Injection foam molding method
By controlling pressure and temperature during the injection foam molding process through a screw stop position and advancement steps, the method achieves uniform expansion and bubble distribution, enhancing product quality.
Patent Information
- Application Number
- JP2020190047
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-11-16
AI Technical Summary
Existing injection foam molding methods face issues with uneven expansion ratio and bubble diameter distribution due to uncontrolled pressure drops and foaming processes, leading to poor surface transferability and defects in foam molded products.
A method involving controlled pressure and temperature management during the injection and filling process, including a screw stop position and subsequent advancement steps to maintain uniform expansion and bubble distribution without expanding the mold cavity volume.
This approach results in a foam molded product with uniform expansion ratio and bubble diameter distribution, improving surface transferability and reducing defects.
Smart Images

Figure 0007589514000001 
Figure 0007589514000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an injection foam molding method for molding a foam-molded product by injecting and filling a molten resin containing a foaming material into a mold cavity. [Background technology]
[0002] There are roughly two types of injection foam molding methods for forming foam molded products. In one method, molten resin containing a foaming material that has been plasticized (melted) in an injection device is injected into a mold cavity formed by clamping the mold to fill the mold cavity to a volume that does not fill the mold cavity (so-called short shot filling), and then the mold cavity is filled, including the unfilled portion from the initial injection filling, with the increase in volume of the molten resin due to the foaming and expansion of the foaming material contained in the molten resin. One example is Patent Document 1. This method is referred to as the "SS (short shot) foam molding method" in this application.
[0003] The other method is to inject and fill the mold cavity with molten resin containing a foaming material (so-called full pack filling), and then expand the volume of the mold cavity to foam and expand the foaming material contained in the molten resin. One example is Patent Document 2. This method is referred to as the "CB (core-back) foam molding method" in this application.
[0004] In the CB foam molding method, the volume expansion of the mold cavity is often achieved by opening the movable mold from the fixed mold by a predetermined amount using a mold with a shear edge structure. The shear edge structure of the mold is also called a cut-in structure or a spigot structure, and is a commonly known structure for the fitting structure that forms the dividing surface of the mold. By forming a fitting part between the fixed mold and the movable mold that extends in the mold opening and closing direction and can be inserted and removed while sliding against each other, the mold cavity is not opened even when the mold is opened by a predetermined amount, and the molten resin injected and filled in the mold cavity is prevented from leaking out of the mold.
[0005] The former SS foam molding method has the advantage of not requiring a large injection pressure because it is a short shot filling method, but it has the problem of filling defects and poor appearance quality (transfer defects) because the unfilled part in the mold cavity is filled with molten resin only by the foaming expansion force of the foaming material contained in the molten resin during injection filling (paragraphs 0003 and 0004 of the specification of Patent Document 1).
[0006] In addition, in the SS foam molding method, the pressure of the molten resin filled in the mold cavity is not controlled at all, so the foaming expansion of the foaming material contained in the molten resin occurs naturally. As a result, the pressure at the flow front of the molten resin in the mold cavity is extremely low, and the foaming expansion cannot be suppressed, so the bubbles (foam cells) become coarse and may burst. Alternatively, the unfilled parts at the time of injection filling are filled only by the volume expansion of the molten resin due to foaming expansion, so the bubbles grow large and become coarse. On the other hand, the pressure of the molten resin near the gate in the mold cavity is high, so bubbles do not occur, or if they do occur, they remain small and do not grow to an appropriate size. As a result, the distribution of the expansion ratio and bubble diameter in the foam molded product is inevitably uneven (uneven).
[0007] In the latter CB foam molding method, the volume of the mold cavity is expanded after full-pack filling, and the pressure in the mold cavity is reduced by a controlled operation, thereby foaming and expanding the foaming material contained in the molten resin. Therefore, compared to foam molded products by the SS foam molding method, full-pack filling provides superior appearance quality (transferability). In addition, the mold cavity volume is expanded with high precision by moving the movable platen in the mold opening direction using a mold clamping device equipped with a toggle-type mold clamping mechanism, and the pressure drop can be controlled with high precision, making it possible to control the foaming ratio, bubble diameter, thickness, etc. of the foam molded product with high precision (paragraphs 0002 and 0003 of the specification of Patent Document 2). Furthermore, this mold cavity volume expansion expands the mold cavity volume uniformly in the thickness direction of the foam molded product, so that the distribution of the foaming ratio and bubble diameter in the foam molded product becomes uniform. However, compared to normal molds, molds with a share edge structure have the disadvantage of being expensive.
[0008] On the other hand, a SS foam molding method that aims to eliminate the disadvantages of the former SS foam molding method has been disclosed. One example is Patent Document 3. In the manufacturing method of foam molded products in Patent Document 3, after the molten resin containing the foaming material is injected and filled into the mold cavity (60% or more of the mold cavity volume), a pullback process is performed in which the screw is retracted from the injection filling completion position. This pullback process causes the molten resin injected and filled into the mold cavity to flow back to the nozzle side of the injection device, and moves the bubbles (foam cells) unevenly distributed in the molten resin at the flow tip of the mold cavity to the flow start side of the mold cavity (the nozzle side of the injection device), thereby controlling the position of the bubbles (foam cells) (paragraphs 0010 and 0011 of the specification of Patent Document 3). Naturally, this pullback process is performed in a state in which the mold cavity and the injection device are communicated via the injection nozzle. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 08-103919 [Patent Document 2] JP 2008-143061 A [Patent Document 3] JP 2020-111029 A Summary of the Invention [Problem to be solved by the invention]
[0010] In order to move the bubbles (foam cells) in the molten resin at the flow front of the mold cavity to an arbitrary part of the flow path, for example, the vicinity of the gate of the mold cavity, by the pullback process of Patent Document 3, a corresponding pullback stroke is required. If the pullback stroke is small, the bubbles (foam cells) in the molten resin at the flow front only move slightly from the flow front to the flow start side (gate side). If the pullback stroke is large, filling failure occurs due to insufficient amount of resin at the flow front. Therefore, even if the manufacturing method of the foam molded product of Patent Document 3 can control the position of the bubbles (foam cells) at the flow front to some extent, it must be said that it is insufficient to prevent the expansion ratio and the distribution of the bubble diameter in the foam molded product from becoming uneven (uneven).
[0011] In addition, the drop in pressure of the molten resin caused by this pullback process is also a problem. The largest pressure drop is not in the mold cavity, but in the molten resin in the storage area in front of the screw of the injection device. In an in-line screw type injection device that has a built-in screw that can rotate and move forward and backward, the screw is rotated in the metering process to plasticize (melt) the resin material and cause the molten resin to flow forward of the screw. As the volume of the molten resin in front of the screw increases, the screw is moved backward while applying a certain resistance force (back pressure), and the amount of molten resin required for one injection filling is stored in front of the screw at a pressure equivalent to the back pressure. The space in front of the screw in the injection device where the plasticized molten resin is stored in this way is called the storage area.
[0012] The next largest pressure drop occurs in the molten resin near the gate of the mold cavity. Therefore, this pullback process moves the bubbles (foam cells) in the molten resin at the front end of the flow to the flow start side (gate side), but in exchange, the large pressure drop described above causes large bubbles (foam cells) to grow in the molten resin near the gate of the mold cavity and in the reservoir of the injection device. As a result, the foam molded product molded by the foam molded product manufacturing method of Patent Document 3 has a non-uniform (uneven) distribution of the expansion ratio and bubble diameter in the foam molded product, that is, a defective product with poor surface transferability in which coarse and unfoamed regions of bubbles (foam cells) are mixed.
[0013] In addition, due to this pullback process, large bubbles (foam cells) generated in the molten resin in the storage section of the injection device cannot maintain the bubbly state and burst. The foaming gas that flows out from the bubbles into the molten resin is not completely remelted in the molten resin within the range of a series of molding cycles. Therefore, the foaming gas may be integrated together, or may be completely separated from the molten resin, or may be released to the outside of the injection device. In the next injection filling, in the former case, the integrated foaming gas is directly filled into the mold cavity, which causes a poor foaming molded product having a large cavity inside. Alternatively, if the integrated bubbles burst during injection filling, it causes a poor appearance of the foaming molded product, such as swirl marks. In the latter case, the foaming material disappears, and the molten resin without bubbles (foam cells) is stored in the storage section without being mixed with the molten resin containing the foaming material that is newly stored in the storage section, and then injected and filled into the mold cavity. As a result, the molten resin, which does not generate bubbles (foam cells), fills the flow front in particular, forming unfoamed portions.
[0014] An object of the present invention is to provide an injection foam molding method for molding a foam-molded product having a uniform expansion ratio and a uniform distribution of cell diameters without expanding the volume of the mold cavity. [Means for solving the problem]
[0015] In order to achieve the above object, one injection foam molding method according to the present invention includes a metering step of storing a molten resin containing a foaming material in a storage section in front of a screw while maintaining a pressure range that does not cause foaming; The molten resin is filled into the mold cavity in a full pack manner while leaving a predetermined amount of the molten resin in the reservoir. an injection filling step of stopping the screw at a screw stop position L1 where the pressure of the molten resin remaining in the reservoir is maintained within the pressure range; A screw position holding process for holding the screw at the screw stop position L1; The present invention is characterized by comprising:
[0016] In one injection foam molding method according to the present invention, after the screw position holding step, a screw re-advancement step 1 is further provided in which the screw is advanced from the screw stop position L1 with a predetermined forward force F1, The pressure of the molten resin in the reservoir may be maintained within the pressure range by advancing the screw with the predetermined advancing force F1.
[0017] In one injection foam molding method according to the present invention, after the screw position holding step, a screw re-advancement step 2 is further provided in which the screw is advanced from the screw stop position L1 at a predetermined forward speed V1, The pressure of the molten resin in the reservoir may be maintained within the pressure range by advancing the screw at the predetermined forward speed V1. Effect of the Invention
[0018] According to the present invention, it is possible to provide an injection foam molding method for molding a foam-molded product having a uniform expansion ratio and a uniform distribution of cell diameters without expanding the volume of the mold cavity. [Brief description of the drawings]
[0019] [Figure 1]1 is a schematic cross-sectional side view showing the inside of a mold cavity of a mold and a reservoir of an injection device from the completion of injection filling to the cooling and solidification of a foam-molded product in an injection foam molding method according to a first embodiment. FIG. [Diagram 2] FIG. 11 is a schematic cross-sectional side view showing the inside of a mold cavity of a mold and a reservoir of an injection device during a screw re-forward step of an injection foam molding method according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings.
[0021] [First embodiment] The injection foam molding method according to the first embodiment of the present invention will be described with reference to Fig. 1. Fig. 1 is a schematic side cross-sectional view showing the inside of the mold cavity of the mold and the reservoir of the injection unit from the completion of injection filling to the cooling and solidification of the foam-molded product in the injection foam molding method according to the first embodiment. Note that since the present invention is premised on a standard injection molding machine equipped with an in-line screw type injection unit, a description of the injection unit, mold clamping unit, etc. of the injection molding machine will be omitted.
[0022] 1(a) shows the mold cavity 11 of the mold 10 and the inside of the reservoir 21 of the injection device 20 immediately after the completion of the injection filling process. To facilitate understanding of the present invention, the mold cavity 11 formed by clamping the mold 10 is illustrated as a simple rectangle. Furthermore, the mold cavity 11 will be described by dividing it into three regions, a gate region FG, a flow middle region FM, and a flow front region FE, from the gate side of the mold cavity 11 where the injection device 20 is docked to the mold 10.
[0023] As for the injection device 20, in addition to the storage section 21, only the screw 22, the flight 22a, and the check ring 22b are shown in the figure. The check ring 22b is a general check valve used in an in-line screw type injection device. In the metering process, the check ring 22b is moved forward by the pressing force of the molten resin flowing forward (left side of FIG. 1(a)) by the rotation of the screw 22, and opens a resin flow path of the molten resin to the front of the screw 22. Then, in the injection filling process, the check ring 22b is moved backward by the pressure of the molten resin in the storage section 21 by the advancing screw 22, and closes the resin flow path to the rear of the check ring 22b, preventing the molten resin from flowing back from the storage section 21 during injection filling.
[0024] First, the metering process will be described. Although not shown in the figure, in the metering process, the molten resin containing the foaming material is plasticized, melted, and kneaded while maintaining the pressure range that does not cause foaming, and a predetermined amount is stored in the storage section 21 in front of the screw 22. As described above, the pressure range that does not cause foaming is maintained by a predetermined resistance force (back pressure) that is applied when the screw 22 is retreated. The foaming material may be any of a chemical foaming agent or a thermal expansion microcapsule that is kneaded in advance with a pellet-shaped resin material, or a physical foaming agent such as nitrogen or carbon dioxide that is mixed into the molten resin in the injection device 20 by various methods and devices. The pressure range that does not cause foaming varies depending on the type and amount of foaming agent, the resin temperature, and the like. For example, in the case of a chemical foaming agent, it is preferable to set the pressure range higher than the pressure of the foaming gas generated by the thermal decomposition of the chemical foaming agent in the process of plasticizing the resin material. On the other hand, in the case of a physical foaming agent, it is preferable to set the pressure range higher than the supply pressure (for example, 1 to 15 MPa) required to dissolve nitrogen or carbon dioxide into the molten resin.
[0025] Regardless of the foaming material, it is preferable to maintain the pressure so that the molten resin in storage section 21 does not foam from the start of the injection filling process to the completion of the screw position holding process described below. Suppose that the pressure of the molten resin in storage section 21 just before the start of the injection filling process after the metering process is completed is PS0 (zero), and this PS0 is within the above-mentioned pressure range that does not cause foaming. And, the temperature of the molten resin in storage section 21 just before the start of the injection filling process, in which the molten state is maintained by a heating means (not shown) of injection device 20, is TS0 (zero).
[0026] Next, after the measurement step is completed, the injection filling step is performed. In the injection filling step, the molten resin in the storage section 21 is filled into the mold cavity 11 in a full pack. Naturally, the storage section 21 and the mold cavity 11 are in communication with each other through the injection nozzle of the injection device 20 (details are omitted) and the resin flow path in the mold of the mold 10 (details are omitted). Here, in order to maintain the pressure range in which the molten resin in the storage section 21 does not foam, it is preferable to select a combination of the configurations of the injection device 20 and the mold 10 that allows the storage section 21 to be sealed in other steps except the injection filling step, and allows the storage section 21 and the mold cavity 11 to be in communication with each other only in the injection filling step. The range of the storage section 21 differs depending on this combination. This will be briefly explained.
[0027] In the case where the gate portion on the mold side (the portion connecting the resin flow path in the mold and the mold cavity) is an open gate that is always open, the tip portion of the injection nozzle on the injection device 20 side (the portion connecting to the resin flow path in the mold) is provided with a valve mechanism (shut-off valve, etc.) that blocks / opens the flow of molten resin to maintain the pressure in the storage portion 21. In this case, the storage portion 21 is between the front end of the screw 22 and the shut-off valve. Note that the resin remaining in the resin flow path in the mold and the gate portion beyond the shut-off valve is removed from the mold 10 together with the foam-molded product.
[0028] When the gate part on the mold side is equipped with a valve mechanism (gate valve, etc.) that blocks / opens the molten resin flow, the injection nozzle may be either in a constantly open form (open nozzle, etc.) or equipped with a valve mechanism such as a shut-off valve. In this case, in order to equalize the pressure in the reservoir 21, it is preferable that the pressure in the reservoir 21 is maintained by closing the valve mechanism of the gate part on the mold side, and the shut-off valve of the injection nozzle is set to be constantly open. In this case, the reservoir 21 is between the front end of the screw 22 and the gate valve including the resin flow path in the mold, and only the foam-molded product in the mold cavity 11 is removed from the mold 10. The temperature of the molten resin in the resin flow path in the mold is adjusted in the same way as in the injection device 20.
[0029] Here, the injection filling process of the present invention, as shown in Fig. 1(a), is characterized in that the mold cavity 11 is filled with full pack molten resin while a predetermined amount of molten resin remains in the storage section 21, the pressure of the molten resin remaining in the storage section 21 is maintained within the pressure range that does not cause foaming as explained in the metering process above, and the forward movement of the screw 22 is stopped at the screw stop position L1 that satisfies both of these conditions. Fig. 1(a) shows the mold cavity 11 of the mold 10 and the inside of the storage section 21 of the injection device 20 immediately after the injection filling process is completed.
[0030] Here, full-pack filling generally means filling the entire mold cavity 11 with molten resin. On the other hand, in the present invention, a predetermined amount of molten resin is left in the storage part 21 during full-pack filling. Let the pressure of the molten resin left in the storage part 21 at this time be PS1. Due to the flow resistance of the molten resin in the mold cavity 11, the pressure of the molten resin in the storage part 21 gradually increases with the passage of time from the start of the injection filling process. Therefore, the pressure PS1 of the molten resin in the storage part 21 during full-pack filling is greater than the pressure PS0 of the molten resin in the storage part 21 immediately before the start of the injection filling process (PS0 < PS1). For this reason, PS1 is maintained within a pressure range where foaming does not occur. Also, the temperature of the molten resin in the storage part 21 is constantly controlled by heating means arranged in the injection device 20 and the mold 10. Therefore, the temperature TS1 of the molten resin in the storage part 21 immediately after the completion of the injection filling process is controlled to be the same as the temperature TS0 immediately before the start of the injection filling process.
[0031] The actual mold cavity is different from the simple-shaped mold cavity 11 shown in Fig. 1(a). In a more complex-shaped mold cavity that mimics the molded product, due to changes in the flow resistance caused by the flow cross-sectional area and the curvature of the flow path for each part where the resin flows, as well as changes in the viscosity of the molten resin that vary depending on the flow distance from the gate part of the mold cavity, etc., the pressure of the molten resin in the mold cavity varies depending on the flow part and region. However, generally, the pressure of the molten resin fully packed in the mold cavity is the highest at the gate part and the lowest at the flow tip. Similarly, the temperature of the molten resin fully packed in the mold cavity is the highest at the gate part where the flow distance in the mold cavity is the shortest and the lowest at the flow tip where the flow distance is the longest.
[0032] Therefore, if the pressures / temperatures of the molten resin in the three regions of the gate portion region FG, the flow intermediate region FM, and the flow tip region FE immediately after full-pack filling are PG1 / TG1, PM1 / TM1, and PE1 / TE1, respectively, the relationship between the pressure PS1 / temperature TG1 of the molten resin in the storage portion 21 and the pressures / temperatures of the above three regions is PE1 < PM1 < PG1 < PS1, and TE1 < TM1 < TG1 < TS1 (see Fig. 1(a)). And immediately after the injection filling process is completed, when the pressure of the molten resin becomes lower than the pressure range that does not cause foaming, foaming expansion starts from the foaming material in the molten resin. Therefore, the molten resin at the flow tip of the flow tip region FE, where the pressure and temperature are the lowest, becomes the starting point of foaming expansion.
[0033] Here, foaming expansion is a process in which the foaming gas of the foaming material dissolved in the molten resin changes in the formation of foaming nuclei, the generation of foaming cells, and the growth of foaming cells when released from the molten resin. By appropriately controlling each process of this foaming expansion, a foamed molded product having innumerable bubbles can be obtained. In Fig. 1, the formation of foaming nuclei, the generation, and growth of foaming cells are imaged, and the foaming nuclei and small foaming cells are illustrated as small black circles, and the growing or grown foaming cells are illustrated as small white circles. It should be understood that the regions where these small black circles and small white circles are not drawn are filled with molten resin, and no foaming expansion has occurred in the molten resin, and there are no foaming cells. Also, a dashed line is drawn slightly separated from the inner surface of the mold cavity 11. It should be understood that the space between this dashed line and the inner surface of the mold cavity 11 images the skin layer 12 formed by the molten resin contacting the inner surface of the mold cavity 11 and being heat-extracted during injection filling of the molten resin. And in order to show the passage of time, the number "1" attached to each item such as PG1 / TG1 will be changed to "2", "3" in order of the passage of time hereafter.
[0034] Here, the present invention is characterized by including a screw position holding step for holding the screw 22 at the screw stop position L1 after the injection filling step. Specifically, a predetermined position holding force is generated by a drive source (not shown) of a drive mechanism for advancing and retracting the screw 22, and control is performed to hold the screw 22 at the screw stop position L1 for a predetermined time. By this screw position holding step, the volumes of the mold cavity 11 and the reservoir 21, which are in a communicating state, are maintained constant immediately after the completion of the injection filling step.
[0035] On the other hand, in contrast to the molten resin in reservoir 21, whose temperature is controlled to be constant, the temperature of the molten resin gradually decreases over time in the above-mentioned three regions of mold cavity 11 communicating with reservoir 21.
[0036] Therefore, immediately after the completion of the injection filling process, the growth of foam cells in the molten resin at the flow front of the flow front region FE, which has the lowest temperature, is suppressed by the increase in the viscosity of the molten resin caused by the temperature drop of the molten resin over time. Furthermore, when the viscosity of the molten resin becomes higher than the pressure of the foaming gas in the foam cells, the growth of the foam cells stops before they become coarse, resulting in a collection of fine foam cells. On the other hand, although the temperature of the molten resin in the flow intermediate region FM and the gate region GM, or the molten resin in the storage section 21, is high, the pressure of the molten resin is sufficiently higher than the lower limit of the pressure range that does not cause foaming, so foaming and expansion of the molten resin in these regions does not start, and the foaming gas of the foaming material remains dissolved in the molten resin (see FIG. 1(a)).
[0037] Fig. 1(b) shows the inside of the mold cavity 11 of the mold 10 and the reservoir 21 of the injection device 20 while the molten resin is cooling and solidifying. In Fig. 1(b), which is a state where more time has passed since the state shown in Fig. 1(a), as the pressure in the flow front region FE of the mold cavity 11 decreases, the pressure in the adjacent flow middle region FM also gradually decreases, and when it becomes smaller than the pressure range where foaming does not occur, the molten resin in the flow middle region FM starts to foam and expand, foam nuclei are formed, and grow into foam cells. In this way, the region where foaming and expansion starts due to the propagation of the pressure decrease gradually shifts from the flow front region FE to the gate region FG.
[0038] In addition, at the same time as the transition to foaming and expansion, the growth of the foam cells is suppressed by the increase in viscosity of the molten resin caused by the decrease in temperature of the molten resin over time. When the viscosity of the molten resin becomes higher than the pressure of the foaming gas in the foam cells, the growth of the foam cells stops before they become coarse, and the intermediate flow region FM becomes a collection of fine foam cells (see Figure 1(b)).
[0039] From the flow front region FE to the flow middle region FM, the pressure and temperature of the molten resin become uniform, the growth of foam cells almost stops in the flow front region FE, and in the flow middle region FM, the formation of foam nuclei and the growth of foam cells are partially mixed and proceeding. The temperature TS2 of the molten resin in the storage section 21 at this time is controlled to the same temperature as the temperature TS0 immediately before the start of the injection filling process, just like TS1.
[0040] At this time, the pressure / temperature relationships of the molten resin in the storage section 21 and the three regions in the mold cavity 11 are such that PE2 ≦ PM2 < PG2 < PS2, and TE2 ≦ TM2 < TG2 < TS2 (see Fig. 1(b)). Naturally, with the passage of time, the pressure / temperature relationship of the molten resin in the flow front region FE is such that PE1 > PE2 and TE1 > TE2 (see Fig. 1(b)). Similarly, in other regions, the items marked with the symbol "1" have higher numerical values than those marked with the symbol "2". Also, similar to Fig. 1(a), there is no foaming expansion in the molten resin in the regions where the black and white circles are not drawn, and there are no foam cells. Naturally, the pressure PS2 of the molten resin in the storage section 21 is also maintained within the pressure range where foaming does not occur.
[0041] On the other hand, in the flow front region FE of Fig. 1(b) where the growth of the foam cells has stopped, the temperature drop of the molten resin further progresses, and the cooling and solidification shrinkage of the molten resin begins. Along with this cooling and solidification shrinkage, the volume of the molten resin decreases as the foam cells and all shrink. At this time, in accordance with the volume decreased by the cooling and solidification shrinkage of the molten resin, the molten resin is replenished from the adjacent flowing intermediate region FM where the pressure and temperature of the molten resin are high, towards the flow front region FE. Further, from the gate region FG where the pressure and temperature are high, the molten resin is replenished towards the flowing intermediate region FM in accordance with the volume decreased by the replenishment. Due to this chain of replenishment of the molten resin, the molten resin is sequentially supplied as shown by the arrows in Fig. 1(b). In Fig. 1(b), the molten resin is continuously supplied from the gate region FG to the flowing intermediate region FM, and from the storage section 21 to the gate region FG. Also, the chain of replenishment of the molten resin is accompanied by the propagation of the pressure drop of the molten resin.
[0042] The volume reduction caused by the cooling, solidifying, and shrinking of the molten resin in the mold cavity 11 is prevented by the pressure / temperature deviation of the molten resin in the mold cavity 11, which is higher than that of the gate side, and the molten resin is sequentially replenished in one direction from the gate side to the flow front, thereby naturally supplying the molten resin without artificial control. At the same time, the pressure drop of the replenished molten resin sequentially causes the formation of foam nuclei in the molten resin, the generation of foam cells, and the growth of the foam cells, and the temperature drop of the replenished molten resin sequentially stops the growth of the foam cells in the molten resin. These behaviors proceed sequentially from the flow front region FE to the gate region FG, contributing to the molding of a foam-molded product with a uniform foaming ratio and a uniform distribution of bubble diameter.
[0043] FIG. 1(c) shows the inside of the mold cavity 11 of the mold 10 and the reservoir 21 of the injection device 20 just before the molten resin is cooled and solidified. In FIG. 1(c), the molten resin supplied to the gate region FG from the reservoir 21 starts foaming and expanding due to the pressure drop of the molten resin similar to that in other regions due to the pressure / temperature deviation of the molten resin in FIG. 1(b), and the growth of foam cells stops due to the drop in temperature of the molten resin. As a result, the pressure and temperature of the molten resin become uniform in the entire region of the mold cavity 11 from the flow front region FE to the gate region FG, and the growth of foam cells in the entire region stops with the distribution of the foaming ratio and the bubble diameter being uniform. The temperature TS3 of the molten resin in the reservoir 21 at this time is controlled to the same temperature as the temperature TS0 just before the start of the injection filling process, similar to TS1 and TS2.
[0044] At this time, the pressure / temperature relationships of the molten resin in the storage part 21 and the three regions in the mold cavity 11 are PE3≒PM3≦PG3<PS3, and TE3≒TM3≦TG3<TS3 (see Fig. 1(c)). Naturally, the pressure / temperature relationship of the molten resin in the flow front region FE with the passage of time is PE2>PE3 and TE2>TE3. Similarly, in other regions, the numerical values of the items with the symbol "2" are higher than those of the items with the symbol "3". On the other hand, as in Fig. 1(a) and Fig. 1(b), there is no foaming expansion in the molten resin in the storage part 21 where no black or white small circles are drawn, and there are no foam cells. Naturally, the pressure PS3 of the molten resin in the storage part 21 is also maintained within the pressure range where foaming does not occur.
[0045] The screw position holding process is preferably completed at the timing when the temperature of the molten resin in the mold cavity 11 reaches below the heat distortion temperature of the molten resin, that is, in the first embodiment, at the timing when the temperature TG3 of the molten resin in the gate part region FG, which has the slowest temperature drop, reaches below the heat distortion temperature of the molten resin. Also, depending on the resin type, product shape, etc., the glass transition temperature may be used instead of the heat distortion temperature. Furthermore, it may be based on the timing when the time required to cool the foam molded product in the mold cavity 11 has elapsed until the cooling and solidification temperature that can satisfy the product dimensions and product strength. This timing is regarded as the completion of the cooling and solidification of the molten resin. The pressure of the molten resin in the mold cavity 11 also becomes equal in all regions. In the first embodiment, in order to maintain the pressure of the molten resin in the storage part 21 within the pressure range where foaming does not occur, after the completion of the screw position holding process, the communication state between the mold cavity 11 and the storage part is released, the storage part 21 is made airtight, and then the mold is opened to take out the foam molded product.
[0046] As described above, in the injection foam molding method of the first embodiment, by performing full pack filling in a state where the storage part 21 and the mold cavity 11 are in communication, it is possible to mold a foam molded product with excellent transferability that suppresses filling defects and appearance quality defects (transfer defects) compared to the SS foam molding method.
[0047] In addition, in the injection filling process, the pressure of the molten resin in the reservoir 11 is maintained within a pressure range that does not cause foaming, so that in the screw position holding process after the injection filling process, continuous resin pressure is applied to the molten resin in the mold cavity 11, and the amount of the molten resin that has decreased in volume due to cooling, solidification, and shrinkage is continuously supplied. As a result, it is possible to mold a foam-molded product with a uniform foaming ratio and cell diameter distribution without expanding the volume of the mold cavity.
[0048] Then, even when the screw position holding step is completed, the pressure of the molten resin in storage portion 21 is maintained within a pressure range that does not cause foaming, so that in the next injection molding step, the molten resin in storage portion 21 can be injected and filled into mold cavity 11 as molten resin containing foaming material without foaming the molten resin in storage portion 21. As a result, a foam-molded product with a uniform foaming ratio and bubble diameter distribution in all parts can be molded.
[0049] In addition, in the injection filling process, the specified amount of molten resin to be left in the storage section 21 when the molten resin is fully packed and filled into the mold cavity 11 is preferably determined by test molding, etc., taking into consideration the following: the pressure range of the molten resin in the storage section 21 is set to a "pressure range that does not cause foaming", screw stop position L1 of the screw 22 can be secured, the molten resin in the mold cavity 11 can be reliably supplied in association with the cooling, solidifying and shrinking of the molten resin based on the pressure / temperature deviation, and molten resin maintained in a pressure range that does not cause foaming is secured for the next injection molding process at the time the screw position holding process is completed, or the amount of molten resin in the metering process that is necessary to satisfy the above conditions of the injection filling process in the first embodiment.
[0050] [Second embodiment] Next, an injection foam molding method according to a second embodiment of the present invention will be described with reference to Fig. 2. Fig. 2 is a schematic side cross-sectional view showing the inside of the mold cavity of the mold and the reservoir of the injection device in the screw re-advance step of the injection foam molding method according to the second embodiment. The injection foam molding method according to the second embodiment differs from the injection foam molding method according to the first embodiment in that it further includes a screw re-advance step of advancing the screw 22 from the screw stop position L1 after the screw position holding step.
[0051] First, the screw re-advancement step 1 in which the screw 22 is advanced with a predetermined advancement force F1 will be described. Here, Fig. 2(a) shows a state corresponding to Fig. 1(b) described in the first embodiment. Specifically, from the flow front region FE to the flow intermediate region FM, the pressure and temperature of the molten resin become uniform, the growth of foam cells in the flow front region FE has almost stopped, and in the flow intermediate region FM, the formation of foam nuclei and the generation and growth of foam cells are partially occurring in a mixed manner.
[0052] As explained above, in the flow front region FE where the growth of the foam cells has stopped, the temperature of the molten resin continues to drop, and the molten resin begins to cool, solidify, and shrink. As a result of this cooling, solidifying, and shrinking, the volume of the molten resin decreases, including the foam cells. Therefore, in Fig. 2(a), similar to Figs. 1(b) and 1(c), molten resin is continuously supplied from the flow middle region FM to the flow front region FE, from the gate region FG to the flow middle region FM, and from the reservoir 21 to the gate region FG, in accordance with the volume reduced by the cooling, solidifying, and shrinking of the molten resin, to compensate for the volume reduction caused by the cooling and solidifying of the molten resin in the mold cavity 11.
[0053] At this time, the supply of molten resin as described above varies depending on the type of molten resin, the shape of the mold cavity 11, etc., and may be insufficient to cover the volume loss caused by the cooling, solidifying, and shrinking of the molten resin in the mold cavity 11. For example, as shown in FIG. 2(a), this may be the case when the pressure difference between the molten resin in the flow middle region FM and the flow front region FE is small, or when the pressure difference between the gate region FG and the flow middle region FM is small (PE2≦PM2≦PG2). Alternatively, this may be the case when the temperature difference between the molten resin in each region is small (TE2≦TM2≦TG2). In such cases, the supply of molten resin in accordance with the cooling, solidifying, and shrinking of the molten resin is not performed appropriately, resulting in poor filling, poor appearance quality (poor transfer), and a poor quality foam-molded product with uneven expansion ratio and cell diameter.
[0054] In such a case, as shown in Figures 2(a) and 2(b), screw re-advance step 1 is performed. Specifically, the amount of molten resin supplied from the reservoir 21 to the gate region FG utilizing the pressure / temperature deviation is increased to a supply amount corresponding to the volume reduction caused by the cooling, solidification, and shrinkage of the molten resin in the mold cavity 11 by advancing the screw 22 from the screw stop position L1 (Figure 2(a)) with a predetermined forward force F1 using the molten resin in the reservoir 21.
[0055] At this time, the predetermined forward force F1 (FIG. 2(a)) of the screw 22 may be determined to have a suitable magnitude by test molding or the like, but it is preferable that the magnitude be such that, in the screw re-forward movement step 1, a pressure / temperature deviation is given to the molten resin in the mold cavity 11 so that the supply of molten resin accompanying cooling solidification shrinkage can be ensured until the cooling of the molten resin is completed, and the pressure of the molten resin in the storage section 21 can be maintained with the lower limit of the pressure range that does not cause foaming as a guide. The reason why the lower limit is preferable is to avoid the occurrence of poor foaming, in which the pressure of the part in the mold cavity 11 to which the molten resin is oversupplied rises excessively to the pressure range that does not cause foaming due to the supply of molten resin in excess of the cooling solidification shrinkage, making it difficult for the molten resin to foam and expand.
[0056] By the screw re-advance step 1 as described above, the volume reduction caused by the cooling, solidifying, and shrinking of the molten resin in the mold cavity 11 is compensated for without significantly changing the natural supply state of the molten resin using the pressure / temperature deviation, and the pressure / temperature deviation of the molten resin in the mold cavity 11 is maintained as in the first embodiment. Then, the formation of foam nuclei in the molten resin (in the intermediate flow region FM in the second embodiment), the generation of foam cells, the amount of foam cells generated, and the coarsening of the foam cells are suppressed, and a foam-molded product with a uniform foaming ratio and a uniform distribution of the bubble diameter of the foam cells can be molded. This is shown in FIG. 2(b). FIG. 2(b) shows the state immediately before the cooling and solidifying of the molten resin is completed, which corresponds to FIG. 1(c) described in the first embodiment.
[0057] In the second embodiment, it is assumed that the supply shortage of the molten resin due to the volume reduction accompanying the cooling, solidifying, and shrinking of the molten resin in the mold cavity 11 occurs in the flow intermediate region FM. However, when such a supply shortage of the molten resin occurs, in which region it occurs, that is, the timing of occurrence from the start of the screw position holding step, differs depending on the type of molten resin and the shape of the mold cavity 11. Therefore, it is preferable to confirm whether or not the supply shortage of the molten resin occurs, and, if it occurs, in which region of the foam-molded product it occurs, by test molding using the injection foam molding method described in the first embodiment, and to determine whether or not the screw re-advancement step 1 is necessary, and, if necessary, the timing of starting the screw re-advancement step 1 after the start of the screw position holding step. In addition, although the predetermined forward force F1 is a fixed value, it is also possible to set multiple stages of pressure as necessary in response to an increase in the forward resistance force of the screw 22 due to an increase in the melt viscosity of the molten resin in the mold cavity 11 over time, or a decrease in the supply amount of the molten resin accompanying the progress of the cooling and solidifying range of the molten resin in the mold cavity 11.
[0058] In addition, the screw re-advance step 1 is preferably completed not based on the movement distance (advance distance) of the screw 22 from the screw stop position L1, but based on the time when the molten resin in the mold cavity 11 cools and solidifies (movement time / advance time). Specifically, as described above in the first embodiment, the step may be completed based on the timing when the temperature TG3 of the molten resin in the gate region FG, which has the slowest temperature drop, reaches the thermal deformation temperature of the molten resin or lower. Alternatively, the step may be completed based on the timing when the cooling and solidification of the molten resin in the mold cavity 11 progresses and it becomes difficult to advance the screw 22 with the predetermined forward force F1, that is, when the flow resistance of the molten resin in the mold cavity 11 becomes greater than the predetermined forward force F1. In either case, after completing the screw re-forward step 1 and sealing the storage section 21, the mold is opened and the foam-molded product is removed from the mold cavity 11, so long as the foam-molded product has reached a strength that does not cause problems such as deformation, then it is appropriate to select the timing that results in the shorter molding cycle.
[0059] Next, the screw re-forward movement process 2 in which the screw 22 is advanced at a predetermined forward movement speed V1 will be described. The difference from the screw re-forward movement process 1 is that in the re-forward movement of the screw 22, the forward movement speed, not the forward movement force, of the screw 22 is controlled. Therefore, similarly to the screw re-forward movement process 1, only the difference from the screw re-forward movement process 1 will be described with reference to Fig. 2. The premise is also the same that a shortage of molten resin supply occurs in the intermediate flow region FM due to a volume reduction accompanying cooling, solidification, and shrinkage of the molten resin in the mold cavity 11.
[0060] In such a case, as shown in Figures 2(a) and 2(b), screw re-advance step 2 is performed. Specifically, the amount of molten resin supplied from the reservoir 21 to the gate region FG utilizing the pressure / temperature deviation is increased to a supply amount corresponding to the volume reduction caused by the cooling, solidification, and shrinkage of the molten resin in the mold cavity 11 by advancing the screw 22 from the screw stop position L1 (Figure 2(a)) at a predetermined forward speed V1 using the molten resin in the reservoir 21.
[0061] At this time, the predetermined forward speed V1 (FIG. 2(a)) of the screw 22 may be determined to be a suitable value by test molding or the like, but it is preferable to set the forward speed of the screw 22 that can supply from the reservoir 21 an amount equal to or slightly more than the amount of supply per unit time required to compensate for the shortage of the volumetric shrinkage (cooling and solidifying speed of the molten resin) caused by cooling and solidifying shrinkage of the molten resin in the mold cavity 11, relative to the amount of molten resin supplied from the reservoir 21 to the gate region FG using the pressure / temperature deviation. The reason why this is a preferable guideline is to avoid the occurrence of poor foaming, in which the pressure in the part of the mold cavity 11 where the molten resin is excessively supplied rises excessively to a pressure range that does not cause foaming, due to the supply of molten resin in excess of the cooling and solidifying shrinkage, making it difficult for the molten resin to foam and expand.
[0062] On the other hand, in order to prevent the molten resin in the storage section 21 from foaming during the screw re-forward movement step 2 as well, it is necessary to maintain the pressure of the molten resin in the storage section 21 within a pressure range that does not cause foaming at the stage of performing the screw re-forward movement step 2. Therefore, if the pressure of the molten resin in the storage section 21 becomes lower than the pressure range that does not cause foaming during the screw re-forward movement step 2, it is necessary to increase the predetermined forward speed V1 of the screw 22.
[0063] However, even in such a case, it is preferable that the predetermined forward speed V1 of the screw 22 does not significantly change the supply state of the molten resin from the screw position holding step in which the natural supply state of the molten resin was maintained using the pressure / temperature deviation. Therefore, the predetermined forward speed V1 of the screw 22 may be a fixed value, but may be set to multiple speeds as necessary in response to an increase in the forward resistance of the screw 22 caused by an increase in the melt viscosity of the molten resin in the mold cavity 11 over time, or a decrease in the supply amount of the molten resin as the molten resin in the mold cavity 11 progresses through the range where it is cooled and solidified.
[0064] By the above-mentioned screw re-advance process 2, the volume reduction accompanying the cooling, solidifying, and shrinking of the molten resin in the mold cavity 11 is compensated for without significantly changing the natural supply state of the molten resin using the pressure / temperature deviation, and the pressure / temperature deviation of the molten resin in the mold cavity 11 is maintained as in the first embodiment. Then, the formation of foam nuclei and the generation of foam cells in the molten resin (in the intermediate flow region FM in the second embodiment), the amount of foam cells generated, and the coarsening of the generated foam cells are suppressed, and a foam-molded product with a uniform expansion ratio and cell diameter distribution of the foam cells can be molded.
[0065] In the screw re-advance step 2 as well, it is preferable to determine whether the screw re-advance step 2 is necessary and, if necessary, the timing to start the screw re-advance step 2 after the start of the screw position holding step, by test molding using the injection foam molding method described in the first embodiment. Also, in the screw re-advance step 2 as well, as in the screw re-advance step 1, it is preferable to complete the step based on the time when the molten resin in the mold cavity 11 cools and solidifies (movement time / forward movement time), rather than the movement distance (forward movement distance) of the screw 22 from the screw stop position L1.
[0066] So far, two screw re-advancement processes have been described: screw re-advancement process 1 for controlling the advancing force of the screw 22, and screw re-advancement process 2 for controlling the advancing speed of the screw 22. Whether these two screw re-advancement processes are necessary, and which one is more suitable when a screw re-advancement process is necessary, is considered to differ depending on the resin material and the shape and size of the foam-molded product. When checking whether a screw re-advancement process is necessary, each screw re-advancement process can be adopted in test molding or the like, and the more suitable one can be selected depending on the type and use of the foam-molded product, for example, by comparing the viewpoint of emphasizing the quality of a foam-molded product having a uniform expansion ratio of foam cells and distribution of bubble diameters with the viewpoint of emphasizing a short molding cycle. [Explanation of symbols]
[0067] 10 mold, 11 mold cavity, 12 skin layer, 20 injection unit, 21 storage section, 22 screw, 22a flight, 22b check ring, FG gate section region, FM flow intermediate region, FE flow front region, L1 screw stop position, PS0 / PS1 / PS2 / PS3 pressure of molten resin in storage section 21, PG1 / PG2 / PG3 pressure of molten resin in gate section region FG, PM1 / PM2 / PM3 / PM2' pressure of molten resin in flow intermediate region FM, PE1 / PE2 / PE3 pressure of molten resin in flow front region FE, TS0 / TS1 / TS2 / TS3 temperature of molten resin in storage section 21, TG1 / TG2 / TG3 temperature of molten resin in gate section region FG, TM1 / TM2 / TM3 temperature of molten resin in flow intermediate region FM, TE1 / TE2 / TE3 temperature of molten resin in flow front region FE, F1 V1: Predetermined forward force of the screw, V2: Predetermined forward speed of the screw
Claims
1. a metering step of storing the molten resin containing the foaming material in a storage section in front of the screw while maintaining the molten resin in a pressure range that does not cause foaming; In a state where the mold cavity and the reservoir are in communication with each other, the mold cavity is filled with the molten resin in a full pack manner while a predetermined amount of the molten resin remains in the reservoir. an injection filling process in which the screw is stopped at a screw stop position L1 where the pressure of the molten resin remaining in the reservoir is maintained within the pressure range; A screw position holding step of holding the screw at the screw stop position L1, An injection foam molding method characterized in that, in the screw position holding process, the volumes of the mold cavity and the storage section, which are in the connected state, are maintained constant, and the molten resin filled in the mold cavity is foamed.
2. After the screw position holding step, the mold cavity and the storage section are in the communicating state, and the screw re-advancement step 1 is further provided in which the screw is advanced from the screw stop position L1 with a predetermined forward force F1, 2. The injection foam molding method according to claim 1, characterized in that, by advancing the screw with the specified forward force F1, the pressure of the molten resin in the storage section is maintained within the pressure range and the volume of the mold cavity is maintained constant, thereby foaming the molten resin filled in the mold cavity.
3. After the screw position holding step, the mold cavity and the storage section are in the communicating state, and the screw re-advancement step 2 is further provided in which the screw is advanced from the screw stop position L1 at a predetermined forward speed V1, 2. The injection foam molding method according to claim 1, characterized in that, by advancing the screw at the specified forward speed V1, the pressure of the molten resin in the storage section is maintained within the pressure range and the volume of the mold cavity is maintained constant, thereby foaming the molten resin filled in the mold cavity.
Citation Information
Patent Citations
Short shot foam molding
JP1996103919A
Method for control of foam injection molding machine and mold used therefor
JP1996336853A
Injection foam molding method / device
JP2008143061A
Method of producing foam molding
JP2012035585A
Method of manufacturing expandable plastic molding, expandable plastic molding, and injection molding machine
JP2012051268A