Olefin polymer and method for producing same
The olefin polymer with specific density, melting index, and TREF distribution, produced using a hybrid catalyst with transition metal compounds, addresses the poor heat-sealing issue of metallocene-catalyzed linear low-density polyethylene, achieving improved heat-sealing properties through high branch content.
Patent Information
- Application Number
- JP2023536580
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-17
- Filing Date
- 2021-12-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-12-10
AI Technical Summary
Linear low-density polyethylene produced using a metallocene catalyst has poor processability due to its narrow molecular weight distribution, resulting in films with poor heat-sealing properties.
An olefin polymer is developed with a density of 0.915 to 0.950 g/cm³, a melting index of 0.5~1.5 g/10 min, a polydispersity index of 2~6, and a temperature rising elution fractionation (TREF) with multimodal distribution, achieved through the use of a hybrid catalyst containing specific transition metal compounds and cocatalysts, which includes at least one first transition metal compound and a second transition metal compound, along with a carrier support.
The olefin polymer exhibits high specific gravity and excellent heat sealability due to the highly branched copolymer derived from comonomers, enhancing the heat-sealing properties of films produced from it.
Smart Images

Figure 0007590580000014 
Figure 0007590580000015 
Figure 0007590580000016
Abstract
Description
[Technical field]
[0001] The present invention relates to an olefin-based polymer and a method for producing the same. Specifically, the present invention relates to an olefin-based polymer having excellent heat sealability and a method for producing the same. [Background technology]
[0002] Metallocene catalysts, which are one of the catalysts used to polymerize olefins, are compounds in which ligands such as cyclopentadienyl, indenyl, and cycloheptadienyl are coordinated to a transition metal or a transition metal halide, and have a sandwich structure as their basic form.
[0003] In contrast to Ziegler-Natta catalysts, another catalyst used to polymerize olefins, in which the metal components that act as active sites are dispersed on the surface of an inert solid, and the properties of the active sites are not uniform, metallocene catalysts are known as single-site catalysts, as they are a single compound with a fixed structure and all active sites have the same polymerization characteristics. Polymers polymerized with such metallocene catalysts have narrow molecular weight distributions, uniform comonomer distributions, and higher copolymerization activity than Ziegler-Natta catalysts.
[0004] Meanwhile, linear low-density polyethylene (LLDPE) is produced by copolymerizing ethylene and alpha-olefins at low pressure using a polymerization catalyst, and has a narrow molecular weight distribution, short chain branches (SCB) of a certain length, and generally does not have long chain branches (LCB). Films made from linear low-density polyethylene have high breaking strength and elongation, excellent tear strength, impact strength, etc. in addition to the properties of general polyethylene, and are widely used in stretch films and overlap films where it is difficult to apply existing low-density polyethylene and high-density polyethylene.
[0005] However, linear low density polyethylene produced by metallocene catalysts has poor processability due to its narrow molecular weight distribution, and films produced therefrom tend to have poor heat sealability.
[0006] Therefore, there is a demand for olefin polymers having excellent heat sealability. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide an olefin polymer having excellent heat sealability.
[0008] Another object of the present invention is to provide a process for producing the above olefin polymer. [Means for solving the problem]
[0009] According to one embodiment of the present invention, (1) density is 0.915 to 0.950 g / cm 3 (2) Melt index (I) measured at 190°C with a load of 2.16 kg 2.16(3) a polydispersity index (Mw / Mn) of 2 to 6; and (4) an olefin polymer having a temperature rising elution fractionation (TREF) of a multimodal distribution that satisfies the following relationship 1: [Equation 1] C 65 -C 45 >15(%) Here, C 45 is the weight percent of polymer eluted at 45°C, C 65 is the weight percent of polymer eluted at 65°C.
[0010] In a specific example of the present invention, the olefin polymer may be prepared by polymerizing an olefin monomer in the presence of a hybrid catalyst including at least one first transition metal compound represented by the following formula 1 and at least one second transition metal compound selected from the group consisting of a compound represented by the following formula 2 and a compound represented by the following formula 3: [ka] In the above Chemical Formulas 1 to 3, M 1 and M. 2 are different from each other and each independently are titanium (Ti), zirconium (Zr) or hafnium (Hf); X is independently halogen, C 1-20 Alkyl, C 2-20 Alkenyl, C 2-20 Alkynyl, C 6-20 Aryl, C 1-20 Alkyl C 6-20 Aryl, C 6-20 Aryl C 1-20 Alkyl, C 1-20 Alkylamide or C 6-20 is an aryl amide, R 1 ~R 10 are each independently hydrogen, substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamides, substituted or unsubstituted C 6-20 Arylamide, substituted or unsubstituted C 1-20 Alkylidene, or substituted or unsubstituted C 1-20 Cyril, R 1 ~R 10 each independently represents a substituted or unsubstituted saturated or unsaturated C 4-20 A ring may be formed.
[0011] In an embodiment of the present invention, M 1 and M. 2 are different from each other and each is zirconium or hafnium, and X is each a halogen or C 1-20 is alkyl, R 1 ~R 10 are hydrogen, substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 1-20 Alkenyl, or substituted or unsubstituted C 6-20 It can be aryl.
[0012] In a preferred embodiment of the present invention, M 1 is hafnium, M 2 is zirconium and X can be chlorine or methyl.
[0013] In a preferred embodiment of the present invention, the first transition metal compound may be at least one of the transition metal compounds represented by the following chemical formulas 1-1 and 1-2, and the second transition metal compound may be at least one of the transition metal compounds represented by the following chemical formulas 2-1, 2-2, and 3-1. [ka] In the above formula, Me is a methyl group.
[0014] In an embodiment of the present invention, the molar ratio of the secondary transition metal compound to the first transition metal compound ranges from 100:1 to 1:100.
[0015] In an embodiment of the present invention, the catalyst may include at least one promoter selected from the group consisting of a compound represented by the following formula 4, a compound represented by the following formula 5, and a compound represented by the following formula 6. [ka] [Chemical formula 6] [LH] + [Z(A) 4 ] - or [L] + [Z(A) 4 ] - In the above Chemical Formula 4, n is an integer of 2 or more, and R a is a halogen atom, C 1-20 C substituted with hydrocarbon or halogen groups 1-20 is a hydrocarbon group, In the above formula 5, D is aluminum (Al) or boron (B), and R b , R c and R d are each independently a halogen atom, C 1-20 Hydrocarbon radicals, halogen-substituted C 1-20 Hydrocarbon group or C 1-20 is an alkoxy group, In the above formula 6, L is a neutral or cationic Lewis base, [LH] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted C 6-20 Aryl group or substituted or unsubstituted C 1-20 It is an alkyl group.
[0016] In an embodiment of the present invention, the catalyst may further comprise a support supporting the transition metal compound, the cocatalyst compound, or both.
[0017] In a preferred embodiment of the present invention, the support may comprise at least one selected from the group consisting of silica, alumina and magnesia.
[0018] Here, the total amount of the mixed transition metal compounds supported on the support is 0.001 to 1 mmole per 1 g of the support, and the total amount of the promoter compounds supported on the support is 2 to 15 mmole per 1 g of the support.
[0019] In a specific embodiment of the present invention, the olefin polymer is a copolymer of an olefin monomer and an olefin comonomer. Specifically, the olefin monomer may be ethylene, and the olefin comonomer may be at least one selected from the group consisting of propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, and 1-hexadecene. Preferably, the olefin polymer is a linear low-density polyethylene in which the olefin monomer is ethylene and the olefin comonomer is 1-hexene.
[0020] According to one embodiment of the present invention, the present invention provides a method for producing an olefin polymer by polymerizing an olefin monomer in the presence of a hybrid catalyst comprising at least one first transition metal compound represented by the above-mentioned Chemical Formula 1 and at least one second transition metal compound selected from the group consisting of a compound represented by the above-mentioned Chemical Formula 2 and a compound represented by the above-mentioned Chemical Formula 3, wherein (1) the density of the olefin polymer is 0.915 to 0.950 g / cm 3 (2) Melt index (I) measured at 190°C with a load of 2.16 kg 2.16(3) a polydispersity index (Mw / Mn) of 2 to 6; and (4) a temperature rising elution fractionation (TREF) of the multimodal distribution satisfies the following relationship 1: [Equation 1] C 65 -C 45 >15(%) Here, C 45 is the weight percent of polymer eluted at 45°C, C 65 is the weight percent of polymer eluted at 65°C.
[0021] In an embodiment of the present invention, the polymerization of the olefinic monomer may be carried out in a gas phase polymerization, specifically, the polymerization of the olefinic monomer may be carried out in a gas phase fluidized bed reactor. Effect of the Invention
[0022] The olefin polymer according to the embodiment of the present invention has a high specific gravity of the copolymer having many branches derived from the comonomer, and therefore has excellent heat sealability. [Brief description of the drawings]
[0023] [Figure 1] 1 is a temperature rising elution fractionation (TREF) graph for explaining Relational Formula 1. [Diagram 2] 1 is a temperature rising elution fractionation (TREF) graph of the olefin polymer of Example 1. [Diagram 3] 1 is a temperature rising elution fractionation (TREF) graph of the olefin polymer of Example 2. [Figure 4] 1 is a temperature rising elution fractionation (TREF) graph of the olefin polymer of Example 3. [Diagram 5] 1 is a temperature rising elution fractionation (TREF) graph of the olefin polymer of Comparative Example 1. [Figure 6] 1 is a temperature rising elution fractionation (TREF) graph of the olefin polymer of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will now be described in more detail.
[0025] Olefin Polymers According to one embodiment of the present invention, (1) density is 0.915 to 0.950 g / cm 3 (2) Melt index (I) measured at 190°C with a load of 2.16 kg 2.16 (3) a polydispersity index (Mw / Mn) of 2 to 6; and (4) an olefin polymer having a temperature rising elution fractionation (TREF) of a multimodal distribution that satisfies the following relationship 1:
[0026] [Equation 1] C 65 -C 45 >15(%)
[0027] Here, C 45 is the weight percent of polymer eluted at 45°C, C 65 is the weight percent of polymer eluted at 65°C.
[0028] In a specific example of the present invention, the olefin polymer has a density of 0.915 to 0.950 g / cm 3 Preferably, the density of the olefin polymer is 0.915 to 0.940 g / cm 3 It can be.
[0029] In an embodiment of the present invention, the olefin polymer has a melt index (I 2.16 The melt index of the olefin polymer measured at 190° C. under a load of 2.16 kg is preferably 0.6 to 1.2 g / 10 min.
[0030] In a specific example of the present invention, the olefin-based polymer has a polydispersity index (Mw / Mn) of 2 to 6. Preferably, the olefin-based polymer has a polydispersity index of 4 to 6.
[0031] In an embodiment of the present invention, the olefin polymer is obtained by temperature-rising elution fractionation of a multi-peak distribution, and the C 65 -C 45 The value exceeds 15(%).
[0032] The area of the TREF peak located between 45 and 65°C in the multimodal TREF curve indicates the amount of copolymer with many branches derived from the comonomer, and the higher the specific gravity, the higher the heat sealability of the polymer obtained.
[0033] The olefin polymer according to an embodiment of the present invention is prepared by polymerizing an olefin monomer in the presence of a hybrid catalyst including at least one first transition metal compound represented by the following formula 1 and at least one second transition metal compound selected from the group consisting of a compound represented by the following formula 2 and a compound represented by the following formula 3:
[0034] [ka]
[0035] In the above Chemical Formulas 1 to 3, M 1 and M. 2 are different from each other and each independently are titanium (Ti), zirconium (Zr) or hafnium (Hf). 1 and M. 2 are different from each other and can each be zirconium or hafnium. 1 is hafnium, M 2 can be zirconium.
[0036] X is independently halogen, C 1-20 Alkyl, C 2-20 Alkenyl, C 2-20 Alkynyl, C6-20 Aryl, C 1-20 Alkyl C 6-20 Aryl, C 6-20 Aryl C 1-20 Alkyl, C 1-20 Alkylamide or C 6-20 Specifically, X is a halogen or C 1-20 Preferably, X is chlorine or methyl.
[0037] R 1 ~R 10 are each independently hydrogen, substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamides, substituted or unsubstituted C 6-20 Arylamide, substituted or unsubstituted C 1-20 Alkylidene, or substituted or unsubstituted C 1-20 Cyril, where R 1 ~R 10 each independently represents a substituted or unsubstituted saturated or unsaturated C 4-20 Specifically, R 1 ~R 10 are hydrogen, substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 1-20 Alkenyl, or substituted or unsubstituted C 6-20 It can be aryl.
[0038] In an embodiment of the present invention, M 1 and M. 2are different from each other and each is zirconium or hafnium, and X is each halogen or C 1-20 is alkyl, R 1 ~R 10 are hydrogen, substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 1-20 Alkenyl, or substituted or unsubstituted C 6-20 It can be aryl.
[0039] In a preferred embodiment of the present invention, M 1 is hafnium, M 2 is zirconium and X can be chlorine or methyl.
[0040] In a preferred embodiment of the present invention, the first transition metal compound may be at least one of the transition metal compounds represented by the following chemical formulas 1-1 and 1-2, and the second transition metal compound may be at least one of the transition metal compounds represented by the following chemical formulas 2-1, 2-2, and 3-1.
[0041] [ka]
[0042] In the above formula, Me is a methyl group.
[0043] In a specific example of the present invention, the molar ratio of the second transition metal compound to the first transition metal compound is in the range of 100:1 to 1:100. Preferably, the molar ratio of the second transition metal compound to the first transition metal compound is in the range of 50:1 to 1:50. Preferably, the molar ratio of the second transition metal compound to the first transition metal compound is in the range of 10:1 to 1:10.
[0044] In an embodiment of the present invention, the catalyst may include at least one promoter compound selected from the group consisting of a compound represented by the following formula 4, a compound represented by the following formula 5, and a compound represented by the following formula 6.
[0045] [ka]
[0046] In the above Chemical Formula 4, n is an integer of 2 or more, and R a is a halogen atom, C 1-20 Hydrocarbon or halogen substituted C 1-20 Specifically, R a can be methyl, ethyl, n-butyl or isobutyl.
[0047] [ka]
[0048] In the above formula 5, D is aluminum (Al) or boron (B), and R b , R c and R d are each independently a halogen atom, C 1-20 Hydrocarbon radicals, halogen-substituted C 1-20 Hydrocarbon group or C 1-20 Specifically, when D is aluminum (Al), R b , R c and R d can each independently be methyl or isobutyl, and when D is boron (B), R b , R c and R d can each be pentafluorophenyl.
[0049] [Chemical formula 6] [LH] + [Z(A) 4 ] - or [L] + [Z(A) 4 ] -
[0050] In the above formula 6, L is a neutral or cationic Lewis base, [LH] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted C 6-20 Aryl group or substituted or unsubstituted C 1-20 It is an alkyl group. Specifically, [LH] + can be a dimethylanilinium cation, [Z(A) 4 ] - is [B(C 6 F 5 ) 4 ] - [L] + is [(C 6 H 5 ) 3 C] + It can be.
[0051] Specifically, examples of the compound represented by the above formula 4 include methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, butylaluminoxane, etc., and methylaluminoxane is preferred, but is not limited thereto.
[0052] Examples of the compound represented by Chemical Formula 5 include trimethylaluminum, triethylaluminum, triisobutylaluminum, tripropylaluminum, tributylaluminum, dimethylchloroaluminum, triisopropylaluminum, tri-s-butylaluminum, tricyclopentylaluminum, tripentylaluminum, triisopentylaluminum, trihexylaluminum, trioctylaluminum, ethyldimethylaluminum, methyldiethylaluminum, triphenylaluminum, tri-p-tolylaluminum, dimethylaluminum methoxide, dimethylaluminum ethoxide, trimethylboron, triethylboron, triisobutylboron, tripropylboron, and tributylboron, and are preferably, but not limited to, trimethylaluminum, triethylaluminum, and triisobutylaluminum.
[0053] Examples of the compound represented by Chemical Formula 6 include triethylammonium tetraphenyl boron, tributylammonium tetraphenyl boron, trimethylammonium tetraphenyl boron, tripropylammonium tetraphenyl boron, trimethylammonium tetra(p-tolyl) boron, trimethylammonium tetra(o,p-dimethylphenyl) boron, tributylammonium tetra(p-trifluoromethylphenyl) boron, trimethylammonium tetra(p-trifluoromethylphenyl) boron, tributylammonium tetrapentafluorophenyl boron, N,N-diethylanilinium tetraphenyl boron, N,N-diethylanilinium tetrapentafluorophenyl boron, diethylammonium tetrapentafluorophenyl boron, triphenylphosphonium tetraphenyl boron, trimethylphosphonium tetraphenyl boron, triethylammonium tetraphenyl aluminum, and tributylammonium tetraphenyl aluminum. ammonium, trimethylammonium tetraphenylaluminum, tripropylammonium tetraphenylaluminum, trimethylammonium tetra(p-tolyl)aluminum, tripropylammonium tetra(p-tolyl)aluminum, triethylammonium tetra(o,p-dimethylphenyl)aluminum, tributylammonium tetra(p-trifluoromethylphenyl)aluminum, trimethylammonium tetra(p-trifluoromethylphenyl)aluminum, tributylammonium tetrapentafluorophenylaluminum, N,N-diethylanilinium tetraphenylaluminum, N,N-diethylanilinium tetrapentafluorophenylaluminum, diethylammonium tetrapentatetraphenylaluminum, triphenylphosphonium tetraphenylaluminum, trimethylphosphonium tetraphenylaluminum, tripropylammonium tetra(p-tolyl)boron, triethylammonium tetra(o,p-dimethylphenyl) boron, tributylammonium tetra(p-trifluoromethylphenyl) boron, triphenylcarbonium tetra(p-trifluoromethylphenyl) boron, triphenylcarbonium tetrapentafluorophenyl boron, etc.
[0054] In an embodiment of the present invention, the catalyst may further comprise a support supporting the transition metal compound, the cocatalyst compound, or both. Specifically, the support may support both the transition metal compound and the cocatalyst compound.
[0055] Here, the carrier may include a material containing a hydroxyl group on the surface, and preferably, a material having a highly reactive hydroxyl group and a siloxane group that has been dried to remove moisture from the surface may be used. For example, the carrier may include at least one selected from the group consisting of silica, alumina, and magnesia. Specifically, silica, silica-alumina, and silica-magnesia that have been dried at high temperatures may be used as the carrier, and these are usually Na 2 OK 2 CO 3 , BaSO 4 , and Mg(NO 3 ) 2 The carrier may contain oxides, carbonates, sulfates, and nitrates such as those mentioned above. These may also contain carbon, zeolite, magnesium chloride, etc. However, the carrier is not limited to these, and is not particularly limited as long as it can support the transition metal compound and the promoter compound.
[0056] The carrier may have an average particle size of 10 to 250 μm, preferably an average particle size of 10 to 150 μm, and more preferably an average particle size of 20 to 100 μm.
[0057] The volume of the micropores in the support may be 0.1 to 10 cc / g, preferably 0.5 to 5 cc / g, and more preferably 1.0 to 3.0 cc / g.
[0058] The specific surface area of the support is 1 to 1,000 m 2 / g, preferably 100 to 800 m 2 / g, more preferably 200 to 600 m 2 / g.
[0059] In a preferred embodiment of the present invention, the support may be silica. Here, the drying temperature for silica may be 200 to 900° C. The drying temperature may be preferably 300 to 800° C., more preferably 400 to 700° C. If the drying temperature is less than 200° C., there may be too much moisture on the surface, causing a reaction between the moisture and the promoter compound, and if the drying temperature exceeds 900° C., the structure of the support may collapse.
[0060] The concentration of hydroxyl groups in the dried silica may be 0.1 to 5 mmole / g, preferably 0.7 to 4 mmole / g, and more preferably 1.0 to 2 mmole / g. If the concentration of hydroxyl groups is less than 0.1 mmole / g, the amount of the first promoter compound supported will be low, and if it exceeds 5 mmole / g, a problem of inactivation of the catalyst component may occur.
[0061] The total amount of the transition metal compound supported on the carrier can be 0.001 to 1 mmole per 1 g of carrier. When the ratio of the transition metal compound to the carrier satisfies the above range, appropriate supported catalytic activity is exhibited, which is advantageous in terms of maintaining the activity of the catalyst and in terms of economic efficiency.
[0062] The total amount of the promoter compounds supported on the carrier may be 2 to 15 mmole per gram of carrier. If the ratio of the promoter compounds to the carrier satisfies the above range, it is advantageous in terms of maintaining the activity of the catalyst and in terms of economy.
[0063] One or more types of carriers may be used. For example, both the transition metal compound and the co-catalyst compound may be supported on one carrier, or the transition metal compound and the co-catalyst compound may be supported on two or more carriers. Also, only one of the transition metal compound and the co-catalyst compound may be supported on the carrier.
[0064] As a method for supporting a transition metal compound and / or a cocatalyst compound usable in an olefin polymerization catalyst, a physical adsorption method or a chemical adsorption method can be used.
[0065] For example, the physical adsorption method may be a method in which a solution in which a transition metal compound is dissolved is brought into contact with a support and then dried; a method in which a solution in which a transition metal compound and a promoter compound are dissolved is brought into contact with a support and then dried; or a method in which a solution in which a transition metal compound is dissolved is brought into contact with a support and then dried to produce a support on which the transition metal compound is supported, and separately, a solution in which a promoter compound is dissolved is brought into contact with a support and then dried to produce a support on which the promoter compound is supported, and then these are mixed together.
[0066] The chemical adsorption method may be a method in which a promoter compound is first supported on the surface of a support, and then a transition metal compound is supported on the promoter compound, or a method in which a catalyst compound is covalently bonded to a functional group on the surface of the support (e.g., in the case of silica, a hydroxyl group (-OH) on the surface of the silica).
[0067] In an embodiment of the present invention, the olefin polymer may be a homopolymer of an olefin monomer or a copolymer of an olefin monomer and a comonomer. Preferably, the olefin polymer is a copolymer of an olefin monomer and an olefin comonomer.
[0068] Here, the olefin monomer is C 2-20 Alpha-olefin, C 1-20 Diolefin, C 3-20Cycloolefin and C 3-20 At least one selected from the group consisting of cyclodiolefins.
[0069] For example, the olefin monomer may be ethylene, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, or 1-hexadecene, and the olefin polymer may be a homopolymer containing only one of the olefin monomers exemplified above, or a copolymer containing two or more of them.
[0070] In an exemplary embodiment, the olefin polymer comprises ethylene and C 3-20 The olefin polymer may be a copolymer in which an alpha-olefin is copolymerized. Preferably, the olefin polymer may be a linear low-density polyethylene in which the olefin monomer is ethylene and the olefin comonomer is 1-hexene.
[0071] In this case, the content of ethylene is preferably 55 to 99.9% by weight, more preferably 90 to 99.9% by weight, and the content of the alpha-olefin comonomer is preferably 0.1 to 45% by weight, more preferably 0.1 to 10% by weight.
[0072] Method for producing olefin polymer According to one embodiment of the present invention, there is provided a method for producing an olefin polymer, comprising the step of polymerizing an olefin monomer in the presence of a hybrid catalyst comprising at least one first transition metal compound represented by the following chemical formula 1 and at least one second transition metal compound selected from a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3, to obtain an olefin polymer:
[0073] [ka]
[0074] In the above chemical formula, M 1 , M 2 , X, R 1 ~R 10 is as explained in the section on olefin-based polymers above.
[0075] As described above, the olefin polymer produced by the production method according to one embodiment of the present invention has the following characteristics: (1) a density of 0.915 to 0.950 g / cm 3 (2) Melt index (I 2.16 (3) the polydispersity index (Mw / Mn) is 2-5; and (4) the temperature rising elusion fractionation (TREF) of the multimodal distribution satisfies the following relationship 1:
[0076] [Equation 1] C 65 -C 45 >15(%)
[0077] Here, C 45 is the weight percent of polymer eluted at 45°C, C 65 is the weight percent of polymer eluted at 65°C.
[0078] In an embodiment of the present invention, the olefin polymer may be polymerized by a polymerization reaction such as, but not limited to, free radical, cationic, coordination, condensation, and addition.
[0079] As an embodiment of the present invention, the olefin polymer may be produced by a gas phase polymerization method, a solution polymerization method, a slurry polymerization method, etc. Preferably, the polymerization of the olefin monomer may be carried out by gas phase polymerization, specifically, the polymerization of the olefin monomer may be carried out in a gas phase fluidized bed reactor.
[0080] When olefin polymers are produced by solution polymerization or slurry polymerization, examples of usable solvents include C tetrahydrofurans such as pentane, hexane, heptane, nonane, decane, and their isomers. 5-12 Examples of the solvent include, but are not limited to, aliphatic hydrocarbon solvents; aromatic hydrocarbon solvents such as toluene and benzene; chlorine-substituted hydrocarbon solvents such as dichloromethane and chlorobenzene; and mixtures thereof.
[0081] Working Example The present invention will be described in more detail with reference to the following examples. However, the following examples are for illustrating the present invention, and the scope of the present invention is not limited to these examples.
[0082] Manufacturing Example The transition metal compound of formula 1-2 (dimethylbis(n-propylcyclopentadienyl)hafnium dichloride) and the transition metal compound of formula 3-1 ((pentamethylcyclopentadienyl)(n-propylcyclopentadienyl)zirconium dichloride) were purchased from MCN and used without further purification.
[0083] 4.07g of the transition metal compound of formula 1-2 and 1.68g of the transition metal compound of formula 3-1 were added to 892g of a 10% methylaluminoxane toluene solution and stirred at room temperature for 1 hour. After the reaction was completed, the solution was added to 200g of silica (XPO-2402), and 1.5L of toluene was added and stirred at 70°C for 2 hours. The catalyst after the loading was completed was washed with 500ml of toluene and dried overnight in a vacuum at 60°C to obtain 280g of a powdered supported catalyst.
[0084] Examples 1 to 3 Using a gas-phase fluidized bed reactor, an ethylene / 1-hexene copolymer was produced in the presence of the supported catalyst obtained in each of the Production Examples. The ethylene partial pressure in the reactor was about 15 kg / cm. 3 The polymerization temperature was maintained at 70 to 90°C.
[0085] The polymerization conditions for the above examples are shown in Table 1 below.
[0086] [Table 1]
[0087] Comparative Examples 1-2 For comparison, Hanwha Solutions' linear low density polyethylenes M1810HN (Comparative Example 1) and M2010EN (Comparative Example 2) were used.
[0088] Test Example The physical properties of the olefin polymers of the above examples were measured according to the following methods and standards, and the results are shown in Tables 2 and 3 below.
[0089] (1) Density Measured according to ASTM D1505.
[0090] (2) Melt index and melt flow ratio (MFR) According to ASTM D 1238, the melt index was measured at 190°C under a load of 21.6 kg and 2.16 kg, and the ratio (MI 21.6 / MI 2.16 ) was sought.
[0091] (3) Polydispersity index The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured by gel permeation chromatography (GPC), and the polydispersity index was calculated as the ratio between them.
[0092] (4) TREF Using cross-fractionation chromatography (CFC) equipment, the difference between the wt% value when the temperature was 65°C and the wt% value when the temperature was 45°C in a TREF graph showing the cumulative weight percentage (sum wt%) eluted by temperature was used.
[0093] [Table 2] [Industrial Applicability]
[0094] As can be seen from Table 2 and FIGS. 1 to 3, the olefin polymer according to the embodiment of the present invention has a high specific gravity of the copolymer having many branches derived from the comonomer, and therefore has excellent heat sealability.
Claims
1. (1) Density is 0.915 to 0.950 g / cm 3 (2) Melt index (I) measured at 190° C. under a load of 2.16 kg 2.16 (3) a polydispersity index (Mw / Mn) of 2 to 6; and (4) a temperature rising elution fractionation (TREF) of a multimodal distribution satisfies the following relationship 1: The olefin polymer is produced by polymerizing an olefin monomer and an olefin comonomer in the presence of a hybrid catalyst containing at least one first transition metal compound selected from the compounds represented by the following chemical formulas 1-1 and 1-2, and a second transition metal compound represented by the following chemical formula 3-1: An olefin polymer, wherein the olefin monomer is ethylene and the olefin comonomer is 1-hexene. [Relationship 1] C 65 -C 45 >15(%) Here, C 45 is the weight percent of polymer dissolved at 45° C., C 65 is the weight percent of polymer eluted at 65°C. 【Chemistry 1】
2. (1) The density of the olefin polymer is 0.915 to 0.940 g / cm 3 (2) a melt index, measured at 190° C. under a load of 2.16 kg, of 0.5 to 1.5 g / 10 min; and (3) a polydispersity index of 4 to 6.
3. 2. The olefin polymer according to claim 1, wherein the molar ratio of the secondary transition metal compound to the primary transition metal compound is in the range of 100:1 to 1:
100.
4. The olefin polymer according to claim 1, wherein the catalyst comprises at least one promoter compound selected from the group consisting of compounds represented by the following chemical formula 4, compounds represented by the following chemical formula 5, and compounds represented by the following chemical formula 6: 【Chemistry 2】 [Chemical formula 6] [L-H] + [Z(A) 4 ] - Or [L] + [Z(A) 4 ] - In the above formula 4, n is an integer of 2 or more, R a is a halogen atom, C 1-20 C substituted with a hydrocarbon group or halogen 1-20 is a hydrocarbon group, In the above formula 5, D is aluminum (Al) or boron (B), R b , R c and R d are each independently a halogen atom, C 1-20 Hydrocarbon groups, halogen-substituted C 1-20 Hydrocarbon group or C 1-20 is an alkoxy group, In the above formula 6, L is a neutral or cationic Lewis base, [L-H] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted C 6-20 an aryl group or a substituted or unsubstituted C 1-20 It is an alkyl group.
5. The olefin-based polymer according to claim 4, wherein the catalyst further comprises a support supporting the transition metal compound, the cocatalyst compound, or both.
6. The olefin-based polymer according to claim 5, wherein the support comprises at least one selected from the group consisting of silica, alumina and magnesia.
7. The olefin polymer according to claim 5, wherein the total amount of the mixed transition metal compounds supported on the support is 0.001 to 1 mmole per 1 g of the support, and the total amount of the co-catalyst compounds supported on the support is 2 to 15 mmole per 1 g of the support.
8. 2. The olefin polymer according to claim 1, which is a linear low-density polyethylene in which the olefin monomer is ethylene and the olefin comonomer is 1-hexene.
9. The method includes the steps of: polymerizing an olefin monomer and an olefin comonomer in the presence of a hybrid catalyst comprising at least one first transition metal compound selected from the compounds represented by the following chemical formulas 1-1 and 1-2; and a second transition metal compound represented by the following chemical formula 3-1 to obtain an olefin polymer; the olefin monomer is ethylene and the olefin comonomer is 1-hexene; The olefin polymer (1) has a density of 0.915 to 0.950 g / cm 3 (2) Melt index (I) measured at 190° C. under a load of 2.16 kg 2.16 (3) a polydispersity index (Mw / Mn) of 2 to 6; and (4) a temperature rising elution fractionation (TREF) of the multimodal distribution satisfies the following relationship 1: [Relationship 1] C 65 -C 45 >15(%) 【Chemistry 3】 In the above formula, C 45 and C. 65 is as defined in claim 1.
10. The method for producing an olefin polymer according to claim 9, wherein the polymerization of the olefin monomer is carried out by gas phase polymerization.
Citation Information
Patent Citations
Addition polymerization catalyst component, production method for addition polymerization catalyst and addition polymer, and use of metallocene transition metal compound
JP2003096125A
Ethylene polymer excellent in processability
JP2004149760A
Polyethylene resin composition and packaging film using the same
JP2006321986A
Dual Metallocene Catalysts for Making Film Resins with Excellent Machine Direction (md) Elmendorf Tear Strength
JP2007518871A
Mixed composition of hafnium compound and zirconium compound and method for producing the same