the steps of: a polymerization step of adding a styrene-based monomer containing styrene and having the flame retardant dissolved therein to an aqueous medium, and carrying out suspension polymerization of the styrene-based monomer in the aqueous medium to obtain styrene-based resin particles containing the flame retardant, In the polymerization step, a first organic peroxide of an aliphatic peroxy ester type and / or an aliphatic peroxy ketal type having a 10-hour half-life temperature of 65° C. or more and 90° C. or less and a second organic peroxide having a 10-hour half-life temperature of more than 90° C. and 110° C. or less are used as a polymerization initiator, The flame retardant is a brominated styrene-butadiene copolymer, The blending amount of the flame retardant is 0.05 to 2 parts by mass per 100 parts by weight of the styrene-based monomer, The method for producing expandable styrene-based resin particles is characterized in that the expandable styrene-based resin particles have a styrene content of 25 mass ppm or less (including 0) and a benzene content of 1.5 mass ppm or less (including 0). Effect of the Invention

[0009] In the manufacturing method of the present invention, the specific first organic peroxide and the specific second organic peroxide are used as polymerization initiators, and the specific flame retardant is used while performing suspension polymerization of a styrene monomer in which the flame retardant is dissolved in an aqueous medium. This makes it possible to manufacture expandable styrene resin particles containing a flame retardant, the styrene content being 25 mass ppm or less and the benzene content being 1.5 mass ppm or less. With such expandable styrene resin particles, it becomes possible to manufacture a styrene resin expanded bead molding having excellent flame retardancy and low styrene and benzene contents. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Next, a preferred embodiment of the expandable styrene-based resin particles will be described. In this specification, expandable styrene-based resin particles are appropriately referred to as "expandable particles". Expanded styrene-based resin particles obtained by expanding expandable styrene-based resin particles are appropriately referred to as "expanded particles". Expanded styrene-based resin beads molded by molding styrene-based resin expanded beads in a mold are appropriately referred to as "expanded molded bodies". In this specification, when a numerical value or a physical property value is expressed before and after "~", it is used as including the values ​​before and after. In addition, when a numerical value or a physical property value is expressed as a lower limit, it means that it is equal to or higher than that numerical value or physical property value, and when a numerical value or a physical property value is expressed as an upper limit, it means that it is equal to or lower than that numerical value or physical property value. In this specification, "parts by mass" and "parts by weight", "% by mass" and "% by weight" are substantially synonymous. "ppm" means "ppm by mass" unless otherwise specified.

[0011] In the polymerization step, the styrene monomer in which the flame retardant is dissolved is added to an aqueous medium, and the styrene monomer is suspended in the aqueous medium. That is, the styrene monomer is suspended in the presence of the flame retardant. This results in styrene resin particles containing the flame retardant. The flame retardant contains a brominated styrene-butadiene copolymer. In the following description, the brominated styrene-butadiene copolymer is appropriately referred to as "Br-SBC". As the Br-SBC, for example, a brominated styrene-butadiene block copolymer can be used. As the flame retardant, a brominated flame retardant other than Br-SBC can be used in combination within the scope in which the intended object of the present invention is achieved.

[0012] The suspension polymerization of the styrene-based monomer in the polymerization step is carried out in an aqueous medium containing, for example, a suspending agent. The aqueous medium is a liquid such as water. The flame retardant is added to the aqueous medium in a state in which it is dissolved in the styrene-based monomer in advance.

[0013] In the polymerization step, suspension polymerization of a styrene-based monomer is carried out. Therefore, unlike the so-called seed polymerization method in which, for example, a styrene-based monomer is impregnated and polymerized into a core particle containing a styrene-based resin, there is no need to produce a core particle. Therefore, the production efficiency of the expandable particles is high. In addition, in the polymerization step, a styrene-based monomer in which a predetermined flame retardant is dissolved as described above is added to an aqueous medium, and suspension polymerization is carried out using a predetermined polymerization initiator. As a result, in a state in which the polymerization of the styrene-based monomer progresses and the concentration of the styrene-based monomer decreases, the generation of benzene derived from the polymerization initiator, for example, is suppressed, and the polymerization of the styrene-based monomer progresses sufficiently. As a result, it is possible to produce expandable particles that contain a flame retardant and have a styrene content of 25 mass ppm or less (including 0) and a benzene content of 1.5 mass ppm or less (including 0). The reason for this is considered as follows.

[0014] In general, when a styrene-based monomer is subjected to suspension polymerization in the presence of a flame retardant, polymerization inhibition is likely to occur, and the styrene-based monomer tends to remain in the expandable particles. As described above, when a styrene-based monomer in which a flame retardant is dissolved is added to an aqueous medium to perform suspension polymerization, polymerization inhibition is suppressed, the amount of remaining styrene is reduced, and flame retardancy is improved by using Br-SBC as a flame retardant. However, when Br-SBC is used as a flame retardant in the suspension polymerization of a styrene-based monomer, benzene was sometimes detected in the expandable particles. The present inventors have found that this is caused by decarboxylation of the polymerization initiator radical. Furthermore, they have found that this decarboxylation is likely to occur when an aromatic polymerization initiator such as benzoyl peroxide is used in the suspension polymerization, and the polymerization of the styrene-based monomer progresses and the amount of the styrene-based monomer is reduced to an extremely small amount. Specifically, it was found that when, for example, benzoyl peroxide is used as a polymerization initiator, in an environment where the concentration of styrene-based monomer is extremely low, the reaction between the benzoyl peroxide radical and the styrene-based monomer is difficult to occur, and the radical undergoes decarboxylation to generate benzene. As in the manufacturing method of the present disclosure, by using the above-mentioned predetermined first organic peroxide and second organic peroxide as the polymerization initiator, the generation of benzene is suppressed even in an environment where the concentration of styrene-based monomer is extremely low, and expandable particles with a low benzene content can be obtained.

[0015] The amount of the flame retardant to be blended relative to 100 parts by weight of the styrene monomer is preferably 0.05 to 2 parts by weight. In this case, the flame retardancy can be further improved, and an increase in the production cost due to an increase in the amount of the flame retardant to be blended can be prevented. Furthermore, the polymerization inhibition of the styrene monomer can be further prevented, and the content of styrene in the foam molded product can be further reduced. From the viewpoint of further reducing the content of styrene, the amount of the flame retardant to be blended relative to 100 parts by weight of the styrene resin is preferably less than 1 part by weight, more preferably less than 0.5 parts by weight, and particularly preferably 0.1 parts by weight or less. The amount of the flame retardant blended above is usually equal to the content of the flame retardant in the foam molded product.

[0016] As the styrene-based monomer, styrene can be used. In addition to styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-methoxystyrene, pn-butylstyrene, pt-butylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,4,6-tribromostyrene, divinylbenzene, styrenesulfonic acid, sodium styrenesulfonate, and other styrene compounds can be used. The styrene-based monomers may be used alone or in combination of two or more kinds. From the viewpoint of product cost and ease of processing of the foamed molded product, it is preferable that the main component of the styrene-based monomer is styrene.

[0017] In addition, a vinyl monomer copolymerizable with the styrene monomer may be used together with the styrene monomer. Examples of such vinyl monomers include (meth)acrylic acid, (meth)acrylic acid esters, vinyl monomers containing a nitrile group, organic acid vinyl compounds, olefin compounds, diene compounds, halogenated vinyl compounds, halogenated vinylvinylidene compounds, and maleimide compounds. Note that "(meth)acrylic acid" is a concept that includes "acrylic acid" and "methacrylic acid", and means either one or both of these.

[0018] Examples of (meth)acrylic acid esters include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, 1,4-butanediol diacrylate, 1,6-hexadiol diacrylate, trimethylolpropane trimethacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate. Examples of vinyl monomers containing a nitrile group include acrylonitrile and methacrylonitrile. Examples of organic acid vinyl compounds include vinyl acetate and vinyl propionate. Examples of olefin compounds include ethylene, propylene, 1-butene, and 2-butene. Examples of diene compounds include butadiene, isoprene, and chloroprene. Examples of halogenated vinyl compounds include vinyl chloride and vinyl bromide. Examples of the vinylidene halide compound include vinylidene chloride, etc. Examples of the maleimide compound include N-phenylmaleimide, N-methylmaleimide, etc.

[0019] The phenylacetylene concentration in the styrene-based monomer is preferably 5 ppm by mass or more and 20 ppm by mass or less. By making the phenylacetylene concentration 20 ppm by mass or less, the styrene content can be further reduced. In addition, even if the phenylacetylene concentration is 5 ppm by mass or more, the production method of the present disclosure makes it possible to sufficiently reduce the styrene content and the benzene content, so that it is possible to avoid the use of a high-cost styrene-based monomer having a phenylacetylene concentration of less than 5 ppm by mass (including 0).

[0020] In the polymerization step, for example, a styrene-based monomer having a flame retardant dissolved therein is dispersed in an aqueous medium in a sealed container equipped with a stirrer to initiate the polymerization reaction. The polymerization step can include a first polymerization step in which polymerization is performed using a specific first organic peroxide as a polymerization initiator, and a second polymerization step in which polymerization is performed using a specific second organic peroxide as a polymerization initiator. The first polymerization step is a step in which most of the styrene-based monomer is polymerized at a relatively low temperature, and the second polymerization step is a step in which the remaining unreacted styrene-based monomer is polymerized at a temperature higher than the first polymerization step. Specifically, the polymerization step preferably includes a first polymerization step in which the styrene-based monomer is polymerized at a temperature of 110°C or lower until the polymerization conversion rate reaches 90% by mass or more, and a second polymerization step in which the styrene-based monomer is further polymerized at a temperature higher than 115°C and lower than 135°C until the content of the unreacted styrene-based monomer is 25 ppm by mass or less (including 0). In this case, it is possible to suppress a decrease in the weight average molecular weight of the styrene-based resin, improve the mechanical strength of the foamed molded article, and further reduce the amount of residual styrene.

[0021] The polymerization initiator is an organic peroxide, and as described above, a first organic peroxide and a second organic peroxide are used. The first organic peroxide has a 10-hour half-life temperature of 65° C. or more and 90° C. or less, and is an aliphatic peroxyester type and / or aliphatic peroxyketal type organic peroxide. If the 10-hour half-life temperature of the first organic peroxide is higher than 90° C., it may be difficult to reduce the amount of residual styrene. In addition, the mechanical strength of the resulting foamed molded article may be reduced. From the viewpoint of further reducing the amount of residual styrene and further improving the mechanical strength of the foamed molded article, the 10-hour half-life temperature of the first organic peroxide is preferably 85° C. or less, more preferably 80° C. or less. On the other hand, if the 10-hour half-life temperature of the first organic peroxide is less than 65° C., it may be difficult to reduce the amount of residual styrene. From the viewpoint of further reducing the amount of residual styrene, the 10-hour half-life temperature of the first organic peroxide is preferably 68° C. or more, more preferably 70° C. or more. The first organic peroxide is used, for example, mainly as a polymerization initiator in the first polymerization step, and is appropriately referred to as a "first polymerization initiator."

[0022] The second organic peroxide is an organic peroxide having a 10-hour half-life temperature of more than 90°C and not more than 110°C. When the 10-hour half-life temperature of the second organic peroxide is higher than 110°C, it may be difficult to reduce the amount of residual styrene. From the viewpoint of further reducing the amount of residual styrene, the 10-hour half-life temperature of the second organic peroxide is preferably 105°C or lower, more preferably 102°C or lower. On the other hand, when the 10-hour half-life temperature of the second organic peroxide is 90°C or lower, it may be difficult to reduce the amount of residual styrene. From the viewpoint of further reducing the amount of residual styrene, the 10-hour half-life temperature of the second organic peroxide is preferably 92°C or higher, more preferably 95°C or higher. The second organic peroxide is used, for example, mainly as a polymerization initiator in the latter polymerization step. The second organic peroxide is appropriately referred to as a "second polymerization initiator".

[0023] The second organic peroxide preferably has a 10-hour half-life temperature 10°C or more higher than that of the first organic peroxide. In this case, the second organic peroxide is more suitable as a polymerization initiator (i.e., a second polymerization initiator) in the latter polymerization step. The second organic peroxide is preferably an aliphatic peroxydicarbonate-type and / or an aliphatic peroxyester-type organic peroxide. Since an aliphatic peroxydicarbonate-type and / or an aliphatic peroxyester-type organic peroxide is a general-purpose polymerization initiator and can be obtained at low cost, the manufacturing cost of the expandable particles can be reduced. In addition, in the manufacturing method of the present disclosure, even if an aliphatic peroxydicarbonate-type and / or an aliphatic peroxyester-type organic peroxide is used as the second polymerization initiator, the styrene content and the benzene content can be sufficiently reduced.

[0024] The 10-hour half-life temperature is defined as the temperature at which 50% of the organic peroxide charged in an inert solvent decomposes thermally in 10 hours. The 10-hour half-life temperature can be measured, for example, as follows. First, the organic peroxide is dissolved in benzene to obtain a solution with a concentration of 0.1 mol / L. This solution is sealed in a glass tube in which the air inside has been replaced with nitrogen. The glass tube is then immersed in a thermostatic bath set to a specified temperature to thermally decompose the organic peroxide. Here, the decomposition rate constant is k, time is t, the initial concentration of the organic peroxide is [PO]0, and the concentration of the organic peroxide after time t is [PO] t Then, kt=ln[PO]0 / [PO] t Therefore, the relationship between time t and ln[PO]0 / [PO] t By plotting the relationship between k and x on a graph, the decomposition rate constant k can be calculated from the slope.

[0025] Half-life time t 1 / 2 So [PO]0 / [PO] t Since the relationship of =2 holds, t 1 / 2 = ln2 / k, the half-life time at a certain temperature t 1 / 2 The half-life time t can be calculated for multiple temperatures. 1 / 2 Seeking, lnt 1 / 2By plotting vs. 1 / T on a graph, the 10-hour half-life temperature can be obtained, where T is absolute temperature (unit: K). In addition, the 10-hour half-life temperature data listed in the catalogs or technical documents issued by the manufacturers of organic peroxides can also be used as the value of the 10-hour half-life temperature.

[0026] The first organic peroxide is t-butylperoxy-2-ethylhexanoate. , t-hexylperoxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, t-amylperoxy-2-ethylhexanoate, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)-2-methylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and the like. Examples of the second organic peroxide include t-butylperoxy-2-ethylhexyl carbonate, t-butylperoxyisopropyl carbonate, t-butylperoxyacetate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, t-amylperoxy-2-ethylhexyl carbonate, t-hexylperoxyacetate, 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, and 2,2-bis(t-butylperoxy)butane.

[0027] Among the above organic peroxides, it is preferable to use a first organic peroxide made of t-butylperoxy-2-ethylhexanoate as a polymerization initiator and a second organic peroxide made of t-butylperoxy-2-ethylhexyl monocarbonate as a polymerization initiator. In this case, the amount of residual styrene in the expandable particles can be further reduced, and the generation of benzene in a state where the styrene monomer is in an extremely low concentration in the polymerization process can be further suppressed, so that the content of benzene can be further reduced. Furthermore, the variation in the average particle size of the expandable particles (specifically, the degree of dispersion) can be reduced.

[0028] The amount of organic peroxide added is preferably 0.01 to 2 parts by mass relative to 100 parts by mass of the styrene-based monomer. In this case, the polymerization rate can be increased and the productivity can be sufficiently increased while suppressing the increase in production cost associated with the amount of organic peroxide used. From the same viewpoint, the amount of organic peroxide added is more preferably 0.1 to 1 part by mass relative to 100 parts by mass of the styrene-based monomer.

[0029] When t-butylperoxy-2-ethylhexanoate is used as the first organic peroxide, it is preferable to add a polymerization inhibitor to the aqueous medium within a range that does not inhibit the polymerization of the styrene monomer. In this case, the variation in the average particle size of the expandable particles can be reduced. Examples of the polymerization inhibitor include oil-soluble polymerization inhibitors such as 4-t-butylcatechol (p-TBC), hydroquinone, p-benzoquinone, chloro-p-benzoquinone, 2,5-dichlorobenzoquinone, 2,6-dichlorobenzoquinone, 2,3-dimethyl-p-benzoquinone, 2,5-dimethyl-p-benzoquinone, methoxy-p-benzoquinone, tetrabromo-p-benzoquinone, tetrachloro-p-benzoquinone, dimethyl-p-benzoquinone, o-dinitrobenzene, m-dinitrobenzene, p-dinitrobenzene, 2,4-dinitrotoluene, 1,3,5-trinitrobenzene, 1,3,5-trinitroanisole, and 2,4,6-trinitrophenol; and water-soluble polymerization inhibitors such as sodium nitrite, potassium nitrate, ammonium nitrite, L-ascorbic acid, and citric acid. The timing of adding the polymerization inhibitor is not particularly limited, but it is preferable to add the styrene-based monomer in which the flame retardant, the polymerization initiator, and the polymerization inhibitor are dissolved, to the aqueous medium in the polymerization step. The amount of the polymerization inhibitor added is preferably 0.0001 to 0.01 parts by mass with respect to 100 parts by mass of the styrene-based monomer.

[0030] In addition, as described above, Br-SBC is used as a flame retardant in the polymerization process. Compared with conventionally used bromine-based flame retardants such as 1,2,5,6,9,10-hexabromocyclododecane and 2,2-bis[4'-(2",3"-dibromo-2"-methylpropoxy)-3',5'-dibromophenyl]propane, Br-SBC is less likely to inhibit the polymerization of styrene monomers, and enables the reduction of unreacted styrene monomers by increasing the polymerization temperature in the latter stage, and does not significantly reduce the molecular weight of the styrene resin even if the polymerization temperature in the latter stage is increased. Therefore, by performing the multi-stage polymerization process as described above, resin particles having a low content of unreacted styrene and a high molecular weight can be obtained, even though they contain a flame retardant. The polymerization temperature in the latter polymerization process is appropriately referred to as the "final polymerization temperature".

[0031] In addition, in the manufacturing method of the present disclosure, the styrene-based monomer in which the flame retardant is dissolved is added to an aqueous medium to carry out suspension polymerization. This can increase the stability of the suspension polymerization. In contrast, for example, if the flame retardant and the polymerization initiator are dissolved in an aqueous medium, and the styrene-based monomer in which the flame retardant is not dissolved in advance is added to the aqueous medium to carry out suspension polymerization, the flame retardant is not uniformly impregnated into the expandable particles, and the flame retardancy of the foamed molded product may be impaired. From the viewpoint of further reducing the content of unreacted styrene (i.e., the amount of remaining styrene), it is preferable to add the styrene-based monomer in which the flame retardant and the polymerization initiator are dissolved to an aqueous medium to carry out suspension polymerization. Note that the styrene-based monomer in which the flame retardant is dissolved and the styrene-based monomer in which the polymerization initiator is dissolved can also be added separately to an aqueous medium to carry out suspension polymerization.

[0032] From the viewpoint of suppressing the decrease in the weight average molecular weight of the styrene resin and improving the mechanical strength of the foamed molded product, the polymerization temperature in the first polymerization step is preferably 110° C. or less, and more preferably 105° C. or less, as described above. On the other hand, from the viewpoint of polymerization efficiency, the lower limit is about 70° C. Furthermore, from the viewpoint of more sufficiently reducing the unreacted styrene monomer in the second polymerization step performed following the first polymerization step, it is preferable to carry out polymerization in the first polymerization step until the polymerization conversion rate of the styrene monomer becomes 90% by mass or more, as described above, more preferably until it becomes 95% by mass or more, and even more preferably until it becomes 98% by mass or more.

[0033] From the viewpoint of efficiently reducing the amount of unreacted styrene-based monomer and further preventing a decrease in the weight-average molecular weight of the styrene-based resin, the final polymerization temperature in the second polymerization step is preferably more than 115° C. and not more than 135° C., as described above, and more preferably 118° C. to 130° C. The amount of unreacted styrene-based monomer in the second polymerization step can be controlled by the holding time of the final polymerization temperature.

[0034] In the polymerization step, it is preferable to carry out suspension polymerization under conditions where the polymerization rate is 14% / hr or more and 18% / hr or less until the polymerization conversion rate reaches 90%. In this case, the amount of residual styrene can be further reduced, and the variation in the average particle size of the expandable particles can be reduced. The polymerization rate can be controlled within the above range by changing the polymerization temperature, the type and amount of the polymerization initiator, etc. The polymerization rate until the polymerization conversion rate reaches 90% can be calculated by dividing the polymerization conversion rate of 90% by the time (hr) required for the polymerization conversion rate to reach 90%.

[0035] In addition, in the polymerization step, a flame retardant assistant can be used as necessary. As the flame retardant assistant, a radical generator having a one-hour half-life temperature of more than 130°C can be used. The mass ratio of the flame retardant to the flame retardant assistant is preferably 1:0.1 to 1:5 (where flame retardant: flame retardant assistant). In this case, the flame retardancy of the foamed molded article can be further improved. As the flame retardant assistant, dicumyl peroxide, di-t-butyl peroxide, cumyl hydroperoxide, 2,3-dimethyl-2,3-diphenylbutane, 3,4-dimethyl-3,4-diphenylhexane, poly(1,4-diisopropylbenzene), etc. can be used.

[0036] In the suspension polymerization of the styrene-based monomer, a suspending agent can be used. That is, the polymerization of the styrene-based monomer can be carried out in a dispersion medium such as water to which the suspending agent is added. As the suspending agent, for example, a hydrophilic polymer such as polyvinyl alcohol, methyl cellulose, polyvinylpyrrolidone, etc. can be used. In addition, as the suspending agent, a poorly water-soluble inorganic salt such as tricalcium phosphate, magnesium pyrophosphate, hydroxyapatite, aluminum oxide, talc, kaolin, bentonite, etc. can also be used. In addition, a surfactant can be used in combination with the suspending agent as necessary. In addition, when a poorly water-soluble inorganic salt is used as the suspending agent, it is preferable to use an anionic surfactant such as sodium alkylsulfonate or sodium dodecylbenzenesulfonate in combination.

[0037] The amount of the suspending agent used is preferably 0.01 to 5 parts by mass relative to 100 parts by mass of the styrene-based monomer. When the suspending agent made of a poorly water-soluble inorganic salt and the anionic surfactant are used in combination as described above, it is preferable to use 0.05 to 3 parts by mass of the suspending agent and 0.0001 to 0.5 parts by mass of the anionic surfactant relative to 100 parts by mass of the styrene-based monomer.

[0038] In addition, additives such as bubble nucleating agents (bubble regulators), plasticizers, chain transfer agents, phosphorus-based flame retardants, inorganic flame retardants, antistatic agents, antioxidants, ultraviolet absorbers, light stabilizers, conductive fillers, organic antibacterial agents, and inorganic antibacterial agents can be added to the styrene-based monomer as long as the effects of the present invention are not impaired.

[0039] As the bubble nucleating agent, for example, polyethylene wax, talc, silica, ethylene bisstearylamide, methyl methacrylate copolymer, silicone, etc. can be used. As the plasticizer, for example, liquid paraffin, glycerin diacetomonolaurate, glycerin tristearate, di-2-ethylhexyl phthalate, di-2-ethylhexyl adipate, etc. can be used. As the chain transfer agent, for example, octyl mercaptan, dodecyl mercaptan, α-methylstyrene dimer, etc. can be used.

[0040] Examples of phosphorus-based flame retardants that can be used include trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, tributoxyethyl phosphate, triphenyl phosphate, and tricreadyl phosphate. As the inorganic flame retardant, aluminum hydroxide, magnesium hydroxide, calcium carbonate, antimony trioxide, expandable graphite, red phosphorus, etc. can be used.

[0041] As the antistatic agent, alkyldiethanolamine, glycerin fatty acid ester, sodium alkylsulfonate, etc. can be used. As the antioxidant, phenol-based, phosphorus-based, sulfur-based, and other antioxidants can be used.

[0042] As the ultraviolet absorbing agent, a benzotriazole type, a benzophenone type, or the like ultraviolet absorbing agent can be used. As the light stabilizer, a hindered amine-based light stabilizer or the like can be used.

[0043] As the conductive filler, conductive carbon black, graphite powder, copper-zinc alloy powder, copper powder, silver powder, gold powder, etc. can be used. As the organic antibacterial agent, for example, silver-based, copper-based, zinc-based, titanium oxide-based, etc. antibacterial agents can be used. Furthermore, a rubber component such as butadiene rubber, styrene-butadiene rubber, isoprene rubber, or ethylene-propylene rubber may be added to the styrene-based monomer as long as the effect of the present invention is not impaired.

[0044] Next, in the blowing agent impregnation step, a blowing agent is added during and / or after the suspension polymerization, and the styrene-based resin particles are impregnated with the blowing agent to obtain expandable particles. The blowing agent impregnation step may be performed on resin particles in the middle of polymerization, on resin particles after polymerization, or on both. That is, the "resin particles" in the blowing agent impregnation step are a concept that includes at least either resin particles in the middle of polymerization or resin particles after polymerization. It is preferable to add the blowing agent when the polymerization conversion rate of the styrene-based monomer is 80% by mass or more. In this case, the content of unreacted styrene can be reduced.

[0045] In the foaming agent impregnation step, it is more preferable to add the foaming agent when the polymerization conversion rate of the styrene monomer is 90% by mass or more. In this case, the polymerization inhibition by the foaming agent is suppressed, so that the amount of styrene in the expandable particles is further reduced. From the viewpoint of improving this effect, the timing of adding the foaming agent is more preferably when the polymerization conversion rate is 95% by mass or more, and particularly preferably when it is 98% by mass or more. On the other hand, from the viewpoint of shortening the polymerization time and preventing, for example, the occurrence of depressions on the surface and improving the appearance of the foamed molded product, it is more preferable to add the foaming agent when the polymerization conversion rate is 99.5% by mass or less, and even more preferably when it is 99% by mass or less.

[0046] As the organic physical blowing agent, a hydrocarbon having 3 to 6 carbon atoms can be used, such as propane, n-butane, isobutane, n-pentane, isopentane, cyclopentane, n-hexane, cyclohexane, etc. These blowing agents can be used alone or in combination of two or more kinds.

[0047] In the foaming agent impregnation step, it is preferable to add butane and pentane as the foaming agent. In this case, the foaming agent can be retained well, the cells of the foamed molded article do not become too fine, and the surface depression is less likely to occur.

[0048] The content of the blowing agent in the expandable particles is preferably 2 to 10% by mass. In the blowing agent impregnation step, the blowing agent is supplied, for example, into a sealed container in such an amount that the blowing agent content in the expandable particles is 2 to 20% by mass.

[0049] The content of styrene in the expandable particles is 25 ppm by mass or less (including 0). In this case, the content of styrene in the foamed molded product can be easily reduced to, for example, 10 ppm by mass or less (including 0). From the viewpoint of more reliably reducing the content of styrene in the foamed molded product to 10 ppm by mass or less (including 0) and further reducing the amount of styrene emitted from the foamed molded product, the content of styrene in the expandable particles is more preferably 20 ppm by mass or less (including 0), and even more preferably 18 ppm by mass or less (including 0). There is no particular limit to the lower limit of the content of styrene in the expandable particles, but it is generally 5 ppm by mass or more. The content of styrene in the expandable particles can be measured using a headspace gas chromatograph mass spectrometer. As a measurement sample, a solution obtained by dissolving the expandable particles in dimethylformamide can be used.

[0050] The benzene content in the expandable particles is 1.5 ppm by mass or less (including 0). In this case, the benzene content in the foamed molded product can be easily reduced to, for example, 0.4 ppm by mass or less (including 0). From the viewpoint of more reliably reducing the benzene content in the foamed molded product to 0.4 ppm by mass or less (including 0) and further reducing the amount of benzene emitted from the foamed molded product, the benzene content in the expandable particles is more preferably 1 ppm by mass or less (including 0), and even more preferably 0.8 ppm by mass or less (including 0). There is no particular limit to the lower limit of the benzene content in the expandable particles, but it is generally 0.1 ppm by mass or more. The benzene content in the expandable particles can be measured using a headspace gas chromatograph mass spectrometer. As a measurement sample, a solution obtained by dissolving the expandable particles in dimethylformamide can be used.

[0051] The moisture content in the expandable particles is preferably 1.5% by mass or less. By using Br-SBC as a flame retardant, the moisture content in the expandable particles can be reduced to within the above range. In this case, it becomes easier to suppress the coarsening of the bubbles in the expanded particles obtained by using the expandable particles, and the maturation period until the size of the bubbles becomes uniform can be shortened. Even if the maturation period of the expandable particles is shortened, it is possible to further suppress the decrease in the mechanical strength of the expanded molded body and to further improve the appearance of the expanded molded body. The maturation period is the period during which the expandable particles are stored in a sealed container in a low-temperature environment of, for example, 10°C or less. The moisture content of the expandable particles is more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and even more preferably 0.3% by mass or less. The moisture content in the expandable particles can be determined by a Karl Fischer moisture meter equipped with a heating vaporizer.

[0052] The expandable particles are used for producing expanded particles. Specifically, the expanded particles can be obtained by carrying out an expansion step in which the expandable particles are expanded. In the expansion step, the expandable particles are heated with a heating medium such as steam to expand the particles, thereby obtaining the expanded particles. The expanded particles are also generally called pre-expanded particles. The expansion step can be carried out, for example, by supplying steam to the expandable particles introduced into a batch-type pre-expanding machine equipped with a stirrer.

[0053] The bulk density of the expanded beads can be controlled by adjusting the expansion conditions. Examples of the expansion conditions include the steam pressure (specifically, the gauge pressure) and the heating time with steam. Increasing the bulk density of the expanded beads improves the strength of the expanded molded article, while decreasing the bulk density makes it lighter and reduces the cost of raw materials. From this viewpoint, the bulk density of the expanded beads is set to 12 to 100 kg / m 3 is preferably 16 to 50 kg / m 3 More preferably, it is 20 to 50 kg / m 3 It is even more preferable that:

[0054] The bulk density of the expanded beads can be determined by the following method. The expanded beads are air-dried for a day and night, then filled into a 1-L measuring cylinder up to the 1-L standard position, and the weight of the expanded beads (=Wp) is measured to the first decimal place. The bulk density of the expanded beads (kg / m2) is calculated from the weight of the expanded beads Wp (g) using the following formula (1): 3 ) can be obtained. Bulk density of foam particles (kg / m 3 ) = Wp(g)÷1(L) (1)

[0055] The expanded beads are used to produce a foamed molded article. The molding step can be carried out by an in-mold molding method. Specifically, the expanded beads are fused together in a mold to be molded into a desired shape to obtain a foamed molded article. In the in-mold molding method, a heating medium such as steam is supplied to the expanded beads filled in the mold to heat them, thereby obtaining a foamed molded article.

[0056] Next, a preferred embodiment of the foam molded product will be described. The foam molded product uses a styrene-based resin as a base resin obtained by suspension polymerization of a styrene-based monomer in the presence of a flame retardant as described above. In the foam molded product, a large number of foam particles containing a flame retardant are fused to each other. The flame retardant contained in the foam molded product is as described above, and contains at least a brominated styrene-butadiene copolymer.

[0057] The weight average molecular weight Mw of the styrene resin in the foam molded product is preferably 150,000 or more. In this case, the strength of the foam molded product is sufficiently high. From the viewpoint of further improving the strength of the foam molded product, the weight average molecular weight Mw is preferably 180,000 or more, and more preferably 200,000 or more. From the viewpoint of improving the expandability of the expandable particles, the weight average molecular weight Mw is preferably 350,000 or less, and more preferably 300,000 or less. From the viewpoint of improving the strength of the foam molded product, the number average molecular weight Mn of the styrene resin is preferably 80,000 or more, more preferably 85,000 or more, and even more preferably 90,000 or more. From the viewpoint of improving the expandability, the number average molecular weight Mn of the styrene resin is preferably 150,000 or less, more preferably 140,000 or less, and even more preferably 120,000 or less. From the viewpoint of improving the strength of the foam molded product, the z-average molecular weight Mz of the styrene resin is preferably 300,000 or more, more preferably 400,000 or more, and even more preferably 450,000 or more. From the viewpoint of improving the expandability, the z-average molecular weight Mz of the styrene resin is preferably 700,000 or less, more preferably 600,000 or less, and even more preferably 550,000 or less. The weight-average molecular weight Mw, the number-average molecular weight Mn, and the z-average molecular weight Mz are values ​​calculated as standard polystyrene measured by gel permeation chromatography (i.e., GPC).

[0058] The styrene content in the foamed molded product is preferably 10 ppm by mass or less. In this case, the amount of styrene emitted from the foamed molded product can be sufficiently reduced. This makes the foamed molded product more suitable for use in narrow spaces such as automobile interior materials. From the same viewpoint, the styrene content in the molded product is preferably 5 ppm by mass or less. In addition, the amount of styrene emitted from the foamed molded product is preferably 50 μg / m 3 The styrene content in the foamed molded product can be measured using a headspace gas chromatograph mass spectrometer, similar to the above-mentioned expandable particles. As a measurement sample, a solution obtained by dissolving a test piece taken from the foamed molded product in dimethylformamide can be used.

[0059] The benzene content in the foamed molded product is preferably 0.4 ppm by mass or less. In this case, the amount of benzene emitted from the foamed molded product can be sufficiently reduced. This makes the foamed molded product more suitable for use in narrow spaces such as automobile interior materials. From the same viewpoint, the benzene content in the foamed molded product is preferably 0.3 ppm by mass or less. In addition, the amount of benzene emitted from the foamed molded product is 11 μg / m 3 The benzene content in the foamed molded product can be measured by the same method as that for the expandable particles described above. As a measurement sample, a dissolved material obtained by dissolving a test piece taken from the foamed molded product in dimethylformamide can be used.

[0060] The apparent density of the foamed molded body is 12 to 100 kg / m 3 In this case, it is possible to achieve both physical properties such as strength and flame retardancy of the foamed molded article and light weight. From the viewpoint of improving this effect, the apparent density of the foamed molded article is preferably 16 to 50 kg / m 3 More preferably, it is 20 to 50 kg / m 3 It is even more preferable that: The apparent density of the foamed molded article can be determined by dividing the mass of the foamed molded article by the volume determined from its outer dimensions.

[0061] The foam molded article is used for interior and exterior materials for vehicles such as automobiles, insulation materials for homes, cold storage boxes, etc. The foam molded article has excellent flame retardancy and a low content of styrene and benzene, and is therefore suitable for interior materials for vehicles, and is particularly suitable for debia pads and floor spacers. EXAMPLES

[0062] Examples and comparative examples of the expandable particles and the foamed molded article will be described below.

[0063] Example 1 The manufacturing method of the expandable particles and the expanded molded article of this example will be described below. First, 16 kg of deionized water, 14.4 g of tribasic calcium phosphate (suspending agent), 0.6 g of sodium α-olefin sulfonate (surfactant), 0.2 g of disodium alkylbiphenyl disulfonate (surfactant), and 24.4 g of sodium acetate (electrolyte) were charged into an autoclave equipped with a stirrer and having an internal volume of 50 L. Next, 43.2 g of t-butylperoxy-2-ethylhexanoate ("Perbutyl O" manufactured by NOF Corp., first polymerization initiator), which is an organic peroxide having a 10-hour half-life temperature of 72.1°C, 25.6 g of t-butylperoxy-2-ethylhexyl monocarbonate ("Perbutyl E" manufactured by NOF Corp., second polymerization initiator), which is an organic peroxide having a 10-hour half-life temperature of 99°C, and 25.6 g of brominated styrene-butadiene block copolymer ("Emerald Innovation Polymer" manufactured by Chemtura Japan Co., Ltd.) were added. 12.8g of dicumyl peroxide (NOF Corp.'s "Percumyl D", flame retardant), 51.2g of dicumyl peroxide, an organic peroxide with a half-life temperature of 136°C (NOF Corp.'s "Percumyl D", flame retardant), 128g of liquid paraffin (MORESCO Corp.'s "Moresco White P-60", plasticizer), 3.2g of polyethylene wax powder (TOYO ADOLE Corp.'s "Polyethylene Wax 1000", cell regulator), and 0.32g of 4-t-butylcatechol (DIC Corp.'s "DIC-TBC", polymerization inhibitor) were mixed with 16kg of styrene, and the mixture was stirred at a rotation speed of 210 rpm and put into an autoclave. The flame retardant used in this example will be referred to as "E3000" hereinafter.

[0064] Next, the air in the autoclave was replaced with nitrogen, and the temperature was raised to 90°C over 1.5 hours. After reaching the temperature of 90°C, the temperature in the autoclave was further raised to 100°C over 6 hours and 30 minutes (first-stage polymerization step). Thereafter, the temperature in the autoclave was further raised to 120°C over 2 hours, and the autoclave was kept at the temperature of 120 for 5 hours (second-stage polymerization step). Thereafter, the temperature was cooled to 30°C over about 6 hours. During the temperature rise from the above-mentioned temperature 90°C to the temperature 100°C, 5 hours and 30 minutes after reaching 90°C, 320g of pentane (a mixture of 80% n-pentane and 20% isopentane) and 880g of butane (a mixture of 70% n-butane and 30% isobutane) were injected into the autoclave as a blowing agent over 30 minutes. At the start of the addition of the blowing agent, i.e., 5 hours and 30 minutes after the temperature reached 90°C, the polymerization conversion rate of styrene was 98% by mass. At the end of the first polymerization step, i.e., when the temperature reached 100°C, the polymerization conversion rate of styrene was 99% by mass. The method for measuring each polymerization conversion rate is described below. The polymerization rate up to a polymerization conversion rate of 90% was 15% / hr. The method for measuring the polymerization rate is described below.

[0065] After cooling, the contents (expandable particles) were removed from the autoclave, and in order to remove the tribasic calcium phosphate adhering to the surface of the expandable particles, nitric acid was added to the expandable particles, which were then dehydrated using a centrifuge and the moisture adhering to the surface was removed using a fluidized bed dryer. In this way, expandable particles with an average particle size of about 1.0 mm were obtained.

[0066] Next, the expandable particles were sieved to select and take out particles of 0.5 to 1.4 mm. Then, 0.005 parts by mass of N,N-bis(2-hydroxyethyl)alkylamine (antistatic agent) was added to 100 parts by mass of the expandable particles to coat the expandable particles with an antistatic agent. Furthermore, 0.1 parts by mass of zinc stearate, 0.05 parts by mass of glycerin tristearate, and 0.05 parts by mass of glycerin monostearate were added to 100 parts by mass of the expandable particles to coat the expandable particles with the mixture. Then, the expandable particles were placed in a sealed container and stored in a refrigerator at 6°C to allow maturation.

[0067] The polymerization conditions for the expandable particles are shown in Table 1. The polymerization conversion rate was measured as follows.

[0068] "Polymerization conversion rate at the end of the first polymerization step" A separate first-stage polymerization step was carried out under the same conditions as the first-stage polymerization step carried out when the expandable particles were produced. At the same time as the first-stage polymerization step was completed, the temperature of the contents of the autoclave was rapidly cooled to 30°C or less within 10 minutes to stop the polymerization reaction. After cooling, the styrene resin particles in the middle of polymerization were taken out of the autoclave, dehydrated with a centrifuge, and the moisture attached to the surface was removed with a fluidized dryer. In this way, the styrene resin particles at the end of the first-stage polymerization step were obtained, and the content of unreacted styrene monomer in the obtained styrene resin particles was determined by gas chromatography. The method for measuring the content of styrene monomer by gas chromatography will be described later. Then, the polymerization conversion rate was calculated from the following formula (2). This operation was carried out three times, and the arithmetic average value of each polymerization conversion rate was calculated. Polymerization conversion rate (mass%) = 100 - styrene monomer content (mass%) (2)

[0069] "Polymerization conversion rate when foaming agent is impregnated" Polymerization was carried out separately under the same conditions as those for producing the expandable particles, and the temperature of the contents of the autoclave was rapidly cooled to 30°C or less within 10 minutes immediately before the start of the addition of the blowing agent to terminate the polymerization reaction. The polymerization conversion rate at the time of impregnation with the blowing agent was then determined by carrying out the same operation as that for measuring the polymerization conversion rate at the end of the above-mentioned first-stage polymerization step. This operation was carried out three times, and the arithmetic average value of each polymerization conversion rate is shown in the table.

[0070] "Polymerization rate up to 90% polymerization conversion" Polymerization was carried out separately under the same conditions as those for producing the expandable particles, and the temperature of the contents of the autoclave was rapidly cooled to 30°C or less within 10 minutes after the temperature of the autoclave was increased and any time had elapsed, to stop the polymerization reaction. The polymerization conversion rate was then determined by the same method as the method for measuring the polymerization conversion rate at the end of the first-stage polymerization process described above. This operation was carried out at multiple time intervals, and a diagram was created in which the relationship between the polymerization conversion rate and the time required to reach that polymerization conversion rate was plotted. The time (hr: hour) required for the polymerization conversion rate to reach 90% was then determined from the relationship between the obtained polymerization conversion rate and the time required to reach that polymerization conversion rate. The polymerization rate until the polymerization conversion rate reached 90% was determined by dividing the polymerization conversion rate of 90% by the time (hr: hour) required for the polymerization conversion rate to reach 90%.

[0071] The expandable particles of this example were measured for the blowing agent content, styrene content, benzene content, water content (i.e., WC), average particle diameter d63, average particle diameter variation, average molecular weight of the styrene resin, and expandability. The results are shown in Table 3.

[0072] "Foaming agent content" The content of the blowing agent was measured by performing gas chromatography on the solution obtained by dissolving the expandable particles in dimethylformamide (DMF). Specifically, first, about 5 g of cyclopentanol was precisely weighed out to three decimal places in a 100 ml measuring flask. This weight is hereinafter referred to as Wi (g). Furthermore, DFM was added to the measuring flask to make the total volume 100 mL. This DMF solution was further diluted 100 times with DMF. This was used as the internal standard solution. Next, about 1 g of the expandable particles to be measured was precisely weighed out to three decimal places. This weight is hereinafter referred to as Ws (g). The precisely weighed sample of the expandable particles was dissolved in about 18 ml of DMF, and then 2 ml of the internal standard solution was added using a whole pipette. 1 μL of the solution thus obtained was collected using a microsyringe and introduced into gas chromatography to obtain a chromatogram. The peak areas of the foaming agent components and the internal standard were determined from the obtained chromatogram, and the concentrations of each component were calculated from the following formula (4).

[0073] Component concentration (mass%)=(Wi / 10000)2×(An / Ai)×Fn / Ws×100 (4) Wi: weight (g) of cyclopentanol when the internal standard solution was prepared, Ws: weight (g) of the sample dissolved in DMF, An: peak area of ​​each component during gas chromatographic measurement, Ai: peak area of ​​the internal standard substance during gas chromatographic measurement, Fn: correction coefficient of each component obtained from the calibration curve prepared in advance.

[0074] The analysis conditions for the gas chromatograph are as follows: Equipment used: Shimadzu Corporation gas chromatograph GC-6AM Detector: FID (Flame Ionization Detector) Column material: Glass column with inner diameter of 3 mm and length of 5000 mm Column packing material: [Liquid phase name] FFAP (free fatty acids), [Liquid phase content] 10% by mass, [Carrier name] Chomasorb W, diatomaceous earth for gas chromatography, [Carrier particle size] 60 / 80 mesh, [Carrier treatment method] AW-DMCS (washed with water, calcined, acid treated, silane treated), [Packing volume] 90 ml Inlet temperature: 250℃ Column temperature: 120℃ Detector temperature: 250℃ Carry gas: N2 Fluid volume: 40ml / min

[0075] "Styrene content, benzene content" The contents of unreacted styrene monomer and benzene in the expandable particles were measured using a gas chromatograph mass spectrometer using the headspace method. As a sample, a solution obtained by dissolving the expandable particles in dimethylformamide (i.e., DMF) was used. Specifically, first, a standard solution was prepared so that the styrene or benzene concentration in DMF was 5 mass ppm, 50 mass ppm, and 500 mass ppm. Next, 0.2 g of the standard solution was precisely weighed into a 20 ml vial, 1 ml of DMF was poured in, and the vial was sealed. The vial was kept warm in a headspace sampler, and the gas phase was measured using a gas chromatograph mass spectrometer, and a calibration curve was created from the obtained chromatogram. Next, 0.2 g of the sample was precisely weighed into a 20 ml vial, 1 ml of DMF was poured in, the vial was sealed, and the vial was kept at room temperature for one day to completely dissolve it. The mixture was kept warm in a headspace sampler, and the gas phase was measured with a gas chromatograph mass spectrometer. The contents of unreacted styrene and benzene were determined from a calibration curve previously prepared from the obtained chromatogram.

[0076] The conditions of gas chromatography mass spectrometry for measuring the styrene content and the benzene content are as follows. Gas chromatograph mass spectrometer: Shimadzu Corporation GCMS-QP2020 Headspace sampler: Shimadzu Corporation HS-20 Capillary column: GL Sciences, Stabilwax, inner diameter 0.32 mm, length 30 m Headspace sampler incubation conditions: 90℃ for 1 hour Column temperature: 50°C, 2 minutes ⇒ (heating rate: 10°C / min) ⇒ 90°C ⇒ (heating rate: 5°C / min) ⇒ 120°C ⇒ (heating rate: 20°C / min) ⇒ 230°C, 2 minutes Ion source temperature: 200℃ Carry gas: Helium Carrier gas column flow rate: 2 ml / min Split ratio: 1 / 10

[0077] "Moisture content" The moisture content of the expandable particles was measured using a Karl Fischer moisture meter. Specifically, about 0.28 g of the expandable particle sample was precisely weighed. Next, the sample was heated at a temperature of 160°C using a moisture vaporizer CHK-501 manufactured by Kyoto Electronics Manufacturing Co., Ltd. to vaporize the moisture, and the moisture content was measured using a Karl Fischer moisture meter (coulometric titration method) MKC-610 manufactured by Kyoto Electronics Manufacturing Co., Ltd.

[0078] "Molecular weight" The molecular weight (number average molecular weight, weight average molecular weight, Z-average molecular weight) of the styrene resin in the expandable particles can be measured by gel permeation chromatography (GPC) using polystyrene as a standard substance. Specifically, the measurement was performed using HLC-8320GPC EcoSEC manufactured by Tosoh Corporation under the following measurement conditions: eluent: tetrahydrofuran (THF), THF flow rate: 0.6 ml / min, sample concentration: 0.1 wt%. As the column, one TSKguardcolumn SuperH-H and two TSK-GEL SuperHM-H columns connected in series were used. That is, the test piece taken from the expandable particles was dissolved in tetrahydrofuran (THF), and the molecular weight was measured by gel permeation chromatography (GPC). The measured value was calibrated with standard polystyrene to determine the number average molecular weight, weight average molecular weight, and Z-average molecular weight, respectively.

[0079] "Average particle size, dispersity" The 63% volume average particle diameter d63, 90% volume average particle diameter d90, and 10% volume average particle diameter d10 of the expandable particles were measured. The 63% volume average particle diameter d63, 90% volume average particle diameter d90, and 10% volume average particle diameter d10 are the particle diameters at 63%, 90%, and 10% of the volume accumulated value, respectively, in the particle size distribution obtained by the laser diffraction / scattering method. The average particle diameter value in the table indicates the value of the 63% volume average particle diameter d63. The specific measurement method is as follows. The particle size distribution of the expandable particles was measured using a particle size distribution measuring device "Militrack JPA" manufactured by KISO Co., Ltd. Specifically, 30 g of expandable particles were allowed to fall freely from the sample supply feeder of the measuring device, and the projected image was captured by a CCD camera. Next, calculation and combination processing was performed sequentially on the captured image information, and measurements were performed under the conditions of an image analysis method that outputs particle size distribution and shape index results. In this way, the particle sizes (d10, d63, d90) mm at volumetric integrated values ​​of 10%, 63%, and 90% in the particle size distribution were obtained. From these values, the dispersity of the 63% average particle size was calculated based on the following formula (5). Note that the average particle size is for expandable particles immediately after production, and is a value for expandable particles that have not been classified by sieving or the like. The smaller the dispersity value, the smaller the particle size variation. Dispersion index of 63% volume average particle size = (d90-d10) / d63 (5)

[0080] "Effervescent" The expandable particles that had completed the aging were expanded in a shelf-type expansion machine by heating them with steam at 3 kPa (gauge pressure) for 270 seconds. The expanded particles were then air-dried for one day and night. The expanded particles were then filled into a 1-L measuring cylinder up to the standard 1-L position, and the weight of the expanded particles (=Wp) was measured to one decimal place. The bulk density (Kg / m) of the expanded particles was calculated from the weight Wp (g) of the expanded particles using the following formula (5): 3 The expandability was determined from the bulk density of the expanded beads. Bulk density of foam particles (Kg / m 3 ) = Wp(g)÷1(L) (5)

[0081] Next, 3.6 kg of the aged expandable particles were placed in a pressurized batch expansion machine (DYHL-500U, manufactured by Daisen Kogyo Co., Ltd.), and heated for 130 seconds by supplying steam at a gauge pressure of 0.15 MPa so that the pressure (gauge pressure) inside the expansion machine became 0.023 MPa. The expansion ratio was about 50 times (bulk density: 20 kg / m 3 ) foam particles were obtained.

[0082] Next, the expanded beads were aged at room temperature (specifically, 23°C) for one day, then filled into the mold of a molded product molding machine manufactured by DABO Co., Ltd., and heated for 15 seconds at a steam pressure of 0.08 MPa (gauge pressure). Then, after cooling for a predetermined time, the expanded molded product was removed from the mold. In this way, a 300 mm x 300 mm x 25 mm plate-shaped expanded molded product in which a large number of expanded beads were fused to each other was obtained. Next, the apparent density, the content of unreacted styrene and benzene, the amount of styrene and benzene emitted, and the bending strength of the expanded molded product were measured, and the flame retardancy (specifically, burning rate and self-extinguishing property) and moldability were evaluated. The results are shown in Table 3.

[0083] "Apparent density" The apparent density was calculated by dividing the mass of the foamed molded article by the volume determined from its outer dimensions.

[0084] "Styrene and benzene content" The sample was measured in the same manner as in the case of the expandable granules, except that a solution obtained by dissolving a part of the foamed molded article in dimethylformamide (ie, DMF) was used.

[0085] "Styrene and benzene emissions" A foam molded body was produced under the same molding conditions as above, except that a molded die for molding a plate-shaped foam molded body with dimensions of 100 mm x 80 mm x 15 mm was used. This foam molded body was dried at 40°C for one day. Thereafter, the foam molded body was placed in a 10 L Tedlar (registered trademark) bag, and the gas (specifically, air) in the bag was expelled by nitrogen purging three times, after which 4 L of nitrogen was injected into the bag and the temperature was kept at 40°C for two hours. Styrene and benzene generated from the foam molded body were collected in a Tenax-TA collection tube. The flow rate to the collection tube was 0.1 ml / min, and the collected amount was 1.0 L. Next, the styrene and benzene in the collection tube were quantified using a thermal desorption-gas chromatograph mass spectrometer, and the amount of styrene and benzene per 1 m of gas was measured. 3 The amount of styrene and benzene per unit (unit: μg / m 3 ) was calculated. 3 If it was less than 5, it was indicated in the table as "<5."

[0086] "Flame retardancy (burning speed)" The evaluation of the burning rate was performed in accordance with FMVSS No. 302. Specifically, the foam molded body was first left at a temperature of 40°C for three days and then at room temperature for one day to allow maturation. The foam molded body was then left at a temperature of 40°C for three days and then at room temperature for one day to allow curing. Five flat test pieces measuring 356 mm long x 102 mm wide x 13 mm thick were then cut out from the foam molded body, and a burning test was performed using an MVSS flammability tester MVSS-2 manufactured by Suga Test Instruments Co., Ltd. Specifically, the test piece was fixed horizontally to a U-shaped fixture, and the free end of the test piece was exposed to the flame of a Bunsen burner with the flame length adjusted to 38 mm for 15 seconds to ignite the test piece. The time required for the test piece to burn from the fixed end located on the opposite side of the free end to a point 38 mm away was measured, and the burning rate (mm / min) was calculated from the burning distance and burning time. If the specimen did not reach the specified end, the burning rate was calculated from the burning distance to the point where the flame stopped and the burning time. If the specimen did not ignite, the burning rate was set to 0 mm / min. The arithmetic average of the burning rates of the five specimens was taken as the burning rate, and compliance with FMVSS No. 302 (burning rate of 102 mm / min or less) was determined.

[0087] "Flame retardant (self-extinguishing)" The self-extinguishing property of the foam molded body was evaluated based on the combustion test (A method) of JIS A 9511:2006R. Specifically, the foam molded body was first left at a temperature of 40°C for 3 days and then left at room temperature for 1 day to cure. Then, five rectangular parallelepiped test pieces measuring 200 mm long x 25 mm wide x 10 mm thick were cut out from the foam molded body. Next, the test pieces were ignited using a candle up to the ignition limit indicator line and the flammability limit indicator line, and the candle was quickly moved back from the test pieces. Then, the time from the moment the candle was moved back to the time the flame of the test pieces went out (extinguishing time) was measured, and the arithmetic average of the extinction times of the five test pieces was calculated. The self-extinguishing property (extinguishing time of 3 seconds or less) was judged from the arithmetic average value of the extinction time. In addition, when the extinction time exceeded 10 seconds, it was indicated as ">10" in the table.

[0088] "Bending strength" The foam molded article was cut to prepare a rectangular parallelepiped test piece measuring 300 mm in length, 75 mm in width, and 25 mm in thickness. A three-point bending test was performed on the test piece in accordance with JIS K 7221-2 Appendix 1, and the mechanical strength of the foam molded article was evaluated by measuring the bending strength.

[0089] "Moldability" The surface of the foamed molded article was visually inspected, and the absence of depressions was rated as "◯ (absent)", while the presence of depressions was rated as "× (present)".

[0090] (Examples 2 to 9) The polymerization conditions were changed as shown in Tables 1 and 2, and the same measurements and evaluations as in Example 1 were performed. In Example 4, the expansion ratio of the expanded beads was set to 30 times, and the expanded molded article was evaluated. In Example 5, the expansion ratio of the expanded beads was set to 20 times, and the expanded molded article was evaluated. In Example 6, the first polymerization initiator was changed from t-butylperoxy-2-ethylhexanoate ("Perbutyl O" manufactured by NOF Corp.) having a 10-hour half-life temperature of 72.1°C to 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate ("Perocta O" manufactured by NOF Corp.) having a 10-hour half-life temperature of 65.3°C. In Example 7, the first polymerization initiator was changed from t-butylperoxy-2-ethylhexanoate ("Perbutyl O" manufactured by NOF Corp.) having a 10-hour half-life temperature of 72.1°C to 1,1-bis(t-butylperoxy)cyclohexane ("Perhexa HC" manufactured by NOF Corp.) having a 10-hour half-life temperature of 87.1°C. In Example 8, the temperature was raised to 100°C over 1.5 hours, and after reaching the temperature of 100°C, the temperature inside the autoclave was further raised to 110°C over 6 hours and 30 minutes. Thereafter, the temperature inside the autoclave was further raised to 120°C over 2 hours, and the autoclave was maintained at the temperature of 120 for 5 hours. Thereafter, the temperature was cooled to 30°C over about 6 hours. During the temperature increase from 100°C to 110°C, 5 hours and 30 minutes after reaching 100°C, the flow was changed to injecting 320 g of pentane (a mixture of 80% n-pentane and 20% isopentane) and 880 g of butane (a mixture of 70% n-butane and 30% isobutane) into the autoclave over a period of 30 minutes as a blowing agent.

[0091] Comparative Example 1 In this example, the same procedure as in Example 1 was carried out except that no polymerization inhibitor was used and t-butylperoxy-2-ethylhexanoate ("Perbutyl O" manufactured by NOF Corp.) was used as the first polymerization initiator and benzoyl peroxide ("Niper BW" manufactured by NOF Corp., water-dilutable powder product, polymerization initiator) was used.

[0092] (Comparative Example 2 and Comparative Example 3) Comparative Examples 2 and 3 are examples in which the amount of foaming agent added was changed from that of Comparative Example 1. Specifically, Comparative Example 2 was performed in the same manner as Comparative Example 1, except that no polymerization inhibitor was used, and 320 g of pentane (a mixture of 80% n-pentane and 20% isopentane) and 928 g of butane (a mixture of 70% n-butane and 30% isobutane) were used as the foaming agent. Comparative Example 3 was performed in the same manner as Comparative Example 1, except that no polymerization inhibitor was used, and 320 g of pentane (a mixture of 80% n-pentane and 20% isopentane) and 976 g of butane (a mixture of 70% n-butane and 30% isobutane) were used as the foaming agent.

[0093] Comparative Example 4 No polymerization inhibitor was used, and the air in the autoclave was replaced with nitrogen, after which the temperature was raised to 90°C over 1.5 hours, and after the polymerization temperature reached 90°C, the temperature in the autoclave was raised to 100°C over 6 hours and 30 minutes, all of which were carried out in the same manner as in Comparative Example 1. The temperature was then further raised to 115°C over 2 hours, and the temperature was maintained at 115°C for 5 hours. Thereafter, the temperature was cooled to 30°C over approximately 6 hours. The cooling operation and subsequent steps were carried out in the same manner as in Comparative Example 1.

[0094] Comparative Example 5 In this example, the same procedure as in Comparative Example 1 was carried out except that no polymerization inhibitor was used and 160 g of 2,2-bis(4'-(2",3"-dibromo-2"-methylpropoxy-3',5'-dibromophenyl)propane was used as the flame retardant. The flame retardant used in this example will hereinafter be referred to as "SR130" where appropriate.

[0095] Comparative Example 6 In this example, the same procedure as in Comparative Example 1 was carried out except that 160 g of SR130 was used as the flame retardant and Perbutyl O was used as the first polymerization initiator.

[0096] Comparative Example 7 In this example, the same procedure as in Comparative Example 1 was carried out except that no polymerization inhibitor was used, and the flame retardant, the first polymerization initiator, and the second polymerization initiator were added to the aqueous phase without being dissolved in the styrene-based monomer.

[0097] Comparative Example 8 In this example, the flame retardant, the first polymerization initiator, and the second polymerization initiator were added to the aqueous phase without being dissolved in the styrene monomer, and Perbutyl O was used as the first polymerization initiator. Then, after the air in the autoclave was replaced with nitrogen, the temperature was raised to 90°C over 1.5 hours, and after the polymerization temperature reached 90°C, the temperature in the autoclave was raised to 100°C over 6 hours and 30 minutes in the same manner as in Comparative Example 1. Next, the temperature was further raised to 115°C over 2 hours, and the temperature was kept at 115°C for 5 hours. Then, it was cooled to 30°C over about 6 hours. The cooling operation and subsequent operations were performed in the same manner as in Comparative Example 1.

[0098] Comparative Example 9 Comparative Example 9 is an example in which the timing of adding the foaming agent was changed from that of Comparative Example 1. Specifically, Comparative Example 9 was carried out in the same manner as Comparative Example 1, except that the timing of adding the foaming agent was changed from 5.5 hours to 6.5 hours after the temperature reached 90°C.

[0099] Comparative Example 10 In this example, the same procedures as in Example 1 were carried out except that t-butylperoxyisopropyl monocarbonate ("Perbutyl I" manufactured by NOF Corporation) was used as the first polymerization initiator.

[0100] The details of the organic peroxides in the table are as follows: Perbutyl O is t-butylperoxy-2-ethylhexanoate, and its structure is represented by the following structural formula (1).

[0101] [ka]

[0102] Perhexa HC (manufactured by NOF Corporation) is 1,1-di(t-hexylperoxy)cyclohexane, and its structure is represented by the following structural formula (3).

[0103] [ka]

[0104] BPO (specifically, NOF Corp.'s "Niper BW", a water-dilutable powder product) is dibenzoyl peroxide, and its structure is represented by the following structural formula (3).

[0105] [ka]

[0106] Perbutyl I (manufactured by NOF Corporation) is t-butylperoxyisopropyl monocarbonate, and its structure is represented by the following structural formula (4).

[0107] [ka]

[0108] Perbutyl E (manufactured by NOF Corporation) is t-butylperoxy-2-ethylhexyl monocarbonate, and its structure is represented by the following structural formula (5).

[0109] [ka]

[0110] Perocta O (manufactured by NOF Corporation) is 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, and its structure is represented by the following structural formula (6).

[0111] [ka]

[0112] For each of the Examples and Comparative Examples, the polymerization conditions, the properties of the expandable particles, and the results of the expansion / molding evaluation are shown in Tables 1 to 6.

[0113] [Table 1]

[0114]

Table 2

[0115]

Table 3

[0116]

Table 4

[0117]

Table 5

[0118]

Table 6

[0119] As can be seen from Tables 1 to 3, Examples 1 to 5 and Example 8 are examples in which a polymerization inhibitor is used and t-butylperoxy-2-ethylhexanoate is used as the first polymerization initiator, Example 9 is an example in which a polymerization inhibitor is not used and t-butylperoxy-2-ethylhexanoate is used as the first polymerization initiator, Example 6 is an example in which a polymerization inhibitor is used and 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate is used as the first polymerization initiator, and Example 7 is an example in which a polymerization inhibitor is used and 1,1-di(t-hexylperoxy)cyclohexane is used as the first polymerization initiator. The expandable particles and expanded molded products of Examples 1 to 9 have low contents of styrene and benzene. Therefore, the amount of styrene and benzene emitted from the expanded molded products is low. In addition, since the weight average molecular weight of the styrene resin is maintained at 150,000 or more, it has excellent bending strength, contains brominated styrene-butadiene copolymer as a flame retardant, and complies with the flammability test of FMVSS No 302. Example 3 is an example in which the amount of flame retardant is increased, and also passed the flammability test (Method A) of JIS A 9511:2006R.

[0120] In particular, when t-butylperoxy-2-ethylhexanoate is used as the first polymerization initiator and t-butylperoxy-2-ethylhexyl monocarbonate is used as the second polymerization initiator, the degree of dispersion is small and the particle size variation of the resulting expandable particles is small. Also, when t-butylperoxy-2-ethylhexanoate is used as the first polymerization initiator and a polymerization inhibitor is added, the degree of dispersion is small and the particle size variation of the resulting expandable particles is small.

[0121] On the other hand, as can be seen from Tables 4 to 6, Comparative Examples 1 to 4, 7, and 9, in which benzoyl peroxide ("Niper BW" manufactured by NOF Corporation, a water-dilutable powder product) was used as the first polymerization initiator, had a low styrene content and a low amount of styrene-based monomer emissions, but a high benzene content and a high amount of benzene emissions.

[0122] Comparative Examples 5 and 6 are examples in which 2,2-bis(4'-(2",3"-dibromo-2"-methylpropoxy-3',5'-dibromophenyl)propane was used as the flame retardant. In these cases, the polymerization of the styrene monomer in the polymerization step was easily inhibited, and the styrene content in the expandable particles increased. Thus, the styrene content in the foamed molded product also increased. In addition, since the weight-average molecular weight of the styrene resin is low at 140,000, the mechanical strength of the foamed molded product, such as bending strength, is low. In Comparative Examples 5 and 6, no high benzene content was detected.

[0123] Comparative Examples 7 and 8 are examples in which a flame retardant was added to the aqueous phase and suspension polymerization was carried out. In this case, the burning rate was high and the flame retardancy was insufficient. This is considered to be because the flame retardant was difficult to be sufficiently blended into the interior of the expandable particles. In addition, the moldability was not evaluated sufficiently. Comparative Example 10 is an example in which an organic peroxide with a high 10-hour half-life temperature was used as the first polymerization initiator. As a result, polymerization inhibition was likely to occur, and the styrene content in the expandable particles was high.

Claims

1. A method for producing expandable styrene-based resin particles containing a flame retardant and a blowing agent, comprising: a polymerization step of adding a styrene-based monomer containing styrene, in which the flame retardant and a polymerization initiator are dissolved, to an aqueous medium, and carrying out suspension polymerization of the styrene-based monomer in the aqueous medium to obtain styrene-based resin particles containing the flame retardant, In the polymerization step, a first organic peroxide of an aliphatic peroxyester type and / or an aliphatic peroxyketal type having a 10-hour half-life temperature of 65° C. or more and 90° C. or less and a second organic peroxide having a 10-hour half-life temperature of more than 90° C. and 110° C. or less are used as a polymerization initiator, The flame retardant is a brominated styrene-butadiene copolymer, The blending amount of the flame retardant is 0.05 to 2 parts by mass per 100 parts by weight of the styrene-based monomer, The method for producing expandable styrene-based resin particles, wherein the expandable styrene-based resin particles have a styrene content of 25 ppm by mass or less (including 0) and a benzene content of 1.5 ppm by mass or less (including 0).

2. 2. The method for producing expandable styrene-based resin particles according to claim 1, wherein the phenylacetylene concentration in the styrene-based monomer is 5 ppm by mass or more and 20 ppm by mass or less.

3. 3. The method for producing expandable styrene-based resin particles according to claim 1 or 2, wherein the second organic peroxide is an aliphatic peroxydicarbonate-type and / or aliphatic peroxyester-type organic peroxide having a 10-hour half-life temperature 10° C. or more higher than that of the first organic peroxide.

4. The method for producing expandable styrene-based resin particles according to any one of claims 1 to 3, wherein the polymerization step comprises a first-stage polymerization step of polymerizing the styrene-based monomer at a temperature of 110°C or less until a polymerization conversion rate reaches 90% by mass or more, and a second-stage polymerization step of polymerizing the styrene-based monomer at a temperature of more than 115°C and 135°C or less until a content of unreacted styrene reaches 25 ppm by mass or less (including 0).

5. The method for producing expandable styrene-based resin particles according to any one of claims 1 to 4, wherein the first organic peroxide is t-butylperoxy-2-ethylhexanoate, and the second organic peroxide is t-butylperoxy-2-ethylhexyl monocarbonate.

6. The method for producing the expandable styrene-based resin particles according to any one of claims 1 to 5, further comprising a blowing agent impregnation step of adding the blowing agent when the polymerization conversion rate of the styrene-based monomer is 90 mass% or more, and impregnating the styrene-based resin particles with the blowing agent.

7. 7. The method for producing expandable styrene-based resin particles according to claim 6, wherein butane and pentane are added as the foaming agent in the foaming agent impregnation step.

8. The method for producing expandable styrene-based resin particles according to any one of claims 1 to 7, wherein in the polymerization step, suspension polymerization is carried out under conditions such that a polymerization rate until a polymerization conversion rate of the styrene-based monomer reaches 90% is 14% / hr or more and 18% / hr or less.

9. The method for producing expandable styrene-based resin particles according to any one of claims 1 to 8, wherein the styrene-based monomer is subjected to suspension polymerization in the presence of a polymerization inhibitor.

Citation Information

Patent Citations

  • Styrene-based foaming resin particulate

    JP1999106548A

  • Expanded styrene resin bead and molded object formed from expanded styrene resin bead

    JP2009108237A

  • Foamable styrene resin particle and production method therefor

    JP2016037573A

  • Manufacturing method of expandable styrene resin particle to which flame retardancy is added

    JP2017071669A

  • Method of producing expandable styrenic resin particles

    JP2020147668A