Manufacturing method of press-molded products

By pre-forming a convex shape on the outer blank to align cross-sectional line lengths, the method addresses misalignment and joint breakage in cold press patchwork, enabling efficient and cost-effective manufacturing of vehicle body frame parts.

JP7590700B2Active Publication Date: 2024-11-27JFE STEEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022188001
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-12
Filing Date
2022-11-25
Publication Date
2024-11-27
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

Cold press patchwork methods for manufacturing vehicle body frame parts with ultra-high tensile steel plates face issues of misalignment and joint breakage due to differing cross-sectional line lengths at bends, leading to inefficiencies and increased costs.

Method used

A method involving pre-forming a convex shape on the outer blank to match the bending direction, followed by joining and press-molding to align cross-sectional line lengths, minimizing misalignment and joint breakage.

Benefits of technology

Stable and efficient production of press-formed products with reduced joint breakage, achieving target shapes without misalignment, thus improving production efficiency and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590700000002
    Figure 0007590700000002
  • Figure 0007590700000003
    Figure 0007590700000003
  • Figure 0007590700000004
    Figure 0007590700000004
Patent Text Reader

Abstract

To provide a method of manufacturing a press-formed article that can obtain a press-formed article of a target shape without causing breakage of a junction of blanks that are stacked after press-forming.SOLUTION: A method of manufacturing a press-formed article 1 is for manufacturing a press-formed article 1 of a target shape having a U-shaped cross-sectional shape or a hat-shaped cross-sectional shape by stacking a plurality of blanks made of metal plates followed by press-forming, includes: a first forming step of forming a pre-formed blank 15 provided with a convex shape 13 extending in a ridge direction of bending, on a blank arranged outside of bending in a bent part in the press-forming; a joint blank preparing step of joining a blank arranged inside of bending in the bent part in the press-forming to a surface opposite a surface on which the convex shape 13 in the pre-formed blank 15 has been formed, and preparing a joint blank 25; and a second forming step of press-forming the joint blank 25 into the target shape by arranging the joint blank 25 in a metal mold 11 such that the convex shape 13 of the joint blank 25 lies outside of the bending.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a press-formed product having a U-shaped or hat-shaped cross-sectional shape, and more particularly to a method for manufacturing a press-formed product by stacking and press-forming a plurality of blanks to produce a press-formed product. [Background technology]

[0002] As collision safety standards become stricter, the strength of the body frame parts of automobiles is being further increased. For example, automobile pillars are important parts for protecting passengers in the cabin during a collision, and they require strength that can withstand collision loads. Therefore, efforts are being made to use high-strength materials such as high-tensile steel plates for these parts.

[0003] Increasing the overall thickness of autobody frame components that make up the cabin, such as pillars, in order to improve their strength increases the weight of the vehicle, reducing the vehicle's fuel efficiency and increasing carbon dioxide emissions.

[0004] Therefore, it is possible to reinforce only the necessary areas rather than the entire part. Because the load during a collision is transmitted mainly through the bending ridges of the parts, auto body frame parts are often partially reinforced by adding reinforcing parts to parts near the bending ridges. To manufacture such a partially reinforced part, for example, the main part and the reinforcing part may be press-molded separately and then joined together in a subsequent process. However, with this method, it is necessary to prepare separate dies for the main body component and the reinforcing component and press-molding them separately, which poses the problem of increased die manufacturing costs and increased man-hours for press molding.

[0005] In response to this, there is a press molding method called patchwork, in which a blank for a main body part and a blank for a reinforcing part are joined in advance in an overlapping state, and the joined blank is press molded in one die, as described in, for example, Patent Documents 1 and 2. With this patchwork method, the main body part and the reinforcing part can be press molded as a single unit, thereby reducing die manufacturing costs and press molding man-hours. Furthermore, compared to a press-formed product in which the main part and reinforcing part are press-formed separately and then joined together, a press-formed product formed by press-forming a patchwork of parts has close contact between the main part and reinforcing part, making it less likely to buckle even when a compressive load is applied, and is more efficient in improving performance.

[0006] Patent Document 1 describes a manufacturing method in which blanks are stacked by hot pressing, in which the blanks are heated and press-formed, and simultaneously quenched in a die. In Patent Document 1, the blanks are given protrusions; however, these protrusions are intended to form a space for escaping Zn vapor generated from the blanks (plated sheets) in order to prevent surface cracks that may occur when the blanks are stacked and heated; in order to form this space, the protrusions are formed in a convex shape on the inner surface where the blanks are stacked together.

[0007] Furthermore, Patent Document 2 discloses that in order to reduce misalignment between overlapping blanks during press forming, the overlapping blanks are curved in the same direction as the bending direction of the press-formed product, then joined and press-formed. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2013-184221 A [Patent Document 2] JP 2020-121336 A Summary of the Invention [Problem to be solved by the invention]

[0009] The hot press disclosed in Patent Document 1 requires high costs for heating the blank and requires time for rapid cooling, resulting in low production efficiency. Therefore, in recent years, cold press forming has been carried out using ultra-high tensile steel sheets for cold press, such as 1470 MPa class, which can reduce heating costs and improve production efficiency. However, in patchwork cold press forming, the cross-sectional line lengths differ between the inside and outside of the bend at bending areas such as the punch shoulder R section, which can cause misalignment between stacked blanks during press forming, and the joints that have been previously joined by stacking the blanks can break during press forming.

[0010] In this regard, as disclosed in Patent Document 2, by bending overlapping blanks in the same direction as the bending direction of the press-formed product, joining them, and press-forming them, it is possible to reduce the misalignment between overlapping blanks during press forming. However, in the method of Patent Document 2, two blanks are curved using multiple jigs, so it is not possible to impart deformation that corresponds to the large bending angle between the top plate portion and the vertical wall portion during press forming. As a result, the misalignment between the stacked blanks during press forming may not be sufficiently eliminated, which may result in the joint breaking.

[0011] The present invention has been made to solve such problems, and aims to provide a method for manufacturing a press-formed product that uses a steel plate for cold pressing to sufficiently eliminate the misalignment between stacked blanks during press forming, and that can obtain a press-formed product of a target shape without causing fracture of the joint after press forming. [Means for solving the problem]

[0012] Before describing the specific means, the misalignment that occurs between overlapping blanks when the overlapping blanks are press-molded by patchwork will be described with reference to Figs. 11 and 12.

[0013] Fig. 11 shows an example of a press-formed product 1 manufactured by patchwork and consisting of a main body part 3 having a hat-shaped cross-sectional shape and a reinforcing part 5 having a U-shaped cross-sectional shape arranged inside the main body part 3, Fig. 11(a) is a perspective view, and Fig. 11(b) is a cross-sectional view in a direction perpendicular to the axial direction of the press-formed product 1 shown in Fig. 11(a). The reinforcing part 5 forms a ridge portion 27 so as to cover both punch shoulder R parts 1c (see Fig. 12(b)) in the main body part 3, is arranged across both vertical wall parts 1b, and is joined to the main body part 3 by spot welds 6. Note that in Fig. 11, the R shape of the punch shoulder R parts 1c is omitted for simplicity. Figure 12 is an enlarged view of a portion of the blank corresponding to the punch shoulder R portion before press forming (Figure 12(a)), and an enlarged view of the punch shoulder R portion 1c extending from the top plate portion 1a to the vertical wall portion 1b after press forming (Figure 12(b)). The thickness of the main body blank 7 which becomes the main body part 3 is t1, and the thickness of the reinforcing blank 9 which becomes the reinforcing part 5 is t2. In this specification, when the term "punch shoulder R portion 1c" is used, it generally refers to the portion of the press-molded product 1 formed by the punch shoulder R portion 11c of the die 11, and when referring to the punch shoulder R portion of the die, it is written as "punch shoulder R portion 11c of the die 11."

[0014] When two overlapping flat blanks are press-formed simultaneously without being joined, the cross-sectional line length of the main blank 7 located on the outside at the punch shoulder R portion 1c (between AB) becomes longer, and if the positions of the two overlapping blanks in the top plate portion 1a are made the same, the portions S1 and S2 corresponding to the vertical walls of the overlapping blanks will be misaligned by ΔL (see Figure 12(b)). This ΔL is the difference in cross-sectional line length between the main blank 7 and the reinforcing blank 9 after press forming.

[0015] This ΔL changes due to deformation caused by expansion and contraction of the blank, but if such deformation is not taken into account, it can be calculated geometrically from the blank thickness and die shape. If the angle between the top plate portion 11a and the vertical wall portion 11b at the punch shoulder R portion 11c of the die 11 is θ (radian), the radius of the punch shoulder R portion 11c of the die 11 is R (mm), and the radii of the punch shoulder R portion 1c at the thickness centers of the main body blank 7 and the reinforcing blank 9 are R1 (mm) and R2 (mm), respectively, then the cross-sectional line length at the thickness center of the main body blank 7 at the punch shoulder R portion 1c is L1 (mm), and the cross-sectional line length at the thickness center of the reinforcing blank 9 is L2 (mm), L1 = R1θ, L2 = R2θ (1) This can be expressed as:

[0016] Also, R1 = R + t1 / 2 + t2, R2 = R + t2 / 2 (2) It becomes. Hereinafter, the cross-sectional line length refers to the cross-sectional line length at the center of the plate thickness. Assuming that there is no expansion or contraction of the cross-sectional line length of the main blank 7 and the reinforcing blank 9, the geometric cross-sectional line length difference ΔL between the main blank 7 and the reinforcing blank 9 * can be expressed as follows: ΔL * =L1-L2=(R1-R2)θ=(t1+t2)θ / 2 (3) As can be seen from formula (3), the thicker the plate thickness of the main body blank 7 and the reinforcing blank 9 are, and the larger the angle between the top plate portion 1a and the vertical wall portion 1b is, the smaller the cross-sectional line length difference ΔL * becomes larger.

[0017] In this way, press forming results in a difference in cross-sectional line length between the main body blank 7 and the reinforcing blank 9. This difference in cross-sectional line length causes a misalignment between the thickness centers of the blanks, so it is necessary to minimize the difference in cross-sectional line length between the main body blank 7 and the reinforcing blank 9 after press forming. In this regard, if the main body blank 7 and the reinforcing blank 9 can be joined while the cross-sectional line length in the target shape of each is ensured, no misalignment will occur at the joint between the main body blank 7 and the reinforcing blank 9 during press forming. As a result of extensive research, the inventors have found that the difference in cross-sectional line length when forming into a target shape can be eliminated by preforming the main body blank 7, which is located on the outside of the bend in the punch shoulder R portion 1c and has a long cross-sectional line length, so that the cross-sectional line length is long before the main body blank 7 and the reinforcing blank 9 are joined. The present invention is based on this finding and specifically has the following configuration.

[0018] (1) A method for manufacturing a press-formed product according to the present invention is a method for manufacturing a press-formed product having a target shape having a U-shaped cross-sectional shape or a hat-shaped cross-sectional shape by stacking and press-forming a plurality of blanks made of a metal plate, A first forming step of forming a preformed blank by imparting a convex shape extending in a ridge line direction of the bend to a blank to be placed on the outer side of the bend in the bent portion in the press forming; a joined blank preparation process for preparing a joined blank by joining a blank to be disposed on the inside of a bend in a bent portion in the press forming process to a surface of the preformed blank opposite to a surface on which a convex shape is formed; and a second forming process in which the joined blank is placed in a die so that the convex shape of the joined blank is on the outside of the bend and press-formed into a target shape.

[0019] (2) In the above-mentioned (1), the convex shape of the preformed blank is formed at a portion that will become a bending ridge portion in the press-formed product of the target shape.

[0020] (3) In addition, in the above-mentioned (1) or (2), the convex shape in the preformed blank is formed so as to be parallel to a bending ridge portion in the press-formed product of the target shape.

[0021] (4) In the above-mentioned (1) to (3), the convex shape of the preformed blank is shorter than a bend ridge of the press-formed product having the target shape.

[0022] (5) Furthermore, in the above-described (1) to (4), the bending angle between the top plate portion and the vertical wall portion at the bending ridge portion in the target shape is θ, the sheet thickness of the preformed blank is t1, and the sheet thickness of the blank to be joined to the preformed blank is t2, and the cross-sectional line length difference ΔL between the length of the sheet thickness center obtained by connecting the start point and end point of the convexity in a cross section of the convex shape in the preformed blank with a straight line and the length of the sheet thickness center obtained by connecting the start point and end point of the convexity with a curved line along the convexity satisfies the following formula. 0.3(t1+t2)θ≦ΔL≦0.7(t1+t2)θ Effect of the Invention

[0023] According to the present invention, it is possible to suppress breakage of joints, which is an issue with patchwork produced by cold pressing, and to stably and efficiently produce press-formed products. [Brief description of the drawings]

[0024] [Figure 1] 3A to 3C are explanatory diagrams of each step of the manufacturing method of the press-molded product according to the embodiment. [Diagram 2] FIG. 2 is an explanatory diagram of a preformed blank formed in a first forming step in the embodiment. [Diagram 3] FIG. 1 is an explanatory diagram for explaining the arrangement of convex shapes in a preformed blank (part 1). [Figure 4] FIG. 2 is an explanatory diagram for explaining the arrangement of convex shapes in a preformed blank (part 2). [Diagram 5] FIG. 11 is an explanatory diagram (part 3) for explaining the arrangement of convex shapes in a preformed blank. [Figure 6] 1 is an explanatory diagram of a difference in cross-sectional line length before and after forming a convex shape formed in a preformed blank. FIG. [Figure 7] FIG. 13 is an explanatory diagram of parameters for changing the shape of a convex shape formed in a preformed blank. [Figure 8] 10A to 10C are explanatory diagrams of a joined blank produced in a joined blank producing step of the embodiment. [Figure 9] FIG. 4 is an explanatory diagram of another embodiment of a press-molded product produced by the present invention. [Figure 10]FIG. 2 is an explanatory diagram of a press-molded product produced in the examples. [Figure 11] FIG. 1 is an explanatory diagram for explaining the problem to be solved by the present invention (part 1). [Figure 12] FIG. 2 is an explanatory diagram for explaining the problem to be solved by the present invention (part 2). [Figure 13] 11 is an explanatory diagram (part 2) of another form of a joined blank produced in the joined blank producing step of the embodiment. FIG. [Figure 14] 11 is an explanatory diagram (part 3) of another form of a joined blank produced in the joined blank producing step of the embodiment. FIG. [Figure 15] FIG. 13 is a diagram showing a reinforcing part applied to a center pillar. [Figure 16] FIG. 13 is a diagram showing a reinforcing part applied to a front pillar. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The manufacturing method for a press-formed product in this embodiment is a manufacturing method for a press-formed product in which multiple blanks made of metal plate are stacked and press-formed to produce a press-formed product 1 (see Figure 1(d)) of a target shape having a U-shaped or hat-shaped cross-sectional shape, and as shown in Figure 1, the manufacturing method for a press-formed product includes a first forming process (see Figure 1(a)), a joining blank creation process (see Figure 1(b)), and a second forming process (see Figure 1(c)). The press-molded product 1 of this embodiment, like that shown in FIG. 11, has a reinforcing part 5 having a U-shaped cross-section joined to the inside of a main body part 3 having a hat-shaped cross-section (see FIG. 1(d)). In addition, in FIG. 1, the same parts as those in FIG. 11 and FIG. 12 are denoted by the same reference numerals. Each step will be described in detail below.

[0026] <1st molding process> The first forming step is a step of forming a preformed blank 15 by imparting a convex shape 13 extending in the direction of a ridge line 27 of the bend to a main body blank 7 that is to be placed on the outer side of the bend in the bent portion during press forming. 1(a), the mold 11 used in the first molding step is composed of a convex mold 19 having a convex streak portion 17 and a concave mold 23 having a concave streak portion 21. The main body blank 7 is set between the convex mold 19 and the concave mold 23, and the convex mold 19 or the concave mold 23 is moved relatively to sandwich the main body blank 7 therebetween, thereby molding. It does not matter whether the convex die 19 and the concave die 23 are arranged above or below each other, and either one may be arranged above or below. FIG. 2 shows an example of a preformed blank 15 produced in this process.

[0027] The portion of the main body blank 7 to which the convex shape 13 is given in the first forming step is preferably a portion corresponding to the punch shoulder R portion 1c in the target shape of the press-formed product 1. The reasons are as follows: During press forming, the material at the punch shoulder R portion 1c deforms significantly, so that the convex shape 13 imparted to the area corresponding to the punch shoulder R portion 1c is crushed, and the cross-sectional line length can be increased along the punch shoulder R portion 1c. This makes it possible to easily eliminate the difference in cross-sectional line length between the main body blank 7 and the reinforcing blank 9, and prevents the occurrence of cracks due to misalignment at the joint.

[0028] On the other hand, when the convex shape 13 is imparted to a portion of the main body blank 7 corresponding to a flat portion such as the top plate portion 1a or the vertical wall portion 1b of the press-formed product 1 shown in Figure 3, after the press-formed product 1 is press-formed into the target shape in the second forming process, the convex shape 13 may not be completely flattened and may remain as a bending tendency, resulting in an impairment of the surface precision (flatness of the surface) of the target shape. Therefore, by making the convex shape 13 fall within the range of the punch shoulder R portion 1c of the target shape as shown in Fig. 3, the convex shape 13 can be flattened and the bending tendency can be reduced. In other words, it is advisable to make it within the range indicated by the arrow, which is the punch shoulder R portion 1c of the target shape, as shown by tracing the lines connecting the lines along the center of the plate thickness of the main body part 3 after forming in Fig. 3(b), with the same length as the dashed line connecting the lines of the line connecting the lines of the convex shape 13 of the preformed blank 15 before forming in Fig. 3(a). Also, even if a part of the convex shape 13 overlaps with the punch shoulder R portion 1c as in Fig. 4 or Fig. 5, the convex shape 13 can be flattened and the bending tendency can be reduced. In other words, it is preferable to make it the same length as the dashed line at the plate thickness center connecting the ● and ● of the convex shape 13 of the preformed blank 15 before forming in Fig. 4(a) or Fig. 5(a), and to make it overlap within the range indicated by the arrow, which is the punch shoulder R portion 1c of the target shape, as traced by connecting the ● and ● along the plate thickness center of the main body part 3 after forming in Fig. 4(b) or Fig. 5(b).

[0029] Next, the cross-sectional line length of the convex shape 13 imparted to the body blank 7 in this process will be described. Figure 6 shows the cross-sectional shapes of the main body blank 7 before the convex shape 13 is imparted in this process, and the preformed blank 15 to which the convex shape 13 has been imparted. The cross-sectional line length between A1 and B1 of the main body blank 7 before the convex shape 13 is imparted (the length of the dashed line connecting ● and ●) is L0, and the cross-sectional line length between A2 and B2 of the preformed blank 15 to which the convex shape 13 has been imparted (the length of the dashed line connecting ● and ●) is L. By imparting the convex shape 13, the cross-sectional line length of the preformed blank 15 becomes longer than that of the main body blank 7 before forming (L>L0), and the cross-sectional line length difference ΔL (=L-L0) before and after imparting the convex shape 13 can be absorbed by press forming by bending the punch shoulder R portion 1c in the second forming process.

[0030] In order to prevent a misalignment from occurring at the joint between the main blank 7 and the reinforcing blank 9 during press forming, the difference in cross-sectional line length ΔL before and after the convex shape 13 is given must be ΔL as shown in the following formula (3) described above. * (ΔL = ΔL * ) can be done. ΔL * =L1-L2=(R1-R2)θ=(t1+t2)θ / 2 (3)

[0031] However, ΔL shown in equation (3) * does not take into account deformation due to expansion and contraction of the blank. Since the blank deforms in the in-plane direction when an external force is applied, there is an optimal range for the cross-sectional line length difference ΔL at which no cracks occur at the joint during press forming. The inventors have considered the preferable range of the cross-sectional line length difference ΔL and have found that ΔL is ΔL shown in formula (3). * It was found that the range of ±40% of the value of (1), i.e., 0.6 to 1.4 times, is sufficient. Therefore, the cross-sectional line length difference ΔL is within the range shown in the following formula (4). 0.3(t1+t2)θ≦ΔL≦0.7(t1+t2)θ···(4)

[0032] Therefore, it is advisable to design and manufacture a preforming die that gives a convex shape 13 that has a cross-sectional line length difference ΔL within this preferable range, and then perform the first forming step. The cross-sectional line length of the convex shape 13 can be adjusted by changing the height h or width w between the center of the plate thickness of the convex shape 13 shown in FIG.

[0033] The direction in which the convex shape 13 extends is preferably parallel to the bending ridgeline. Even if a tensile load is generated in a direction perpendicular to the bending ridgeline during bending, the convex shape 13 allows the load to be bent and stretched, preventing misalignment of the joint. As an example of the length in the ridge direction of the convex shape 13, it may be the entire length of the bent ridge portion 27, i.e., the entire length of the preformed blank 15, as shown in Fig. 8, or it may be the case that the convex shape 13 extends over the entire length of the reinforcing blank 9 but not the entire length of the preformed blank 15, as shown in Fig. 13. Also, it may not extend over the entire length of both the preformed blank 15 and the reinforcing blank 9, as shown in Fig. 14.

[0034] An example of application of the present invention to a vehicle body frame part will now be described. Fig. 15 shows an example of the arrangement of the main body part 3 and the reinforcing part 5 when the present invention is applied when the main body part 3 is a center pillar, and Fig. 16 shows an example of the arrangement of the main body part 3 and the reinforcing part 5 when the main body part 3 is a front pillar. Generally, from the viewpoint of weight reduction, the reinforcing parts 5 arranged in a patchwork manner are often short enough to be a part of the main body part 3 in the longitudinal direction. The convex shape 13 given to the main body blank 7 only needs to be near the joint with the reinforcing part 5 to prevent the joint from shifting, and the convex shape 13 is not necessarily required at the ridge line portion 27 where the reinforcing part 5 does not exist. From the above, it is preferable that the convex shape 13 given to the main body blank 7 is shorter than the bent ridge line portion 27 of the main body part 3 as shown in Figs. 13 and 14.

[0035] <Joining blank production process> The joined blank creation process is a process of creating a joined blank 25 by joining a reinforcing blank 9, which will be placed on the inside of the bend in the bending section during press molding, to the side of the preformed blank 15 opposite the side on which the convex shape 13 is formed, as shown in Figures 1(b) and 8. The joining here can be any method for joining blanks, which are metal plates, such as resistance spot welding, arc welding, laser welding, seam welding, or mechanical joining.

[0036] <Second forming process> The second forming step is a step of placing the joined blank 25 in the die 11 so that the convex shape 13 is on the outside of the bend, and press-forming it into a target shape, as shown in FIG. 1(c). In this process, as shown in Figures 3 to 5, the convex shape 13 is crushed and absorbed during the forming process of the punch shoulder R portion 1c, and the portion of the preformed blank 15 where the convex shape 13 was formed abuts against the reinforcing blank 9. Therefore, there is no difference in cross-sectional line length at the portion of the preformed blank 15 corresponding to the punch shoulder R portion 1c before and after forming, and no misalignment occurs between the preformed blank 15 and the reinforcing blank 9 at the joined vertical wall portion. The molding method in the second molding step may be foam molding or draw molding. In addition, the second forming step may involve performing multiple press forming steps to form the target shape.

[0037] As described above, according to the present invention, it is possible to suppress breakage of joints, which is a problem in patchwork produced by cold pressing, and to stably and efficiently produce the press-formed product 1.

[0038] The present invention can be suitably applied to the press forming of crash-resistant parts made of ultra-high strength materials, such as front pillars, center pillars, and floor cloths. Furthermore, the press-molded product 1 to which the present invention can be applied may have a structure in which a reinforcing part 5 is arranged inside a main body part 3 as shown in Figures 11 and 1(d), or a structure in which a reinforcing part 5 is arranged outside a main body part 3 as shown in Figure 9. Moreover, the blank to be formed into the press-formed product 1 is not limited to a steel plate, but may be, for example, a metal plate such as an aluminum alloy plate, a magnesium alloy plate, a titanium alloy plate, etc. Furthermore, there is no limitation regarding the strength of the blank. EXAMPLES

[0039] The effects of the method of the present invention were examined by carrying out specific press molding experiments, and an example of the experiment will be described below. 10, the shape of the press-formed product 1, which is the target shape, is composed of a main body part 3 having a hat-shaped cross-sectional shape and a reinforcing part 5 having a U-shaped cross-sectional shape, and the reinforcing part 5 having the U-shaped cross-sectional shape is disposed inside the main body part 3 having the hat-shaped cross-sectional shape to form a ridge line portion 27. The reinforcing part 5 having the U-shaped cross-sectional shape is disposed across both vertical wall portions 1b so as to cover both punch shoulder R portions 1c of the main body part 3.

[0040] The main body blank 7 formed into the main body part 3 is a 590 MPa class steel plate with a thickness of 1.0 mm, and the reinforcing blank 9 formed into the reinforcing part 5 is a 1470 MPa class steel plate with a thickness of 1.4 mm. The angle θ between the top plate part 1a and the vertical wall part 1b at the punch shoulder R part 1c of the press-formed product 1 is 80° (approximately 1.39 radians), and the bending radius R of the punch shoulder R part 1c is 7 mm. The main body part 3 and the reinforcing part 5 were joined at their respective vertical wall parts 1b by spot welds 6 that were multiple-point joined in the longitudinal direction of the parts with a center-to-center distance of 40 mm (see FIG. 10(c)).

[0041] The manufacturing process of the press-formed product 1 of the present invention is as shown in Fig. 1 described in the above embodiment. That is, in the first forming step, a convex shape 13 is given to a main body blank 7, and then in the joining blank preparation step, a preformed blank 15, which has been given the convex shape 13 and is placed on the outside (the side opposite to the surface where the blanks are overlapped), is joined to a flat reinforcing blank 9 by multiple spot welds 6 to prepare a joining blank 25 (see Fig. 8), which is then formed into a target shape by form forming in the second forming step.

[0042] Regarding the convex shape 13 formed in the first forming process, when forming the press-formed product 1 into the target shape, the geometrically optimal value ΔL of the cross-sectional line length difference ΔL that can avoid cracks at the joint is * is calculated from the equation (3) using the plate thickness of the main blank 7, the plate thickness of the reinforcing blank 9, and the bending angle of the top plate portion 1a and the vertical wall portion 1b at the punch shoulder R portion 1c of the press-formed product 1. * =1.67mm.

[0043] In this example, in the first forming step, the height and width of the thickness center of the convex shape 13 imparted to the main body blank 7 were changed to create six levels of preformed blanks 15 with different cross-sectional line lengths. Then, the joining blank creation step and the second forming step were carried out, and the presence or absence of cracks in the spot welds 6 under each condition was evaluated. As a conventional example, the first forming step was omitted, and in the joined blank preparation step, flat blanks were stacked and joined to prepare a joined blank, and press forming was performed in the second forming step.

[0044] Table 1 shows the height h and width w (FIG. 7) of the thickness center of the convex shape 13 imparted to the main body blank 7 under each condition of the conventional example and the example of the present invention, the cross-sectional line length difference ΔL of the thickness center of the main body blank 7 before and after the convex shape 13 is imparted, and the geometric cross-sectional line length difference ΔL at which no deviation occurs between the thickness center of the main body blank 7 and the thickness center of the reinforcing blank 9 in the vertical wall portion joined in the second forming process. * The error with ((ΔL-ΔL * ) / ΔL * ) and the results of whether or not cracks occurred in the joints of the press-molded product 1 are shown.

[0045] [Table 1]

[0046] In the conventional example, because the main body blank 7 was not preformed, a misalignment (approximately 1.67 mm) occurred between the main body blank 7 and the reinforcing blank 9 in the second forming process, causing cracks in all of the multi-point joints. In the present invention example 1, the main body blank 7 was preformed, but the cross-sectional line length difference after press forming was ΔL = 0.7 mm, which is the optimal value without deviation ΔL * Because it was 58% shorter than the standard, the difference in cross-sectional line length during press molding could not be fully absorbed, and cracks occurred in some (20%) of the multi-point joints. On the other hand, in Examples 2 to 5 of the present invention, ΔL * The error was within 40%, and no cracks occurred at the joints of the press-molded product 1. In addition, in Example 6 of the present invention, the cross-sectional line length difference after press molding ΔL = 2.5 mm, which is the optimal value without deviation ΔL * Since the difference in cross-sectional line length was 50% longer than the required length, the cross-sectional line length of the main body blank 7 was left over in the second forming process, resulting in a shift in the opposite direction to that of the conventional example and invention example 1, and as a result, a crack occurred in part (10%) of the joint.

[0047] From the above, it has been found that the present invention can suppress breakage of joints, which is a problem in patchwork produced by cold pressing, and can produce the press-formed product 1 stably and efficiently. [Explanation of symbols]

[0048] 1 Press-molded products 1a Top plate 1b Vertical wall section 1c Punch shoulder R part 3 Main body parts 5 Reinforcement parts 6 Spot welds 7 Body Blank 9 Reinforcement Blanks 11 Mold 11a Top plate 11b Vertical wall section 11c Punch shoulder R part 13 Convex shape 15 Preformed Blanks 17 Convex stripe 19 Convex mold 21 Concave section 23 Concave mold 25 Bonded Blanks 27 Ridge

Claims

1. A method for manufacturing a press-molded product, which produces a press-molded product having a target shape having a U-shaped or hat-shaped cross-sectional shape, in which a reinforcing part made of a steel plate is attached to a part of a main body part made of a steel plate, comprising: a first forming step of forming a preformed blank in which a convex shape extending in a ridge direction of the bend is imparted to a portion of a main body blank that is to be the main body component and that is to be disposed on an outer side of the bend in the bent portion in the press forming, and that is to be a bend ridge portion; a joined blank preparation process in which a reinforcing blank that is to be the reinforcing part and that is disposed on the inside of the bend in the bent portion in the press forming is joined to a surface of the preformed blank opposite to a surface on which a convex shape is formed, thereby preparing a joined blank; A second forming process in which the joined blank is placed in a mold so that the convex shape of the joined blank is on the outside of the bend, and press-formed into a target shape by form forming. The convex shape of the preformed blank is shorter than a bending ridge portion of a press-formed product having the target shape; and A manufacturing method for a press-formed product, characterized in that the bending angle between the top plate portion and the vertical wall portion at the bending ridge portion in the target shape is θ, the plate thickness of the preformed blank is t1, and the plate thickness of the reinforcing blank to be joined to the preformed blank is t2, and the cross-sectional line length difference ΔL between the length of the plate thickness center connecting the start point and end point of the convexity in a cross section of the convex shape in the preformed blank with a straight line and the length of the plate thickness center connecting with a curve along the convexity satisfies the following formula. 0.33 (t 1 + t 2 )θ≦ΔL≦0.69 (t 1 +t 2 )θ

2. The method for manufacturing a press-formed product according to claim 1, characterized in that the convex shape in the preformed blank is formed so as to be parallel to a bending ridge portion in the press-formed product of the target shape.

Citation Information

Patent Citations

  • Method for pressing spot welded part

    JP1995232223A

  • Laminated hot press member and method of producing the same

    JP2013184221A

  • Method for manufacturing vehicle structure member

    JP2020121336A

  • Structural member for vehicle

    JP2022129059A

  • Overlapped blank and method for molding the same

    JP2023077210A