Resin composition and method for producing resin composition

The resin composition with a polymethylpentene continuous phase, thermoplastic elastomer dispersed phase, and interface-compatible phase addresses compatibility issues, achieving superior tensile properties and maintaining desirable resin characteristics.

JP7590638B2Active Publication Date: 2024-11-27NIPPON STEEL CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020167675
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-02
Publication Date
2024-11-27
Estimated Expiration
2040-10-02

AI Technical Summary

Technical Problem

Existing resin materials struggle to combine multiple properties such as heat resistance, chemical resistance, toughness, and processability due to poor compatibility and interfacial adhesion between different resin components, leading to inferior tensile properties.

Method used

A resin composition comprising a continuous phase of polymethylpentene, a dispersed phase of thermoplastic elastomer, and a compatible phase at the interface between the two, with a controlled area ratio of the dispersed phase, enhancing interfacial adhesion and stress dispersion.

Benefits of technology

The composition achieves improved tensile strength and elongation beyond additive expectations, leveraging a synergistic effect through a phase-separated structure with well-maintained interfacial adhesion, while retaining properties like lightness, heat resistance, and chemical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590638000003
    Figure 0007590638000003
  • Figure 0007590638000004
    Figure 0007590638000004
  • Figure 0007590638000005
    Figure 0007590638000005
Patent Text Reader

Abstract

To provide a resin composition that allows improved tensile characteristics while using polyolefin resin.SOLUTION: A resin composition contains polymethylpentene and a thermoplastic elastomer, the resin composition having a continuous phase composed of the polymethylpentene, a dispersed phase composed of the thermoplastic elastomer, and a compatible phase that lies at an interface between the continuous phase and the dispersed phase and in which the polymethylpentene and the thermoplastic elastomer are compatible with each other. The dispersed phase constitutes 0.6-12.0% of the resin composition by area.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing polymethylpentene and a thermoplastic elastomer, and a method for producing the resin composition. [Background technology]

[0002] Resin materials are used in a wide range of fields, and there is a demand for the development of resin materials that meet the increasingly diverse and complex required characteristics. In recent years, there are many cases in which contradictory characteristics are required. For example, automotive resins are required to be lightweight, as well as heat resistance, chemical resistance, toughness, and processability. However, it is difficult for a single existing resin to combine multiple properties. For example, the toughness and heat resistance of a resin are often in a trade-off relationship, and improving one can result in a significant decrease in the other.

[0003] For example, polyolefin resins such as polypropylene are lightweight general-purpose resins with various excellent properties, and are therefore used in a wide range of applications, such as home appliance parts, food packaging applications, medical supplies, automotive parts, etc. However, depending on the application, problems arise such as insufficient heat resistance and relatively poor elasticity and elongation.

[0004] Polymethylpentene, a polyolefin resin, has the chemical resistance and water resistance characteristic of polyolefins, and also has the lowest specific gravity among thermoplastic resins and excellent heat resistance with a melting point of 200 to 250° C. However, it still has issues such as relatively poor elasticity and elongation.

[0005] On the other hand, thermoplastic elastomers have excellent rubber elasticity, sufficient flexibility and large elongation, and furthermore, because they are thermoplastic, they can be processed relatively easily, but they are inferior in heat resistance and chemical resistance.

[0006] As mentioned above, it is becoming difficult to satisfy the complex needs of recent years with a single material, and resin materials with improved tensile properties are desired in addition to the light weight, heat resistance, and chemical resistance unique to polyolefins. As one of the solutions, efforts are being made to develop new materials that combine multiple properties that cannot be achieved with a single material by mixing multiple resins or resins and thermoplastic elastomers. When expecting improvement in tensile properties by mixing resins, compatibility between mixed materials such as resins and resins or resins and elastomers is important, and in the case of complete compatibility, the properties are expressed in an additive manner according to the addition ratio. On the other hand, when the main material and the additive material are not compatible and form a dispersion structure, it is expected to express a synergistic effect that cannot be achieved by each material alone. However, the synergistic effect is not expressed unconditionally, and in many cases, the compatibility between the two is poor, so a large dispersed phase is formed, or the physical properties are lower than those of the single material due to poor interfacial adhesion. Therefore, in order to express the synergistic effect by mixing, the development of a resin material with a controlled dispersion structure is desired.

[0007] For example, Patent Document 1 discloses a thermoplastic elastomer composition having a partially compatible continuous phase obtained by mixing a thermoplastic resin and a rubber, and describes that it is possible to provide a thermoplastic elastomer composition having an excellent balance of tensile strength, elongation, etc.

[0008] Patent Document 2 describes that by adding a predetermined amount of a thermoplastic elastomer to 4-methyl-1-pentene, it is possible to provide a packaging film that has high heat sealability without impairing the gas permeability of 4-methyl-1-pentene. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2019-70079 A [Patent Document 2] JP 2012-201392 A Summary of the Invention [Problem to be solved by the invention]

[0010] In Patent Document 1, it is described that the mechanism for providing a thermoplastic elastomer composition with an excellent balance of tensile strength, elongation, etc. is that the resin and rubber have a continuous phase in which they are partially compatible. However, it is not difficult to imagine that the partially compatible continuous phase makes the composition soft overall, and the tensile strength of the provided thermoplastic elastomer is lower than that of the added thermoplastic resin. In addition, kneading is required in a high-temperature environment until the partially compatible continuous phase is formed, which is 180°C for 30 minutes according to the example in Patent Document 1, but depending on the resin component or rubber component used, thermal degradation due to kneading cannot be avoided. Furthermore, the additive material is limited to rubber, that is, a material that requires the separate addition of a crosslinking agent, so while a composition mainly composed of a thermoplastic resin is obtained, the rubber component does not have plasticity and moldability is an issue.

[0011] Patent Document 2 aims to improve the heat sealability of the film while maintaining gas permeability, but does not improve tensile strength and elongation. In many cases, the compatibility between resins or between resins and elastomers is poor. Therefore, a large dispersed phase is formed, and the physical properties are often lower than those of a simple material due to poor interfacial adhesion, and tensile properties are not easily improved by resin blending. In addition, the addition of a propylene (co)polymer as a third additive is mentioned, but it is described as being compatible with the thermoplastic elastomer that constitutes the dispersed phase, and the purpose of adding it is to suppress blocking during kneading of raw materials or film formation, and to improve film formability.

[0012] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a resin composition which uses a polyolefin resin having the above-mentioned excellent properties and has improved tensile properties. [Means for solving the problem]

[0013] After thorough investigation into the conditions necessary to solve this problem, it was discovered that in order to obtain superior properties through the synergistic effect of a resin blend compared to each material alone, it is important to form a phase-separated structure and to maintain good interfacial adhesion by having partially compatible sites at the interface between the dispersed phase and the continuous phase.

[0014] That is, it was found that a partially compatible portion in the continuous phase as described in Patent Document 1 is not necessarily required, but it is important that a partially compatible phase exists at the interface between the continuous phase and the dispersed phase, and as a result, the stress propagating from the continuous phase reaches the elastomer which is the dispersed phase, and the stress is dispersed within the elastomer, so that the subsequent crack propagation is suppressed and the tensile strength and elongation are improved. These findings led to the invention.

[0015] The gist of the present invention is as follows. [1] A resin composition containing polymethylpentene and a thermoplastic elastomer, A continuous phase consisting of the polymethylpentene; A dispersed phase consisting of the thermoplastic elastomer; a compatible phase in which the polymethylpentene and the thermoplastic elastomer are compatible with each other and is present at the interface between the continuous phase and the dispersed phase; The resin composition, wherein the area ratio of the dispersed phase in the resin composition is 0.6 to 12.0%. [2] The resin composition according to [1], wherein the thermoplastic elastomer is at least one selected from the group consisting of styrene-ethylene-butylene-styrene (SEBS), styrene-butadiene-styrene (SBS), and styrene-butadiene rubber (SBR). [3] The tensile strength A (MPa) of the polymethylpentene alone, the tensile strength B (MPa) of the thermoplastic elastomer alone, the tensile strength C (MPa) of the resin composition, and the area ratio X (%) of the dispersed phase in the resin composition are C>(BA)X / 100+A The resin composition according to [1] or [2], which satisfies the above. [4] A method for producing a resin composition, comprising the steps of: A step of melt-kneading polymethylpentene and a thermoplastic elastomer; and cooling the melt-kneaded resin to room temperature. In the melt-kneading step, the thermoplastic elastomer is added in an amount of 1 to 18% based on the total volume ratio of the polymethylpentene and the thermoplastic elastomer; A continuous phase of the polymethylpentene, a dispersed phase of the thermoplastic elastomer, and a compatible phase in which the polymethylpentene and the thermoplastic elastomer are dissolved and which exists at the interface between the continuous phase and the dispersed phase are formed. A method for producing a resin composition. [5] The method for producing a resin composition according to [4], wherein the thermoplastic elastomer is at least one selected from the group consisting of styrene-ethylene-butylene-styrene (SEBS), styrene-butadiene-styrene (SBS), and styrene-butadiene rubber (SBR). [6] The tensile strength A (MPa) of the polymethylpentene alone, the tensile strength B (MPa) of the thermoplastic elastomer alone, the tensile strength C (MPa) of the resin composition, and the area ratio X (%) of the dispersed phase in the resin composition are C>(BA)X / 100+A The method for producing a resin composition according to [4] or [5], Effect of the Invention

[0016] According to the present invention, it is possible to improve the tensile properties of a polyolefin resin that has excellent light weight, heat resistance, chemical resistance, and further easy processability due to thermoplasticity. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is an explanatory diagram illustrating a phase-separated structure of a resin composition according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an example of a binarized contrast image of a resin composition according to an embodiment of the present invention, showing a binarized image of a visual field of 100 μm square. [Diagram 3] FIG. 1 is an example of visualization of the compatible phase of a resin composition according to an embodiment of the present invention by STXM, showing an STXM image with a field of view of 5 μm square. [Figure 4] 1 is an example of a K-shell X-ray absorption near-edge fine structure spectrum of a resin composition according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] An embodiment of the resin composition of the present invention will be described with reference to Fig. 1. The resin composition of this embodiment has a continuous phase 11 made of polymethylpentene and a dispersed phase 13 made of a thermoplastic elastomer, and has a phase separation structure in which the thermoplastic elastomer is dispersed as domains in the polymethylpentene matrix. The phase separation structure is also called a sea-island structure, in which the continuous phase is the sea and the dispersed phase is the islands.

[0019] The resin composition in this embodiment has a compatible phase 12 at the interface between the continuous phase and the dispersed phase. The compatible phase refers to a phase in which the molecular chains of the polymethylpentene and the thermoplastic elastomer penetrate and dissolve in each other.

[0020] The phase separation structure and the presence or absence of a compatible phase can be examined by STXM (Scanning Transmission X-ray Microscopy).

[0021] The resin composition is prepared into a thin film of about 100 nm by an ultramicrotome and measured, and the phase separation structure and the compatible phase can be identified from the obtained contrast image. The area ratio of the dispersed phase is calculated by binarizing the contrast image of a field of view of 100 μm square obtained by STXM under the condition of 100 nm / pixel. When the continuous phase is black and the dispersed phase is white and the binarization process is performed under the above conditions, the area ratio shown in white with respect to the entire contrast image of a field of view of 100 μm square is the area ratio of the dispersed phase. An example is shown in Figure 2. Furthermore, the presence or absence of a compatible phase can be determined from the binarized image, but it can be further clarified by obtaining a K-shell X-ray absorption near edge fine structure spectrum. For example, in the case of a resin composition having aromatic rings only in the thermoplastic elastomer, the absorption energy of the aromatic ring of 285 eV is irradiated to obtain a contrast image of a field of view of 5 μm square, and the regions of the continuous phase 31, the dispersed phase 33, and the compatible phase 32 are identified. An example is shown in Figure 3. The wavelength of the incident X-ray is scanned within each region. Then, the X-ray absorption spectrum of each phase can be obtained. An example is shown in FIG. 4. Comparing the spectra obtained for each phase (spectrum 41 of the continuous phase, spectrum 42 of the compatible phase, and spectrum 43 of the dispersed phase in FIG. 4), a spectrum having both the characteristics of the continuous phase and the dispersed phase is obtained for the compatible phase. From this, it is clear that a compatible phase exists. In the resin composition of this embodiment, it is not possible to obtain a sufficient effect simply by including a continuous phase made of polymethylpentene and a dispersed phase made of a thermoplastic elastomer, and it is important that a compatible phase exists at the interface between these phases. The presence of a compatible phase improves the interfacial adhesion, and as a result, the stress propagated from the continuous phase reaches the elastomer, which is the dispersed phase, and the stress is dispersed within the elastomer, so that it is considered that the progress of the crack is suppressed and the tensile strength and elongation are improved.

[0022] The addition ratio of the thermoplastic elastomer is preferably 1 to 18 vol% relative to the total of 100 vol% when polymethylpentene and the thermoplastic elastomer are added, and a resin composition is obtained that exhibits a superadditive law that exceeds the additive law tensile strength predicted from the tensile strength of each of polymethylpentene and the thermoplastic elastomer alone. In addition, the improvement in tensile elongation is also remarkable. A particularly preferred addition ratio of the thermoplastic elastomer is 1 to 15 vol% or 4 to 10 vol% relative to the total of 100 vol% when polymethylpentene and the thermoplastic elastomer are added. Here, the superadditive law that exceeds the additive law tensile strength predicted from the tensile strength of each of polymethylpentene and the thermoplastic elastomer alone means that the following formula (1-1) is established. C>(BA)X / 100+A Equation (1-1) In the above formula (1-1), A is the tensile strength (MPa) of the polymethylpentene alone, B is the tensile strength (MPa) of the thermoplastic elastomer alone, C is the tensile strength (MPa) of the resin composition, and X is the area ratio (%) of the dispersed phase in the resin composition. C is preferably 101% or more of A or B, more preferably 105% or more of A, even more preferably 110% or more of A, and most preferably 120% or more of A.

[0023] The area ratio of the dispersed phase calculated by the above method is 0.6 to 12.0% with respect to the entire contrast image of the resin composition in a field of view of 100 μm square. If the area ratio of the dispersed phase is too small, even if the stress propagated from the continuous phase reaches the elastomer which is the dispersed phase, the stress is not dispersed in the elastomer, and the progress of the crack cannot be stopped, so that the tensile strength and elongation are not improved. Therefore, the area ratio of the dispersed phase is 0.6% or more, and may be 1.0% or more, 1.5% or more, 2.0% or more, or 2.5% or more. On the other hand, if the area ratio of the dispersed phase is too high, the adhesion between the continuous phase and the dispersed phase is reduced, so that the improvement of the tensile strength and elongation cannot be expected. Therefore, the area ratio of the dispersed phase is 12.0% or less, and may be 11.0% or less, 10.0% or less, 9.0% or less, or 8.0% or less.

[0024] The thermoplastic elastomer in this embodiment is not particularly limited as long as it can form a compatible phase with polymethylpentene, and examples thereof include olefin-based elastomers and / or styrene-based elastomers. The thermoplastic elastomer is preferably a styrene-based elastomer, and more preferably at least one selected from the group consisting of styrene-ethylene-butylene-styrene (SEBS), styrene-butadiene-styrene (SBS), and styrene-butadiene rubber (SBR).

[0025] In this embodiment, the resin composition may be composed of only polymethylpentene and a thermoplastic elastomer, or may further contain other additives within a range that does not impair the purpose. Examples of these other additives include talc, mica, clay, basic magnesium carbonate, aluminum hydroxide, glass flakes, glass fibers, glass beads, carbon fibers, aramid fibers, boron fibers, silicon carbide fibers, steel fibers, PBO fibers, alumina fibers, high-strength polyethylene fibers, calcium carbonate, silica sand, barium sulfate, titanium oxide, antioxidants, flame retardants, flame retardant assistants, ultraviolet absorbers, antibacterial agents, heat stabilizers, antistatic agents, colorants, foaming agents, crosslinking agents, coupling agents, compatibilizers, etc. The content of other additives other than polymethylpentene and a thermoplastic elastomer is preferably 10% by mass or less, and may be 8% by mass or less, 5% by mass or less, 3% by mass or less, or 1% by mass or less.

[0026] The presence of polymethylpentene or thermoplastic elastomer in the resin composition can be confirmed by solid-state NMR measurement of the resin composition, especially 1 H and 13 It can be identified by C measurement.

[0027] The blend of polymethylpentene and thermoplastic elastomer is performed by melt kneading in a heated environment. The kneading temperature is a temperature equal to or higher than the melting points of the thermoplastic resin and the thermoplastic elastomer, for example, 180°C or higher or 220°C or higher, and the kneading is performed under conditions suitable for the materials, for example, a kneading time of 1 minute or more or 2 minutes or more, and a mixer rotation speed of 80 rpm or more or 90 rpm or more, and the resin composition is removed from the kneading mixer and cooled. The kneading temperature may be 300°C or lower or 280°C or lower, and the kneading time may be 10 minutes or lower or 5 minutes or less. The mixer rotation speed may be 150 ppm or lower or 120 ppm or lower. In order to prevent thermal deterioration due to long-term exposure to the high temperature of the kneading mixer, the resin composition is removed from the kneading mixer after kneading, but since a phase separation structure is formed during melt kneading, the subsequent cooling rate does not matter. Kneading can be performed with a known kneading mixer.

[0028] The resin composition of the present embodiment is a resin composition that has excellent tensile properties that show the superadditivity rule while mainly using a polyolefin resin that has excellent light weight, heat resistance, and chemical resistance as described above. Therefore, the resin composition can be used in a wide range of applications such as home appliance parts, food packaging applications, medical supplies, and automobile parts. EXAMPLES

[0029] The following examples of the present invention are described, but the present invention is not limited to these examples. The methods for producing various resin compositions and the methods for measuring the properties are as follows. Table 1 shows the raw materials for each example and comparative example.

[0030] [Table 1]

[0031] Example 1 Polymethylpentene (A1) and SEBS (B1), which had been previously dried in a vacuum at 70°C for 24 hours, were weighed out so that A1:B1 was 96:4 vol%, and melt-kneaded in a kneader at 225°C. A Toyo Seiki R-30 was used as the kneading mixer, and the kneading mixer volume was 30 cm3 The raw materials were charged so that the filling rate was 80%. After the entire amount of the raw materials was charged, the mixture was mixed for 3 minutes at a rotation speed of 100 rpm, and the resin composition was removed from the mixer and allowed to cool naturally. The mixture was then pressed at 250°C for 5 minutes at 4 MPa in a hot press (Toyo Seiki Co., Ltd., tabletop mini hot press), and cooled with water to produce a sheet with a thickness of 0.2 mm. The results were evaluated by a tensile test. The results are shown in Table 2.

[0032] Example 2 A1 and B1, which had been previously dried in a vacuum at 70° C. for 24 hours, were weighed out so that A1:B1 was 95:5 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0033] Example 3 A1 and B1, which had been previously dried in a vacuum at 70° C. for 24 hours, were weighed out so that A1:B1 was 90:10 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0034] Example 4 A1 and B1, which had been previously dried in a vacuum at 70° C. for 24 hours, were weighed out so that A1:B1 was 85:15 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0035] Example 5 A1 and SEBS (B2), which had been previously dried in a vacuum at 70° C. for 24 hours, were weighed out so that A1:B2 was 90:10 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0036] Example 6 A1 and SBS (B3), which had been previously dried in a vacuum at 70° C. for 24 hours, were weighed out so that A1:B3 was 90:10 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0037] Example 7 A1, which had been previously dried in a vacuum at 70° C. for 24 hours, and SBR (B4) were weighed out so that A1:B4 was 90:10 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0038] Comparative Example 1 A1, which had been previously dried in a vacuum at 70° C. for 24 hours, was weighed and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0039] Comparative Example 2 A1 and B1, which had been previously dried in a vacuum at 70° C. for 24 hours, were weighed out so that A1:B1 was 80:20 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0040] Comparative Example 3 A1, which had been previously dried in a vacuum at 70°C for 24 hours, and styrene-isoprene-styrene (SIS) (B5) were weighed out so that A1:B5 was 90:10 vol%, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0041] Comparative Example 4 A1, which had been previously dried in a vacuum at 70° C. for 24 hours, and Bondfast (B6), a glycidyl methacrylate-modified polyethylene copolymer, were weighed out so that A1:B6 was 90:10 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0042] Comparative Example 5 A1, which had been previously dried in a vacuum at 70°C for 24 hours, and the thermoplastic polyester elastomer Hytrel (B7) were weighed out so that A1:B7 was 90:10 vol%, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0043] Comparative Example 6 Polypropylene (A2) previously dried in a vacuum at 70° C. for 24 hours and B1 were weighed out so that A2:B1 was 95:5 vol %, and kneaded in the same manner as in Example 1. Furthermore, the tensile properties were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0044] The tensile test was carried out using an AGS-H manufactured by Shimadzu Corporation, and the tensile strength (MPa) and tensile elongation at break (%) were evaluated. The resin composition was cut into a size of 75×10×0.2 mm, and the measurements were performed with a gauge length of 10 mm and a crosshead speed of 500 mm / min.

[0045] The visualization of the miscible phase and the confirmation of the dispersed phase were carried out using an STXM. The equipment used was a BRUKER ASC STXM installed at the beamline BL4U of the Extreme Ultraviolet Research Facility (UVSOR) of the Institute for Molecular Science, National Institutes of Natural Sciences. Thin films of approximately 100 nm were prepared using an ultramicrotome and measurements were carried out. Energy of 285 eV was used to acquire the images.

[0046] The preparation conditions and the obtained verification results of Examples 1 to 7 and Comparative Examples 1 to 6 are summarized in Table 2.

[0047] [Table 2]

[0048] As shown in Table 2, the resin composition of the present invention has a continuous phase composed of polymethylpentene, but contains a thermoplastic elastomer as a dispersed phase, and further has a compatible phase in which polymethylpentene and thermoplastic elastomer are compatible at the interface between them, thereby satisfying formula (1-1) and achieving tensile properties showing the superadditivity law. In addition, the resin composition of the present invention also achieved good results in terms of tensile elongation at break, specifically, even the lowest tensile elongation at break of 8% was achieved in Examples 6 and 7, and tensile elongation at break of 15% was achieved in Examples 3 and 5. In addition, since the resin composition of the present invention uses polymethylpentene as a main component, it has the light weight, heat resistance, and chemical resistance peculiar to polyolefin resins, and further has ease of processing derived from thermoplasticity, and in fact, all of the produced resin compositions had thermoplasticity and were easy to process. On the other hand, the tensile properties of the resin compositions of Comparative Examples 1 to 6 were below the additivity law and were inferior. [Industrial Applicability]

[0049] The resin composition of the present invention combines the excellent characteristics of polyolefins with superadditive tensile strength, and can therefore be used in a wide range of applications, such as home appliance parts, food packaging, medical supplies, and automobile parts. [Explanation of symbols]

[0050] 11: Continuous phase 12: Compatible phase 13: Dispersed phase 31: Continuous phase 32: Compatible phase 33: Dispersed phase 41:31 Spectrum The 42:32 Spectrum The 43:33 Spectrum

Claims

1. A resin composition comprising polymethylpentene and a thermoplastic elastomer, The thermoplastic elastomer is at least one selected from the group consisting of styrene-ethylene-butylene-styrene (SEBS) and styrene-butadiene-styrene (SBS); A continuous phase consisting of the polymethylpentene; A dispersed phase consisting of the thermoplastic elastomer; a compatible phase in which the polymethylpentene and the thermoplastic elastomer are compatible with each other and which is present at the interface between the continuous phase and the dispersed phase; The resin composition has an area ratio of a dispersed phase of 0.6 to 12.0%.

2. The tensile strength A (MPa) of the polymethylpentene alone, the tensile strength B (MPa) of the thermoplastic elastomer alone, the tensile strength C (MPa) of the resin composition, and the area ratio X (%) of the dispersed phase in the resin composition are C>(B-A)X / 100+A The resin composition according to claim 1, which satisfies the above.

3. A resin composition described in claim 1 or 2, having a phase separation structure in which the dispersed phase is dispersed in the continuous phase which serves as a matrix.

4. A method for producing a resin composition, comprising: A step of melt-kneading polymethylpentene and a thermoplastic elastomer; and cooling the melt-kneaded resin to room temperature. In the melt-kneading step, the thermoplastic elastomer is added in an amount of 1 to 18% based on the total volume ratio of the polymethylpentene and the thermoplastic elastomer; A continuous phase of the polymethylpentene, a dispersed phase of the thermoplastic elastomer, and a compatible phase in which the polymethylpentene and the thermoplastic elastomer are dissolved and which exists at the interface between the continuous phase and the dispersed phase are formed, The thermoplastic elastomer is at least one selected from the group consisting of styrene-ethylene-butylene-styrene (SEBS) and styrene-butadiene-styrene (SBS). A method for producing a resin composition.

5. The tensile strength A (MPa) of the polymethylpentene alone, the tensile strength B (MPa) of the thermoplastic elastomer alone, the tensile strength C (MPa) of the resin composition, and the area ratio X (%) of the dispersed phase in the resin composition are C>(B-A)X / 100+A The method for producing a resin composition according to claim 4, which satisfies the above.

6. A method for producing a resin composition described in claim 4 or 5, which has a phase separation structure in which the dispersed phase is dispersed in the continuous phase which serves as a matrix.

Citation Information

Patent Citations

  • Packaging film, laminated packaging film, method for manufacturing packaging film and packaging method using packaging film

    JP2012201392A

  • 4-methyl-1-pentene-based resin composition and molded article thereof

    JP2013216817A

  • Thermoplastic elastomer composition

    JP2019070079A