Moisture-curable composition
The moisture-curable composition with polyoxyalkylene polymer and surface-treated calcium carbonate addresses low toughness and separation issues, ensuring enhanced adhesiveness and storage stability with optimized molecular weights and distributions.
Patent Information
- Application Number
- JP2020217393
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-25
- Filing Date
- 2020-12-25
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-12-25
AI Technical Summary
Existing room temperature curable adhesives exhibit low toughness and adhesiveness, and organic and inorganic components separate during storage.
A moisture-curable composition containing a polyoxyalkylene polymer with hydrolyzable silyl groups and surface-treated calcium carbonate, optimized with specific molecular weights and distributions, to enhance toughness and prevent component separation.
The composition achieves improved toughness, adhesiveness, and storage stability by suppressing component separation, maintaining low viscosity and excellent coating properties across varying temperatures.
Smart Images

Figure 0007590760000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a moisture-curable composition. [Background technology]
[0002] Modified silicone-based curable compositions containing a polyoxyalkylene polymer having a hydrolyzable silyl group form a crosslinked structure by condensation polymerization while the hydrolyzable silyl group is hydrolyzed by moisture in the air as necessary, and are safe as they do not generate toxic substances during curing and have elasticity and toughness after curing. For these reasons, modified silicone-based curable compositions are often used as sealants, adhesives, paints, and the like.
[0003] The adhesive is designed to have a low viscosity in order to improve the handling during application. Specifically, Patent Document 1 describes a composition comprising 100 parts by mass of a polyoxyalkylene polymer having a hydrolyzable silyl group, a number average molecular weight of 15,000 to 50,000, and a molecular weight distribution (weight average molecular weight (Mw) / number average molecular weight (Mn)) of 1.3 or less, and a tertiary ethyl ketone (TTA) copolymer having a BET specific surface area of 19 m. 2 The adhesive disclosed is a room-temperature curable adhesive containing 30 to 300 parts by mass of precipitated calcium carbonate having a viscosity of 1000 g / g or more and 1 to 10 parts by mass of an aminosilane coupling agent. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-210839 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the above room temperature curable adhesive has a problem in that the toughness of the cured product is low and the adhesiveness is low. Furthermore, the above room temperature curable adhesive has another problem in that the organic component and the inorganic component separate during storage.
[0006] The present invention provides a moisture-curable composition which has low viscosity and excellent coatability, and when cured, has excellent toughness. Furthermore, separation of the organic component and the inorganic component during storage is suppressed, and the composition has excellent storage stability. [Means for solving the problem]
[0007] The moisture-curable composition of the present invention contains a polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule, and surface-treated ground calcium carbonate.
[0008] [Polyoxyalkylene polymer having hydrolyzable silyl group in the molecule] The moisture-curable composition contains a polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule (hereinafter, simply referred to as a "polyoxyalkylene polymer"). The main chain of the polyoxyalkylene polymer is preferably a polymer containing a repeating unit represented by general formula (1). -(R 1 -O) n - (1) (In the formula, R 1 represents an alkylene group having 1 to 14 carbon atoms, and n is the number of repeating units and is a positive integer.
[0009] The main chain of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units.
[0010] Examples of the main chain skeleton of the polyoxyalkylene polymer include polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymer, and polyoxypropylene-polyoxybutylene copolymer, with polyoxypropylene being preferred.
[0011] The hydrolyzable silyl group refers to a group that undergoes a condensation reaction in the presence of moisture or a crosslinking agent, and if necessary, using a catalyst, such as a silicon-containing group or a silanol group having a hydrolyzable group bonded to a silicon atom. Note that a silanol group refers to a hydroxy group (≡Si-OH) that is directly bonded to a silicon atom.
[0012] Examples of the hydrolyzable silyl group include monoalkoxysilyl groups such as a methoxysilyl group, an ethoxysilyl group, a dimethylmethoxysilyl group, and a dimethylethoxysilyl group; dialkoxysilyl groups such as a dimethoxysilyl group, a methyldimethoxysilyl group, and a methyldiethoxysilyl group; trialkoxysilyl groups such as a trimethoxysilyl group and a triethoxysilyl group; and halogenated silyl groups to which a halogen is bonded, such as a trichlorosilyl group. Of these, a dialkoxysilyl group is preferred, and a dimethoxysilyl group is more preferred.
[0013] The polyoxyalkylene polymer (A) preferably does not contain a urethane bond. Since the polyoxyalkylene polymer (A) does not contain a urethane bond, the moisture-curable composition is prevented from increasing in viscosity even in winter, and has excellent coatability.
[0014] The polyoxyalkylene polymer (A) preferably has a hydrolyzable silyl group at the molecular end, and more preferably has hydrolyzable silyl groups at both molecular ends, since this suppresses an increase in viscosity of the moisture-curable composition even in winter and provides excellent coatability.
[0015] The polyoxyalkylene polymer (A) preferably has a hydrolyzable silyl group at the molecular terminal without a urethane bond, and more preferably has a hydrolyzable silyl group at both molecular terminals without a urethane bond, in order to suppress an increase in viscosity of the moisture-curable composition even in winter and to have excellent coatability.
[0016] The polyoxyalkylene polymer (A) having a hydrolyzable silyl group at the end of the polyoxyalkylene chain without a urethane bond can be produced, for example, by reacting a polyoxyalkylene polymer having a functional group such as a hydroxyl group at the end with an organic compound having an active group and an unsaturated group that are reactive with the functional group, and then allowing a hydrosilane having a hydrolyzable group to act on the resulting reaction product to carry out hydrosilylation.
[0017] The polyoxyalkylene polymer (A) is a polyoxyalkylene polymer (A1) having a hydrolyzable silyl group in the molecule, a molecular weight distribution of less than 1.4, and a number average molecular weight of 8,000 or more and less than 19,000; It is a mixture with a polyoxyalkylene polymer (A2) having a hydrolyzable silyl group in the molecule and a number average molecular weight of 19,000 or more and 50,000 or less.
[0018] The number average molecular weight of the polyoxyalkylene polymer (A1) is 8000 or more, preferably 9000 or more, more preferably 10000 or more, and more preferably 11000 or more. The number average molecular weight of the polyoxyalkylene polymer (A1) is less than 19000, preferably 18700 or less, more preferably 18500 or less, and more preferably 16000 or less. When the number average molecular weight of the polyoxyalkylene polymer (A1) is 8000 or more, the elasticity of the cured product of the moisture-curable composition is improved, and separation of the organic component and the inorganic component is suppressed, thereby improving storage stability. When the number average molecular weight of the polyoxyalkylene polymer (A1) is less than 19000, the coatability of the moisture-curable composition is improved.
[0019] The number average molecular weight of the polyoxyalkylene polymer (A2) is 19000 or more, preferably 19500 or more, more preferably 20000 or more, more preferably 20500 or more, and more preferably 21000 or more. The number average molecular weight of the polyoxyalkylene polymer (A2) is 50000 or less, preferably 40000 or less, more preferably 35000 or less, more preferably 30000 or less, and more preferably 25000 or less. When the number average molecular weight of the polyoxyalkylene polymer (A2) is 19000 or more, the toughness of the cured product of the moisture-curable composition is improved, and separation of the organic component and the inorganic component is suppressed, thereby improving storage stability. When the number average molecular weight of the polyoxyalkylene polymer (A2) is 50000 or less, the coatability of the moisture-curable composition is improved.
[0020] In this way, since the polyoxyalkylene polymer (A) is a mixture of two kinds of polyoxyalkylene polymers (A1) and (A2) having different number average molecular weights, the crosslinking density is appropriately varied in the cured product of the moisture-curable composition, thereby imparting excellent elasticity and toughness to the cured product of the moisture-curable composition. The polyoxyalkylene polymer (A1) reduces the viscosity of the moisture-curable composition and improves the coatability of the moisture-curable composition, while the polyoxyalkylene polymer (A2) suppresses separation of the organic component and the inorganic component, thereby improving the storage stability of the moisture-curable composition.
[0021] The molecular weight distribution of the polyoxyalkylene polymer (A1) is less than 1.4, preferably less than 1.3, more preferably less than 1.2, and more preferably less than 1.15. When the molecular weight distribution of the polyoxyalkylene polymer (A1) is less than 1.4, the viscosity of the moisture-curable composition is reduced, and the moisture-curable composition has excellent coatability regardless of the use environment, and the moisture-curable composition has excellent toughness as a cured product.
[0022] The molecular weight distribution of the polyoxyalkylene polymer (A2) is preferably less than 1.4, more preferably less than 1.3, more preferably less than 1.2, and more preferably less than 1.15. When the molecular weight distribution of the polyoxyalkylene polymer (A2) is less than 1.4, the viscosity of the moisture-curable composition is reduced, and the moisture-curable composition has excellent coatability regardless of the use environment, and the moisture-curable composition has excellent toughness in its cured product.
[0023] In the present invention, the number average molecular weight and weight average molecular weight of the polyoxyalkylene polymer having a hydrolyzable silyl group are values measured by GPC (gel permeation chromatography) and converted into polystyrene. Specifically, 6 to 7 mg of the polyoxyalkylene polymer having a hydrolyzable silyl group is collected, the collected polyoxyalkylene polymer is fed to a test tube, and then an o-DCB (ortho-dichlorobenzene) solution containing 0.05% by mass of BHT (dibutylhydroxytoluene) is added to the test tube to dilute the polyoxyalkylene polymer to a concentration of 1 mg / mL to prepare a diluted solution.
[0024] The dilution solution is shaken at 145° C. and 25 rpm for 1 hour using a dissolution filter to dissolve the polyoxyalkylene polymer in the o-DCB solution containing BHT to obtain a measurement sample. The number average molecular weight and weight average molecular weight of the polyoxyalkylene polymer can be measured by the GPC method using this measurement sample.
[0025] The number average molecular weight and weight average molecular weight of the polyoxyalkylene polymer having a hydrolyzable silyl group can be measured, for example, using the following measuring device and under the following measuring conditions. Measuring device: TOSOH product name "HLC-8121GPC / HT" Measurement conditions Column: TSKgelGMHHR-H(20)HT x 3 TSKguardcolumn-HHR(30)HT x 1 Mobile phase: o-DCB 1.0mL / min Sample concentration: 1mg / mL Detector: Bryce type refractometer Standard material: Polystyrene (TOSOH, molecular weight: 500-8420000) Elution conditions: 145℃ SEC temperature: 145℃
[0026] In the polyoxyalkylene polymer (A), the content of the polyoxyalkylene polymer (A1) is preferably 50% by mass or more, more preferably 55% by mass or more, and more preferably 60% by mass or more. In the polyoxyalkylene polymer (A), the content of the polyoxyalkylene polymer (A1) is preferably 98% by mass or less, more preferably 97% by mass or less, and more preferably 95% by mass or less. When the content of the polyoxyalkylene polymer (A1) is 50% by mass or more, the coatability of the cured product of the moisture-curable composition is improved. When the content of the polyoxyalkylene polymer (A1) is 98% by mass or less, the toughness of the cured product of the moisture-curable composition is improved.
[0027] In the polyoxyalkylene polymer (A), the content of the polyoxyalkylene polymer (A2) is preferably 2% by mass or more, more preferably 3% by mass or more, and more preferably 5% by mass or more. In the polyoxyalkylene polymer (A), the content of the polyoxyalkylene polymer (A2) is preferably 50% by mass or less, more preferably 45% by mass or less, and more preferably 40% by mass or less. When the content of the polyoxyalkylene polymer (A2) is 2% by mass or more, the toughness and elasticity of the cured product of the moisture-curable composition are improved. When the content of the polyoxyalkylene polymer (A2) is 50% by mass or less, the coatability of the cured product of the moisture-curable composition is improved.
[0028] The ratio of the content of the polyoxyalkylene polymer (A1) to the content of the polyoxyalkylene polymer (A2) [mass of the polyoxyalkylene polymer (A1) / mass of the polyoxyalkylene polymer (A2)] is preferably 1 or more, more preferably 1.5 or more, and more preferably 2 or more. The ratio of the content of the polyoxyalkylene polymer (A1) to the content of the polyoxyalkylene polymer (A2) [mass of the polyoxyalkylene polymer (A1) / mass of the polyoxyalkylene polymer (A2)] is preferably 50 or less, more preferably 35 or less, more preferably 25 or less, and more preferably 20 or less. When the ratio of the content of the polyoxyalkylene polymer (A1) to the content of the polyoxyalkylene polymer (A2) [mass of the polyoxyalkylene polymer (A1) / mass of the polyoxyalkylene polymer (A2)] is 1 or more, the coatability of the moisture-curable composition is improved. When the ratio of the content of the polyoxyalkylene polymer (A1) to the content of the polyoxyalkylene polymer (A2) [mass of the polyoxyalkylene polymer (A1) / mass of the polyoxyalkylene polymer (A2)] is 50 or less, the elasticity and toughness of the cured product of the moisture-curable composition are improved.
[0029] [Calcium carbonate] The moisture-curable composition contains surface-treated heavy calcium carbonate. The moisture-curable composition contains a mixture of polyoxyalkylene polymers (A1) and (A2) as the polyoxyalkylene polymer (A), and also contains surface-treated heavy calcium carbonate. Therefore, the moisture-curable composition has excellent storage stability since separation of the polyoxyalkylene polymer (A) and the heavy calcium carbonate during storage is suppressed, and the cured product has excellent elasticity and toughness.
[0030] The surface treatment of the heavy calcium carbonate is not particularly limited, but is preferably a treatment with a fatty acid, a fatty acid ester, or a fatty acid metal salt, and more preferably a treatment with a fatty acid. By containing the surface-treated heavy calcium carbonate, the storage stability of the moisture-curable composition is improved.
[0031] Examples of fatty acids include caproic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, alaic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, obscylic acid, caroleic acid, undecylenic acid, Linderic acid, tsuzuic acid, physeteric acid, moristoleic acid, palmitoleic acid, petroselinic acid, oleic acid, elaidic acid, asclevic acid, vaccenic acid, gadoleic acid, gondoic acid, cetoleic acid, erucic acid, brassidic acid, selacholeic acid, xymenic acid, lumecic acid, sorbic acid, and linoleic acid. Of these, lauric acid, myristic acid, palmitic acid, stearic acid, and oleic acid are preferred.
[0032] Examples of fatty acid esters include stearyl stearate, lauryl stearate, stearyl palmitate, and lauryl palmitate.
[0033] Examples of the fatty acid metal salts include the sodium and potassium salts of the above-mentioned fatty acids, and preferred are the sodium salt of lauric acid, the sodium salt of myristic acid, the sodium salt of palmitic acid, the sodium salt of stearic acid, and the sodium salt of oleic acid.
[0034] The average particle size of the primary particles of the surface-treated heavy calcium carbonate is preferably 10 μm or less, more preferably 6 μm or less, more preferably 5 μm or less, more preferably 3 μm or less, and more preferably 2 μm or less. The average particle size of the primary particles of the surface-treated heavy calcium carbonate is more preferably 0.05 μm or more, more preferably 0.1 μm or more, more preferably 0.5 μm or more, and more preferably 0.8 μm or more. When the average particle size of the primary particles is 10 μm or less, the toughness of the cured product of the moisture-curable composition is improved. When the average particle size of the primary particles is 0.05 μm or more, the viscosity of the moisture-curable composition is prevented from increasing, and the coatability can be improved.
[0035] The average particle size of the primary particles of the surface-treated heavy calcium carbonate refers to a value calculated based on the following formula using the specific surface area per gram of heavy calcium carbonate before the surface treatment. The specific surface area per gram of heavy calcium carbonate before the surface treatment can be measured using, for example, a powder specific surface area measuring device commercially available from Shimadzu Corporation under the product name "SS-100 Model." Average particle size of primary particles of surface-treated ground calcium carbonate (μm) =6×10000 / (specific gravity×specific surface area)
[0036] In the moisture-curable composition, the content of the surface-treated heavy calcium carbonate is preferably 50 parts by mass or more, more preferably 80 parts by mass or more, more preferably 100 parts by mass or more, and more preferably 130 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. In the moisture-curable composition, the content of the surface-treated heavy calcium carbonate is preferably 400 parts by mass or less, more preferably 350 parts by mass or less, more preferably 300 parts by mass or less, and more preferably 250 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When the content of the surface-treated heavy calcium carbonate is 50 parts by mass or more, the toughness of the cured product of the moisture-curable composition is improved. When the content of the surface-treated heavy calcium carbonate is 400 parts by mass or less, the coatability of the moisture-curable composition is improved.
[0037] The moisture-curable composition preferably contains surface-treated precipitated calcium carbonate. When the moisture-curable composition contains precipitated calcium carbonate, the viscosity of the moisture-curable composition is suppressed to improve the coatability, and separation of the organic component and the inorganic component during storage is suppressed to impart excellent storage stability to the moisture-curable composition. Furthermore, excellent elasticity and toughness can be imparted to the cured product of the moisture-curable composition.
[0038] The surface treatment of the precipitated calcium carbonate is not particularly limited, but is preferably a treatment with a fatty acid, a fatty acid ester, or a fatty acid metal salt, and more preferably a treatment with a fatty acid. The moisture-curable composition has improved storage stability due to the inclusion of the surface-treated heavy calcium carbonate. Note that the fatty acid, fatty acid ester, and fatty acid metal salt are omitted because they are the same as those used in the surface treatment of heavy calcium carbonate.
[0039] The average particle size of the primary particles of the surface-treated precipitated calcium carbonate is preferably 5 μm or less, more preferably 3 μm or less, and more preferably 2.5 μm or less. The average particle size of the primary particles of the surface-treated precipitated calcium carbonate is more preferably 0.01 μm or more, and more preferably 0.03 μm or more. When the average particle size is 5 μm or less, the moisture-curable composition has high thixotropy and excellent coatability. When the average particle size is 0.01 μm or more, the viscosity of the moisture-curable composition can be suppressed from increasing, and the coatability can be improved. The average particle size of the primary particles of the precipitated calcium carbonate is measured in the same manner as that of the surface-treated heavy calcium carbonate, and therefore the description thereof will be omitted.
[0040] In the moisture-curable composition, the content of the surface-treated precipitated calcium carbonate is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and more preferably 15 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. In the moisture-curable composition, the content of the surface-treated precipitated calcium carbonate is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and more preferably 100 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When the content of the precipitated calcium carbonate is 5 parts by mass or more, the moisture-curable composition can be given excellent thixotropy. When the content of the precipitated calcium carbonate is 200 parts by mass or less, the viscosity of the moisture-curable composition can be suppressed from increasing, and the coatability can be improved.
[0041] In the moisture-curable composition, the ratio of the content of the surface-treated heavy calcium carbonate to the content of the surface-treated precipitated calcium carbonate (mass of the surface-treated heavy calcium carbonate / mass of the surface-treated precipitated calcium carbonate) is preferably 1.5 or more, more preferably 1.6 or more, more preferably 1.8 or more, more preferably 2 or more, more preferably 3 or more, and more preferably 4 or more. In the moisture-curable composition, the ratio of the content of the surface-treated heavy calcium carbonate to the content of the surface-treated precipitated calcium carbonate (mass of the surface-treated heavy calcium carbonate / mass of the surface-treated precipitated calcium carbonate) is more preferably 30 or less, more preferably 28 or less, more preferably 25 or less, more preferably 20 or less, and more preferably 15 or less. When the ratio of the content of the surface-treated heavy calcium carbonate to the content of the surface-treated precipitated calcium carbonate is 1.5 or more, the moisture-curable composition can be imparted with thixotropy, and the coatability is improved. When the ratio of the content of the surface-treated heavy calcium carbonate to the content of the surface-treated precipitated calcium carbonate is 30 or less, the viscosity of the moisture-curable composition can be kept low, the coatability of the moisture-curable composition can be improved, and further, the moisture-curable composition can be easily removed from a container, which is preferable.
[0042] [Silane coupling agents] The moisture-curable composition may further contain a silane coupling agent. By containing a silane coupling agent, the moisture-curable composition has excellent curability and adhesive strength even if it has a low viscosity.
[0043] The silane coupling agent preferably contains an amino group-containing silane coupling agent or an epoxy group-containing silane coupling agent, and more preferably contains an amino group-containing silane coupling agent, since this improves the adhesive strength of the cured product of the moisture-curable composition.
[0044] The silane coupling agent more preferably contains an amino group-containing silane coupling agent and an epoxy group-containing silane coupling agent. When the silane coupling agent contains an amino group-containing silane coupling agent and an epoxy group-containing silane coupling agent, the adhesive strength of the cured product of the moisture-curable composition is improved.
[0045] The amino group-containing silane coupling agent means a compound containing, in one molecule, a silicon atom to which an alkoxy group is bonded and a functional group containing a nitrogen atom. The amino group-containing silane coupling agent is not particularly limited, and examples thereof include 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N,N'-bis-[3-(trimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(triethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(methyldimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(trimethoxysilyl)propyl]hexamethylenediamine, and N,N'-bis-[3-(triethoxysilyl)propyl]hexamethylenediamine, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane is preferred.
[0046] The epoxy group-containing silane coupling agent means a compound that contains a silicon atom with an alkoxy group bonded to it in one molecule and a functional group that contains an epoxy group.The epoxy group-containing silane coupling agent is not particularly limited, and can be, for example, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and is preferably 3-glycidoxypropyltriethoxysilane.
[0047] The content of the silane coupling agent in the moisture-curable composition is preferably 0.1 parts by mass or more, more preferably 2 parts by mass or more, and particularly preferably 3 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) in the molecule. The content of the silane coupling agent in the moisture-curable composition is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and particularly preferably 6 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) in the molecule. When the content of the silane coupling agent is 0.1 parts by mass or more, the adhesive strength of the cured product of the moisture-curable composition is improved. When the content of the silane coupling agent is 10 parts by mass or less, the cured product of the moisture-curable composition is prevented from becoming brittle, and excellent adhesive strength can be imparted to the cured product, and the storage stability of the moisture-curable composition can be improved.
[0048] When an amino group-containing silane coupling agent is contained in the moisture-curable composition, the content of the amino group-containing silane coupling agent in the moisture-curable composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When an amino group-containing silane coupling agent is contained in the moisture-curable composition, the content of the amino group-containing silane coupling agent in the moisture-curable composition is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and particularly preferably 6 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When the content of the amino group-containing silane coupling agent is 0.5 parts by mass or more, the adhesive strength of the cured product of the moisture-curable composition is improved. When the content of the amino group-containing silane coupling agent is 20 parts by mass or less, the moisture-curable composition has excellent curability.
[0049] When an epoxy group-containing silane coupling agent is contained in the moisture-curable composition, the content of the epoxy group-containing silane coupling agent in the moisture-curable composition is preferably 0.3 parts by mass or more, more preferably 0.4 parts by mass or more, more preferably 0.45 parts by mass or more, and particularly preferably 0.5 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When an epoxy group-containing silane coupling agent is contained in the moisture-curable composition, the content of the epoxy group-containing silane coupling agent in the moisture-curable composition is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, more preferably 6 parts by mass or less, and particularly preferably 3 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When the content of the epoxy group-containing silane coupling agent is 0.3 parts by mass or more, the adhesive strength of the cured product of the moisture-curable composition is improved. When the content of the epoxy group-containing silane coupling agent is 20 parts by mass or less, the adhesive strength of the cured product of the moisture-curable composition is improved.
[0050] [Plasticizer] The moisture-curable composition may contain a plasticizer. The plasticizer is not particularly limited, and examples thereof include phthalates such as dibutyl phthalate, di(2-ethylhexyl)phthalate, diisononyl phthalate, diisodecyl phthalate, and butyl benzyl phthalate; non-aromatic dibasic acid esters such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, and isodecyl succinate; aliphatic esters such as butyl oleate and methyl acetyl ricinoleate; esters of polyalkylene glycols such as diethylene glycol dibenzoate, triethylene glycol dibenzoate, and pentaerythritol ester; phosphates such as tricresyl phosphate and tributyl phosphate; trimellitic acid esters; polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, polychloroprene, and the like. Examples of suitable plasticizers include: chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; polyether polyols such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, and polyether polyols such as derivatives in which the hydroxyl groups of polyether polyols are converted to ester groups, ether groups, and the like; epoxy plasticizers such as epoxidized soybean oil and epoxy benzyl stearate; polyester plasticizers obtained from dibasic acids such as sebacic acid, adipic acid, azelaic acid, and phthalic acid and dihydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and dipropylene glycol; and vinyl polymers obtained by polymerizing vinyl monomers such as acrylic plasticizers by various methods. The plasticizers may be used alone or in combination of two or more.
[0051] The content of the plasticizer in the moisture-curable composition is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. The content of the plasticizer in the moisture-curable composition is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When the content of the plasticizer is 20 parts by mass or more, the coatability of the moisture-curable composition is improved. When the content of the plasticizer is 100 parts by mass or less, the toughness of the cured product of the moisture-curable composition is improved.
[0052] [Silanol condensation catalyst] The moisture-curable composition preferably contains a silanol condensation catalyst. The silanol condensation catalyst is a catalyst for promoting a dehydration condensation reaction between silanol groups formed by hydrolysis of a hydrolyzable silyl group contained in a polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. The silanol group means a hydroxyl group (≡Si-OH) directly bonded to a silicon atom.
[0053] The silanol condensation catalyst is not particularly limited, and examples thereof include dibutyltin diacetylacetonate, dibutyltin dilaurate, dibutyltin oxide, dibutyltin diacetate, dibutyltin phthalate, bis(dibutyltin laurate) oxide, dibutyltin bis(acetylacetonate), dibutyltin bis(monoester maleate), tin octoate, dibutyltin octoate, dioctyltin oxide, dibutyltin bis(triethoxysilicate), dioctyltin bis(triethoxysilicate), dioctyltin dilaurate, bis(dibutyltin bistriethoxysilicate) oxide, and dibutyltin bis(triethoxysilicate). Organotin compounds such as tin oxybisethoxysilicate; organotitanium compounds such as tetra-n-butoxy titanate and tetraisopropoxy titanate; cycloamidine compounds such as 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, 6-dibutylamino-1,8-diazabicyclo[5.4.0]undec-7-ene, and 1,5-diazabicyclo[4.3.0]non-5-ene; dibutylamine-2-ethylhexoate. Other acidic and basic catalysts can also be used as silanol condensation catalysts. The silanol condensation catalysts may be used alone or in combination of two or more. As the silanol condensation catalyst, an organotin compound is preferred since it can improve the curing property of the moisture-curable composition.
[0054] The content of the silanol condensation catalyst in the moisture-curable composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. The content of the silanol condensation catalyst in the moisture-curable composition is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When the content of the silanol condensation catalyst is 0.1 parts by mass or more, the curability of the moisture-curable composition is improved. When the content of the silanol condensation catalyst is 10 parts by mass or less, the adhesive strength of the cured product of the moisture-curable composition is improved.
[0055] [Dehydrating agent] The moisture-curable composition may contain a dehydrating agent. The dehydrating agent can suppress the moisture in the air or the like from curing the moisture-curable composition during storage.
[0056] Examples of the dehydrating agent include silane compounds such as vinyltrimethoxysilane, dimethyldimethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, phenyltrimethoxysilane, and diphenyldimethoxysilane; and ester compounds such as methyl orthoformate, ethyl orthoformate, methyl orthoacetate, and ethyl orthoacetate.The dehydrating agent is preferably nivyltrimethoxysilane.The dehydrating agent may be used alone or in combination of two or more.
[0057] The content of the dehydrating agent in the moisture-curable composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and particularly preferably 1.1 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. The content of the dehydrating agent in the moisture-curable composition is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and particularly preferably 5 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. When the content of the dehydrating agent is in the above range, it is possible to reduce the occurrence of an unexpected curing reaction during storage of the moisture-curable composition.
[0058] [Other additives] The moisture-curable composition may contain other additives such as antioxidants, ultraviolet absorbers, light stabilizers, pigments, dyes, and antisettling agents. Among these, antioxidants are preferred. The moisture-curable composition preferably does not contain a solvent.
[0059] Examples of the antioxidant include hindered phenol-based antioxidants, monophenol-based antioxidants, bisphenol-based antioxidants, and polyphenol-based antioxidants, and hindered phenol-based antioxidants are preferred. The content of the antioxidant in the moisture-curable composition is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule. The content of the antioxidant in the moisture-curable composition is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, per 100 parts by mass of the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule.
[0060] The viscosity of the moisture-curable composition at 23°C is preferably 15,000 mPa·s or more, more preferably 20,000 mPa·s or more, and more preferably 30,000 mPa·s or more. The viscosity of the moisture-curable composition at 23°C is preferably 200,000 mPa·s or less, more preferably 150,000 mPa·s or less, and more preferably 130,000 mPa·s or less. The viscosity of the moisture-curable composition at 23°C refers to a value measured using a B-type viscometer in accordance with JIS K6833 at 23°C and a rotation speed of 10 rpm.
[0061] For the moisture-curable composition, the ratio of the viscosity at 10 rpm at 23 ° C. to the viscosity at 1 rpm at 23 ° C. (viscosity at 1 rpm / viscosity at 10 rpm) is preferably 3 or more, preferably 4 or more, more preferably 4.1 or more, and more preferably 4.5 or more. For the moisture-curable composition, the ratio of the viscosity at 10 rpm at 23 ° C. to the viscosity at 1 rpm at 23 ° C. (viscosity at 1 rpm / viscosity at 10 rpm) is preferably 10 or less, more preferably 9 or less, more preferably 8.5 or less, and more preferably 8 or less. When the ratio of the viscosity at 10 rpm at 23 ° C. to the viscosity at 1 rpm at 23 ° C. is within the above range, the moisture-curable composition has high thixotropy despite its low viscosity. Therefore, the moisture-curable composition has better coatability.
[0062] For the moisture-curable composition, the viscosity at 23° C. and 10 rpm and 1 rpm refers to a value measured using a B-type viscometer in accordance with JIS K6833 at 23° C. and a rotation speed of 10 rpm or 1 rpm.
[0063] The moisture-curable composition can be produced by mixing the polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule, the surface-treated heavy calcium carbonate, and other additives as necessary. The mixing is preferably carried out under reduced pressure.
[0064] The moisture-curable composition is preferably used as an adhesive, for example, in the construction of a floor structure. The floor structure is constructed, for example, by adhering and integrating a floor finishing material onto a floor underlayment laid on a floor base via a cured product layer formed by curing the moisture-curable composition. The floor structure includes a floor base, a floor underlayment laid on the floor base, a cured product layer formed by curing the moisture-curable composition formed on the floor underlayment and adhesively integrated with the floor underlayment, and a floor finishing material laid on the cured product layer and adhesively integrated with the cured product layer.
[0065] Examples of components that make up floor finishing materials include wood-based materials such as plywood and medium density fiberboard (MDF), tiles, polyvinyl chloride sheets, and stone materials, and among these, the use of thin, soft materials such as polyvinyl chloride sheets is preferable.
[0066] Examples of materials that make up the floor underlayment include plywood, particle board, wooden joists, gypsum board, slate boards, and concrete boards. Effect of the Invention
[0067] The moisture-curable composition of the present invention has a low viscosity and therefore has excellent coatability in both low temperature winter and high temperature summer environments.
[0068] Despite its low viscosity, the moisture-curable composition is inhibited from separating from the polyoxyalkylene polymer and the surface-treated ground calcium carbonate during storage, and has excellent storage stability.
[0069] The moisture-curable composition has excellent toughness when cured to form a cured product, and when used as an adhesive, it exhibits excellent adhesive properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. EXAMPLES
[0071] The following compounds were used in the preparation of the moisture-curable compositions of the Examples and Comparative Examples.
[0072] [Polyoxyalkylene polymer (A) having hydrolyzable silyl group in the molecule] Polyoxyalkylene polymer having hydrolyzable silyl group in the molecule (A11) (polyoxypropylene polymer having dimethoxysilyl group as hydrolyzable silyl group and having polyoxypropylene as main chain skeleton, no urethane bond, number average molecular weight: 15000, molecular weight distribution: 1.10, Asahi Glass Co., Ltd., product name "Exestar 6250") Polyoxyalkylene polymer having hydrolyzable silyl groups in the molecule (A12) (polyoxypropylene polymer having dimethoxysilyl groups as hydrolyzable silyl groups and having a polyoxypropylene main chain skeleton, no urethane bond, number average molecular weight: 18,000, molecular weight distribution: 1.40, manufactured by Asahi Glass Co., Ltd., product name "Exestar 3430") Polyoxyalkylene polymer having hydrolyzable silyl group in the molecule (A21) (polyoxypropylene polymer having dimethoxysilyl group as hydrolyzable silyl group and having polyoxypropylene as main chain skeleton, no urethane bond, number average molecular weight: 20000, molecular weight distribution: 1.16, Asahi Glass Co., Ltd., product name "Exestar 4530") Polyoxyalkylene polymer having hydrolyzable silyl groups in the molecule (A22) (polyoxypropylene polymer having dimethoxysilyl groups as hydrolyzable silyl groups and having a polyoxypropylene main chain skeleton, no urethane bond, number average molecular weight: 21,000, molecular weight distribution: 1.39, manufactured by Asahi Glass Co., Ltd., product name "Exestar 2420") Polyoxyalkylene polymer having hydrolyzable silyl groups in the molecule (A3) (polyoxypropylene polymer having dimethoxysilyl groups as hydrolyzable silyl groups and having a polyoxypropylene main chain skeleton, no urethane bond, number average molecular weight: 4500, molecular weight distribution: 1.40, Kaneka Corporation product name "SAX015")
[0073] [Calcium carbonate] Surface-treated ground calcium carbonate (average primary particle size: 1.0 μm, surface treatment with stearic acid, manufactured by Nitto Funka Co., Ltd., product name "NCC2310") Heavy calcium carbonate with an untreated surface (average particle size of primary particles: 5 μm, product name "Whiten P-30" manufactured by Toyo Fine Chemical Co., Ltd.) Surface-treated precipitated calcium carbonate (average primary particle size: 0.05 μm, surface treatment with fatty acid, product name "Kalfine 200M" manufactured by Maruo Calcium Co., Ltd.)
[0074] [Silane coupling agents] Amino group-containing silane coupling agent [N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, Shin-Etsu Chemical Co., Ltd. product name "KBM-603"]
[0075] [Silanol condensation catalyst] Dibutyltin bis(triethoxysilicate)
[0076] (Example 1 to 10 , Comparative Example 1~ 8 ) Moisture-curable compositions were prepared by uniformly mixing polyoxyalkylene polymers (A1) and (A2) having hydrolyzable silyl groups in the molecule, calcium carbonate, an amino group-containing silane coupling agent, and a silanol condensation catalyst in the amounts shown in Table 1 under reduced pressure in a sealed stirrer. In Table 1, the polyoxyalkylene polymer having a hydrolyzable silyl group in the molecule is simply referred to as "polyoxyalkylene polymer."
[0077] The viscosity at 23°C and the ratio of the viscosity at 10 rpm at 23°C to the viscosity at 1 rpm at 23°C (viscosity at 1 rpm / viscosity at 10 rpm) of the obtained moisture-curable composition were measured in the manner described above, and the results are shown in Table 1. The ratio of the viscosity at 10 rpm at 23°C to the viscosity at 1 rpm at 23°C was expressed as "viscosity ratio (1 rpm / 10 rpm)."
[0078] The dumbbell physical properties [maximum stress and elongation] and storage stability of the obtained moisture-curable composition were measured in the following manner. The results are shown in Table 1.
[0079] (Dumbbell properties) The moisture-curable composition was applied to a substrate to a thickness of 3 mm and cured for one week in an environment of 23°C and 50% relative humidity to produce a cured product. Dumbbell size No. 3 test pieces were prepared from the cured product in accordance with JIS K6251, and the maximum stress (Tmax) and elongation (Emax) of the dumbbell physical properties were measured in accordance with JIS K6251.
[0080] (Storage stability) 300 g of the moisture-curable composition was filled into a glass bottle. The air in the glass bottle was removed and filled with nitrogen, and then the glass bottle was sealed to be in a hermetically sealed state. The mayonnaise bottle was left at 50° C. for one month. The presence or absence of separation between the polyoxyalkylene polymer and calcium carbonate was visually observed. A: No separation occurred between the polyoxyalkylene polymer and calcium carbonate. B: Polyoxyalkylene polymer in a portion extending from the surface to less than 0.5 mm There was separation of calcium carbonate. C: Polyoxyalkylene polymer in the area extending 0.5 mm or more from the surface There was separation of calcium carbonate.
[0081] [Table 1]
Claims
1. a polyoxyalkylene polymer (A) having a hydrolyzable silyl group in the molecule, the polyoxyalkylene polymer (A1) having a hydrolyzable silyl group in the molecule, a molecular weight distribution of less than 1.4, and a number average molecular weight of 8,000 or more and less than 19,000, and a polyoxyalkylene polymer (A2) having a hydrolyzable silyl group in the molecule and a number average molecular weight of 19,000 to 50,000; A surface-treated ground calcium carbonate; a surface-treated precipitated calcium carbonate; A moisture-curable composition comprising:
2. 2. The moisture-curing composition according to claim 1, wherein the ratio of the content of the surface-treated heavy calcium carbonate to the content of the surface-treated precipitated calcium carbonate (mass of the surface-treated heavy calcium carbonate / mass of the surface-treated precipitated calcium carbonate) is 1.5 or more.
3. 3. The moisture-curable composition according to claim 1, wherein the polyoxyalkylene polymer (A2) has a molecular weight distribution of less than 1.
4.
4. The moisture-curable composition according to any one of claims 1 to 3, characterized in that the ratio of the content of the polyoxyalkylene polymer (A1) to the content of the polyoxyalkylene polymer (A2) [mass of the polyoxyalkylene polymer (A1) / mass of the polyoxyalkylene polymer (A2)] is 1 or more.
5. The moisture-curable composition according to any one of claims 1 to 3, characterized in that the ratio of the content of the polyoxyalkylene polymer (A1) to the content of the polyoxyalkylene polymer (A2) [mass of the polyoxyalkylene polymer (A1) / mass of the polyoxyalkylene polymer (A2)] is 50 or less.
Citation Information
Patent Citations
Room temperature curing composition
JP1994329896A
Room-temperature-setting composition
JP1996225738A
Room temperature curable adhesive
JP2016210839A
Curable composition
JP2018162437A
Curable composition
WO2012117902A1