Toughened degradable polyglycolic acid composition, toughened degradable polyglycolic acid material, and method for preparing same and use thereof
A composition of polyglycolic acid, biodegradable polyester, and compatibilizers forms a network structure to enhance toughness and processability, addressing the low toughness and melt strength issues of polyglycolic acid materials, resulting in improved mechanical properties and biodegradability.
Patent Information
- Application Number
- JP2023506198
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-19
- Filing Date
- 2021-07-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-07-19
AI Technical Summary
Polyglycolic acid materials suffer from low toughness, low melt strength, and poor processability, and the addition of non-degradable resins during modification leads to material deterioration.
A composition comprising polyglycolic acid, biodegradable polyester, and a compatibilizer, such as an epoxy compound, maleic anhydride graft polymer, or isocyanate compound, is melt-extruded to form a network structure, enhancing compatibility and toughness, and improving melt strength and processability.
The resulting toughened degradable polyglycolic acid material exhibits increased notch impact strength, elongation at break, and improved processing performance, with enhanced melt strength and biodegradability.
Smart Images

Figure 0007588708000005 
Figure 0007588708000006 
Figure 0007588708000007
Abstract
Description
Detailed Description of the Invention
[0001] Related Applications This application claims the benefit of Chinese patent application No. 202010837326.5, filed on Aug. 19, 2020, the contents of which are incorporated herein by reference.
[0002] [Technical field] The present invention relates to the field of polyglycolic acid modification, specifically to a toughened degradable polyglycolic acid composition, a toughened degradable polyglycolic acid material and its preparation method and application.
[0003] [Background technology] Polyglycolic acid (PGA for short) is an aliphatic polyester polymer with the smallest carbon number, a completely degradable ester structure, and the fastest decomposition rate. It can be biodegraded and hydrolyzed, is non-toxic, and is eventually decomposed into water and carbon dioxide, so it is recognized worldwide as a material that protects the global environment and life. Polyglycolic acid has excellent mechanical properties, and its flexural strength and tensile strength are higher than those of ordinary resins and superior to many engineering plastics. Due to its excellent biocompatibility, PGA is widely used in high-value-added products such as medical absorbable surgical sutures, drug release, simulated human tissue materials, and biodegradable polymer scaffolds. However, PGA has the disadvantages of being brittle and having low melt strength, which greatly restricts its processing applications in many fields. Therefore, it is very important to toughen and modify PGA and prepare high-toughness PGA materials. However, there is currently little research on the toughening and modification of PGA.
[0004] CN102993654A discloses a biodegradable barrier film, the preparation raw materials include, in mass%, 0-80wt% biodegradable homopolyester, 0-80wt% biodegradable copolyester, 1-30wt% ethylene-vinyl alcohol copolymer, and 0-5wt% additives, the biodegradable homopolyester is obtained by condensation reaction or ring-opening polymerization reaction from hydroxy fatty acid monomer, and the biodegradable copolyester is obtained by polymerization reaction from dibasic monomer and aliphatic diol. It is used to overcome the drawback that biodegradable film does not have barrier property. However, there is no content about toughening or weight increase.
[0005] CN107083032A discloses a method for preparing a biodegradable polylactic acid-based composite material with high strength and high toughness by a crosslinking reaction during processing and extrusion, the biodegradable polylactic acid-based composite material includes, by weight fraction, 60-100 parts of polylactic acid, 5-60 parts of biodegradable polyester, and 3-20 parts of polyol or polyol ether crosslinker, the biodegradable polylactic acid-based composite material is prepared by a melt-kneading-extrusion method, specifically, the steps include: (1) uniformly mixing dry polylactic acid resin, biodegradable polyester, and polyol or polyol ether crosslinker; and (2) adding the mixture obtained in step (1) to a twin-screw extruder and extruding by melt-kneading reaction. This invention solves the problem that the compatibility and strength of polylactic acid materials are reduced by the addition of flexible polyester in the preparation of polylactic acid-based composite materials. This patent is mainly related to crosslinking using polyol and polyether, which is significant for improving strength and not so much for improving toughness.
[0006] CN107987494A discloses a biodegradable polyethylene terephthalate blend, which contains, by weight, 50-70 parts polyethylene terephthalate, 10-40 parts polyglycolic acid, 5-10 parts compatibilizer, 0.1-0.5 parts antioxidant, and 1-2 parts hydrolysis inhibitor. However, this patent only adds polyglycolic acid to improve the decomposition performance of PET, and does not necessarily improve the toughness of the material. Furthermore, since PET itself is not biodegradable, it also affects the complete biodegradability of the entire material.
[0007] At present, polyglycolic acid materials need to solve the problems of toughening the materials and improving their compatibility, and there is a need to develop highly tough degradable materials.
[0008] Summary of the Invention The object of the present invention is to overcome the problems of conventional polyglycolic acid materials, such as low toughness, low melt strength, low processability, and deterioration and destruction due to decomposition of the material itself caused by the addition of a non-degradable resin in modification, and to provide a toughened degradable polyglycolic acid composition, a toughened degradable polyglycolic acid material, and a method for preparing and use thereof.
[0009] In order to achieve the above object, a first aspect of the present invention provides a toughened degradable polyglycolic acid composition comprising polyglycolic acid, a biodegradable polyester, and a compatibilizer, wherein the biodegradable polyester comprises a biodegradable homopolyester and / or copolyester, and the compatibilizer comprises at least one selected from an epoxy compound, a maleic anhydride graft polymer, a maleic anhydride polyolefin copolymer, and an isocyanate-based compound.
[0010] A second aspect of the invention provides a method for preparing a toughened degradable polyglycolic acid material comprising the step of melt extruding a composition of the invention to obtain a toughened degradable polyglycolic acid material.
[0011] A third aspect of the present invention provides a toughened degradable polyglycolic acid material produced by the preparation method of the present invention.
[0012] A fourth aspect of the present invention provides the use of the material provided by the present invention in injection molding, blister molding and blow molding.
[0013] According to the above technical solution, in the composition provided by the present invention, the compatibilizer can chemically react with PGA and other degradable esters to form a network structure, enhance the compatibility of both phases, reduce the dispersion size of the degradable esters in PGA, and even form a fine fiber continuous phase structure, greatly improving the toughness of the resulting composite material, and obtaining a highly tough and completely biodegradable material. Furthermore, the melt viscosity and melt index of the composition can be adjusted to improve the processing performance of the PGA material and expand its application field.
[0014] BRIEF DESCRIPTION OF THE DRAWINGS FIG. 1 is an infrared spectrum of the raw materials PGA, PBAT, MDI, and the toughened degradable polyglycolic acid material obtained in Example 1 of the present invention.
[0015] [Figure 2] SEM image of the polyglycolic acid material obtained in Comparative Example 4.
[0016] FIG. 3 is an SEM image of the toughened degradable polyglycolic acid material obtained in Example 6.
[0017] FIG. 4 is a diagram showing the complex viscosity-frequency of the polyglycolic acid material obtained in Comparative Example 4 and the toughened degradable polyglycolic acid material obtained in Example 6.
[0018] [Mode for carrying out the invention] The endpoints of the ranges and any values disclosed herein should be understood not to be limited to that particular range or value, but to encompass values close to that range or value. For numerical ranges, the endpoints of each range can be combined with each other, with each of the individual points, and with each of the individual points to obtain one or more new numerical ranges, which numerical ranges are considered to be specifically disclosed herein.
[0019] A first aspect of the present invention provides a toughened degradable polyglycolic acid composition comprising polyglycolic acid, a biodegradable polyester, and a compatibilizer, wherein the biodegradable polyester comprises a biodegradable homopolyester and / or copolyester, and the compatibilizer comprises at least one selected from an epoxy compound, a maleic anhydride graft polymer, a maleic anhydride polyolefin copolymer, and an isocyanate-based compound.
[0020] In some embodiments of the present invention, the use of the biodegradable polyester can improve the toughness and processing performance of the resulting polyglycolic acid material. A specific biodegradable polyester can be selected to match the polyglycolic acid and ensure not only complete degradability of the prepared material, but also to maintain the material performance of the polyglycolic acid. Preferably, the biodegradable polyester includes at least one selected from polyadipic acid / butylene terephthalate, polycaprolactone, polybutylene glycol succinate, polylactic acid, polyhydroxybutyl ester, and polyhydroxy fatty acid ester. More preferably, polyadipic acid / butylene terephthalate (PBAT) can have the properties of high toughness, biodegradability, and high thermal stability. For example, it is commercially available, such as Ecoflex F blend C1200 from BASF, and polycaprolactone is soft, has high stretch properties, provides a plasticizing effect, and can be a commercially available product, such as 6800 from Solvay, USA.
[0021] Furthermore, in some embodiments of the present invention, the weight ratio of the biodegradable polyester to the compatibilizer is 2 to 40: 1, preferably 6 to 30: 1. If the weight ratio of the biodegradable polyester to the compatibilizer is not within the above range, the compatibility with polyglycolic acid will be poor, the toughness of the polyglycolic acid will not be improved, the melt strength of the material will be affected, and the processability will be impaired.
[0022] In some embodiments of the present invention, the amount of each component provided by the composition satisfies the following relationship: polyglycolic acid is 20-90 parts by weight, the biodegradable polyester is 10-80 parts by weight, and the compatibilizer is 0.2-10 parts by weight. The composition of this composition can further produce polyglycolic acid materials with higher toughness and improved processing performance.
[0023] In some embodiments of the present invention, preferably, the polyglycolic acid is 30-70 parts by weight, the biodegradable polyester is 30-70 parts by weight, and the compatibilizer is 0.5-5 parts by weight.
[0024] In some embodiments of the present invention, the polyglycolic acid preferably has a melt index of 2 to 100 g / 10 min, preferably 20 to 85 g / 10 min, at 240° C. and a load of 2.16 kg. The weight average molecular weight of the polyglycolic acid is preferably 50,000 to 300,000, preferably 90,000 to 250,000. By selecting a polyglycolic acid having these performance parameters, the effects of sufficient mechanical strength and good processability can be obtained. The polyglycolic acid may be a commercially available product, such as the polyglycolic acid of Shanghai Pu Jing Chemical Co., Ltd.
[0025] In some embodiments of the present invention, the polyglycolic acid and the composition preferably have melt indices MFR1 and MFR2, respectively, at 240° C. and a load of 2.16 kg, and MFR2≦60%×MFR1, preferably MFR2 is (10 to 40%)×MFR1. When the melt index between the polyglycolic acid and the composition satisfies the above relationship, it is possible to increase the melt strength and improve the processing performance.
[0026] In some embodiments of the present invention, the melt viscosity of the composition is preferably 1000 to 30000 Pa·s. In the present invention, the melt viscosity of the composition is measured by a rotational rheometer. The measurement is performed under the conditions of 240°C, strain 2%, and frequency 0.05 rad / s. As a result, the composition provided by the present invention can have better processing performance.
[0027] In the present invention, when the polyglycolic acid and the composition satisfy the above relationship, the action or effect of improving melt strength and processing performance can be achieved.
[0028] In some embodiments of the present invention, the compatibilizer can provide a technical effect of improving compatibility and melt strength by reacting with the hydroxyl group at the chain end. Preferably, the epoxy compound is made of a copolymer containing a glycidyl methacrylate (GMA) group, but is not limited thereto, and preferably the GMA content is 0.5% by weight to 20% by weight. Preferably, the epoxy compound is at least one selected from styrene-acrylonitrile-glycidyl methacrylate copolymer, ethylene-methyl acrylate-glycidyl methacrylate copolymer, ethylene-ethyl acrylate-glycidyl methacrylate copolymer, POE elastomer-glycidyl methacrylate copolymer, and styrene-methacrylate-glycidyl methacrylate copolymer. The epoxy compound can exert an action or effect of reacting with both components in the composition to form crosslinks. It can be a commercial product such as BASF's ADR-4468 (GMA content 10% by weight, weight average molecular weight about 6680).
[0029] In some embodiments of the present invention, preferably, the maleic anhydride graft polymer is at least one selected from ethylene-maleic anhydride graft copolymer, POE elastomer-maleic anhydride graft copolymer, and propylene-maleic anhydride graft copolymer, and preferably, the graft ratio of the maleic anhydride graft polymer is 0.2-5 wt%. The weight average molecular weight of the maleic anhydride graft polymer is 20,000-150,000, and it can be a commercial product such as JOYAL GR216 (graft ratio 0.5 wt%-1.0 wt%). By selecting a maleic anhydride graft polymer that satisfies the above performance parameters, the high toughness of the toughened degradable polyglycolic acid material obtained by providing the composition can be further promoted.
[0030] In some embodiments of the present invention, the maleic anhydride polyolefin copolymer preferably has the structure shown in Formula 1:
[0031] [ka]
[0032] where R is H, C1-C6 alkyl, phenyl or C1-C6 alkoxy, and n is an integer equal to or greater than 2. For example, SMA1000 from Yusuo New Materials Technology Co., Ltd., where R is phenyl, n is 27, and the weight average molecular weight M w is about 5,500.
[0033] In some embodiments of the present invention, the isocyanate compound is preferably at least one selected from toluene-2,4-diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, lysine diisocyanate, and polyisocyanate. The isocyanate compound can react with components in the composition to improve melt strength and system compatibility. The polyisocyanate has a viscosity (25°C) of 150-250 mPa·s and a functionality of 2.6-2.7. The polyisocyanate is a commercially available product, such as PM200 (viscosity at 25°C of 150-250 mPa·s, -NCO content of 30.2-32 wt%, functionality of 2.6-2.7) manufactured by Wanhua Chemical.
[0034] More preferably, the compatibilizer is an epoxy compound and / or an isocyanate-based compound.
[0035] A second aspect of the invention provides a method for preparing a toughened degradable polyglycolic acid material comprising the step of melt extruding a composition of the invention to obtain a toughened degradable polyglycolic acid material.
[0036] In a specific embodiment provided by the present invention, the preparation method comprises the steps of:
[0037] 1) According to the recipe, weigh out the polyglycolic acid and biodegradable ester and place them in a vacuum oven to dry, removing moisture at a drying temperature of 50-80°C for 4-10 hours.
[0038] 2) Mix the dried polyglycolic acid, degradable polyester, and compatibilizer uniformly according to the recipe.
[0039] 3) The mixture obtained in step 2) is added to a twin-screw extruder and melt-kneaded reactive extrusion is carried out.
[0040] In some specific embodiments of the present invention, the melt kneading conditions are preferably a temperature of 220 to 245°C, preferably 230 to 240°C, a time of 4 to 10 minutes, preferably 5 to 8 minutes, and an extruder rotation speed of 60 to 110 rpm, preferably 80 to 100 rpm.
[0041] In the present invention, the inventors have studied the melt-kneading conditions and found that when the toughening degradable polyglycolic acid composition is melt-kneaded under the above conditions, it is possible to avoid decomposition of polyglycolic acid during the extrusion process and to avoid deterioration of the performance of the obtained polyglycolic acid composition.
[0042] A third aspect of the present invention provides a toughened degradable polyglycolic acid material obtained by the preparation process of the present invention.
[0043] The toughened degradable polyglycolic acid material obtained in the present invention has improved performance, and preferably, in some embodiments, the toughened degradable polyglycolic acid material has a notched impact strength of 5 kJ / m 2 The breaking elongation is 80% or more.
[0044] The toughened degradable polyglycolic acid material provided by the present invention contains a biodegradable polyester and a compatibilizer in addition to polyglycolic acid, and therefore, in addition to toughening, the material can have increased system melt strength and improved processing performance. Preferably, the toughened degradable polyglycolic acid material has a complex viscosity of 1000 to 30000 Pa s, and preferably 2000 to 20000 Pa s, at 240°C, 2% strain, and 0.05 rad / s frequency.
[0045] A fourth aspect of the present invention provides the use of the materials provided herein in the preparation of injection moulded, blister moulded and blow moulded products, for example in the preparation of films, fibres and sheets.
[0046] The present invention will now be described in detail with reference to examples. The obtained toughened degradable polyglycolic acid material was observed with a SEM and a Nova NanoSEM 450. The sample was frozen in liquid nitrogen, subjected to brittle fracture, and the cross section was sprayed with carbon. The dispersion and particle size of each component in the material were then observed at a magnification of 10,000x.
[0047] The melt index is measured according to the GB / T 3682-2000 method. The complex viscosity was measured by the rotational rheology frequency scan method (240°C, strain 2%, frequency 0.05-100 rad / s). The notch impact strength of the samples was measured according to GB / T 1043-2008, and at least 5 samples were tested and the average value was taken. Test the tensile performance of injection molded small sample strips according to GB / T 16421-1996, test at least 5 samples, and take the average value. Polyglycolic acid (PGA) was purchased from Shanghai Pu Jing Chemical Technology Co., Ltd. and was classified into PGA-1 (melt index 64.0g / 10min, weight average molecular weight 150,000), PGA-2 (melt index 85.0g / 10min, weight average molecular weight 90,000), PGA-3 (melt index 45.0g / 10min, weight average molecular weight 200,000), Biodegradable polyester PBAT, BASF Ecoflex F blend C1200, Maleic anhydride polyolefin copolymer: SMA1000 (R is phenyl, n is 27, weight average molecular weight M w (approximately 5500), Yusuo New Materials Technology Co., Ltd. MDI was purchased from Innochem, Polyisocyanate (PMDI), PM200 manufactured by Wanhua Chemical (viscosity at 25°C is 150-250 mPa.s, -NCO content is 30.2-32 wt%, and functional group number is 2.6-2.7); Epoxy compound: BASF ADR-4468 (GMA content: 10% by weight, weight average molecular weight: approximately 6680).
[0048] <Example 1> 70 parts by weight of polyglycolic acid PGA-1, 30 parts by weight of PBAT, and 5 parts by weight of MDI were uniformly mixed, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm to obtain a toughened degradable polyglycolic acid material.
[0049] The composition recipes and test results are shown in Table 1.
[0050] The raw materials PGA, PBAT, MDI and the toughened degradable polyglycolic acid material obtained in Example 1 are tested by infrared spectroscopy, and the spectrum results are shown in Figure 1. As can be seen from the figure, the 2300 cm belonging to MDI in the PGA / PBAT / MDI blend is -1 The characteristic peak of -N=C=O disappears and 3320 cm -1 A new -NH- group was generated at the position of -OH, which is the reaction product of -OH and -N=C=O, indicating that MDI can react with the -OH at the chain ends of PGA and PBAT to form a crosslinked network structure.
[0051] <Example 2> 50 parts by weight of polyglycolic acid PGA-1, 50 parts by weight of PBAT, and 2 parts by weight of MDI are uniformly mixed, melt-kneaded in a twin-screw extruder at 235°C for 8 minutes, and extrusion-granulated at an extruder speed of 80 rpm to obtain a toughened degradable polyglycolic acid material.
[0052] The composition recipes and test results are shown in Table 1.
[0053] <Example 3> 40 parts by weight of polyglycolic acid PGA-1, 60 parts by weight of PBAT, and 5 parts by weight of MDI are uniformly mixed, melt-kneaded in a twin-screw extruder at 230°C for 5 minutes, and extrusion-granulated at an extruder speed of 90 rpm to obtain a toughened degradable polyglycolic acid material.
[0054] The composition recipes and test results are shown in Table 1.
[0055] <Example 4> 30 parts by weight of polyglycolic acid PGA-1, 70 parts by weight of PBAT, and 5 parts by weight of a compatibilizer (MDI) are uniformly mixed, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm to obtain a toughened degradable polyglycolic acid material.
[0056] The composition recipes and test results are shown in Table 1.
[0057] <Example 5> 50 parts by weight of polyglycolic acid PGA-1, 50 parts by weight of PBAT, and 5 parts by weight of a compatibilizer (ADR-4468) are uniformly mixed, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm to obtain a toughened degradable polyglycolic acid material.
[0058] The composition recipes and test results are shown in Table 1.
[0059] <Example 6> 50 parts by weight of polyglycolic acid PGA-1, 50 parts by weight of PBAT, and 5 parts by weight of PMDI are uniformly mixed, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm to obtain a toughened degradable polyglycolic acid material.
[0060] The composition recipes and test results are shown in Table 1.
[0061] The toughened degradable polyglycolic acid material obtained in Example 6 is observed by SEM, and the SEM diagram shown in Figure 3 is obtained. It can be seen that after adding the reactive compatibilizer MDI, PGA-2 reacts with PBAT, which enhances the compatibility of both phases and can further form a continuous phase structure of fine fibers.
[0062] <Example 7> 50 parts by weight of polyglycolic acid PGA-1, 50 parts by weight of PBAT, and 5 parts by weight of a compatibilizer (SMA1000) are uniformly mixed, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm to obtain a toughened degradable polyglycolic acid material.
[0063] <Example 8> 50 parts by weight of polyglycolic acid PGA-2, 50 parts by weight of PBAT, and 5 parts by weight of MDI are uniformly mixed, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm to obtain a toughened degradable polyglycolic acid material.
[0064] The composition recipes and test results are shown in Table 1.
[0065] <Example 9> 50 parts by weight of polyglycolic acid PGA-3, 50 parts by weight of PBAT, and 5 parts by weight of MDI are uniformly mixed, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm to obtain a toughened degradable polyglycolic acid material.
[0066] The composition recipes and test results are shown in Table 1.
[0067] <Comparative Example 1> 100 parts by weight of polyglycolic acid PGA-1 was melt-extruded and granulated in a twin-screw extruder at 240°C for 6 minutes, and the rotation speed was 100 rpm. The test results are shown in Table 1.
[0068] <Comparative Example 2> 100 parts by weight of polyglycolic acid PGA-1 and 5 parts by weight of MDI are uniformly mixed, melt-kneaded in a twin-screw extruder at 240° C. for 6 minutes, and extruded and granulated at an extruder speed of 100 rpm.
[0069] <Comparative Example 3> 70 parts by weight of polyglycolic acid PGA-1 and 30 parts by weight of PBAT are mixed uniformly, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm. The composition recipe and test results are shown in Table 1.
[0070] <Comparative Example 4> 50 parts by weight of polyglycolic acid PGA-1 and 50 parts by weight of PBAT are mixed uniformly, melt-kneaded in a twin-screw extruder at 240°C for 6 minutes, and extrusion-granulated at an extruder speed of 100 rpm. The composition recipe and test results are shown in Table 1.
[0071] The polyglycolic acid material obtained in Comparative Example 4 was observed by SEM to obtain the SEM image shown in Figure 2. It can be seen that the compatibility between the two phases in Comparative Example 4 was poor, and a phase-separated structure due to the absence of a compatibilizer was clearly evident.
[0072] The viscosity of the polyglycolic acid material obtained in Comparative Example 4 and the toughened degradable polyglycolic acid material obtained in Example 6 is measured to obtain the rheological complex viscosity-frequency diagram shown in Figure 4. It can be seen that after adding the reactive compatibilizer MDI, PGA and PBAT can react with each other, the molecular chains grow, the entanglement of the molecular chains increases, and the melt viscosity increases significantly.
[0073] [Table 1]
[0074] [Table 2]
[0075] As can be seen from the results of the Examples, Comparative Examples and Table 1, the toughened degradable polyglycolic acid material obtained by toughening and modifying using the composition, biodegradable resin and extender provided by the present invention can have higher notch impact strength, breaking elongation and tensile strength. For example, comparing Example 1 with Comparative Example 3, Examples 2, 5-9 with Comparative Example 4, the melt strength of the composition is improved, has better processing performance, and the toughness and tensile performance of the obtained material are significantly improved. The technical effects obtained in Examples 3 and 4 are also better than those of the Comparative Examples. The toughness and tensile performance of the materials provided by Comparative Examples 1 and 2 are both lower than the performance of the toughened degradable polyglycolic acid material provided by the present invention.
[0076] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited thereto. Within the scope of the technical idea of the present invention, various simple modifications can be made to the technical solutions of the present invention, and each technical feature can be combined in any other suitable manner, and these simple modifications and combinations are also considered as the disclosure of the present invention, and all are included in the protection scope of the present invention. [Brief description of the drawings]
[0077] [Figure 1] 1 is an infrared spectrum of raw materials PGA, PBAT, MDI and the toughened degradable polyglycolic acid material obtained in Example 1 of the present invention. [Diagram 2] FIG. 1 is an SEM image of a polyglycolic acid material obtained in Comparative Example 4. [Diagram 3] FIG. 1 is an SEM image of the toughened degradable polyglycolic acid material obtained in Example 6. [Figure 4] FIG. 1 is a diagram showing the complex viscosity-frequency of the polyglycolic acid material obtained in Comparative Example 4 and the toughened degradable polyglycolic acid material obtained in Example 6.
Claims
1. A toughened degradable polyglycolic acid composition comprising polyglycolic acid, polyadipic acid / butylene terephthalate and a compatibilizer, the compatibilizer comprising at least one selected from an epoxy compound, a maleic anhydride grafted polymer, a maleic anhydride polyolefin copolymer and an isocyanate-based compound; The polyglycolic acid and the composition have melt indices of MFR1 and MFR2, respectively, at 240° C. and a load of 2.16 kg, and MFR2≦60%×MFR1; The composition has a complex viscosity at 240°C of 1000 to 30000 Pa s, The weight ratio of the polyadipic acid / butylene terephthalate and the compatibilizer is 2 to 40:1; The epoxy compound comprises a copolymer containing glycidyl methacrylate groups.
2. 2. The composition of claim 1, wherein the polyglycolic acid is 20 to 90 parts by weight, the polyadipic acid / butylene terephthalate is 10 to 80 parts by weight, and the compatibilizer is 0.2 to 10 parts by weight.
3. The composition of claim 2, wherein said polyglycolic acid is 30 to 70 parts by weight, said polyadipic acid / butylene terephthalate is 30 to 70 parts by weight, and said compatibilizer is 0.5 to 5 parts by weight.
4. The composition according to any one of claims 1 to 3, wherein the polyglycolic acid has a melt index of 2 to 100 g / 10 min at 240°C under a load of 2.16 kg.
5. The composition according to any one of claims 1 to 4, wherein MFR2 is (10 to 40%) x MFR1.
6. The composition of claim 5, wherein the weight ratio of polyadipic acid / butylene terephthalate and compatibilizer is 6-30:
1.
7. The epoxy compound is at least one selected from styrene-acrylonitrile-glycidyl methacrylate copolymer, ethylene-methyl acrylate-glycidyl methacrylate copolymer, ethylene-ethyl acrylate-glycidyl methacrylate copolymer, POE elastomer-glycidyl methacrylate copolymer, and styrene-methacrylate-glycidyl methacrylate copolymer; The maleic anhydride graft polymer is at least one selected from the group consisting of ethylene-maleic anhydride graft copolymer, POE elastomer-maleic anhydride graft copolymer, and propylene-maleic anhydride graft copolymer; The maleic anhydride polyolefin copolymer has a structure shown in Formula 1: 【Chemistry 1】 Here, R is H, C 1 -C 6 alkyl, phenyl or C 1 -C 6 alkoxy, n is an integer of 2 or more, The composition according to any one of claims 1 to 5, wherein the isocyanate compound is at least one selected from toluene-2,4-diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, lysine diisocyanate and polyisocyanate.
8. 8. The composition according to claim 7, wherein the graft ratio of the maleic anhydride grafted polymer is 0.2 to 5% by weight.
9. A method for preparing a toughened degradable polyglycolic acid material, comprising melt extruding the composition according to any one of claims 1 to 8 to obtain a toughened degradable polyglycolic acid material.
Citation Information
Patent Citations
Polybutylene succinate 3D printing wire and preparation method thereof
CN105111699A
Low-cost bio-based fully-degradable high-transmittance film and preparation method thereof
CN107652641A
Quick-shaping degradable composite material and preparation method thereof
CN109280350A
Polyglycolic acid full-biodegradable composite fibers and preparation method thereof
CN110468468A
Recovery method and application of polyglycolic acid
CN111718569A