Rubber composition, its manufacturing method, and rubber product using same
A rubber composition with carboxylic acid-modified ethylene-α-olefin elastomer and carboxyl group-containing oil addresses the adhesion issue with RFL adhesives, providing enhanced bonding strength and affinity, suitable for applications like power transmission belts and tires.
Patent Information
- Application Number
- JP2020135003
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-07
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-08-07
AI Technical Summary
Existing rubber compositions do not exhibit excellent adhesion to resorcinol formaldehyde latex (RFL) adhesives, which is crucial for bonding with fiber members like polyester.
A rubber composition containing a carboxylic acid-modified ethylene-α-olefin elastomer and a carboxyl group-containing oil, where the carboxyl group-containing oil is composed of paraffin and naphthenic oils, is developed to enhance adhesion to RFL adhesives.
The composition achieves superior adhesiveness with RFL adhesives, enabling strong bonding with fiber members, as demonstrated by higher room temperature adhesive strength and improved affinity with latex in RFL aqueous solutions.
Smart Images

Figure 0007590829000004 
Figure 0007590829000001 
Figure 0007590829000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition, a method for producing the same, and a rubber product using the same. [Background technology]
[0002] It is known that ethylene-α-olefin elastomers are modified with carboxylic acids. For example, Patent Document 1 discloses that maleic anhydride and an organic peroxide are added to ethylene propylene copolymer (EPM) and the temperature is raised to the decomposition temperature of the organic peroxide, thereby grafting maleic anhydride onto the EPM. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 62-41245 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a rubber composition having excellent adhesion to a resorcinol-formaldehyde-latex (RFL) adhesive. [Means for solving the problem]
[0005] The present invention relates to a rubber composition comprising a carboxylic acid-modified ethylene-α-olefin elastomer and a carboxyl group-containing oil. The carboxyl group-containing oil includes a carboxylic acid-modified oil, and the oil before modification in the carboxylic acid-modified oil includes a paraffin oil and a naphthenic oil. .
[0006] The present invention relates to a rubber product having a product body formed from the rubber composition according to the present invention.
[0007] The present invention includes a step of preparing a carboxylic acid-modified ethylene-α-olefin elastomer by modifying an ethylene-α-olefin elastomer with a carboxylic acid, and a step of kneading the prepared carboxylic acid-modified ethylene-α-olefin elastomer with a carboxyl group-containing oil. The carboxyl group-containing oil includes a carboxylic acid-modified oil, and the oil before modification in the carboxylic acid-modified oil includes a paraffin oil and a naphthenic oil. A method for producing a rubber composition. Effect of the Invention
[0008] According to the present invention, by containing a carboxylic acid-modified ethylene-α-olefin elastomer and a carboxyl group-containing oil, excellent adhesion to a resorcinol-formaldehyde-latex (RFL) adhesive can be obtained. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a perspective view of a test piece for an adhesion test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The embodiments will be described in detail below.
[0011] The rubber composition according to the embodiment contains a rubber component. The rubber component contains an ethylene-α-olefin elastomer as a main component. The content of the ethylene-α-olefin elastomer in the rubber component is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 100% by mass. The rubber component may contain chloroprene rubber (CR), hydrogenated nitrile rubber (H-NBR), etc., in addition to the ethylene-α-olefin elastomer.
[0012] The ethylene-α-olefin elastomer contained in the rubber component is partially or entirely a carboxylic acid-modified ethylene-α-olefin elastomer. Hereinafter, the ethylene-α-olefin elastomer before modification in the carboxylic acid-modified ethylene-α-olefin elastomer is referred to as "elastomer A".
[0013] Examples of the elastomer A include ethylene propylene diene monomer (EPDM), ethylene propylene copolymer (EPM), ethylene butene copolymer (EBM), ethylene octene copolymer (EOM), etc. The elastomer A preferably contains one or more of these, and more preferably contains at least one of EPDM and EPM.
[0014] The ethylene content of the elastomer A is preferably from 40% by mass to 85% by mass, and more preferably from 50% by mass to 80% by mass.
[0015] When the elastomer A is EPDM, examples of the diene component include ethylidene nobornene (ENB), dicyclopentadiene (DCPD), and 1,4-hexadiene. Of these, the diene component is preferably ethylidene nobornene (ENB) or dicyclopentadiene (DCPD). When the diene component is ENB, the ENB content of the EPDM is preferably 0.5% by mass or more and 20.0% by mass or less, more preferably 1.5% by mass or more and 15.0% by mass or less. When the diene component is DCPD, the DCPD content of the EPDM is preferably 0.5% by mass or more and 10.0% by mass or less, more preferably 1.5% by mass or more and 8.0% by mass or less.
[0016] Examples of the carboxylic acid used for the carboxylic acid modification of the elastomer A include maleic anhydride, maleic acid, fumaric acid, itaconic anhydride, itaconic acid, and oleic acid. The carboxylic acid preferably contains one or more of these, and more preferably contains at least one of maleic anhydride and maleic acid. The content of the carboxylic acid in the carboxylic acid modified ethylene-α-olefin elastomer is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, more preferably 0.05 parts by mass or more and 3.0 parts by mass or less, based on 100 parts by mass of the elastomer A.
[0017] The carboxylic acid modified ethylene-α-olefin elastomer can be obtained by kneading elastomer A, carboxylic acid, and organic peroxide at a predetermined temperature. At this time, radicals are generated in the molecular chain of elastomer A by the action of the organic peroxide, and carboxylic acid is grafted to the radicals. An example of a commercially available organic peroxide is Perkadox 16 manufactured by Kayaku Akzo Co., Ltd. The amount of the organic peroxide to be blended at this time is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, more preferably 0.05 parts by mass or more and 3.0 parts by mass or less, based on 100 parts by mass of elastomer A.
[0018] The ethylene-α-olefin elastomer contained in the rubber component may be a partly carboxylic acid-modified ethylene-α-olefin elastomer, and the remainder may be an ethylene-α-olefin elastomer that is not carboxylic acid-modified (hereinafter referred to as "elastomer B").
[0019] The elastomer B may be, as in the case of the elastomer A, for example, EPDM, EPM, EBM, EOM, etc. The elastomer B preferably contains one or more of these, and more preferably contains at least one of EPDM and EPM. The elastomer B is preferably the same as the elastomer A.
[0020] The ethylene content of the elastomer B is preferably 40% by mass or more and 85% by mass or less, more preferably 50% by mass or more and 80% by mass or less. The ethylene content of the elastomer B is preferably the same as or higher than the ethylene content of the elastomer A.
[0021] When the elastomer B is EPDM, examples of the diene component include ENB, DCPD, and 1,4-hexadiene. Of these, the diene component is preferably ENB or DCPD. When the diene component is ENB, the ENB content is preferably 0.5% by mass or more and 20.0% by mass or less, more preferably 1.5% by mass or more and 15.0% by mass or less. When the diene component is DCPD, the DCPD content is preferably 0.5% by mass or more and 10.0% by mass or less, more preferably 1.5% by mass or more and 8.0% by mass or less. When both the elastomer A and the elastomer B are EPDM, the diene content (ENB content or DCPD content) of the elastomer B is preferably the same as the diene content of the elastomer A.
[0022] The content of elastomer B in the rubber component is preferably the same as or greater than the content of elastomer A.
[0023] The rubber composition according to the embodiment contains an oil component. A part or all of the oil component is a carboxyl group-containing oil. Examples of the carboxyl group-containing oil include fats and oils having a carboxyl group and carboxylic acid-modified oils. It is preferable that the carboxyl group-containing oil contains at least one of these.
[0024] The fats and oils having a carboxyl group include one or more selected from the group consisting of oleic acid, linoleic acid, linoleic acid, palmitoleic acid, petroselinic acid, elaidic acid, ricinoleic acid, linoelaidic acid, arachidonic acid, stearidonic acid, eicosapentaenoic acid, docosapentaenoic acid, docosahexaenoic acid, docosatetraenoic acid, vaccenic acid, paulic acid, erucic acid, nervonic acid, sapienic acid, etc. The fats and oils having a carboxyl group may be the same as the carboxylic acid used for the carboxylic acid modification of the elastomer A.
[0025] Examples of the oil before modification in the carboxylic acid modified oil (hereinafter referred to as "oil P") include paraffin oil, naphthenic oil, aromatic oil, etc. Oil P preferably contains one or more of paraffin oil, naphthenic oil, and aromatic oil, more preferably contains two of paraffin oil and naphthenic oil, and further preferably contains all three.
[0026] Paraffin oil contains a large amount of paraffin-based hydrocarbons, which are saturated chain compounds. Examples of commercially available paraffin oils include Diana Process Oil PW-90 (manufactured by Idemitsu Kosan Co., Ltd.) and Diana Process Oil PW-380 (manufactured by Idemitsu Kosan Co., Ltd.).
[0027] Naphthenic oil contains a large amount of naphthenic hydrocarbons, which are hydrocarbons having at least one saturated ring (naphthenic ring) in one molecule. Commercially available naphthenic oils include, for example, Diana Process Oil NS90S (manufactured by Idemitsu Kosan Co., Ltd.) and Diana Process Oil NS100 (manufactured by Idemitsu Kosan Co., Ltd.).
[0028] Aroma oil contains a large amount of aromatic hydrocarbons, which are hydrocarbons having at least one aromatic ring in one molecule. Commercially available aroma oils include, for example, Diana Process Oil AC-12 (manufactured by Idemitsu Kosan Co., Ltd.), Diana Process Oil AC-460 (manufactured by Idemitsu Kosan Co., Ltd.), Diana Process Oil AH-16 (manufactured by Idemitsu Kosan Co., Ltd.), etc.
[0029] When the oil P contains both paraffin oil and naphthenic oil, the content of the paraffin oil is preferably greater than the content of the naphthenic oil. The mass ratio of the paraffinic hydrocarbon components to the oil P is preferably 60% or more and 95% or less, more preferably 70% or more and 90% or less. The mass ratio of the naphthenic hydrocarbon components to the oil P is preferably 5% or more and 40% or less, more preferably 10% or more and 30% or less. The mass ratio (%) of each hydrocarbon component to the oil P is measured based on ASTM D3238 (hereinafter the same).
[0030] When the oil P contains three types of oil, namely, paraffin oil, naphthenic oil, and aromatic oil, the content of paraffin oil is preferably greater than the content of naphthenic oil, and the content of naphthenic oil is preferably greater than the content of aromatic oil. The mass ratio of paraffinic hydrocarbon components to the oil P is preferably 55% or more and 90% or less, more preferably 60% or more and 85% or less. The mass ratio of naphthenic hydrocarbon components to the oil P is preferably 9.9% or more and 38% or less, more preferably 14% or more and 34% or less. The mass ratio of aromatic hydrocarbon components to the oil P is preferably 0.1% or more and 7% or less, more preferably 1% or more and 6% or less.
[0031] Examples of the carboxylic acid used for the carboxylic acid modification of the oil P include maleic anhydride, maleic acid, fumaric acid, itaconic anhydride, and itaconic acid. The carboxylic acid preferably contains one or more of these, and more preferably contains at least one of maleic anhydride modified oil and maleic acid modified oil. The carboxylic acid used for the carboxylic acid modification of the oil P is preferably the same as the carboxylic acid used for the carboxylic acid modification of the elastomer A. The content of the carboxylic acid in the carboxylic acid modified oil is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, more preferably 0.05 parts by mass or more and 3.0 parts by mass or less, based on 100 parts by mass of the oil P.
[0032] The carboxylic acid modified oil can be obtained by mixing Oil P, carboxylic acid, and organic peroxide at a predetermined temperature. At this time, radicals are generated in the molecules of Oil P by the action of the organic peroxide, and carboxylic acid is bonded to the radicals. Commercially available organic peroxides include, for example, Perkadox 16 manufactured by Kayaku Akzo Co., Ltd. The amount of the organic peroxide to be blended at this time is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, more preferably 0.05 parts by mass or more and 3.0 parts by mass or less, relative to 100 parts by mass of Oil P.
[0033] The oil component may be a part of a carboxyl group-containing oil, and the remainder of the oil may be an oil not containing a carboxyl group (hereinafter referred to as "oil Q"). As with oil P, examples of oil Q include paraffin oil, naphthenic oil, and aromatic oil. It is preferable that oil Q contains one or more of paraffin oil, naphthenic oil, and aromatic oil.
[0034] In this case, the content of oil Q in the oil component is preferably lower than the content of oil P. The ratio of the content of oil Q to the content of oil P is preferably 0.01 or more and 0.5 or less, more preferably 0.05 or more and 0.4 or less.
[0035] The content of the oil component in the rubber composition according to the embodiment is preferably 0.5 parts by mass to 50.0 parts by mass, more preferably 1.0 parts by mass to 30.0 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of improving adhesion to the RFL adhesive. The content of the carboxyl group-containing oil is preferably 0.25 parts by mass to 25.0 parts by mass, more preferably 0.5 parts by mass to 15.0 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of improving adhesion to the RFL adhesive.
[0036] Here, the "RFL adhesive" is used to bond a fiber material such as polyester to rubber. The RFL adhesive is attached to the surface of the fiber material by immersing the fiber material in an RFL aqueous solution in which a precondensate (RF) of resorcin (R) and formalin (F) is mixed with latex (L) and then heating the solution. The fiber material and rubber are bonded via this RFL adhesive. In this specification, the RFL adhesive refers to an object to be bonded to which the rubber composition according to the embodiment is bonded.
[0037] The molar ratio (R / F) of resorcin (R) to formalin (F) in the RFL aqueous solution is, for example, 1 / 2 or more and 1 / 1 or less. The solids mass ratio (RF / L) of the initial condensate (RF) of resorcin (R) and formalin (F) to the latex (L) in the RFL aqueous solution is, for example, 1 / 20 or more and 1 / 5 or less. The solids concentration of the RFL aqueous solution is, for example, 3 mass% or more and 30 mass% or less.
[0038] Examples of the latex (L) include vinylpyridine-styrene butadiene copolymer rubber (VP-SBR) latex, chloroprene rubber (CR) latex, chlorosulfonated polyethylene rubber (CSM) latex, 2,3-dichlorobutadiene polymer rubber (2,3-DCB) latex, nitrile butadiene rubber (NBR) latex, etc. The latex (L) preferably contains one or more of these, and more preferably contains vinylpyridine-styrene butadiene copolymer rubber (VP-SBR) latex from the viewpoint of enhancing the adhesion between the rubber composition according to the embodiment and the RFL adhesive.
[0039] The immersion time of the fiber material in the RFL aqueous solution is, for example, 0.5 to 10 seconds. The heating temperature (heating furnace setting temperature) after immersion in the RFL aqueous solution is, for example, 200° C. to 280° C., and the heating time is, for example, 30 to 600 seconds.
[0040] In the rubber composition according to the embodiment, rubber molecules of the rubber component are crosslinked. For this crosslinking, an organic peroxide may be used as a crosslinking agent, or sulfur may be used as a crosslinking agent, or these may be used in combination. From the viewpoint of enhancing adhesion to the RFL adhesive, the rubber composition according to the embodiment preferably uses at least an organic peroxide as a crosslinking agent. In that case, from the same viewpoint, the blending amount of the organic peroxide in the uncrosslinked rubber composition before crosslinking is preferably 0.5 parts by mass or more and 8.0 parts by mass or less, more preferably 1.0 parts by mass or more and 6.0 parts by mass or less, relative to 100 parts by mass of the rubber component. In addition, it is preferable that the organic peroxide used for crosslinking the rubber component is different from the organic peroxide used for the carboxylic acid modification of the elastomer A or the oil P. It is preferable that the organic peroxide used for crosslinking the rubber component has a higher decomposition temperature than the organic peroxide used for the carboxylic acid modification of the elastomer A or the oil P.
[0041] From the viewpoint of enhancing adhesion to the RFL adhesive, the rubber composition according to the embodiment preferably further contains a carbodiimide as a rubber compounding agent. Carbodiimides include monocarbodiimides having one carbodiimide group in the molecule and polycarbodiimides having two or more carbodiimide groups in the molecule.
[0042] Examples of monocarbodiimides include bis(2,6-diisopropylphenyl)carbodiimide, diphenylcarbodiimide, di-β-naphthylcarbodiimide, N,N′-diisopropylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, and the like.
[0043] Examples of polycarbodiimides include poly(1,6-hexamethylenecarbodiimide), poly(4,4'-methylenebiscyclohexylcarbodiimide), poly(1,3-cyclohexylenecarbodiimide), poly(1,4-cyclohexylenecarbodiimide), poly(4,4'-dicyclohexylmethanecarbodiimide), and the like.
[0044] The carbodiimide preferably contains one or more of these, and from the viewpoint of improving adhesion to the RFL adhesive, it preferably contains a monocarbodiimide, and more preferably contains bis(2,6-diisopropylphenyl)carbodiimide.
[0045] In order to enhance adhesion to the RFL adhesive, the content of the carbodiimide in the rubber composition according to the embodiment is preferably 0.25 parts by mass or more and 25.0 parts by mass or less, and more preferably 0.5 parts by mass or more and 15.0 parts by mass or less, per 100 parts by mass of the rubber component.
[0046] The rubber composition according to the embodiment may contain, in addition to the carbodiimide, reinforcing materials such as carbon black and short fibers, processing aids, vulcanization accelerators, vulcanization acceleration assistants, plasticizers, and the like as rubber compounding agents.
[0047] The rubber composition according to the embodiment having the above configuration can provide excellent adhesion to the RFL adhesive. This is believed to be because the rubber composition according to the embodiment contains a carboxyl group-containing oil, which improves the affinity between the latex contained in the RFL aqueous solution and the rubber composition according to the embodiment.
[0048] The rubber composition according to the above embodiment can be used as a material for forming a product body in which a fiber member is combined with an RFL adhesive for rubber products such as a transmission belt, a conveyor belt, a tire, or a hose.
[0049] Next, a method for producing the rubber composition according to the embodiment will be described.
[0050] [Manufacturing method example 1] In the example of the production method 1, fats and oils having a carboxyl group are used as the carboxyl group-containing oil.
[0051] First, elastomer A is charged into a kneader such as a Banbury mixer and masticated, and then carboxylic acid and organic peroxide are charged therein and heated to perform carboxylic acid modification treatment of elastomer A. The treatment temperature for this carboxylic acid modification treatment is preferably 60°C or higher and 130°C or lower.
[0052] Next, the kneaded product is discharged from the kneader and cooled, and then the unreacted carboxylic acid is removed by sublimation to obtain a carboxylic acid-modified ethylene-α-olefin elastomer.
[0053] Next, the rubber component containing the obtained carboxylic acid-modified ethylene-α-olefin elastomer is added to a kneader such as a Banbury mixer and masticated, and various rubber compounding agents including oils and fats having carboxyl groups and a crosslinking agent are added thereto and kneaded.
[0054] Next, the kneaded mixture is discharged from the kneader and cooled to obtain an uncrosslinked rubber composition.
[0055] The resulting uncrosslinked rubber composition is then held for a predetermined time under conditions of a predetermined temperature and a predetermined pressure to crosslink the rubber component, thereby obtaining the rubber composition according to the embodiment.
[0056] In addition, when the fat or oil having a carboxyl group is the same as the carboxylic acid used for the carboxylic acid modification of elastomer A, an excess of fat or oil having a carboxyl group as the carboxylic acid can be added to elastomer A to obtain a mixture of a carboxylic acid-modified ethylene-α-olefin elastomer and a fat or oil having a carboxyl group, and therefore a step of further adding a fat or oil having a carboxyl group to the obtained carboxylic acid-modified ethylene-α-olefin elastomer is not necessary.
[0057] [Manufacturing method example 2] In the example of the production method 2, a carboxylic acid-modified oil is used as the carboxyl group-containing oil. In this case, a step of preparing the carboxylic acid-modified ethylene-α-olefin elastomer and a step of preparing the carboxylic acid-modified oil are simultaneously carried out in a single step.
[0058] First, elastomer A is charged into a kneading machine such as a Banbury mixer and masticated, and oil P is then charged therein and kneaded.
[0059] A carboxylic acid and an organic peroxide are added to the obtained kneaded product, and the temperature is raised to perform a carboxylic acid modification treatment of the elastomer A and the oil P. The treatment temperature for this carboxylic acid modification treatment is preferably 60°C or higher and 190°C or lower.
[0060] Next, the kneaded product is discharged from the kneader and cooled, and then the unreacted carboxylic acid is removed by sublimation to obtain a carboxylic acid-modified ethylene-α-olefin elastomer and a carboxylic acid-modified oil.
[0061] Next, the rubber component containing the obtained carboxylic acid-modified ethylene-α-olefin elastomer and the carboxylic acid-modified oil is added to a kneader such as a Banbury mixer and kneaded, and various rubber compounding agents including a crosslinking agent are added thereto and further kneaded.
[0062] The subsequent steps are the same as in Example 1 of the manufacturing method.
[0063] [Manufacturing method example 3] In the example of the manufacturing method 3, a carboxylic acid-modified oil is used as the carboxyl group-containing oil. At this time, a step of preparing the carboxylic acid-modified ethylene-α-olefin elastomer and a step of preparing the carboxylic acid-modified oil are separately carried out as mutually independent steps.
[0064] First, elastomer A is charged into a kneader such as a Banbury mixer and masticated, and then carboxylic acid and organic peroxide are charged therein and heated to perform carboxylic acid modification treatment of elastomer A. The treatment temperature for this carboxylic acid modification treatment is preferably 60°C or higher and 130°C or lower.
[0065] Next, the kneaded product is discharged from the kneader and cooled, and then the unreacted carboxylic acid is removed by sublimation to obtain a carboxylic acid-modified ethylene-α-olefin elastomer.
[0066] In addition, the oil P, a carboxylic acid, and an organic peroxide are put into a sample tube or the like, mixed, and heated to perform a carboxylic acid modification treatment of the oil P. The treatment temperature of this carboxylic acid modification treatment is preferably 60° C. or higher and 130° C. or lower. In this way, a carboxylic acid modified oil is obtained.
[0067] Next, the rubber component containing the obtained carboxylic acid-modified ethylene-α-olefin elastomer and the obtained carboxylic acid-modified oil is added to a kneader such as a Banbury mixer and kneaded, and various rubber compounding agents including a crosslinking agent are added thereto and further kneaded.
[0068] The subsequent steps are the same as in Example 1 of the manufacturing method. EXAMPLES
[0069] [Test evaluation 1] Uncrosslinked rubber compositions of Examples 1-1 to 1-7 and Comparative Example 1-1 were prepared. The configurations of each are also shown in Table 1.
[0070] <Example 1-1> First, 100 parts by mass of EPM (EP11 manufactured by JSR, ethylene content 52% by mass) was put into an open roll and masticated, and 10 parts by mass of oil (1) was put therein and kneaded. This oil (1) contains paraffin oil, naphthene oil and aromatic oil, and contains paraffinic hydrocarbons, naphthenic hydrocarbons and aromatic hydrocarbons in a mass ratio of 73:23:4.
[0071] Next, the kneaded material obtained was put into a Banbury mixer, and the rotor speed was set to 30 rpm and kneaded for 1 minute, after which 0.8 parts by mass of maleic anhydride was put into 100 parts by mass of EPM and kneaded for 1 minute. Furthermore, 0.8 parts by mass of organic peroxide (Perkadox 16, manufactured by Kayaku Akzo) was put into 100 parts by mass of EPM and kneaded at a rotor speed of 30 rpm until the temperature reached 100°C. Here, the mixture was held at 100°C for 7 minutes and subjected to maleic anhydride modification treatment. The rotation speed was adjusted so as to hold the mixture at 100°C.
[0072] Then, the kneaded product was discharged from the Banbury mixer, formed into a sheet by a calendar roll, cooled, and then wrapped around a heated roll to heat it, so that the unreacted maleic anhydride was sublimated and removed, and formed into a sheet by a calendar roll again, thereby producing the uncrosslinked rubber composition of Example 1-1.
[0073] <Example 1-2> First, 100 parts by mass of EPDM (1) (Nordel IP 4640 manufactured by Dow Chemical, ethylene content 55%, ENB content 4 to 5%) was put into a Banbury mixer, and the rotor speed was set to 30 rpm and masticated for 1 minute. 0.8 parts by mass of maleic anhydride was put into 100 parts by mass of EPDM (1) and kneaded for 1 minute, and further, 0.8 parts by mass of organic peroxide was put into 100 parts by mass of EPDM (1), and the rotor speed was set to 30 rpm and kneaded until the temperature reached 100 ° C. Here, the mixture was held at 100 ° C. for 7 minutes and subjected to maleic anhydride modification treatment. The rotation speed was adjusted to hold the mixture at 100 ° C.
[0074] Next, the kneaded product was discharged from the Banbury mixer, formed into a sheet using a calendar roll, cooled, and then wrapped around a heated roll to heat it, sublimating and removing the unreacted maleic anhydride, and formed into a sheet using a calendar roll again, thereby producing a modified EPDM.
[0075] Next, 100 parts by mass of oil (1), 1.5 parts by mass of maleic anhydride, and 1.5 parts by mass of organic peroxide (Perkadox 16, manufactured by Kayaku Akzo) were added to the sample tube, mixed, and heated. The liquid was then held at 100°C for 7 minutes to carry out maleic anhydride modification treatment. This produced modified oil (1). The composition of modified oil (1) is also shown in Table 2.
[0076] 100 parts by mass of modified EPDM was put into an open roll and masticated, 4.1 parts by mass of modified oil (1) was put therein and kneaded, and the mixture was formed into a sheet shape by a calendar roll, thereby preparing an uncrosslinked rubber composition of Example 1-2.
[0077] <Example 1-3> An uncrosslinked rubber composition was prepared in the same manner as in Example 1-1, except that EPDM (1) was used instead of EPM, and the amount of oil (1) was changed to 4 parts by mass per 100 parts by mass of EPDM (1). This was designated as Example 1-3.
[0078] <Example 1-4> An uncrosslinked rubber composition was prepared in the same manner as in Example 1-1 except that EPDM(2) (EPT1045 manufactured by Mitsui Chemicals, Inc., ethylene content 58%, DCPD content 5%) was used instead of EPM. The uncrosslinked rubber composition was designated as Example 1-4.
[0079] <Example 1-5> Example 1-5 was an uncrosslinked rubber composition prepared in the same manner as in Example 1-1, except that EPDM (2) was used instead of EPM and the amount of maleic anhydride was changed to 1.6 parts by mass per 100 parts by mass of EPDM (2).
[0080] <Examples 1-6> First, 100 parts by mass of EPDM (2) was charged into an open roll and masticated, and 2.3 parts by mass of oleic acid was charged thereto and kneaded.
[0081] Next, the obtained kneaded material was put into a Banbury mixer, and the rotor speed was set to 30 rpm and kneaded for 1 minute, and then 0.8 parts by mass of organic peroxide was put into 100 parts by mass of EPDM (2), and the rotor speed was set to 30 rpm and kneaded until the temperature reached 100°C. Here, the mixture was held at 100°C for 7 minutes to carry out oleic acid modification treatment, and a mixture of oleic acid modified EPDM and oleic acid was obtained. The rotation speed was adjusted to maintain the temperature at 100°C.
[0082] Subsequently, the kneaded product was discharged from the Banbury mixer and formed into a sheet using a calendar roll, thereby producing an uncrosslinked rubber composition of Example 1-6 containing oleic acid-modified EPDM and oleic acid.
[0083] <Example 1-7> Modified oil (2) was prepared in the same manner as modified oil (1) prepared in Example 1-2, except that oil (2) was used instead of oil (1). Oil (2) contains paraffin oil and naphthene oil, and contains paraffinic hydrocarbons and naphthenic hydrocarbons in a mass ratio of 72:28. The composition of modified oil (2) is also shown in Table 2.
[0084] An uncrosslinked rubber composition was prepared in the same manner as in Example 1-2, except that modified oil (2) was used instead of modified oil (1) in Example 1-2, and designated as Example 1-7.
[0085] <Comparative Example 1-1> An uncrosslinked rubber composition was prepared in the same manner as in Example 1-2, except that unmodified oil (1) was used instead of modified oil (1) in Example 1-2, and used as Comparative Example 1-1.
[0086] [Table 1]
[0087] [Table 2]
[0088] (Test evaluation method) For each of the uncrosslinked rubber compositions of Examples 1-1 to 1-7 and Comparative Example 1-1, the uncrosslinked rubber compositions were left at room temperature for two weeks. After that, the occurrence of bleeding was confirmed by touching each uncrosslinked rubber composition. When oil was attached to the hand, it was judged as A, and when oil was not attached to the hand, it was judged as B.
[0089] (Test evaluation results) The test results are shown in Table 1.
[0090] According to Table 1, bleeding occurred in the rubber composition of Comparative Example 1-1, which does not contain a carboxyl group-containing oil such as modified oil (1) or modified oil (2), whereas bleeding did not occur in the rubber compositions of Examples 1-1 to 1-7, which contain a carboxyl group-containing oil.
[0091] [Test evaluation 2] The rubber fiber composites of Examples 2-1 to 2-9 and Comparative Examples 2-1 to 2-4 were prepared. The rubber compositions of Example 2-10 and Comparative Example 2-5 were also prepared. The configurations of each are shown in Table 3.
[0092] <Example 2-1> First, 55.8 parts by mass of the uncrosslinked rubber composition of compounding number [1] according to Example 1-1 and 50 parts by mass of EPDM (2) were put into a Banbury mixer and kneaded, and then 5 parts by mass of zinc oxide, 1.5 parts by mass of stearic acid, 0.5 parts by mass of metal soap-fatty acid amide compound, 35 parts by mass of carbon black, 20 parts by mass of silica, 10 parts by mass of unsaturated carboxylic acid compound, 0.1 parts by mass of insoluble sulfur, and 4 parts by mass of organic peroxide (1) (Peroximon F40, NOF Corp., peroxide component 40%) were put therein and further kneaded to prepare an uncrosslinked rubber composition containing various rubber compounding agents. The uncrosslinked rubber composition of compounding number [1] contains 50 parts by mass of EPM and 5 parts by mass of oil (1), and the EPM and oil (1) are modified with maleic anhydride. The uncrosslinked rubber composition containing the various rubber compounding agents contains, as rubber components, 50 parts by mass of the unmodified EPM contained in the uncrosslinked rubber composition of compounding number [1] and 50 parts by mass of unmodified EPDM (2).
[0093] A twisted yarn made of polyester fibers was given a primer treatment and an RFL treatment.
[0094] In the primer treatment, a solution with a solid content concentration of 16 mass % obtained by dissolving polymethylene polyphenyl polyisocyanate (manufactured by Sumika Bayer Urethane Co., Ltd., product name: Sumidur 44V20) in toluene was used as the primer solution. The twisted yarn was immersed in the primer solution for 0.5 seconds, and the heating temperature (heating furnace setting temperature) after immersion was 245±11°C, and the heating time was 60 seconds.
[0095] For the RFL treatment, an RFL aqueous solution was prepared using vinylpyridine-styrene butadiene copolymer rubber (VP-SBR) latex. The molar ratio (R / F) of resorcinol (R) to formalin (F) was 1 / 1.4, the solid mass ratio (RF / L) of the initial condensate (RF) of resorcinol (R) and formalin (F) to the latex (L) was 1 / 6.1, and the solid concentration was 16.1 mass%. The immersion time of the twisted yarn in the RFL aqueous solution was 1.0 second, the heating temperature (heating furnace setting temperature) after immersion was 230±10℃, and the heating time was 60 seconds.
[0096] Using the uncrosslinked rubber composition containing the various rubber compounding agents and the twisted yarn that had been subjected to the primer treatment and the RFL treatment, an adhesion test specimen 10 was press-molded in which seven twisted yarns 11 as shown in FIG. 1 were embedded in the surface layer of a plate-shaped rubber sheet 12 formed of the uncrosslinked rubber composition containing the various rubber compounding agents so as to extend parallel to each other at intervals. The press molding conditions were a temperature of 160°C, a pressure of 4 MPa, and a time of 40 minutes. The adhesion test specimen 10 was a rubber fiber composite in which the crosslinked rubber composition was bonded to the twisted yarns 11 via the RFL adhesive, and this adhesion test specimen 10 was designated Example 2-1.
[0097] <Example 2-2> A specimen 10 for adhesion test similar to that of Example 2-1 was prepared, except that 40.2 parts by mass of the uncrosslinked rubber composition of Compounding Number [4] according to Example 1-4 was used instead of the uncrosslinked rubber composition of Compounding Number [1], and the compounding amount of EPDM (2) was changed to 64 parts by mass, and this was designated as Example 2-2. The uncrosslinked rubber composition of Compounding Number [4] contains 36 parts by mass of EPDM (2) and 3.6 parts by mass of oil (1), and EPDM (2) and oil (1) are modified with maleic anhydride. The uncrosslinked rubber composition containing various rubber compounding agents contains, as a rubber component, 36 parts by mass of EPDM (2) before modification and 64 parts by mass of unmodified EPDM (2) contained in the uncrosslinked rubber composition of Compounding Number [4].
[0098] <Example 2-3> A specimen 10 for adhesion test similar to that of Example 2-1 was prepared, except that 56.2 parts by mass of the uncrosslinked rubber composition of Compounding No. [5] according to Example 1-5 was used instead of the uncrosslinked rubber composition of Compounding No. [1], and 1 part by mass of fatty acid ester was further added, and this specimen was designated as Example 2-3. The uncrosslinked rubber composition of Compounding No. [5] contains 50 parts by mass of EPDM (2) and 5 parts by mass of oil (1), and the EPDM (2) and oil (1) are modified with maleic anhydride. The uncrosslinked rubber composition containing various rubber compounding agents contains, as a rubber component, 50 parts by mass of the unmodified EPDM (2) contained in the uncrosslinked rubber composition of Compounding No. [5] and 50 parts by mass of unmodified EPDM (2).
[0099] <Example 2-4> A specimen 10 for adhesion test similar to that of Example 2-1 was prepared, except that 25.8 parts by mass of the uncrosslinked rubber composition of Compounding Number [6] according to Example 1-6 was used instead of the uncrosslinked rubber composition of Compounding Number [1], and the compounding amount of EPDM (2) was changed to 75 parts by mass, and this was designated as Example 2-4. The uncrosslinked rubber composition of Compounding Number [6] contains 25 parts by mass of EPDM (2) and 0.6 parts by mass of oleic acid, and EPDM (2) is modified with oleic acid, and is composed of a mixture of oleic acid-modified EPDM (2) and oleic acid. The uncrosslinked rubber composition containing various rubber compounding agents contains, as a rubber component, 25 parts by mass of EPDM (2) before modification contained in the uncrosslinked rubber composition of Compounding Number [6] and 75 parts by mass of unmodified EPDM (2).
[0100] <Example 2-5> A specimen 10 for adhesion test was prepared similarly to that of Example 2-1, except that 104.1 parts by mass of the uncrosslinked rubber composition of Compounding Number [2] according to Example 1-2 was used instead of the uncrosslinked rubber composition of Compounding Number [1] and EPDM (2), and this specimen was designated as Example 2-5. The uncrosslinked rubber composition of Compounding Number [2] contains 98 parts by mass of EPDM (1) and 4 parts by mass of oil (1), and the EPDM (1) and oil (1) are modified with maleic anhydride. The uncrosslinked rubber composition containing various rubber compounding agents contains 98 parts by mass of EPDM (1) before modification contained in the uncrosslinked rubber composition of Compounding Number [2] as a rubber component.
[0101] <Example 2-6> A specimen 10 for adhesion test similar to that of Example 2-1 was prepared, except that 27.9 parts by mass of the uncrosslinked rubber composition of Compounding Number [4] according to Example 1-4 was used instead of the uncrosslinked rubber composition of Compounding Number [1], the amount of EPDM (2) was changed to 75 parts by mass, and 2 parts by mass of the carbodiimide compound and 2.5 parts by mass of oil (1) were further added, and this specimen was designated as Example 2-6. The uncrosslinked rubber composition of Compounding Number [4] contains 25 parts by mass of EPDM (2) and 2.5 parts by mass of oil (1), and EPDM (2) and oil (1) are modified with maleic anhydride. The uncrosslinked rubber composition containing various rubber compounding agents contains, as a rubber component, 25 parts by mass of EPDM (2) before modification and 75 parts by mass of unmodified EPDM (2) contained in the uncrosslinked rubber composition of Compounding Number [4].
[0102] <Example 2-7> A specimen 10 for adhesion test was prepared similarly to Example 2-1, except that 28.1 parts by mass of the uncrosslinked rubber composition of compounding number [5] according to Example 1-5 was used instead of the uncrosslinked rubber composition of compounding number [1], the amount of EPDM (2) was changed to 75 parts by mass, and 0.5 parts by mass of fatty acid ester, 2 parts by mass of carbodiimide compound, and 2.5 parts by mass of oil (1) were further added, and this specimen was designated as Example 2-7. The uncrosslinked rubber composition of compounding number [5] contains 25 parts by mass of EPDM (2) and 2.5 parts by mass of oil (1), and EPDM (2) and oil (1) are modified with maleic anhydride. The uncrosslinked rubber composition containing various rubber compounding agents contains, as a rubber component, 25 parts by mass of EPDM (2) before modification and 75 parts by mass of unmodified EPDM (2) contained in the uncrosslinked rubber composition of compounding number [5].
[0103] <Example 2-8> A specimen 10 for adhesion test similar to that of Example 2-1 was prepared, except that 51.6 parts by mass of the uncrosslinked rubber composition of Compounding No. [6] according to Example 1-6 was used instead of the uncrosslinked rubber composition of Compounding No. [1], stearic acid was not added, and 2 parts by mass of a carbodiimide compound was further added, and this specimen was designated as Example 2-8. The uncrosslinked rubber composition of Compounding No. [6] contains 50 parts by mass of EPDM (2) and 1.2 parts by mass of oleic acid, and the EPDM (2) is modified with oleic acid, and is composed of a mixture of oleic acid-modified EPDM (2) and oleic acid. The uncrosslinked rubber composition containing various rubber compounding agents contains, as a rubber component, 50 parts by mass of the unmodified EPDM (2) contained in the uncrosslinked rubber composition of Compounding No. [6] and 50 parts by mass of unmodified EPDM (2).
[0104] <Example 2-9> A specimen 10 for adhesion test was prepared similarly to Example 2-1, except that the amount of the uncrosslinked rubber composition of compounding number [1] was changed to 111.6 parts by mass, EPDM (2) was not added, and 2 parts by mass of a carbodiimide compound was further added, and this specimen was designated as Example 2-9. The uncrosslinked rubber composition of compounding number [1] contains 100 parts by mass of EPM and 10 parts by mass of oil (1), and the EPM and oil (1) are modified with maleic anhydride. The uncrosslinked rubber composition containing various rubber compounding agents contains 100 parts by mass of EPM before modification contained in the uncrosslinked rubber composition of compounding number [1] as a rubber component.
[0105] <Example 2-10> First, 105.6 parts by mass of the uncrosslinked rubber composition of compounding number [3] according to Example 1-3 was wound around an open roll, 5 parts by mass of zinc oxide was added thereto, and the mixture was left until the zinc oxide was incorporated. Next, 100 parts by mass of calcium carbonate was added, and the mixture was left until the calcium carbonate was incorporated. After turning over, the roll was cooled to bring the rubber composition to room temperature. The rubber composition was wound around an open roll, and 1 part by mass of an organic peroxide (Percumyl D, NOF Corp., peroxide content 98% or more) was added. Furthermore, turning over was performed once each to the left and right to obtain a sheet-like rubber composition with a thickness of about 0.6 mm. This produced the rubber composition of Example 2-10. The uncrosslinked rubber composition of compounding number [3] contained 100 parts by mass of EPDM (1) and 4 parts by mass of oil (1), and the EPDM (1) and oil (1) were modified with maleic anhydride. The uncrosslinked rubber composition containing various rubber compounding agents contains, as a rubber component, 100 parts by mass of the unmodified EPDM (1) contained in the uncrosslinked rubber composition of compounding number [3].
[0106] <Comparative Example 2-1> A specimen 10 for adhesion test was prepared similarly to Example 2-1, except that 50 parts by mass of EPM was used instead of the uncrosslinked rubber composition of compounding number [1], and 5 parts by mass of oil (1) was added, and this specimen was designated as Comparative Example 2-1. The uncrosslinked rubber composition containing various rubber compounding agents contains 50 parts by mass of unmodified EPM and 50 parts by mass of unmodified EPDM (2) as rubber components.
[0107] <Comparative Example 2-2> A specimen 10 for adhesion test was prepared similarly to Example 2-1, except that the uncrosslinked rubber composition of compounding number [1] was not added, the compounding amount of EPDM (2) was changed to 100 parts by mass, and 3.6 parts by mass of oil (1) was added, and this specimen was designated as Comparative Example 2-2. The uncrosslinked rubber composition containing various rubber compounding agents contains 100 parts by mass of unmodified EPDM (2) as the rubber component.
[0108] <Comparative Example 2-3> A specimen 10 for adhesion test was prepared similarly to Example 2-1, except that 100 parts by mass of EPDM (1) was used instead of the uncrosslinked rubber composition of compounding number [1] and EPDM (2), and 4 parts by mass of oil (1) was added, and this specimen was designated as Comparative Example 2-3. The uncrosslinked rubber composition containing various rubber compounding agents contains 100 parts by mass of unmodified EPDM (1) as the rubber component.
[0109] <Comparative Example 2-4> A specimen 10 for adhesion test was prepared similarly to Example 2-1, except that the uncrosslinked rubber composition of compounding number [1] was not added, the compounding amount of EPDM (2) was changed to 100 parts by mass, stearic acid was not added, and 2.3 parts by mass of oleic acid was added, and this specimen was designated as Comparative Example 2-4. The uncrosslinked rubber composition containing various rubber compounding agents contains 100 parts by mass of unmodified EPDM (2) as the rubber component.
[0110] <Comparative Example 2-5> A rubber composition prepared in the same manner as in Example 2-10, except that 100 parts by mass of EPDM (1) was used instead of the uncrosslinked rubber composition of compounding number [3] and 4 parts by mass of oil (1) was added, was designated as Comparative Example 2-5. The uncrosslinked rubber composition containing various rubber compounding agents contains 100 parts by mass of unmodified EPDM (1) as the rubber component.
[0111] [Table 3]
[0112] (Test evaluation method) <Adhesion evaluation test> For each of the adhesion test specimens 10 of Examples 2-1 to 2-9 and Comparative Examples 2-1 to 2-4, after leaving the specimens for adhesion test in an atmosphere at 23° C. for 24 hours or more, the rubber plate 12 was fixed to one chuck of a tensile tester, and three twisted threads 11 arranged every other one of the seven twisted threads 11 embedded in the rubber plate 12 were folded back and pulled out in a direction forming an angle of 180° with the rubber plate 12 and fixed to the other chuck, and 100 mm of the three twisted threads 11 were peeled off from the rubber plate 12 at a peeling speed of 100 mm / min. The value measured based on JIS K6274 was taken as the room temperature adhesive strength.
[0113] <Viscoelasticity property evaluation test> For Examples 2-10 and Comparative Examples 2-5, test pieces with a thickness of 1 mm, width of 3 mm, and length of 20 mm were cut out from each rubber composition. The storage modulus (E') and loss factor (tan δ) of the test pieces were measured at 23°C and 120°C with a strain amplitude of 0.1% and a frequency of 10 Hz. A dynamic viscoelasticity measuring device Rheogel-E4000 manufactured by UBM was used for the measurements.
[0114] (Test evaluation results) The test results are shown in Table 3. According to the results of the adhesion evaluation test, it is found that Examples 2-1 to 2-9 have significantly higher room temperature adhesive strength than Comparative Examples 2-1 to 2-4. Therefore, it is found that the rubber composition containing a carboxyl group-containing oil has excellent adhesive strength to the RFL adhesive. Furthermore, it is found that, among Examples 2-1 to 2-9, Examples 2-6 to 2-9 containing a carbodiimide have higher room temperature adhesive strength than Examples 2-1 to 2-5 not containing a carbodiimide. Therefore, it is found that the rubber composition further containing a carbodiimide has better adhesive strength to the RFL adhesive.
[0115] According to the results of the viscoelasticity property evaluation test, it is found that Example 2-10 has lower storage modulus (E') and loss factor (tan δ) than Comparative Example 2-5. [Industrial Applicability]
[0116] The present invention is useful in the technical fields of a rubber composition, a method for producing the same, and a rubber product using the same. [Explanation of symbols]
[0117] 10. Adhesion test specimen 11 Twisted Yarn 12 Rubber plate
Claims
1. A rubber composition comprising a carboxylic acid-modified ethylene-α-olefin elastomer and a carboxyl group-containing oil, The carboxyl group-containing oil includes a carboxylic acid-modified oil, A rubber composition in which the oil before modification in the carboxylic acid modified oil contains paraffin oil and naphthene oil.
2. The rubber composition according to claim 1, The rubber composition, wherein the carboxylic acid modified oil comprises maleic anhydride modified oil or maleic acid modified oil.
3. The rubber composition according to claim 1 or 2, The rubber composition, wherein the oil before modification further contains an aromatic oil.
4. The rubber composition according to any one of claims 1 to 3, The rubber composition, wherein the carboxylic acid-modified ethylene-α-olefin elastomer comprises a maleic anhydride-modified ethylene-α-olefin elastomer or a maleic acid-modified ethylene-α-olefin elastomer.
5. The rubber composition according to any one of claims 1 to 4, The rubber composition further comprises a carbodiimide.
6. The rubber composition according to any one of claims 1 to 5, The rubber composition further comprises a non-carboxylic acid modified ethylene-α-olefin elastomer.
7. A rubber product having a main body formed from the rubber composition according to any one of claims 1 to 6.
8. A step of modifying an ethylene-α-olefin elastomer with a carboxylic acid to prepare a carboxylic acid modified ethylene-α-olefin elastomer; a step of kneading the prepared carboxylic acid-modified ethylene-α-olefin elastomer with a carboxyl group-containing oil; Including, The carboxyl group-containing oil includes a carboxylic acid-modified oil, The method for producing a rubber composition, wherein the oil before modification in the carboxylic acid modified oil contains paraffin oil and naphthenic oil.
9. The method for producing a rubber composition according to claim 8, The method for producing a rubber composition further comprises a step of modifying an oil with a carboxylic acid to prepare a carboxylic acid modified oil to be contained in the carboxyl group-containing oil.
10. The method for producing a rubber composition according to claim 9, The ethylene-α-olefin elastomer and the oil are kneaded while being modified with a carboxylic acid, thereby simultaneously carrying out a step of preparing the carboxylic acid-modified ethylene-α-olefin elastomer and a step of preparing the carboxylic acid-modified oil in a single step.
11. The method for producing a rubber composition according to claim 9, The method for producing a rubber composition, wherein the step of preparing the carboxylic acid-modified ethylene-α-olefin elastomer and the step of preparing the carboxylic acid-modified oil are carried out separately as mutually independent steps.
Citation Information
Patent Citations
Vulcanized rubber composition
JP1987041245A
Soundproof panel
JP1994049813A
Thermoplastic elastomer composition
JP2004269608A
Hot melt adhesive
WO2018074070A1
Crosslinked rubber composition and rubber product using same
WO2020122054A1