cBN sintered body
A cBN sintered body with controlled cubic boron nitride content and balanced transition metal compound groups in the binder phase addresses wear and chipping issues, enhancing cutting tool durability for high-hardness steel applications.
Patent Information
- Application Number
- JP2021043149
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-17
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2041-03-17
AI Technical Summary
Existing cubic boron nitride (cBN) sintered bodies lack sufficient wear resistance and chipping resistance when used as cutting tools for high-hardness steel, due to uncontrollable impurity mixing and unspecified binder phase compositions.
A cBN sintered body with controlled ratios of cubic boron nitride particles (30 to 85% by volume) and a binder phase containing specific transition metal compound groups (VB and VC, TaB and TaC, NbB and NbC, CrB and CrC) with a balanced 111 diffraction line intensity ratio (1.0≦I MB /I MC ≦3.0) is developed.
The improved cBN sintered body exhibits enhanced wear resistance and fracture resistance, extending tool life and ensuring reliable performance in cutting high-hardness steel.
Smart Images

Figure 0007590695000004 
Figure 0007590695000001 
Figure 0007590695000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a cubic boron nitride sintered body (hereinafter sometimes referred to as a cBN sintered body), which is a hard composite material. [Background technology]
[0002] Although cBN sintered compacts are inferior in hardness to diamond, they have the property of low reactivity with Fe-based and Ni-based materials, and therefore are also used as cutting tools. There have been proposals to improve the performance of cBN sintered compacts.
[0003] For example, Patent Document 1 describes a cBN sintered body containing 40 to 85 volume % cBN, at least one metal selected from Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Ni, and Al, a binder phase consisting of at least one metal selected from the group consisting of at least one carbide, nitride, carbonitride, boride, oxide, and mutual solid solutions of these metals, and the remainder being unavoidable impurities, with Mo content of 0.2 to 3.0 mass %, Ni content of 0.2 to 3.0 mass %, and Ta content of 0.5 to 3.0 mass %, and it is said that when the sintered body is used as a cutting tool, it has excellent wear resistance and chipping resistance.
[0004] Furthermore, for example, Patent Document 2 describes polycrystalline cBN in which protruding borides are formed on the surface of the cBN, the average particle size of which is 4 to 8 μm, the volume ratio of which is 70 to 85 volume %, and the borides are formed within 100 nm of the surface of the cubic boron nitride particles, with sizes of 0.001 to 1 μm, and this polycrystalline cBN is said to have excellent impact resistance and wear resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5614460 [Patent Document 2] Patent No. 6715349 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above circumstances and proposals, and has an object to obtain a cBN sintered body having improved wear resistance and fracture resistance when used, for example, as a cutting tool for high-hardness steel. [Means for solving the problem]
[0007] The cubic boron nitride sintered body according to the embodiment of the present invention is It has cubic boron nitride particles and a binder phase, The content of the cubic boron nitride particles is 30 to 85% by volume, The binder phase includes any one of the four combinations of transition metal compounds: VB and VC, TaB and TaC, NbB and NbC, and CrB and CrC; The transition metal element constituting the transition metal compound group is contained in an amount of 0.1 to 0.8 atomic %; The 111 diffraction intensity of the metal borides in the transition metal compound group is I MB , the 111 diffraction intensity of metal carbide is I MC When I MB / I MC <=3.0.
[0008] In addition, the cubic boron nitride sintered body according to the embodiment has the following features (1) to (4): (2) may satisfy one or more of the above.
[0009] (1) The content of cubic boron nitride particles is 40 to 80 volume percent. (2) The average particle size of the cubic boron nitride particles is 2.0 to 8.0 μm. Effect of the Invention
[0010] When the cubic boron nitride sintered body is used as a cutting tool, the wear resistance and chipping resistance can be further improved. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a schematic diagram showing the structure of a cBN sintered body according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] As a result of examining the proposals described in the above-mentioned patent documents, the present inventors have 1) Carbon, an impurity (unavoidable impurity) that is unintentionally mixed in during the manufacturing process, adheres to the cBN particle interfaces, reducing strength. 2) The content ratio of compounds or mutual solid solutions in the binder phase is not specified, so depending on the compounds contained or the content ratio of the compounds, the cutting conditions under which high-hardness steel is subjected to high loads may not be able to be endured. I recognized that.
[0013] Therefore, the present inventors have conducted extensive research in order to obtain a cBN sintered body having improved wear resistance and fracture resistance, taking the above-mentioned knowledge into consideration. As a result, the following findings 1) to 5) have been obtained.
[0014] 1) When an appropriate amount of orthorhombic metal boride is produced by heat treatment from the hexagonal metal diboride, which is added as raw material powder to form the binder phase of the cBN sintered body, the wear resistance and chipping resistance of the cBN sintered body are improved.
[0015] 2) However, simply generating metal borides is not sufficient to improve the wear resistance and fracture resistance of cBN sintered bodies.
[0016] 3) In order to solve the problem 2) above, it is preferable that the carbon inevitably contained in the orthorhombic metal boride during the formation of the orthorhombic metal boride does not exist as elemental carbon but exists as a cubic metal carbide. However, since the cubic metal carbide itself is an embrittlement material, if too much is produced, the wear resistance and fracture resistance will decrease, and therefore unless the amount produced is controlled, the wear resistance and fracture resistance will not improve.
[0017] 4) To this end, the binder phase must contain one of the following four combinations of components: VB and VC, TaB and TaC, NbB and NbC, and CrB and CrC.
[0018] 5) As mentioned above, metal carbides are embrittles, and therefore if too much is produced, the wear resistance and chipping resistance decrease. On the other hand, orthorhombic metal borides are less susceptible to wear when cutting high-hardness steel, but if too much is produced, chipping resistance decreases. Therefore, it is necessary to control the amounts of metal borides and metal carbides produced to an appropriate ratio, and as an indicator of this, the amounts produced can be quantitatively evaluated by comparing the intensity of the 111 diffraction line in the transition metal compound group.
[0019] The cBN sintered body according to the embodiment of the present invention will be described in detail below. In the present specification and claims, when a numerical range is expressed as "A to B" (A and B are both numerical values), this is equivalent to "A or more and B or less," and the range includes an upper limit (B) and a lower limit (A). The units of the upper limit and the lower limit are the same. Furthermore, the numerical values include tolerances.
[0020] As shown in FIG. 1, this embodiment has cBN particles (1) and a binder phase (2), in which metal carbide particles (3) and metal boride particles (4) selected from one of the four combinations of VB and VC, TaB and TaC, NbB and NbC, and CrB and CrC are dispersed. These will be explained below.
[0021] 1. Cubic boron nitride (cBN) particles The average grain size of the cBN grains and the content ratio of the cBN grains in the cBN sintered compact will be described below.
[0022] (1) Average particle size The average particle size of the cBN particles used in this embodiment is not particularly limited, but is more preferably in the range of 2.0 to 8.0 μm.
[0023] The reason is that, in addition to the fact that the inclusion of cBN particles in the sintered body enhances the chipping resistance, if the average grain size is 2.0 to 8.0 μm, when used as a cutting tool, not only chipping caused by the uneven shape of the cutting edge caused by the falling off of cBN particles on the tool surface is more reliably suppressed, but also the propagation of cracks that develop from the interface between the cBN particles and the binder phase caused by the stress applied to the cutting edge during use, or cracks that develop as the cBN particles break, is more suppressed, resulting in better chipping resistance. The average grain size is more preferably 3.0 to 6.0 μm, and even more preferably 3.5 to 5.0 μm.
[0024] Here, the average particle size of the cBN particles can be determined as follows. The cross section of the cBN sintered body is mirror-finished, and the mirror-finished surface is observed with a scanning electron microscope (SEM) to obtain a secondary electron image. Next, the cBN grains in the obtained image are extracted by image processing, and the average grain size (described later) is calculated based on the maximum length of each grain determined by image analysis.
[0025] Here, when extracting the cBN particle portion of the image through image processing, in order to clearly distinguish between the cBN particles and the binder phase, the image is displayed in monochrome with 256 gradations, with 0 being black and 255 being white, and binarization processing is performed so that the cBN particles appear black using an image with pixel values such that the ratio of the pixel values of the cBN particle portion to the pixel values of the binder phase portion is 2 or more.
[0026] In addition, it is desirable to select an area of approximately 0.5 μm × 0.5 μm as the area for determining the pixel value of the cBN particle portion, and to use the average value determined from at least three different points within the same image area as the aforementioned pixel value of cBN.
[0027] After the binarization process, a process is performed to separate the cBN grains that are thought to be in contact with each other, for example, a watershed method is used to separate the cBN grains that are thought to be in contact with each other.
[0028] The areas corresponding to the cBN particles in the image obtained after the binarization process described above (black areas) are subjected to particle analysis, and the maximum length of each particle obtained is taken as the diameter of each particle. In particle analysis to determine the maximum length, the Feret's diameter for one cBN particle is calculated, and the larger of the two lengths obtained is taken as the maximum length, and this value is taken as the diameter of each particle.
[0029] Assuming each particle is an ideal sphere with this diameter, the cumulative volume is calculated as the volume of each particle, and a graph is drawn based on this cumulative volume with the vertical axis representing volume percentage (%) and the horizontal axis representing diameter (μm), and the diameter when the volume percentage is 50% is taken as the average particle size of the cBN particles. This is done for the three observation areas, and the average value is taken as the average particle size (μm) of the cBN particles.
[0030] When performing this particle analysis, the length per pixel (μm) is set using the scale value known in advance from the SEM. As the observation area used for image processing, if the average particle size of the cBN particles is about 4.0 μm, a field of view of about 40 μm × 40 μm is desirable.
[0031] (2)Content ratio The content (volume %) of cBN particles in the cBN sintered compact is more preferably 40 to 80 volume %.
[0032] The reason is that if the content is less than 40% by volume, the hard material in the cBN sintered body is small, and when used as a cutting tool, the chipping resistance may decrease, while if the content exceeds 80% by volume, voids that become the starting points of cracks are generated in the cBN sintered body, and the chipping resistance may decrease.The content of cBN particles is more preferably 50 to 75% by volume.
[0033] The cBN particle content in a cBN sintered compact can be determined as follows: the cross-sectional structure of the cBN sintered compact is observed by SEM, the cBN particle portion of the obtained secondary electron image is extracted by image processing, the area occupied by the cBN particles is calculated by image analysis, and the images of at least three observation regions are processed and the average value obtained is taken as the cBN particle content (volume %). When the average cBN particle content is about 50 volume %, a field of view of about 40 μm × 40 μm is preferred as the observation region used for image processing.
[0034] 2. Bonded phase The binder phase preferably contains any one of the four combinations of transition metal compounds: VB and VC, TaB and TaC, NbB and NbC, and CrB and CrC, and there are no particular limitations on the other components.
[0035] Examples of other components include one or more of Al borides, nitrides and oxides, and one or more of Ti borides, nitrides, carbides and carbonitrides.
[0036] Then, for the borides and carbides of the transition metal compound group, the 111 diffraction ray intensity of the metal borides was calculated as I MB , the 111 diffraction intensity of metal carbide is I MC When I MB / I MC When it is ≦3.0, the wear resistance and fracture resistance are improved.
[0037] Here, the above I MB , I MC is measured using Cu-Kα radiation as the X-ray source. The wavelength of the X-ray is 1.54 Å.
[0038] The content of the transition metal element in the transition metal compound group is not particularly limited, but is preferably 0.1 to 0.8 atomic %. If the content is within this range, the above-mentioned object can be reliably achieved. Here, the atomic % refers to the ratio of the transition metal atoms contained in the transition metal compound group to all atoms contained in the cBN sintered body.
[0039] The content of the transition metal element in the cBN sintered compact is determined by analyzing the cBN sintered compact with an electron probe micro analyzer (EPMA), and the content (atomic %) of the transition metal element in the cBN sintered compact is obtained by subjecting the detected elements to the ZAF quantitative analysis method. EXAMPLES
[0040] Next, examples will be described, but the present invention is not limited to the examples in any way.
[0041] This example was produced by the following steps (1) to (4).
[0042] (1) To obtain the metal boride of the transition metal compound group, a metal diboride powder having an average particle size of 0.1 μm to 6.0 μm (VB 2 , NbB 2 , TaB 2 ,CrB 2 A container lined with cemented carbide was filled with cemented carbide balls and acetone, and the container was then covered with a lid and crushed using a ball mill. The mixed slurry was then dried and classified using a centrifugal separator to obtain a metal diboride raw powder having an average particle size of 20 to 300 nm.
[0043] (2) Ti compound powder (TiN powder, TiC powder, TiCN powder, TiAl powder, etc. shown in Table 1) 3 At least one of the powders was selected from the above-mentioned (1) and the metal diboride raw powder (MB powder in Table 1). 2 The powder was mixed with cBN powder as the raw material for the hard phase, and the mixture was dried to obtain a raw powder for the sintered body.
[0044] (3) The obtained raw powder for the sintered body was press-molded to a size of 50 mm in diameter and 1.5 mm in thickness at a molding pressure of 1 MPa, and then this molded body was pre-sintered by maintaining it at a predetermined temperature in the range of 900 to 1300°C in a vacuum atmosphere with a pressure of 1 Pa or less. The main purpose of the pre-sintering was to remove the solvent during the wet mixing.
[0045] (4) The green body produced in (3) was placed in an ultra-high pressure sintering apparatus and sintered under ultra-high pressure conditions of a pressure of 5 GPa, a temperature of 1200 to 1400°C, and a holding time of 30 minutes, thereby obtaining the sintered bodies of the present invention (Examples 1 to 12) shown in Table 2.
[0046] For comparison, there are also those which do not have a compound of the transition metal compound group in the binder phase, those which contain only metal borides or only metal carbides as transition metal compounds, those which do not have borides and carbides of the same transition metal, and those which have a range of 1.0≦I MB / I MC Comparative sintered bodies (Comparative Examples 1' to 8') not satisfying the range ≦3.0 were produced by the same steps as in (1) to (4).
[0047] Next, the above-prepared Examples 1 to 12 and Comparative Examples 1' to 8' were cut to a predetermined size by a wire electric discharge machine. This was brazed to the brazing part (corner part) of the WC-based cemented carbide insert body having a composition of Co: 5 mass%, TaC: 5 mass%, WC: remainder, and an insert shape of ISO standard CNGA120408 using a brazing material of Ag alloy having a composition of Cu: 26 mass%, Ti: 5 mass%, Ag: remainder, and the upper and lower surfaces and the outer circumference were polished and honed to produce the cBN-based ultra-high pressure sintered compact cutting tools of the present invention (Examples 1 to 12) and the comparative cBN-based ultra-high pressure sintered compact cutting tools (Comparative Examples 1' to 8') having the insert shape of ISO standard CNGA120408 shown in Table 2.
[0048] In addition, Table 2 shows the I measured by the above-mentioned method in Examples 1 to 12 and Comparative Examples 1' to 8'. MB / I MC , the atomic percentage of the transition metal element, the content of cBN particles, and the average particle size.
[0049] [Table 1]
[0050] [Table 2]
[0051] Next, cutting was carried out under the following cutting conditions for Examples 1 to 12 and Comparative Examples 1' to 8', and the tool life (cutting time) until chipping occurred was measured. <Cutting conditions> Work material: Carburized steel (JIS SCR420, hardness: HRC58~62) round bar Cutting speed: 250m / min Cut: 0.2mm Feed: 0.1mm / rev Dry cutting tests of high hardness steel were conducted under the above conditions.
[0052] The tool life was defined as the time when the cutting edge of each tool was chipped. The cutting edge was observed every 30 seconds of cutting time to check for the presence or absence of chipping on the cutting edge, and the time until the tool life was determined. Table 3 shows the results of the cutting test.
[0053] [Table 3]
[0054] From the results shown in Table 3, it can be seen that in all of the Examples, the tool life was extended without the occurrence of sudden chipping of the cutting edge compared to all of the Comparative Examples, and the toughness was improved, and the effect of excellent chipping resistance was also achieved in the continuous cutting of hardened steel. [Industrial Applicability]
[0055] The cBN sintered body of the present invention, when used as a cutting tool, exhibits excellent fracture resistance over long-term use without the occurrence of fracture, and aims to extend the tool life, and therefore can fully respond to the needs for improving the performance of cutting equipment, as well as for reducing labor and energy consumption in cutting, and for reducing costs. [Explanation of symbols]
[0056] 1 cBN particle 2 Bonded phase 3 Metal carbide particles 4 Metal boride particles
Claims
1. A cubic boron nitride sintered body having cubic boron nitride particles and a binder phase, The content of the cubic boron nitride particles is 30 to 85 volume %, The binder phase includes any one of the four combinations of transition metal compounds: VB and VC, TaB and TaC, NbB and NbC, and CrB and CrC; The transition metal element constituting the transition metal compound group is contained in an amount of 0.1 to 0.8 atomic %; The 111 diffraction intensity of the metal boride in the transition metal compound group is I MB , the 111 diffraction intensity of the metal carbide is I MC When I MB / I MC 3. A cubic boron nitride sintered body, characterized in that:
2. 2. The cubic boron nitride sintered body according to claim 1, wherein the content of said cubic boron nitride particles is 40 to 80 volume %.
3. 3. The cubic boron nitride sintered body according to claim 1, wherein the cubic boron nitride particles have an average particle size of 2.0 to 8.0 μm.
Citation Information
Patent Citations
Novel cement and production method thereof
JP1981014460A
Dense sintered ceramic body containing chromium compound
JP1984089749A
Aluminum nitride sintered compact and its production
JP1995309663A
Sputtering target, its production and resistance film formed by using the same and thermal printer head
JP1997031636A
Rolling support unit
JP2005195165A