Towpreg and fiber reinforced composites
The towpreg with controlled epoxy resin composition and laminar friction coefficient addresses twill drop and void formation issues, enhancing the quality and productivity of fiber-reinforced composite materials in filament winding processes.
Patent Information
- Application Number
- JP2020173753
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-10-15
AI Technical Summary
Existing methods for manufacturing fiber-reinforced composite materials face challenges in preventing twill drop, misalignment of yarn paths, and void formation during filament winding, which affect productivity and product quality.
A towpreg composed of an epoxy resin composition with specific viscosity, fineness, and surface roughness, laminated in a controlled manner to achieve an interlaminar friction coefficient between 0.10 and 0.50, ensuring proper alignment and spreadability.
The solution effectively suppresses twill drop and misalignment, reducing void formation, thereby improving the handling and quality of fiber-reinforced composite materials, particularly in manufacturing hollow containers and cylinders.
Smart Images

Figure 0007589492000006 
Figure 0007589492000007 
Figure 0007589492000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a towpreg that is particularly suitable for use in manufacturing hollow containers and cylinders made of fiber-reinforced composite materials, and more particularly to a towpreg that is easy to handle and capable of producing high-quality molded products with few voids. [Background technology]
[0002] Fiber-reinforced composite materials using reinforcing fibers such as carbon fiber and glass fiber are used in many fields such as aerospace, automobiles, railway vehicles, ships, civil engineering and construction, and sporting goods because of their excellent light weight. In particular, fiber-reinforced composite materials using continuous reinforcing fibers are used in applications that require high performance, and carbon fiber, which has excellent specific strength and specific elastic modulus, is often used as the reinforcing fiber, and epoxy resin, which has excellent adhesion to carbon fiber, is often used as the thermosetting resin.
[0003] In response to the recent expansion of applications of carbon fiber, molding methods are also expanding. Among these, filament winding is a method that is preferably used for manufacturing hollow containers and cylinders such as pressure vessels. Instead of the conventional wet method in which a reinforced fiber bundle unwound from a bobbin is immersed in a liquid thermosetting resin and then wound up on a mold, a method in which a narrow belt-shaped intermediate base material called a tow prepreg, yarn prepreg, or strand prepreg (hereinafter referred to as a tow prepreg) in which a reinforced fiber bundle is pre-impregnated with a thermosetting resin is supplied and wound up on a mold has been attracting attention from the viewpoints of productivity and quality.
[0004] Towpregs are usually supplied in the form of bobbins with hundreds to thousands of meters wound around a paper tube, and are unwound at high speed during the molding process of fiber-reinforced composite materials. For this reason, there are demands for the towpregs to be aligned in a fixed position at the end of the bobbin to prevent twill drop and have a beautiful winding appearance, to be less likely to cause deviation in the yarn path due to slippage of the towpreg during filament winding molding, and to have appropriate spreadability to prevent voids from occurring in the molded product.
[0005] Furthermore, in pressure vessel applications for which towpregs are suitable, they are required to have sufficient heat resistance against the temperature rise that occurs when high-pressure gas is rapidly filled, and to have little performance degradation due to repeated use over a long period of time, etc. In order to satisfy these performance requirements, it is useful to improve the toughness and heat resistance (glass transition temperature) of the matrix resin.
[0006] Patent Document 1 discloses a method for manufacturing a composite container in which the towpreg is heated before being wound around a liner to reduce the viscosity of the matrix resin and suppress void formation, and then cooled after the winding to increase the viscosity of the matrix resin and suppress tow slippage. However, this method is not economically satisfactory because it requires the installation of a heating and cooling mechanism in the manufacturing equipment for winding.
[0007] Patent Document 2 discloses a technology for strengthening tack and preventing slippage of the tow during filament winding molding by applying a high-viscosity, hardener-free second resin to the surface layer of a towpreg impregnated with a low-viscosity first resin that contains a hardener. However, since the resin must be impregnated in two separate steps, this complicates the towpreg manufacturing process and is not economically satisfactory. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2010-234658 A [Patent Document 2] JP 2015-98556 A Summary of the Invention [Problem to be solved by the invention]
[0009] In view of the above background, an object of the present invention is to provide a towpreg that suppresses the occurrence of twill drop, has a beautiful winding appearance, is less susceptible to deviation of the yarn path due to slippage during filament winding molding, and is less susceptible to the formation of voids in the molded product due to inadequate spreadability, and has excellent handleability and productivity, and can produce a high-quality fiber-reinforced composite material. [Means for solving the problem]
[0010] The present invention employs the following means to solve the above problems. That is, the towpreg of the present invention is a towpreg obtained by impregnating a carbon fiber bundle having a fineness of 30 to 4000 g / 1000 m and an arithmetic mean roughness (Ra) of a single fiber surface of 1 to 100 nm with an epoxy resin composition having a viscosity of 1 to 150 Pa s at 25° C., the towpreg has a resin content of 20 to 40 mass %, and the towpreg is laminated in three layers in the same direction, and the interlayer friction coefficient measured by pulling out the central towpreg under conditions of a temperature of 25° C., a humidity of 50% RH, a speed of 1 mm / min, and a normal load of 20.6 N is 0.10 or more and 0.50 or less. Effect of the Invention
[0011] The towpreg of the present invention suppresses the occurrence of twill drop, resulting in a beautiful winding appearance, and is less susceptible to deviations in the yarn path due to slippage during filament winding molding, or formation of voids in the molded product due to inadequate spreadability. As a result, it has excellent handleability and productivity when producing hollow containers such as pressure vessels and cylinders, and a good-quality fiber-reinforced composite material can be obtained. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1A is a cross-sectional view showing the method for measuring an interlayer friction coefficient of the present invention, and FIG. 1B is a plan view showing the method for measuring an interlayer friction coefficient of the present invention. [Diagram 2] 1 is an example of an image of the surface of a towpreg taken with an optical microscope at 200x magnification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention has the following configuration: That is, the towpreg of the present invention is a towpreg obtained by impregnating a carbon fiber bundle having a fineness of 30 to 4000 g / 1000 m and an arithmetic mean roughness (Ra) of a single fiber surface of 1 to 100 nm with an epoxy resin composition having a viscosity of 1 to 150 Pa s at 25° C., the towpreg having a resin content of 20 to 40 mass %, and the towpreg is laminated in three layers in the same direction, and the interlayer friction coefficient measured by pulling out the central towpreg under conditions of a temperature of 25° C., a humidity of 50% RH, a speed of 1 mm / min, and a normal load of 20.6 N is 0.10 or more and 0.50 or less.
[0014] The interlayer friction coefficient in the present invention refers to the static friction coefficient in the friction phenomenon that occurs between layers of towpregs in a towpreg laminate in which towpregs are stacked. Here, the interlayer refers to the boundary region where the surfaces of the towpregs are in contact with each other, and in the present invention, the term interlayer is used even when it is not clearly observed with a microscope or the like.
[0015] In the present invention, the interlaminar friction coefficient is measured by the following method. First, as shown in FIG. 1, one towpreg 3 is sandwiched between two towpregs 4 with the same fiber direction, and a load of 20.6 N is applied vertically to the stacked towpregs using a pressure plate 1 (hereinafter referred to as vertical load). Next, the maximum load obtained when the sandwiched towpreg 3 is pulled out at a temperature of 25° C., a humidity of 50% RH, and a speed of 1 mm / min is read. The static friction coefficient obtained by dividing the read maximum load by twice the vertical load applied to the contact portion between the towpreg 3 and the towpreg 4 is defined as the interlaminar friction coefficient in the present invention. The reason for using a value twice the vertical load is that there are two surfaces of the towpreg that receive frictional resistance. More detailed test methods will be described in the examples below.
[0016] The interlayer friction coefficient of the towpreg of the present invention measured by this method is 0.10 to 0.50. By satisfying this range, slippage during winding into a bobbin shape can be suppressed, the towpreg is aligned in a fixed position at the end, twill drop is unlikely to occur, and a towpreg bobbin with a beautiful winding appearance can be obtained, and a towpreg can be obtained that is less susceptible to misalignment of the yarn path due to slippage during filament winding molding and less likely to form voids in the molded product due to inadequate spreadability. In this way, by using a towpreg in which the occurrence of defects is suppressed, it is possible to improve the yield and the quality of the molded product.
[0017] The interlayer friction coefficient of the towpreg of the present invention can be adjusted within an appropriate range by the viscosity of the epoxy resin composition described below, the arithmetic mean roughness (Ra) of the single fiber surface of the carbon fiber, the resin content (Rc) of the towpreg, etc.
[0018] The viscosity of the epoxy resin composition used in the towpreg of the present invention at 25°C must be 1 to 150 Pa·s, preferably 1 to 100 Pa·s, and more preferably 1 to 50 Pa·s. By setting the viscosity of the epoxy resin composition in this range, the interlaminar friction coefficient can be adjusted to an appropriate range. In the present invention, the lower the viscosity of the epoxy resin composition, the lower the resin content (Rc) of the towpreg can be and the higher the carbon fiber content, which can contribute to weight reduction of the fiber reinforced composite material. In addition, the lower the viscosity of the epoxy resin composition, the simpler the mechanism for adjusting the viscosity by heating and controlling the temperature of the epoxy resin composition in the towpreg manufacturing process can be, which is preferable from the viewpoint of suppressing equipment costs and energy consumption.
[0019] Specific examples of carbon fiber bundles used in the towpreg of the present invention include acrylic, pitch and rayon carbon fiber bundles, and acrylic carbon fiber bundles having particularly high tensile strength are preferably used.
[0020] The carbon fiber bundles used in the towpreg of the present invention must have a fineness of 30 to 4000 g / 1000 m, and typically have 1,000 to 70,000 filaments each having a diameter of 3 to 100 μm. By setting the fineness of the carbon fiber bundles within this range, it is possible to obtain a towpreg that is easy to handle as a belt-shaped intermediate substrate and is uniformly impregnated with the epoxy resin composition all the way to the inside.
[0021] In addition, the carbon fiber bundle used in the towpreg of the present invention must have an arithmetic mean roughness (Ra) of the single fiber surface of the carbon fiber of 1 to 100 nm, and preferably 1 to 20 nm. By setting the arithmetic mean roughness (Ra) of the single fiber surface of the carbon fiber in this range, the interlaminar friction coefficient can be adjusted to an appropriate range. Here, the arithmetic mean roughness (Ra) of the single fiber surface is an index of the unevenness of the carbon fiber surface, and is the arithmetic mean roughness (Ra) calculated from the image of the three-dimensional surface shape obtained by measuring a three-dimensional surface shape of 600 nm x 600 nm by an atomic force microscope (AFM) and approximating the roundness of the fiber with a three-dimensional curved surface as the average line.
[0022] The resin content (Rc) of the towpreg of the present invention must be 20-40% by mass, preferably 20-35% by mass, more preferably 20-30% by mass, and even more preferably 20-27% by mass. Here, the resin content (Rc) of the towpreg is the mass ratio of the epoxy resin composition to the mass of the towpreg. By setting Rc in this range, the interlaminar friction coefficient can be adjusted to an appropriate range. In addition, when Rc is 20% by mass or more, it is possible to suppress the occurrence of defects such as unimpregnated parts and voids inside the obtained fiber reinforced composite material, and when it is 40% by mass or less, it is possible to suppress the exudation of the resin composition from the bobbin of the towpreg and the scattering of the resin composition in the filament winding molding process. The smaller Rc is, the higher the carbon fiber content can be, which contributes to weight reduction of the fiber reinforced composite material, and is therefore preferable. Rc can be changed by controlling the mass of the epoxy resin composition impregnated into the carbon fiber bundle.
[0023] When a solid component is blended with the epoxy resin composition of the towpreg of the present invention, it is preferable that, when the surface of the towpreg is observed using an optical microscope at a magnification of 200 times, the ratio of the area of the portion covered by the solid component not dissolved in the epoxy resin to the area of the field of view (coverage rate) is 2.5% or more and 20% or less.
[0024] In the present invention, the coverage is measured by the following method. First, the surface of the towpreg is imaged with an optical microscope at a magnification of 200 times while applying ring illumination, and a digital image as shown in FIG. 2 is obtained. By applying ring illumination, the reflection of light by the epoxy resin is canceled, and an image in which the solid components not dissolved in the epoxy resin are emphasized can be obtained. Next, the obtained digital image is binarized using image analysis software, and the part covered by the solid components not dissolved in the epoxy resin is recognized and its area is calculated. The area of the part covered by the solid components not dissolved in the epoxy resin obtained by the above method is divided by the area actually captured, and the value expressed as a percentage is taken as the coverage. With this measurement method, it is possible to distinguish a covered part having a size of about 1 μm at the smallest.
[0025] When the coverage rate of the towpreg of the present invention, measured by this method, satisfies this range, slippage when wound into a bobbin shape can be suppressed, the towpreg is aligned in a fixed position at the end, which makes it less likely for twill drop to occur, resulting in a towpreg bobbin with a beautiful wound appearance, and further, a towpreg can be obtained that is less likely to experience misalignment of the yarn path due to slippage during filament winding molding or formation of voids in the molded product due to inadequate spreadability.
[0026] The materials constituting the towpreg of the present invention are described below.
[0027] (About epoxy resin) The epoxy resin in the present invention can be used without any particular limitation, and examples thereof include bisphenol type epoxy resins such as bisphenol A type, bisphenol F type, and bisphenol S type, glycidyl amine type epoxy resins such as glycidyl aniline type, diaminodiphenylmethane type, diaminodiphenyl sulfone type, aminophenol type, metaxylenediamine type, and 1,3-bisaminomethylcyclohexane type, aliphatic epoxy resins such as polyethylene glycol type, polypropylene glycol type, butanediol type, neopentyl glycol type, hexanediol type, and cyclohexanedimethanol type, isocyanurate type, hydantoin type, phenol novolac type, orthocresol novolac type, dicyclopentadiene novolac type, biphenyl type, trishydroxyphenylmethane type, and tetraphenylolethane type epoxy resins. These epoxy resins may be used alone or in appropriate mixture.
[0028] In the present invention, it is preferable that the epoxy resin contains 3 to 20 parts by mass of a bifunctional aliphatic epoxy resin that is liquid at 25°C in 100 parts by mass of the epoxy resin component. By containing such a range of bifunctional aliphatic epoxy resin that is liquid at 25°C, it becomes easy to adjust the interlayer friction coefficient to an appropriate range. In addition, by using it in combination with a carboxyl-terminated butadiene nitrile rubber and / or core-shell rubber particles described later, a specific toughness value improvement effect can be obtained compared to when each component is used alone or when only the two components are used in combination. The reason why such an effect is obtained is unclear, but it is speculated that it is due to the concerted action of the different toughness value improvement mechanisms of each component.
[0029] Examples of such bifunctional aliphatic epoxy resins that are liquid at 25° C. include polyethylene glycol type epoxy resins, polypropylene glycol type epoxy resins, butanediol type epoxy resins, neopentyl glycol type epoxy resins, hexanediol type epoxy resins, and cyclohexanedimethanol type epoxy resins.
[0030] Commercially available bifunctional aliphatic epoxy resins that are liquid at 25°C include "Denacol (registered trademark)" EX-821, "Denacol (registered trademark)" EX-850 (both are polyethylene glycol type epoxy resins, manufactured by Nagase ChemteX Corporation), "Denacol (registered trademark)" EX-920, "Denacol (registered trademark)" EX-941 (both are polypropylene glycol type epoxy resins, manufactured by Nagase ChemteX Corporation), "Denacol (registered trademark)" EX-214 (1,4-butanediol type epoxy resin, manufactured by Nagase ChemteX Corporation), "Araldite (registered trademark)" DY-026 (1,4-butanediol type epoxy resin, manufactured by Huntsman Japan Co., Ltd.), "Denacol (registered trademark)" EX-221 (1,4-butanediol type epoxy resin, manufactured by Nagase ChemteX Corporation), "Denacol (registered trademark)" EX-222 (1,4-butanediol type epoxy resin, manufactured by Nagase ChemteX Corporation), "Denacol (registered trademark)" EX-221 (1,4-butanediol type epoxy resin, manufactured by Nagase ChemteX Corporation), "Denacol (registered trademark)" EX-222 (1,4-butanediol type epoxy resin, manufactured by Huntsman Japan Co., Ltd.), "Denacol (registered trademark)" EX-221 (1,4-butanediol type epoxy resin, manufactured by Nagase ChemteX Corporation ... -212 (1,6-hexanediol type epoxy resin, manufactured by Nagase ChemteX Corporation), "ADEKA RESIN (registered trademark)" ED-503 (1,6-hexanediol type epoxy resin, manufactured by ADEKA Corporation), "Denacol (registered trademark)" EX-211 (neopentyl glycol type epoxy resin, manufactured by Nagase ChemteX Corporation), "ADEKA RESIN (registered trademark)" ED-523 (neopentyl glycol type epoxy resin, manufactured by ADEKA Corporation), "Denacol (registered trademark)" EX-216 (cyclohexane dimethanol type epoxy resin, manufactured by Nagase ChemteX Corporation), "Rikaresin (registered trademark)" DME-100 (cyclohexane dimethanol type epoxy resin, manufactured by New Japan Chemical Co., Ltd.), and the like.
[0031] (About the hardener) The epoxy resin curing agent in the present invention can be used without any particular limitation, and examples thereof include dicyandiamide, cyanamide, aromatic amines such as diethyltoluenediamine, diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and diaminodiphenylsulfone, carboxylic anhydrides such as methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, and methylnadic anhydride, Lewis acids such as boron trifluoride amine complexes and boron trichloride amine complexes, and imidazoles such as 2-ethyl-4-methylimidazole, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. These epoxy resin curing agents may be used alone or in appropriate mixtures.
[0032] Commercially available dicyandiamide products include "jER Cure (registered trademark)" DICY7 and "jER Cure (registered trademark)" DICY15 (both manufactured by Mitsubishi Chemical Corporation).
[0033] Commercially available cyanamide products include "DYHARD (registered trademark)" Fluid 111 (manufactured by AlzChem). Commercially available aromatic amines include "jER Cure (registered trademark)" WA (diethyltoluenediamine, manufactured by Mitsubishi Chemical Corporation), "KAYAHARD (registered trademark)" AA (3,3'-diethyl-4,4'-diaminodiphenylmethane, manufactured by Nippon Kayaku Co., Ltd.), and "SEIKACURE (registered trademark)" S (epoxy resin hardener, 4,4'-diaminodiphenyl sulfone, manufactured by Seika Corporation).
[0034] Commercially available carboxylic acid anhydrides include HN-2200 (methyltetrahydrophthalic anhydride, manufactured by Hitachi Chemical Co., Ltd.), "RIKACID (registered trademark)" HH (hexahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.), and "KAYAHARD (registered trademark)" MCD (methylnadic anhydride, manufactured by Nippon Kayaku Co., Ltd.).
[0035] Commercially available boron halide amine complexes include Accelerator DY 9577 (boron trichloride amine complex, manufactured by Huntsman Japan Co., Ltd.) and LEECURE B-550 (boron trifluoride amine complex, manufactured by Leepoxy Plastics).
[0036] Commercially available imidazole products include "Curezol (registered trademark)" 2E4MZ, "Curezol (registered trademark)" 2MZA-PW, "Curezol (registered trademark)" 2MAOK-PW, and "Curezol (registered trademark)" 2P4MHZ-PW (all manufactured by Shikoku Chemical Industry Co., Ltd.).
[0037] Among these epoxy resin curing agents, dicyandiamide is particularly preferably used because it can provide an epoxy resin composition for towpreg that gives a fiber-reinforced composite material with an excellent balance of mechanical properties.
[0038] In addition, dicyandiamide is a solid component that does not dissolve in epoxy resin under the handling conditions of the towpreg except for the curing process, and therefore is preferable from the viewpoint that it can be used as a component for controlling the interlayer friction coefficient of the towpreg by powdering it for use.
[0039] The primary particle diameter of dicyandiamide is preferably 0.5 to 150 μm, more preferably 0.5 to 100 μm, and even more preferably 0.5 to 10 μm. By setting the primary particle diameter in this range, it becomes easy to adjust the interlayer friction coefficient to an appropriate range, and the mechanical properties of the resin cured material can be improved. Here, the primary particle diameter of dicyandiamide refers to the volume-based particle size distribution, and it is preferable that D10 is equal to or greater than the lower limit of the preferred range of the primary particle diameter, and D90 is equal to or less than the upper limit of the preferred range of the primary particle diameter. The primary particle diameter of dicyandiamide can be measured by a laser diffraction / scattering method or the like.
[0040] The content of dicyandiamide is preferably 1 to 20 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the epoxy resin. By setting the content of dicyandiamide within this range, it becomes easy to adjust the interlayer friction coefficient to an appropriate range, and it is possible to prevent deterioration of heat resistance and mechanical properties due to insufficient curing or excessive reaction heat generation, and to obtain a cured product of good quality.
[0041] The epoxy resin composition used in the towpreg of the present invention preferably contains aromatic urea as a curing accelerator for dicyandiamide. By using aromatic urea in combination with dicyandiamide, the temperature required for curing can be lowered and handling can be improved. Here, aromatic urea refers to a compound having a structure in which a urea group is bonded to an aromatic ring, and specific examples thereof include 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), 3-(4-chlorophenyl)-1,1-dimethylurea, phenyldimethylurea (PDMU), and 2,4-toluenebis(3,3-dimethylurea) (TBDMU). These may be used alone or in appropriate mixture. Commercially available examples of such aromatic ureas include DCMU99 (DCMU, manufactured by Hodogaya Chemical Co., Ltd.), "Omicure (registered trademark)" 24 (TBDMU, manufactured by Chori GLEX Co., Ltd.), and "Dyhard (registered trademark)" UR505 (4,4'-methylenebis(phenyldimethylurea), manufactured by AlzChem).
[0042] Among these aromatic ureas, it is preferable to use TBDMU since it is possible to obtain a cured resin having excellent heat resistance.
[0043] (Additives) In the present invention, in order to adjust the interlayer friction coefficient and improve the performance such as the mechanical properties of the resin cured product, various additives such as viscosity modifiers such as thermoplastic resins and thixotropic agents, toughening agents such as rubber components, and other additives such as defoamers, stabilizers, flame retardants, and pigments can be contained. The thermoplastic resin is preferably a thermoplastic resin that is soluble in epoxy resin. Examples of the thermoplastic resin that is soluble in epoxy resin include polyvinyl acetal resins such as polyvinyl formal and polyvinyl butyral, polyvinyl alcohol, phenoxy resin, polyamide, polyimide, polyvinyl pyrrolidone, and polysulfone. Examples of the thixotropic agent include organic ones such as amide wax and hydrogenated castor oil, and inorganic ones such as silica, alumina, mixed oxides of aluminum and silicon, titanium oxide, light calcium carbonate, smectite clay minerals (montmorillonite, beidellite, bentonite, hectorite, saponite, etc.), sepiolite, and carbon black. The defoaming agent includes non-silicon polymer-based defoaming agents, silicone-based defoaming agents, and the like.
[0044] The epoxy resin composition used in the towpreg of the present invention contains a toughening agent that is compatible with epoxy resins at 25°C and / or a toughening agent having a particle size of 50 nm to 1 μm, and the toughness value KIc of the cured product obtained by curing the epoxy resin composition at 150°C for 4 hours is 1.0 to 3.0 MPa m 0.5 By satisfying these conditions, it is possible to increase the toughness of the cured resin without excessively increasing the interlaminar friction coefficient, and to obtain a fiber-reinforced composite material that exhibits little deterioration in performance due to repeated use.
[0045] Here, being compatible with the epoxy resin at 25°C means that the epoxy resin composition to be impregnated into the towpreg does not substantially contain a solid toughening agent component and does not cause coarse liquid-liquid phase separation. Compatibility can be confirmed by mixing the epoxy resin and the toughening agent and visually observing the mixture.
[0046] In the present invention, the particle size of the toughening agent refers to the volume average particle size, and can be measured by a method such as a laser diffraction / scattering method or a dynamic light scattering method.
[0047] Examples of toughening agents compatible with epoxy resins at 25°C include liquid rubbers such as liquid butadiene nitrile rubber, CTBN (carboxyl-terminated butadiene nitrile rubber), ATBN (amino-terminated butadiene nitrile rubber), and butadiene nitrile rubber modified with a carboxyl group in the main chain. These may be used alone or in appropriate mixtures. Commercially available liquid rubbers include "Hypro (registered trademark)" 1300X31, "Hypro (registered trademark)" 1300X13, "Hypro (registered trademark)" 1300X13NA, and "Hypro (registered trademark)" 1300X8 (all manufactured by CVC Thermoset Specialties).
[0048] Examples of toughening agents having a particle size of 50 nm to 1 μm include rubber particles such as acrylic rubber particles, butadiene rubber particles, butadiene-styrene rubber particles, and silicone rubber particles, as well as core-shell rubber particles having a core-shell structure in which rubber particles are coated with a different polymer, etc. These may be used alone or in appropriate mixture.
[0049] Commercially available examples of such core-shell rubber microparticles include "Kane Ace (registered trademark)" MX-125, "Kane Ace (registered trademark)" MX-150, "Kane Ace (registered trademark)" MX-154, "Kane Ace (registered trademark)" MX-257, "Kane Ace (registered trademark)" MX-267, "Kane Ace (registered trademark)" MX-416, "Kane Ace (registered trademark)" MX-451, and "Kane Ace (registered trademark)" MX-EXP (HM5) (all manufactured by Kaneka Corporation).
[0050] In the present invention, it is preferable to contain both the core-shell rubber particles and the carboxyl-terminated butadiene nitrile rubber, since a particularly excellent effect of improving toughness can be obtained.
[0051] In the present invention, the mass ratio obtained by dividing the mass of the carboxyl-terminated butadiene nitrile rubber by the mass of the core-shell rubber particles is preferably 0.1 to 0.8. By setting the content of the carboxyl-terminated butadiene nitrile rubber relative to the core-shell rubber particles in this range, it is possible to effectively obtain specifically excellent toughness and to simultaneously achieve heat resistance.
[0052] Furthermore, since a more excellent toughness improving effect and a viscosity suitable for manufacturing an intermediate substrate can be obtained, the content of the core-shell rubber microparticles is preferably 5 to 30 parts by mass, more preferably 5 to 15 parts by mass, based on 100 parts by mass of the total epoxy resin components. From the same viewpoint, the content of the carboxyl-terminated butadiene nitrile rubber is preferably 0.5 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the total epoxy resin components. Moreover, the sum of the content of the core-shell rubber microparticles and the content of the carboxyl-terminated butadiene nitrile rubber is preferably 5 to 50 parts by mass, more preferably 9 to 20 parts by mass, based on 100 parts by mass of the total epoxy resin components.
[0053] In the present invention, the glass transition temperature of the cured product obtained by curing the epoxy resin composition at 150° C. for 4 hours is preferably 120 to 160° C., and more preferably 120 to 150° C. By controlling the glass transition temperature of the cured resin product to fall within this range, it is possible to achieve a good balance between the heat resistance and toughness of the cured resin product.
[0054] The epoxy resin composition for use in the towpreg of the present invention can be prepared by various known methods, for example, by kneading using a machine such as a kneader, planetary mixer, mechanical stirrer, dissolver, or three-roll mill, or by hand mixing using a beaker and spatula, etc.
[0055] The towpreg of the present invention can be manufactured by various known methods. That is, the epoxy resin composition used in the towpreg of the present invention can be heated without using an organic solvent to reduce the viscosity, and the reinforcing fiber bundle is immersed in the epoxy resin composition and impregnated therewith; the epoxy resin composition having a low viscosity at room temperature or the epoxy resin composition having a low viscosity by heating is coated on a rotating roll or release paper, and then transferred to one or both sides of the reinforcing fiber bundle, and then the reinforcing fiber bundle is pressed and impregnated by passing through a bending roll or a pressure roll. Since a high-quality towpreg can be manufactured, the manufacturing method of the towpreg of the present invention preferably includes a step of contacting a rotating roll coated with an epoxy resin composition with at least one side of the reinforcing fiber bundle. The towpreg is usually supplied in a bobbin shape wound around a paper tube with hundreds to thousands of meters.
[0056] The fiber-reinforced composite material of the present invention can be obtained by heat curing the towpreg of the present invention. The intermediate substrate of the present invention can be used in many fields such as aerospace, automobiles, railway vehicles, ships, civil engineering and construction, and sporting goods, and can be particularly suitably used for manufacturing hollow containers such as pressure vessels, and cylinders. EXAMPLES
[0057] The present invention will be described in detail below with reference to examples. However, the scope of the present invention is not limited to these examples. The unit "parts" in the composition ratio means parts by mass unless otherwise noted. Furthermore, the measurements of various characteristics (physical properties) were performed in an environment of a temperature of 23°C and a relative humidity of 50%, with the number of measurements being 1, unless otherwise noted.
[0058] <Materials used in the Examples and Comparative Examples> (1) Carbon fiber bundle Carbon fiber manufactured by Toray Industries, Inc. (fineness: 1645g / 1000m, arithmetic mean roughness (Ra): 2.1nm of single fiber surface).
[0059] (2) Epoxy resin "jER (registered trademark)" 807 (liquid bisphenol F type epoxy resin, manufactured by Mitsubishi Chemical Corporation) "jER (registered trademark)" 828 (liquid bisphenol A type epoxy resin, manufactured by Mitsubishi Chemical Corporation) "Sumiepoxy (registered trademark)" ELM-434VL (tetraglycidyldiaminodiphenylmethane, manufactured by Sumitomo Chemical Co., Ltd.) "EPICLON (registered trademark)" HP-7200L (dicyclopentadiene type epoxy resin, manufactured by DIC Corporation) "Denacol (registered trademark)" EX-821 (a bifunctional aliphatic epoxy resin that is liquid at 25°C, a polyethylene glycol type epoxy resin, manufactured by Nagase ChemteX Corporation) "Denacol (registered trademark)" EX-212 (a bifunctional aliphatic epoxy resin that is liquid at 25°C, a 1,6-hexanediol type epoxy resin, manufactured by Nagase ChemteX Corporation).
[0060] (3) Hardener "jER Cure (registered trademark)" DICY7 (dicyandiamide, manufactured by Mitsubishi Chemical Corporation) Accelerator DY 9577 (boron trichloride amine complex, Huntsman Japan Co., Ltd.) "DYHARD®" Fluid 111 (cyanamide, manufactured by AlzChem) "Omicure" (registered trademark) 24 (TBDMU, manufactured by Chori GLEX Co., Ltd.).
[0061] (4) Additives "AEROSIL®" 130 (fumed silica, manufactured by Nippon Aerosil Co., Ltd.) "Kane Ace (registered trademark)" MX-150 (liquid bisphenol A type epoxy resin masterbatch containing 40% polybutadiene rubber type core-shell rubber particles (particle diameter: 100 nm), manufactured by Kaneka Corporation) "Hypro (registered trademark)" 1300X13 (carboxyl-terminated butadiene nitrile rubber, manufactured by CVC Thermoset Specialties) "Vinylec" K (polyvinyl formal resin, manufactured by JNC Corporation).
[0062] <Method of measuring the arithmetic mean roughness (Ra) of a single fiber surface> The carbon fibers were cut to a length of a few mm and fixed on a substrate (silicon wafer) using silver paste, and then an atomic force microscope (AFM) was used to obtain an image of the three-dimensional surface shape at the center of each single fiber. The atomic force microscope used was a Digital Instruments NanoScope IIIa with a Dimension 3000 stage system. The observation conditions were as follows: Scanning mode: Tapping mode Tip: Silicon cantilever Scanning range: 0.6μm×0.6μm Scanning speed: 0.3Hz - Number of pixels: 512 x 512 Measurement environment: Room temperature, in air For each sample, the roundness of the fiber cross section was approximated by a cubic curve for the images obtained by observing one point from each single fiber, and the arithmetic mean roughness (Ra) was calculated for the entire image. The average value of the values obtained for five single fibers was used.
[0063] <Method for preparing epoxy resin composition> After the components other than the curing agent were put into a beaker, it was heated to 100°C and stirred until it became uniform. Next, the temperature of the resin was lowered to 25-60°C, and then the curing agent was put in and stirred until it became uniform to obtain an epoxy resin composition. When a toughening agent compatible with the epoxy resin at 25°C was used, compatibility was confirmed by visual observation. The component content ratios of the examples and comparative examples are shown in Tables 1-3.
[0064] <Method for measuring viscosity of epoxy resin composition at 25°C> According to the "Viscosity measurement method using a cone-plate type rotational viscometer" in JIS Z8803 (2011), measurements were taken using an E-type viscometer (TVE-30H, manufactured by Toki Sangyo Co., Ltd.) equipped with a standard cone rotor (1°34' x R24) at a rotation speed of 5 to 20 revolutions per minute. The temperature inside the sample cup was adjusted to the measurement temperature (25°C), and the epoxy resin composition was poured in, and the value was read when the displayed value stabilized after 1 minute or more had elapsed.
[0065] <How to make a resin cured plate> The epoxy resin composition was degassed in a vacuum and then poured into a mold set to a thickness of 2 mm or 6 mm using a Teflon (registered trademark) spacer. The epoxy resin composition was then cured by increasing the temperature from room temperature to 150°C at a rate of 2.5°C per minute in a hot air oven and maintaining the temperature for 4 hours. The epoxy resin composition was then cooled to room temperature and removed from the mold to produce a cured resin plate.
[0066] <Method of measuring glass transition temperature> A test piece 12.7 mm wide and 45 mm long was cut out from a 2 mm thick resin cured plate, and DMA measurements were performed in the temperature range of 30 to 250°C using a viscoelasticity measuring device (ARES, manufactured by TA Instruments) under conditions of a torsional vibration frequency of 1.0 Hz and a heating rate of 5.0°C / min. The glass transition temperature (Tg) was defined as the temperature at the intersection of the tangent in the glassy state and the tangent in the transition state on the storage modulus G' curve.
[0067] <Method for measuring fracture toughness of cured resin> The test was conducted in accordance with the SENB (Single Edge Notched Bend) test method in accordance with ASTM D5045. A test piece 60 mm long and 12.7 mm wide was cut out from a 6 mm thick resin-cured plate, and a pre-crack was then introduced. Then, using an Instron universal testing machine (Instron Corporation), the span was set to 50.8 mm, the crosshead speed was set to 10 mm / min, and the number of samples was set to n=6, and the fracture toughness value (K IC ) was measured.
[0068] <How to make towpregs> Using a towpreg manufacturing device equipped with a creel, kiss roll, nip roll, and winder, an epoxy resin composition adjusted to a temperature of 20 to 60°C was applied to one side of a carbon fiber bundle, and then the bundle was passed through a nip roll to impregnate the inside of the reinforced fiber bundle with the epoxy resin composition, thereby obtaining a towpreg. The towpreg bobbin was wound up to 2300 m on a cardboard tube with an initial tension of 600 to 1000 gf and a wind ratio of 6 to 10, to form a cylindrical shape with a winding width of 230 to 260 mm.
[0069] <Method of measuring Rc of towpreg> The Rc of the towpreg is the mass of the towpreg bobbin (W A ), the mass of the paper tube (W B ), the mass per unit length of carbon fiber (W C ), the length of the towpreg wound on the bobbin (W D ) according to equation (1).
[0070]
number
[0071] <Method for measuring interlayer friction coefficient> The interlaminar friction coefficient was measured by carrying out the following operations (a), (b), and (c) in this order. (a) First, as shown in FIG. 1, a first layer towpreg 4 cut to a length of 150 mm was placed on a release paper 2 having a width of 40 mm and a length of 150 mm, and a second layer towpreg 3 cut to the same size was laminated on top of it so as to overlap by a length of 60 mm. Next, a towpreg for spacer 5 having a length of 20 mm was laminated on the first layer towpreg 4 so as to contact the overlapping portion of the second layer, and a third layer towpreg 4 having a length of 150 mm was laminated on top of it so as to overlap with the first layer to produce a towpreg laminate. Next, in order to prevent the towpreg laminate from being deformed more than necessary due to a vertical load, a spacer 6 having a thickness equivalent to that of the towpreg laminate was laminated with cellophane tape and placed so as to contact the side of the towpreg laminate. Finally, a release paper 2 having a width of 40 mm and a length of 150 mm was attached so as to overlap with the release paper 2 of the lowest layer to produce a test sample. (b) The test sample was placed in a sample chamber with a temperature of 25°C and a humidity of 50% RH, and a constant vertical load of 20.6 N was applied using pressure plate 1 to the area ranging from 60 mm of the overlap portion to 10 mm in the center of the spacer (area 10 mm wide and 70 mm long). (c) 10 minutes after applying the vertical load, the second layer towpreg 3 was pulled out in the fiber direction at a tensile speed of 1 mm / min, and the pull-out load was measured. The maximum value of the pull-out load that appears after the start of pulling was taken as the static friction force, and the static friction coefficient was calculated according to the following formulas (2) to (6). At this time, since the area of the overlap part where the second layer towpreg receives the vertical load decreases with pulling, the pull-out displacement at the time when the pull-out load becomes maximum is subtracted from the initial overlap part length, and the value obtained by dividing the pull-out load by twice the vertical load received by the area of the overlap part was taken as the static friction coefficient. In addition, at this time, since the towpreg 3 has slack immediately after the start of measurement, the pull-out displacement at the time when the pull-out load becomes maximum was corrected by subtracting the displacement until the slack was eliminated. The interlaminar friction coefficient in the present invention was calculated by measuring this static friction coefficient three times and using the average value.
[0072]
number
[0073] Here, the symbols in the formulas (2) to (6) have the following meanings. F: Maximum pull-out load (static friction force) N: Vertical load applied to the overlapping part of towpreg 3 and towpreg 4 at maximum load P: Vertical pressure applied to the overlapping portion of towpreg 3 and towpreg 4 at maximum load A 34 : Area of overlap between towpreg 3 and towpreg 4 under maximum load A s : Area of spacer 5 W: Towpreg width L 34 : Length of overlap between towpreg 3 and towpreg 4 at maximum load L 0 : Initial overlap length L 1 Displacement until the initial slack of towpreg 3 is eliminated L t : Pull-out displacement at maximum load.
[0074] <Method of measuring coverage> First, the towpreg was cut into a length of 10 mm and placed on a sample stage so that the surface coated with the epoxy resin composition could be observed. The surface of the towpreg was imaged at a magnification of 200 times using a Keyence digital microscope VHX-5000 while illuminating with a ring light, and a digital image as shown in FIG. 2 was obtained. By illuminating with a ring light, the reflection of light by the epoxy resin was canceled, and an image in which the solid components not dissolved in the epoxy resin were emphasized was obtained. The obtained digital image was then binarized using image analysis software ImageJ, and the parts covered by the solid components not dissolved in the epoxy resin were recognized and their area was calculated. The area of the parts covered by the solid components not dissolved in the epoxy resin obtained by the above method was divided by the area actually captured, and the value expressed as a percentage was used as the coverage rate.
[0075] <Bobbin quality evaluation method> The ends of the bobbins of the towpreg wound at 2,300 m were visually inspected to check for the presence of twill drop and steps due to misalignment of the yarn path, and the beauty of the winding appearance was judged. A was assigned to a condition where there was no twill drop, the ends were aligned, and the winding appearance was good, a B was assigned to a condition where the above abnormalities occurred infrequently but were tolerable, and a C was assigned to a condition where the above abnormalities occurred frequently and were unacceptable. A was the best ranking, and C was the worst.
[0076] <How to make a pressure vessel> A 7.5 L polyethylene liner was placed in a filament winding molding device, and the towpreg of the present invention was wound around the entire liner. As the first layer, a hoop layer at ±89° to the axial direction of the liner was wound to a thickness of 1.4 mm. Next, as the second layer, a helical layer at ±20° to the axial direction of the liner was wound to a thickness of 2.2 mm. Furthermore, as the third layer, a hoop layer at ±89° to the axial direction of the liner was wound to a thickness of 0.6 mm to obtain an intermediate body. The thickness of each layer was determined by measuring the outer diameter with a vernier caliper. The intermediate body was rotated in a curing furnace and cured at 150° C. for 4 hours to obtain a pressure vessel.
[0077] <Evaluation method for filament winding formability> In the process of winding the towpreg around the liner in the method for producing the pressure vessel, the presence or absence of misalignment of the yarn path due to slippage and the presence or absence of gaps between adjacent towpregs were visually observed to evaluate the filament winding moldability. In addition, the degree of seepage of the resin composition from the towpreg bobbin and the degree of scattering of the resin composition in the filament winding molding process were also taken into consideration, and the evaluation was made on a three-level scale from A to C. When there was no slippage or gap and the quality of the intermediate pressure vessel after winding was good, B was when the above abnormalities occurred infrequently but were tolerable, and C was when the above abnormalities occurred frequently and were unacceptable. The evaluation order was A, which was the best, and C was the worst.
[0078] Example 1 An epoxy resin composition was prepared according to the above <Method for preparing epoxy resin composition> using 35 parts by mass of "jER (registered trademark)" 807, 65 parts by mass of "Sumiepoxy (registered trademark)" ELM-434VL as the epoxy resin, and 1.0 part by mass of "jER Cure (registered trademark)" DICY7 and 13.6 parts by mass of "Dyhard (registered trademark)" Fluid 111 as the curing agent. The viscosity of this resin composition at 25°C was 47 Pa s. The cured resin obtained according to the above <Method for preparing cured resin plate> had a glass transition temperature of 147°C and a fracture toughness value (K IC ) is 0.8MPa m 0.5 It was.
[0079] Next, a towpreg was obtained using this epoxy resin composition according to the above-mentioned <Towpreg Production Method>. The towpreg had an Rc of 25.6 mass%, a coverage of 2.9%, and an interlaminar friction coefficient of 0.11. The bobbin quality of this towpreg was evaluated and it was rated A, indicating that the quality was good. In addition, the filament winding moldability was evaluated and it was rated A, indicating that the moldability was good.
[0080] As described above, good results were obtained in all tests.
[0081] (Examples 2 to 4) Epoxy resin compositions and towpregs were prepared and evaluated in the same manner as in Example 1, except that the formulation of the epoxy resin composition was changed as shown in Table 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlaminar friction coefficient, bobbin quality, and filament winding moldability were all favorable. In Example 3, in which the viscosity of the resin composition was relatively high, it was necessary to heat the epoxy resin composition during towpreg production, reduce the viscosity to an easy-to-coat level, and control the temperature so as to prevent an increase in viscosity due to the progress of the curing reaction. However, in Examples 2 and 4, since the viscosity was lower than 50 Pa s, simple temperature control was sufficient, and operability was excellent.
[0082] (Examples 5 to 6) Epoxy resin compositions and towpregs were prepared and evaluated in the same manner as in Example 1, except that the formulation of the epoxy resin composition was changed as shown in Table 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlaminar friction coefficient, bobbin quality, and filament winding formability all showed good results. IC showed excellent values with the addition of toughening agents.
[0083] (Examples 7 to 9) Epoxy resin compositions and towpregs were prepared and evaluated in the same manner as in Example 1, except that the formulation of the epoxy resin composition was changed as shown in Tables 1 and 2. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlaminar friction coefficient, bobbin quality, and filament winding formability all showed good results. IC showed particularly excellent values by using the core-shell rubber particles and the carboxyl-terminated butadiene nitrile rubber in combination. Among them, Examples 7 and 8, in which the mass ratio obtained by dividing the mass of the carboxyl-terminated butadiene nitrile rubber by the mass of the core-shell rubber particles is 0.1 to 0.8, showed particularly excellent K IC It achieves both improvement effect and heat resistance.
[0084] Example 10 Except for changing the composition of the epoxy resin composition as shown in Table 2, the epoxy resin composition and towpreg were prepared and evaluated in the same manner as in Example 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlaminar friction coefficient, bobbin quality, and filament winding formability all achieved good results.
[0085] (Examples 11 to 12) Except for changing the composition of the epoxy resin composition as shown in Table 2, the epoxy resin composition and towpreg were prepared and evaluated in the same manner as in Example 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlaminar friction coefficient, bobbin quality, and filament winding formability all showed good results. IC By containing 3 to 20 parts by mass of a bifunctional aliphatic epoxy resin that is liquid at 25°C per 100 parts by mass of epoxy resin, a high value was exhibited despite the low content of toughening agent compared to Examples 8 to 10, and a specifically excellent effect was exhibited.
[0086] Example 13 Except for changing the composition of the epoxy resin composition as shown in Table 2, the epoxy resin composition and towpreg were prepared and evaluated in the same manner as in Example 1. The evaluation results were the viscosity of the resin composition at 25°C, the glass transition temperature of the cured resin, and the fracture toughness value (K IC ), Rc, coverage, interlaminar friction coefficient, bobbin quality, and filament winding formability all achieved good results. However, because the coverage was relatively low at 2.3%, the evaluation results for bobbin quality and filament winding formability were given a B rating.
[0087] (Comparative Examples 1 to 2) Except for changing the composition of the epoxy resin composition as shown in Table 3, an epoxy resin composition and a towpreg were prepared and evaluated in the same manner as in Example 1. As a result of the evaluation, the interlaminar friction coefficient was less than 0.10, and the evaluation results of both the bobbin quality and the filament winding formability were rated C, which was an insufficient result.
[0088] Comparative Example 3 An epoxy resin composition and a towpreg were produced and evaluated in the same manner as in Example 1, except that the composition of the epoxy resin composition was changed as shown in Table 3, and Rc was set to 18.9%, which is smaller than 20%. As a result of the evaluation, the interlaminar friction coefficient was 0.64, which was larger than 0.50, and therefore the bobbin quality was rated A, which was good. However, in the evaluation of filament winding formability, gaps were easily generated between adjacent towpregs, resulting in an unsatisfactory result of C. Furthermore, due to the small Rc, many voids were generated in the pressure vessel after curing.
[0089] Comparative Example 4 An epoxy resin composition and a towpreg were produced and evaluated in the same manner as in Example 1, except that the composition of the epoxy resin composition was changed as shown in Table 3, and Rc was increased to 43.2%, which is greater than 40%. As a result of the evaluation, the interlaminar friction coefficient was 0.033, which was smaller than 0.10, and the evaluation results of the bobbin quality and filament winding moldability were both rated C, which was insufficient. In addition, because Rc was large, there was a lot of seepage of the resin composition from the towpreg bobbin and a lot of scattering of the resin composition during the filament winding molding process, and the processability was insufficient.
[0090] Comparative Example 5 An epoxy resin composition and towpreg were prepared and evaluated in the same manner as in Example 1, except that the formulation of the epoxy resin composition was changed as shown in Table 3, and the viscosity of the resin composition at 25°C was increased to 169 Pa s, which was greater than 150 Pa s. As a result of the evaluation, the interlaminar friction coefficient was 0.55, which was greater than 0.50, and therefore the bobbin quality was rated A, which was good. However, in the evaluation of filament winding formability, gaps were easily generated between adjacent towpregs, resulting in an unsatisfactory result of rated C.
[0091] [Table 1]
[0092] [Table 2]
[0093] [Table 3]
[0094] The compositions in the table are expressed in parts by mass. [Explanation of symbols]
[0095] 1: Pressure plate 2:Release paper 3: 2nd layer towpreg 4: 1st and 3rd towpreg layers 5: Towpreg for spacers 6: Cellophane tape spacer
Claims
1. An epoxy resin composition having a viscosity of 1 to 150 Pa·s at 25°C, Fineness: 30 to 4000g / 1000m, A towpreg is impregnated with a carbon fiber bundle having a single fiber surface with an arithmetic average roughness (Ra) of 1 to 100 nm, the epoxy resin composition contains a toughening agent that is compatible with epoxy resins at 25°C and / or a toughening agent having a particle size of 50 nm to 1 µm, and the toughness value KIc of a cured product obtained by curing the epoxy resin composition at 150°C for 4 hours is 1.0 to 3.0 MPa·m 0.5 , The resin content (Rc) of the towpreg is 20 to 40 mass%; and a towpreg having an interlayer friction coefficient of 0.10 or more and 0.50 or less, the interlayer friction coefficient being measured by stacking three layers of the towpreg in the same direction and pulling out the central towpreg under conditions of a temperature of 25° C., a humidity of 50% RH, a speed of 1 mm / min, and a vertical load of 20.6 N.
2. 2. The towpreg according to claim 1, wherein, when a surface of the towpreg is observed with an optical microscope at a magnification of 200 times, a ratio (coverage rate) of an area of a portion covered by a solid component not dissolved in an epoxy resin to a field of view area is 2.5% or more and 20% or less.
3. 3. The towpreg according to claim 2, wherein the solid component not dissolved in the epoxy resin is dicyandiamide, the dicyandiamide has a primary particle size of 0.5 to 150 μm, and the content of dicyandiamide per 100 parts by mass of the epoxy resin is 1 to 20 parts by mass.
4. The towpreg according to any one of claims 1 to 3, comprising both core-shell rubber particles and a carboxyl group-terminated butadiene nitrile rubber as the toughening agent.
5. The towpreg according to claim 4, wherein a mass ratio obtained by dividing the mass of the carboxyl group-terminated butadiene nitrile rubber by the mass of the core-shell rubber particles is 0.1 to 0.
8.
6. The towpreg according to any one of claims 1 to 5, wherein the cured product obtained by curing the epoxy resin composition at 150°C for 4 hours has a glass transition temperature of 120 to 160°C.
7. A fiber-reinforced composite material obtained by curing the towpreg according to any one of claims 1 to 6.
Citation Information
Patent Citations
Prepreg and its production
JP1988221122A
Protection board
JP1995113599A
Epoxy resin composition for tow prepreg
JP1997087365A
Epoxy resin composition and prepreg using the same
JP2006083216A
Carbon fiber and method for producing the same
JP2006183173A