Aromatic ether ether ketone polymer, its method of production, and resin composition and cured resin using said polymer

An aromatic ether ether ketone polymer with controlled molecular weight and structure addresses the limitations of existing epoxy resins, providing enhanced heat resistance and thermal conductivity for advanced film and sheet applications.

JP7590174B2Active Publication Date: 2024-11-26NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020210423
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-11-26
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Existing epoxy resins, such as those based on bisphenol A or bisphenol F, suffer from inadequate heat resistance, high thermal expansion, and low thermal conductivity, making them unsuitable for applications requiring high performance films or sheets.

Method used

Development of an aromatic ether ether ketone polymer with a specific molecular structure and weight average molecular weight, produced through controlled reactions involving bisphenol compounds and epichlorohydrin, to enhance heat resistance, thermal conductivity, and toughness.

Benefits of technology

The polymer exhibits high heat resistance, low thermal expansion, and improved toughness, suitable for use in multilayer printed wiring boards and adhesives, with controlled molecular weight and solubility for effective application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590174000001
    Figure 0007590174000001
  • Figure 0007590174000002
    Figure 0007590174000002
  • Figure 0007590174000003
    Figure 0007590174000003
Patent Text Reader

Abstract

To provide a polymer used suitably for preparation of a film- or sheet-like epoxy resin composition or epoxy resin cured product excellent in high thermostability, low thermal expansion and high toughness.SOLUTION: An aromatic ether-ether-ketone based polymer and a production method thereof are provided. The content of units represented by the general formula (1) in the figure in the polymer is 20 to 100 wt.%, where each A independently represents a divalent aromatic group and n represents a number from 1 to 50. The polymer has a weight-average molecular weight of 5,000 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel polymer containing an aromatic ether ether ketone skeleton, a method for producing the same, a resin composition using the polymer, and a cured resin product obtained by curing the same. [Background technology]

[0002] Up to now, high molecular weight epoxy resins, such as phenoxy resins, have been used as essential components of epoxy resins used to obtain film- or sheet-shaped epoxy resin cured products. Phenoxy resins with bisphenol A or bisphenol F as the main skeleton have been widely used, but they have problems with heat resistance, low thermal expansion, high thermal conductivity, and the like. For example, Patent Document 1 describes an adhesive-attached copper foil using a bisphenol A-type polymer epoxy resin, but the multilayer printed wiring board produced by this method has the disadvantage of being inferior in heat resistance and low thermal expansion compared to multilayer printed wiring boards produced by conventional techniques. For example, Patent Document 2 discloses a phenoxy resin produced from bisphenol A and bisphenol S (4,4'-dihydroxydiphenyl sulfone) as a phenoxy resin with improved heat resistance, but it is still insufficient in terms of heat resistance. Patent Document 3 also discloses an epoxy resin having an ether ether ketone structure, but in the examples, epichlorohydrin is used in an amount 7 to 10 times the amount of phenolic hydroxyl groups, and does not teach the synthesis of a polymer. The disclosed epoxy resin is a low molecular weight substance having a molecular weight of 1000 or less, judging from the epoxy equivalent, and does not have film properties. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-202418 [Patent Document 2] Japanese Patent Application Publication No. 2-45575 [Patent Document 3] Patent No. 5390491 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a polymer which is excellent in heat resistance, low thermal expansion, low moisture absorption and high toughness and is suitably used for preparing a film- or sheet-shaped cured epoxy resin product, a production method thereof, a resin composition using this polymer, and a cured resin product obtained by curing this resin composition. [Means for solving the problem]

[0005] The present invention relates to a compound represented by the following general formula (1): [ka] (wherein A independently represents a divalent aromatic group, and n represents a number from 1 to 50) is 20 to 100 wt % of a unit containing aromatic ring, and the weight average molecular weight is 5,000 or more.

[0006] The process for producing the aromatic ether ether ketone polymer of the present invention is any one of the following processes. i) The following general formula (3): [ka] (wherein, A independently represents a divalent aromatic group, and n represents a number from 1 to 50), A method for producing an aromatic ether ether ketone polymer, comprising reacting a bisphenol compound represented by the following general formula (4) with at least one compound selected from the group consisting of dihydroxynaphthalenes and dihydroxy compounds represented by the following general formula (5): [ka] (In the formula, m represents a number from 0 to 2; R1 and R2 each independently represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom; and X represents a direct bond, an oxygen atom, a sulfur atom, -SO2-, -CO-, -COO-, -CONH-, -CH2-, -CH(CH3)-, -C(CH3)2-, -φ-, or a 9,9-fluorenyl group, in which φ represents a phenylene group.) [ka] (In the formula, B independently represents a divalent aromatic group, and p represents a number from 1 to 50.)

[0007] ii) The following general formula (6): [ka] (wherein m is a number from 0 to 2, R1 and R2 each independently represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom, and X represents a direct bond, an oxygen atom, a sulfur atom, -SO2-, -CO-, -COO-, -CONH-, -CH2-, -CH(CH3)-, -C(CH3)2-, -φ-, or a 9,9-fluorenyl group, in which φ represents a phenylene group), and [ka] (wherein A independently represents a divalent aromatic group, and n represents a number from 1 to 50) with a dihydroxy compound represented by the following formula:

[0008] iii) A method for producing an aromatic ether ether ketone polymer, which comprises reacting a dihydroxy compound represented by the above general formula (7) with epichlorohydrin in the presence of an alkali metal hydroxide.

[0009] In the above polymer and production method, the divalent aromatic groups A and B are each independently an aromatic group represented by the following general formula (2) or a naphthylene group described below. [ka] (In the formula, m represents a number from 0 to 2; R1 and R2 each independently represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom; and X represents a direct bond, an oxygen atom, a sulfur atom, -SO2-, -CO-, -COO-, -CONH-, -CH2-, -CH(CH3)-, -C(CH3)2-, -φ-, or a 9,9-fluorenyl group, in which φ represents a phenylene group.)

[0010] The present invention also relates to a resin composition comprising the aromatic ether ether ketone polymer, and a cured resin obtained by curing the resin composition. Effect of the Invention

[0011] The polymer of the present invention has crystallinity with a melting point of 100°C or higher, and is expected to have excellent characteristics such as high heat resistance, high thermal conductivity, low thermal expansion and high toughness, and can be suitably used in fields where it is used as a film- or sheet-shaped epoxy resin cured product, such as a multilayer printed wiring board, an adhesive, or a coating material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The polymer of the present invention has an aromatic unit represented by general formula (1) and the ratio is 20 to 100 weight % (wt%), preferably 30 to 100 wt%, more preferably 40 to 100 wt%. If the ratio is less than this, the effects of the present invention, such as high heat resistance, low thermal expansion, and low water absorption, are difficult to achieve. The ratio of the unit represented by general formula (1) that can be contained in the polymer of the present invention can be expressed as the weight ratio of the total amount of the diglycidyl compound represented by general formula (3) and the dihydroxy compound represented by general formula (5) to the total amount of the polymer.

[0013] In the general formula (1), A independently represents a divalent aromatic group. The divalent aromatic group is represented by the following general formula (2): [ka] (wherein m is a number from 0 to 2; R1 and R2 are hydrogen atoms, alkyl groups having 1 to 8 carbon atoms, aryl groups, alkoxy groups, aralkyl groups or halogen atoms; and X is a direct bond, oxygen atom, sulfur atom, -SO2-, -CO-, -COO-, -CONH-, -CH2-, -CH(CH3)-, -C(CH3)2-, -φ- or 9,9-fluorenyl group, where φ is a phenylene group), or a naphthylene group. These aromatic groups and naphthylene groups are derived from the bisphenol compound of general formula (4) or dihydroxynaphthalenes described below, which are the raw materials.

[0014] In the general formula (1), n ​​represents the average number of repetitions and is from 1 to 50, preferably from 1 to 30. If it is greater than this, the viscosity increases and the solubility in solvents decreases, resulting in poor handleability.

[0015] Units other than the unit represented by general formula (1) that may be contained in the polymer of the present invention include mainly units represented by the following general formula (8) or the following general formula (9), but other units may also be contained. [ka] (In the formula, m, R1, R2, and X are the same as those in the above general formula (4).) [ka]

[0016] The weight-average molecular weight of the polymer of the present invention is 5,000 or more. If the molecular weight is less than 5,000, when the resin composition using the polymer is applied and dried on a substrate such as copper foil, SUS foil, polyethylene terephthalate film, polyimide film, or glass plate, or when the resin composition is impregnated and dried on a fiber substrate such as carbon fiber or glass cloth, problems such as curling of the substrate or powder falling off during cutting are likely to occur. Furthermore, if the molecular weight exceeds 200,000, even if the polymer is diluted and dissolved in a solvent, the solution viscosity becomes high at a concentration of 40% by weight to 70% by weight that is generally used industrially, making it difficult to apply the polymer to a substrate. Therefore, the weight-average molecular weight of the polymer of the present invention is preferably 5,000 to 100,000, more preferably 10,000 to 60,000.

[0017] The reduced viscosity of the polymer of the present invention, measured in N-methylpyrrolidone as a solvent at 30° C., is preferably in the range of 0.2 to 1.2 dL / g, more preferably in the range of 0.3 to 0.8 dL / g. If it is lower than this range, the film properties tend to decrease, and if it is higher than this range, the handleability tends to decrease.

[0018] The polymer of the present invention does not necessarily have to be a two-dimensional polymer as long as it essentially contains the unit of general formula (1), and may be a polymer having a branched structure or a polymer that is partially three-dimensionally crosslinked. The branched structure or three-dimensional crosslinked structure can be formed by the reaction of the hydroxyl group of general formula (1) with the epoxy group, or by using a trifunctional or higher epoxy resin and a curing agent in combination.

[0019] The polymer of the present invention is usually in an amorphous glass state, but may be partially or entirely crystallized. By making it a crystalline polymer, properties such as heat resistance, high thermal conductivity, low thermal expansion, low moisture absorption, and high toughness based on crystallinity can be expected. The degree of crystallization can be grasped by differential scanning calorimetry. Specifically, the peak (endothermic peak) of the endothermic curve accompanying the melting of crystals in differential scanning calorimetry measured at a heating rate of 10°C / min is measured, and the temperature is taken as the melting point, and the heat of fusion is obtained from the integral value of this endothermic peak curve. The preferred heat of fusion of the endothermic peak in differential scanning calorimetry as a crystalline polymer is 5 joules / g (hereinafter referred to as "j / g") or more, preferably 10 j / g or more, and more preferably 20 j / g or more. The preferred melting point range of the crystalline polymer is one in which the endothermic peak temperature is in the range of 100°C to 350°C when measured at a heating rate of 10°C / min using a differential scanning calorimetry device. If the melting point is lower than this range, the properties such as heat resistance and low thermal expansion based on the crystallinity will decrease, whereas if the melting point is higher than this range, the handling properties will tend to decrease.

[0020] Examples of the terminal group of the polymer of the present invention include an epoxy group, a hydroxyl group, a carboxylic acid, an amino group, a vinyl group, a mercapto group and an aromatic group, with an epoxy group being preferred.

[0021] The method for producing the polymer of the present invention is generally a method of direct reaction of a dihydric phenol compound with epichlorohydrin in the presence of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide, or a method of addition polymerization reaction of a diglycidyl ether compound with a dihydric phenol compound. The polymer of the present invention may be produced by either method, but depending on the structure and molecular weight, there are problems such as poor solubility in solvents or crystals being precipitated, preventing the molecular weight of the polymer from increasing. Therefore, it is necessary to select a desirable polymerization method and polymerization conditions according to the properties of the target polymer. Each production method is shown below.

[0022] In the case of the direct reaction between a dihydric phenol compound and epichlorohydrin, a dihydroxy compound represented by general formula (7) is used as the dihydric phenol compound, and the proportion of the dihydroxy compound of general formula (7) is preferably 10 mol % or more of the total dihydric phenol compounds used. At 10 mol % or more, the effect of introducing an ether ether ketone skeleton becomes sufficient, and a cured product having heat resistance, low thermal expansion, low moisture absorption, and high toughness can be obtained, which is preferable.

[0023] The amount of epichlorohydrin used in the reaction between a dihydric phenol compound and epichlorohydrin is usually 1 to 5 times the molar amount of epichlorohydrin per mole of hydroxyl groups in the dihydric phenol compound, and is preferably in the range of 1 to 3 times the molar amount. By varying the amount within this range, the molecular weight of the polymer can be adjusted. This reaction is usually carried out at a temperature of 120°C or less.

[0024] In this reaction, a quaternary ammonium salt or a polar solvent such as dimethyl sulfoxide or diglyme may be used. Examples of the quaternary ammonium salt include tetramethylammonium chloride, tetrabutylammonium chloride, and benzyltriethylammonium chloride, and the amount of the quaternary ammonium salt added is preferably in the range of 0.1 to 2.0 wt% relative to the dihydric phenol compound. This range is preferable in terms of the effect of the addition of the quaternary ammonium salt and the amount of hardly hydrolyzable chlorine produced. The amount of the polar solvent added is preferably in the range of 10 to 200 wt% relative to the dihydric phenol compound. This is for the effect of the addition and for optimizing the reactivity and yield due to volumetric efficiency. After the reaction is completed, the excess epichlorohydrin and the solvent are distilled off, and the residue is dissolved in a solvent such as toluene or methyl isobutyl ketone, filtered, and washed with water to remove inorganic salts and remaining solvents, and then the solvent is distilled off to obtain an epoxy resin. More advantageously, the obtained epoxy resin is further added with an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide in an amount 1 to 30 times the amount of the remaining hydrolyzable chlorine, and a ring-closing reaction is carried out. The temperature for this ring-closing reaction is usually 100° C. or lower, preferably 90° C. or lower.

[0025] On the other hand, in the case of a method using an addition polymerization reaction between a diglycidyl ether compound and a dihydric phenol compound, the following i) and ii) can be mentioned. First, i) is a method in which a bisphenol compound represented by general formula (4), a dihydroxynaphthalene, and / or a dihydroxy compound represented by general formula (5) is used as a dihydric phenol compound, and these are reacted with a diglycidyl ether compound represented by general formula (3). On the other hand, ii) is a method in which a diglycidyl ether compound represented by general formula (6) is reacted with a dihydroxy compound represented by general formula (7) as a dihydric phenol compound.

[0026] In the general formulae (4) and (6), R1 and R2 independently represent a substituent selected from a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom, and are preferably a hydrogen atom or a methyl group. The linking positions of the benzene ring include the 1,4-position, the 1,3-position, and the 1,2-position, and the 1,4-position is particularly preferred. This is because the 1,3-position and the 1,2-position cannot be expected to improve physical properties such as heat resistance, low thermal expansion, and high toughness, compared to the 1,4-position.

[0027] Preferable examples of the bisphenol compound represented by the general formula (4) include hydroquinone, resorcinol, bisphenol A, bisphenol F, 3,3',5,5'-tetramethyl-4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxybiphenyl, 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 1,4-bis(4-hydroxyphenoxy)benzene, 1,3-bis(4-hydroxyphenoxy)benzene, 4,4'-bis(4-hydroxyphenoxy)diphenyl ether, 4,4'-dihydroxybenzophenone, 4,4'-dihydroxydiphenyl sulfide, and bisphenol fluorene. Examples of the dihydroxynaphthalenes include 1,4-naphthalenediol, 1,5-naphthalenediol, 1,6-naphthalenediol, 1,7-naphthalenediol, 2,6-naphthalenediol, and 2,7-naphthalenediol. These bisphenol compounds and dihydroxynaphthalenes can be used as a mixture with a dihydroxy compound represented by the general formula (5) described below.

[0028] The dihydroxy compound represented by the general formula (5) or (7) can be synthesized, for example, by reacting a halide of benzophenone such as 4,4'-difluorobenzophenone with a bisphenol compound represented by the general formula (4) or a dihydroxynaphthalene in the presence of a basic compound, but is not limited thereto. The units A and B in the general formulas (5) and (7) are divalent aromatic groups derived from the bisphenol compound or dihydroxynaphthalene thus reacted, respectively, and are preferably the aromatic group represented by the general formula (2) or a naphthylene group as described above.

[0029] The diglycidyl compounds represented by the general formula (3) or (6) are generally obtained by a method of directly reacting the bisphenol compound represented by the general formula (4) or the dihydroxy compound represented by the general formula (7) with epichlorohydrin, and normal reaction conditions can be adopted.

[0030] The reaction by addition polymerization between such a diglycidyl ether compound and a dihydric phenol compound can be carried out in the presence of a catalyst such as an amine, an imidazole, a triphenylphosphine, or a phosphonium salt. The molar ratio of the diglycidyl ether compound to the dihydric phenol compound is usually in the range of 3:1 to 1:3, preferably 2:1 to 1:2, and more preferably 1.1:1 to 1:1.1. The closer the molar ratio of the diglycidyl ether compound to the dihydric phenol compound is to 1, the higher the molecular weight of the resulting polymer. Other conditions for the addition polymerization reaction can be adopted as usual general reaction conditions.

[0031] This reaction can be carried out without a solvent, but if the reaction is carried out without a solvent, branching reactions are likely to occur and gelation may occur. Therefore, it is preferable to use a solvent in this reaction. Examples of the solvent include aliphatic ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and cyclopentanone, aromatics such as benzene, toluene, ortho-xylene, meta-xylene, para-xylene, chlorobenzene, and dichlorobenzene, aliphatic amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone, ethers such as tetrahydrofuran, dioxane, diethylene glycol dimethyl ether, and triethylene glycol dimethyl ether, and dimethyl sulfoxide. Two or more of these organic solvents may be selected and used as a mixed solvent.

[0032] In this polymerization reaction, the diglycidyl ether compound and the dihydric phenol compound can each be used as a mixture of two or more kinds, but the diglycidyl ether compound and the dihydric phenol compound must be selected so that the aromatic unit represented by the general formula (1) is 20 to 100 wt% in the obtained polymer. If it is less than 20 wt%, the effect of introducing the ether ether ketone structure is insufficient, and a cured product having heat resistance, low thermal expansion, and toughness cannot be obtained, which is not preferable.

[0033] In the resin composition of the present invention, when the polymer of the present invention has a weight average molecular weight of 5,000 or more, the resin flow during molding is small and the circuit embedding property is often somewhat insufficient. In this case, in order to obtain sufficient circuit embedding property, another low molecular weight epoxy resin can be further added. In this case, the molecular weight of the low molecular weight epoxy resin is 3,000 or less, preferably 1,500 or less, more preferably 800 or less, in weight average molecular weight.

[0034] In this case, the blending ratio of the polymer of the present invention to the low molecular weight epoxy resin is preferably 10 to 90 parts by weight, more preferably 20 to 60 parts by weight, based on 100 parts by weight of the polymer of the present invention. If the amount is less than this, the improvement in the flowability of the resin during molding is small, and if the amount is more than this, the heat resistance and moisture resistance of the cured product may decrease.

[0035] As the low molecular weight epoxy resin, in order to provide circuit embedding properties without deteriorating physical properties such as flexibility and heat resistance after curing, it is preferable to use an aromatic epoxy resin with an epoxy equivalent of 100 g / eq to 2,000 g / eq. If the epoxy equivalent exceeds 2,000 g / eq, the effect of improving the circuit embedding properties is not obtained sufficiently, and the crosslinking density is likely to be low, making it difficult to obtain a heat-resistant cured film. In addition, with an aliphatic epoxy resin, the circuit embedding properties can be obtained, but the heat resistance is insufficient. In addition, if the epoxy equivalent is less than 100 g / eq, the crosslinking density of the cured product becomes high, which increases the shrinkage rate of the cured product, and the deformation of the cured product tends to increase, as well as the water absorption rate. For these reasons, the epoxy equivalent of the low molecular weight epoxy resin is preferably 130 g / eq to 1,500 g / eq, more preferably 150 g / eq to 1,000 g / eq. Preferred low molecular weight epoxy resins include epoxy resins obtained by reacting a bisphenol compound represented by the above general formula (4) with epichlorohydrin, and examples thereof include, but are not limited to, bisphenol A type epoxy resins, bisphenol F type epoxy resins, tetramethylbisphenol F type epoxy resins, tetrabromobisphenol A type epoxy resins, etc. These epoxy resins may be used alone or in combination of two or more kinds.

[0036] In the present invention, other high molecular weight epoxy resins can be further added for the purpose of improving film properties.

[0037] In this case, the weight blending ratio of the polymer of the present invention to the high molecular weight epoxy resin is preferably in the range of 10 to 90 parts by weight, more preferably 20 to 60 parts by weight, per 100 parts by weight of the total amount of the polymer of the present invention and the high molecular weight epoxy resin. If it is less than this range, the improvement in the film properties of the cured product is small, and if it is more than this range, the heat resistance and low thermal expansion properties of the cured product may decrease.

[0038] The preferred molecular weight of the high molecular weight epoxy resin is, in terms of weight average molecular weight, 5,000 to 100,000, more preferably 10,000 to 60,000. Examples of the high molecular weight epoxy resin include, but are not limited to, bisphenol A type epoxy resin, bisphenol F type epoxy resin, tetramethylbisphenol F type epoxy resin, and tetrabromobisphenol A type epoxy resin.

[0039] The resin composition of the present invention advantageously contains an epoxy resin, a phenoxy resin or a compound containing an epoxy group. Such a resin can be a polymer of the present invention. When the resin composition of the present invention contains an epoxy resin or a compound containing an epoxy group, it is desirable to use a curing agent.

[0040] As the curing agent, all commonly known curing agents can be used, for example, dicyandiamide and its derivatives, imidazoles such as 2-methylimidazole and 2-ethyl-4-methylimidazole and their derivatives, divalent phenol compounds such as bisphenol A, bisphenol F, brominated bisphenol A, naphthalenediol, and dihydroxybiphenyl, novolac-type phenolic resins obtained by condensation reaction of phenols such as phenol, cresol, bisphenol A, naphthol, and naphthalenediol with aldehydes such as formaldehyde or ketones, and phenols such as phenol, cresol, bisphenol A, naphthol, and naphthalenediol with hydroxyl groups. Examples of commonly used epoxy resin curing agents include, but are not limited to, phenolic compounds such as aralkyl phenolic resins obtained by condensation reaction with rylene glycols, acid anhydride compounds such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, and hexahydrophthalic anhydride, amine compounds such as polyamidoamines obtained by condensation reaction between acids such as diaminodiphenylmethane, triethylenetetramine, isophoronediamine, and dimer acid and polyamines, and hydrazides such as adipic acid dihydrazide and isophthalic acid dihydrazide. These curing agents may be used alone or in combination of two or more.

[0041] A solvent may be used in the resin composition, preferably the epoxy resin composition, in the present invention to maintain a suitable viscosity when applied to a substrate. The viscosity adjusting solvent is one that does not remain in the epoxy resin composition when the solvent is dried at 80°C to 200°C, and specific examples thereof include toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, dioxane, ethanol, isopropyl alcohol, methyl cellosolve, ethyl cellosolve, cyclohexanone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc., but are not limited thereto. These solvents may be used alone or in combination of two or more.

[0042] To the resin composition of the present invention, silica, calcium carbonate, talc, aluminum hydroxide, mica, alumina, aluminum nitride, etc. may be added in order to impart heat resistance and flame retardancy, reduce the thermal expansion coefficient, increase the thermal conductivity, etc., and also, to improve adhesive strength, an epoxy silane coupling agent, a rubber component, etc. may be added to the extent that the properties of the cured product of the resin composition are not deteriorated.

[0043] The resin composition of the present invention may contain a curing accelerator as necessary. For example, various known curing accelerators such as amines, imidazoles, triphenylphosphine, and phosphonium salts can be used, but are not limited to these. When a curing accelerator is used, the amount is preferably in the range of 0.01 wt% to 10 wt% based on the resin component. If the amount exceeds 10 wt%, storage stability may be deteriorated, which is not preferable.

[0044] When the resin composition of the present invention is an epoxy resin composition, for example, the viscosity is adjusted to 15 Pa s or less, preferably 10 Pa s or less, using the above-mentioned solvent, an appropriate amount of curing agent is added so as to have a certain curing time, and a curing accelerator is optionally further added to form a varnish, which is applied to a substrate and the solvent is volatilized at 100°C to 160°C to form a prepreg. The obtained prepreg can then be cured by heating to form a cured product. EXAMPLES

[0045] The present invention will be specifically described below based on the embodiments of the invention.

[0046] The present invention will be described in more detail below with reference to examples. In the examples, the molecular weight and physical properties were measured by sample preparation and measurement according to the methods described below. Unless otherwise specified, "parts" refers to "parts by weight".

[0047] 1) Molecular weight of dihydroxy resin and epoxy resin A GPC measuring device (Nihon Waters, 515A GPC) was used, and three TSKgel G2000HXL (Tosoh) columns and one TSKgel G4000HXL (Tosoh) columns were used. The detector was RI, the solvent was tetrahydrofuran, the flow rate was 1.0 ml / min, and the column temperature was 38°C.

[0048] 2) Melt Viscosity The measurements were performed at 150°C to 190°C using a Brookfield CAP2000H rotational viscometer.

[0049] 3) Softening point The temperature was determined at a temperature rise rate of 5° C. / min according to JIS K 7234.

[0050] 4) Measurement of hydroxyl equivalent Using a potentiometric titrator, acetylation was carried out with 1.5 mol / L acetyl chloride in 1,4-dioxane as a solvent, and the excess acetyl chloride was decomposed with water and titrated with 0.5 mol / L potassium hydroxide.

[0051] 5) Measurement of epoxy equivalent A potentiometric titrator was used, and methyl ethyl ketone was used as the solvent. Tetraethylammonium bromide acetate solution was added, and the measurement was performed using a 0.1 mol / L perchloric acid-acetic acid solution in the potentiometric titrator.

[0052] 6) Pyrolysis temperature and residual carbon ratio The measurements were performed using a Hitachi High-Tech Science TG / DTA7300 differential thermal thermogravimetry device under a nitrogen gas flow at a heating rate of 10°C / min. The temperature at which the weight was reduced by 5 wt% (T-5%), the temperature at which the weight was reduced by 10 wt% (T-10%), and the carbon residue rate at 700°C were determined.

[0053] 7) Linear expansion coefficient, glass transition temperature (Tg) The measurements were performed using a Hitachi High-Tech Science TMA7100 thermomechanical measuring device at a heating rate of 10° C. / min.

[0054] 8) Water absorption rate The weight change rate was measured after absorbing moisture for 100 hours at 85°C and a relative humidity of 85%.

[0055] 9) Hydrolyzable chlorine 0.5 g of sample was dissolved in 30 ml of dioxane, 10 ml of 1N-KOH was added, and the mixture was boiled under reflux for 30 minutes. The mixture was then cooled to room temperature, and 100 ml of 80% acetone water was added. The solution was then subjected to potentiometric titration with a 0.002N-AgNO3 aqueous solution.

[0056] Reference example 1 A 2L separable flask was charged with 110g (1.0mol) of resorcinol, 109g (1.0mol) of 4,4'-difluorobenzophenone (DFBP), 276g of anhydrous potassium carbonate, 1200g of N-methylpyrrolidone (NMP), and 200g of toluene, and the mixture was reacted for 4 hours under a nitrogen stream while heating to 140°C and distilling off water. The mixture was then heated to 160°C and reacted for 4 hours under reduced pressure while distilling off NMP. The mixture was cooled to room temperature, dissolved in 1400g of methyl isobutyl ketone (MIBK), neutralized with a 30% aqueous sulfuric acid solution, and washed with water. The MIBK was then removed under reduced pressure, and the mixture was reacted for another 4 hours at 210°C. The remaining resorcinol was removed under reduced pressure to obtain 111g of a resinous solid (dihydroxy resin A). The softening point was 132°C, the melt viscosity at 180°C was 3.3 Pa s, and the hydroxyl (OH) equivalent was 468 g / eq. GPC measurement showed that the product components were p=1 of general formula (5) 10.3%, p=2 13.5%, p=3 14.5%, p=4 12.2%, p=5 9.5%, p=6 7.2%, p≧7 28.2%, and others 4.6%.

[0057] Reference example 2 A 0.5L separable flask was charged with 30g of dihydroxy resin A, 59g of epichlorohydrin (ECH), and 9g of diethylene glycol dimethyl ether, and 5.3g of 48.8% sodium hydroxide aqueous solution was added dropwise over 3 hours at 62°C under reduced pressure. During this time, the water generated was removed from the system by azeotropy with ECH, and the distilled ECH was returned to the system. After the dropwise addition was completed, the reaction was continued for another hour to dehydrate. Then, ECH was removed under reduced pressure, 80g of toluene was added to dissolve it, the salt generated was removed by filtration, and further washing with water was performed. 1.8g of 48.8% potassium hydroxide aqueous solution was added to this, and the reaction was performed for 2 hours at 80°C. After washing with water, the toluene was removed under reduced pressure, and 23.1g of a resin-like material (epoxy resin A) was obtained. The softening point was 94°C, and the melt viscosity at 150°C was 3.6 Pa·s. The hydrolyzable chlorine was 0.3%, and the epoxy equivalent was 422g / eq.

[0058] Reference example 3 A 2L separable flask was charged with 109g (0.5mol) of DFBP, 200g (1.0mol) of 4,4'-dihydroxydiphenylmethane, 123g of anhydrous potassium carbonate, 1120g of NMP, and 120g of toluene, and the mixture was stirred at room temperature for 1 hour under a nitrogen stream. The mixture was then heated to 140°C and stirred for 4 hours while distilling off water. The mixture was then further heated to 205°C and stirred for 4 hours while distilling off NMP. The mixture was then returned to room temperature, slowly poured into 1500mL of water while stirring, dispersed, washed with water, filtered, and then further poured into 1500mL of water and neutralized with a 30% aqueous sulfuric acid solution, after which it was washed with water, filtered, and dried, to obtain 232g of a milky white solid product (dihydroxy resin B). The OH equivalent was 457g / eq. From the GPC measurement, the component ratio of the product was 39.1% for p=1 in the general formula (5), 32.2% for p=2, 15.9% for p=3, 6.0% for p=4, 4.4% for p≧5, and 2.4% for others.

[0059] Reference example 4 50.0 g of dihydroxy resin B obtained in Reference Example 3, 185 g of ECH, and 500 g of NMP were charged and dissolved at 65°C, after which 9.1 g of 48.8% aqueous sodium hydroxide solution was added dropwise and reacted for 4 hours. Then, ECH and the generated water were distilled off at 85°C under reduced pressure, and the generated salt was removed by filtration. The reaction liquid was then added dropwise to 2000 mL of water with stirring to precipitate the product. After repeated washing with water, the product was dried to obtain 50.8 g of a white solid (epoxy resin B). The melt viscosity at 190°C was 0.1 Pa s, and the epoxy equivalent was 579 g / eq.

[0060] Reference example 5 A 2L separable flask was charged with 60g (0.28mol) of DFBP, 176.2g (1.10mol) of 1,6-dihydroxynaphthalene, 152g of anhydrous potassium carbonate, 1000g of NMP, and 150g of toluene, and the mixture was stirred at room temperature for one hour under a nitrogen stream. The mixture was then heated to 140°C and stirred for four hours while distilling off water. The mixture was then heated to 160°C and stirred for four hours while distilling off NMP under reduced pressure. The mixture was then returned to room temperature, and 1000g of MIBK was added and dissolved, neutralized with a 30% aqueous sulfuric acid solution, and repeatedly washed with water. The MIBK was then removed from the MIBK layer under reduced pressure, yielding 196g of resin-like solid (dihydroxy resin C). The softening point was 44°C, the melt viscosity at 150°C was 85mPa·s, and the OH equivalent was 212g / eq. From the GPC measurement, the component ratio of the product was 35.1% unreacted 1,6-naphthalenediol, 30.0% p=1 in the general formula (5), 17.7% p=2, 8.5% p=3, 3.9% p=4, 2.4% p≧5, and 2.3% others.

[0061] Example 1 In a 500 ml glass separable flask equipped with a stirrer, a thermometer, and a nitrogen gas inlet, 20 parts of bisphenol A type epoxy resin (epoxy resin D; manufactured by Nippon Steel Chemical & Material Co., Ltd., YD-8125, epoxy equivalent 173 g / eq.), 54.1 parts of dihydroxy resin A synthesized in Reference Example 1, and 200 parts of NMP were weighed out and taken, and the mixture was heated to 110°C while stirring under a nitrogen stream to dissolve uniformly. Then, 0.2 parts of 2-ethyl-4-methylimidazole was added as a catalyst and reacted at 150°C for 5 hours to obtain a polymer solution. The obtained polymer solution was dropped into a large amount of methanol, and 72 g of a precipitated white polymer (polymer A) was collected. The reduced viscosity of the obtained polymer measured at 30°C using NMP as a solvent was 0.43 dL / g. The proportion of the unit represented by the general formula (1) was 73 wt%. The weight average molecular weight was 38,000.

[0062] Example 2 Using 52.8 parts of dihydroxy resin B instead of dihydroxy resin A, the reaction was carried out in the same manner as in Example 1 to obtain 71 parts of a polymer (Polymer B). The reduced viscosity of the obtained polymer at 30°C using NMP as a solvent was 0.52 dL / g. The proportion of the unit represented by general formula (1) was 72 wt%. The weight average molecular weight was 47,000.

[0063] Example 3 Using 24.5 parts of dihydroxy resin C instead of dihydroxy resin A, the reaction was carried out in the same manner as in Example 1 to obtain 43 parts of a polymer (polymer C). The reduced viscosity of the obtained polymer at 30°C using NMP as a solvent was 0.38 dL / g. The proportion of the unit represented by general formula (1) was 55 wt%. The weight average molecular weight was 28,000.

[0064] Example 4 Using 20 parts of epoxy resin A and 22.2 parts of dihydroxy resin A, a reaction was carried out in the same manner as in Example 1 to obtain 41 parts of a polymer (Polymer D). The reduced viscosity of the obtained polymer at 30°C using NMP as a solvent was 0.41 dL / g. The proportion of the unit represented by general formula (1) was 100 wt%. The weight average molecular weight was 36,000.

[0065] Example 5 Using 40 parts of epoxy resin B and 7.9 parts of bisphenol A (dihydroxy resin D), a reaction was carried out in the same manner as in Example 1 to obtain 45 parts of a polymer (polymer E). The reduced viscosity of the obtained polymer at 30°C using NMP as a solvent was 0.48 dL / g. The proportion of the unit represented by general formula (1) was 83 wt%. The weight average molecular weight was 46,000.

[0066] Example 6 Using 20 parts of a biphenyl-based epoxy resin (epoxy resin E; YX-4000H, manufactured by Mitsubishi Chemical, epoxy equivalent 193 g / eq.) and 22 parts of dihydroxy resin C, a reaction was carried out in the same manner as in Example 1 to obtain 40 parts of a polymer (polymer F). The reduced viscosity of the obtained polymer at 30°C using NMP as a solvent was 0.36 dL / g. The proportion of the unit represented by general formula (1) was 52 wt%. The weight average molecular weight was 27,000.

[0067] Comparative Example 1 Using 30 parts of epoxy resin D and 19.8 parts of dihydroxy resin D, a reaction was carried out in the same manner as in Example 1 to obtain 47 parts of a polymer (polymer G). The reduced viscosity of the obtained polymer at 30°C using NMP as a solvent was 0.56 dL / g. The proportion of the unit represented by general formula (1) was 0 wt%. The weight average molecular weight was 57,000.

[0068] Comparative Example 2 Using 30 parts of epoxy resin E and 17.7 parts of dihydroxy resin D, a reaction was carried out in the same manner as in Example 1 to obtain 46 parts of a polymer (Polymer H). The reduced viscosity of the obtained polymer at 30°C using NMP as a solvent was 0.53 dL / g. The proportion of the unit represented by general formula (1) was 0 wt%. The weight average molecular weight was 53,000.

[0069] Comparative Example 3 Using 40 parts of epoxy resin D, 8.1 parts of dihydroxy resin A, and 24.3 parts of dihydroxy resin D, the reaction was carried out in the same manner as in Example 1 to obtain 68 parts of a polymer (Polymer I). The reduced viscosity of the obtained polymer at 30°C using NMP as a solvent was 0.51 dL / g. The proportion of the unit represented by general formula (1) was 11.2 wt%. The weight average molecular weight was 51,000.

[0070] Examples 7 to 12, Comparative Examples 4 to 6 Test pieces were prepared by press molding using the polymers obtained in Examples 1 to 6 and Comparative Examples 1 to 3, and were subjected to evaluation of various physical properties. The results are shown in Table 1.

[0071] [Table 1]

Claims

1. The following general formula (1) 【Chemistry 1】 (wherein A independently represents a divalent aromatic group, and n represents a number from 1 to 50) is 30 to 100 wt % of a unit containing an aromatic group, and the weight average molecular weight is 27,000 or more.

2. The divalent aromatic group A is represented by the following general formula (2): 【Chemistry 2】 (In the formula, m represents a number from 0 to 2, and R 1 , R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom; X represents a direct bond, an oxygen atom, a sulfur atom, or —SO 2 -, -CO-, -COO-, -CONH-, -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 2. The aromatic ether ether ketone polymer according to claim 1, wherein the aromatic group is an aromatic group represented by the following formula: embedded image wherein φ represents a phenylene group, -φ-, -φ- or 9,9-fluorenyl group, where φ represents a phenylene group, or a naphthylene group.

3. The following general formula (1) 【Chemistry 3】 (wherein A independently represents a divalent aromatic group, and n represents a number from 1 to 50) is 20 to 100 wt % of a unit containing an aromatic group, and the weight average molecular weight is 5,000 or more, The following general formula (3) 【Chemistry 4】 (wherein A independently represents a divalent aromatic group, and n represents a number from 1 to 50), A method for producing an aromatic ether ether ketone polymer, comprising reacting a bisphenol compound represented by the following general formula (4), a dihydroxynaphthalene, and a dihydroxy compound represented by the following general formula (5), 【Chemistry 5】 (In the formula, m represents a number from 0 to 2, and R 1 , R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom; X represents a direct bond, an oxygen atom, a sulfur atom, or —SO 2 -, -CO-, -COO-, -CONH-, -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -φ- or 9,9-fluorenyl group, where φ represents a phenylene group. 【Chemistry 6】 (In the formula, B independently represents a divalent aromatic group, and p represents a number from 1 to 50.)

4. A method for producing the aromatic ether ether ketone polymer according to claim 1 or 2, comprising the steps of: The following general formula (6) 【Chemistry 7】 (In the formula, m represents a number from 0 to 2, and R 1 , R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom; X represents a direct bond, an oxygen atom, a sulfur atom, or —SO 2 -, -CO-, -COO-, -CONH-, -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -φ- or 9,9-fluorenyl group, where φ represents a phenylene group, and 【Chemistry 8】 (wherein A independently represents a divalent aromatic group, and n represents a number from 1 to 50) with a dihydroxy compound represented by the following formula:

5. The following general formula (1) 【Chemistry 9】 (wherein A independently represents a divalent aromatic group, and n represents a number from 1 to 50) is 20 to 100 wt % of a unit containing an aromatic group, and the weight average molecular weight is 5,000 or more, The following general formula (7) 【Chemistry 10】 (wherein A independently represents a divalent aromatic group, and n represents a number from 1 to 50) with epichlorohydrin in the presence of an alkali metal hydroxide.

6. The divalent aromatic groups A and B are independently represented by the following general formula (2): 【Chemistry 11】 (In the formula, m represents a number from 0 to 2, and R 1 , R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom; X represents a direct bond, an oxygen atom, a sulfur atom, or —SO 2 -, -CO-, -COO-, -CONH-, -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 6. The method for producing an aromatic ether ether ketone polymer according to claim 3, wherein the aromatic group is an aromatic group represented by the formula (I) below, wherein φ represents a phenylene group, -φ-, -φ- or 9,9-fluorenyl group, where φ represents a phenylene group, or a naphthylene group.

7. A resin composition comprising the aromatic ether ether ketone polymer according to claim 1 or 2.

8. A cured resin obtained by curing the resin composition according to claim 7.

Citation Information

Patent Citations

  • Printing of * kasuri * thread

    JP1978090491A

  • Self-fusing insulating paint

    JP1990045575A

  • Epoxy resin composition for sealing semiconductor

    JP1992248866A

  • Interlayer adhesive for multilayer printed wiring board, copper foil applied with adhesive and production of multilayer printed wiring board

    JP1995202418A

  • Epoxy resin composition and molded item

    JP2010195854A