Copolymer polyester and molded article made of same and method for producing same
A copolymerized polyester with specific diol and triol units, utilizing biomass-derived materials, addresses impact resistance and environmental impact issues, offering improved hardness and long-term storage resistance.
Patent Information
- Application Number
- JP2020150544
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-08
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-09-08
AI Technical Summary
Existing copolyesters used in extrusion blow molding lack sufficient impact resistance and hardness during long-term storage, and their production does not adequately address environmental impact reduction by utilizing biomass-derived materials.
A copolymerized polyester with specific ratios of diol and triol units, including biomass-derived ethylene glycol and terephthalic acid, is developed, achieving a biomass content of 5% to 40% and optimized intrinsic viscosity for improved impact resistance and hardness.
The copolymerized polyester exhibits excellent drawdown properties, good hardness, and impact resistance during long-term storage, while reducing the environmental impact by minimizing petroleum resource usage and greenhouse gas emissions.
Smart Images

Figure 0007590834000001 
Figure 0007590834000002 
Figure 0007590834000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a copolymer polyester characterized by having a biomass plastic content of 5% or more and 40% or less, suitable as a raw material for extrusion blow molding, a production method thereof, and a molded article made of the same. [Background technology]
[0002] Polyester resins such as polyethylene terephthalate resins are excellent in transparency, mechanical properties, gas barrier properties, flavor barrier properties, etc. Furthermore, polyester resins are less likely to leave residual monomers or harmful additives when molded into articles, and are also excellent in hygiene and safety. For this reason, polyester resins have been widely used in recent years to take advantage of these properties as hollow containers for filling with juices, soft drinks, seasonings, oils, cosmetics, detergents, etc., as a replacement for the conventionally used polyvinyl chloride resins.
[0003] A known molding method for producing hollow molded products made of polyester resin is extrusion blow molding, in which molten plasticized resin is extruded through a die orifice as a cylindrical parison, and while the parison is in a softened state, it is sandwiched between a mold and air or other fluid is blown into the interior to form the product. This method is simpler than injection blow molding, and does not require advanced technology for making and molding the mold, so the equipment costs and mold manufacturing costs are low, making it suitable for high-mix, low-volume production. Another advantage is that it is possible to produce molded products with complex shapes, such as thin, deep, large, and with handles.
[0004] Patent Document 1 describes that, as a copolymer polyester suitable for extrusion blow molding, when a polyester is produced using a dicarboxylic acid component mainly composed of terephthalic acid or an ester-forming derivative thereof and a diol component mainly composed of ethylene glycol, the diol component contains a specific diol component having a benzene nucleus in a specific ratio, and further contains a specific triol component having a benzene nucleus in a specific ratio, a copolymer polyester having high melt viscosity and excellent melt moldability, and further excellent in transparency, mechanical properties such as impact resistance, heat resistance, and the like is obtained.
[0005] In recent years, there has been an increasing demand for biomass polyester resin compositions using plant-derived raw materials such as carbon-neutral biomass, aiming at a recycling-oriented society. Patent Document 2 describes a method for producing bio-based PET and a method for producing a container using bio-based PET, in which monoethylene glycol and terephthalic acid are formed from a bio-based material, the bio-based PET is melt-polymerized, and then solid-phase polymerized to produce a container by extrusion blow molding. Patent Document 3 describes a biomass polyester resin composition that is comparable in physical properties, such as mechanical properties, to polyesters produced from conventional raw materials obtained from fossil fuels, and contains 50 to 95% by mass of polyester, the diol unit of which is biomass-derived ethylene glycol, and the dicarboxylic acid unit is fossil fuel-derived dicarboxylic acid, relative to the entire resin composition, and further contains additives such as plasticizers. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-208818 [Patent Document 2] JP 2012-519748 A [Patent Document 3] JP 2012-097163 A Summary of the Invention [Problem to be solved by the invention]
[0007] Containers formed by extrusion blow molding are widely used as containers suitable for storing medicines, cosmetics, etc. Such containers are required to have impact resistance when dropped and hardness that prevents the container surface from being scratched when colliding with surrounding objects. However, the copolymer polyester of Patent Document 1 has room for improvement in impact resistance and hardness during long-term storage of the molded product, and only polyesters produced from raw materials obtained from fossil fuels have been considered, and raw materials derived from biomass have not been considered, and no consideration has been given to reducing the environmental load of reducing the amount of petroleum resources used or suppressing greenhouse gas emissions. In addition, the bio-based PET of Patent Document 2 is produced by forming monoethylene glycol and terephthalic acid from bio-based materials, but only the reduction of the environmental load has been considered, and the impact resistance of the molded product is insufficient for practical use, and the impact resistance during long-term storage is also poor. Patent Document 3 discusses a polyester in which the diol unit is ethylene glycol derived from biomass and the dicarboxylic acid unit is dicarboxylic acid derived from fossil fuels. However, since 10 parts by mass of porous silica was blended in order to impart strength to the polyester, the polyester was opaque and the molded product had low impact resistance.
[0008] An object of the present invention is to provide a copolymer polyester which has the effect of reducing the environmental load by reducing the consumption of petroleum resources and suppressing greenhouse gas emissions, while being capable of producing molded articles which have excellent parison drawdown properties, hardness, and good impact resistance and color tone during long-term storage, and which can be suitably used as a raw material for the production of thick-walled molded articles and extrusion blow molding, and which further has the effect of reducing the environmental load, and a method for producing the same. [Means for solving the problem]
[0009] Means for Solving the Problems The present inventors conducted intensive research in light of the above problems and discovered that a copolymerized polyester having a biomass plastic content within a specific range and containing specific diol units and triol units having a benzene nucleus in specific proportions can suppress the decrease in impact resistance during long-term storage, thereby completing the present invention. That is, according to the present invention, the above object is to [1] A copolymerized polyester mainly composed of dicarboxylic acid units mainly composed of terephthalic acid units, diol units (α) mainly composed of ethylene glycol units and diol units (I) represented by the following formula (I), and triol units (β) including triol units (II) represented by the following formula (II), characterized in that the copolymerized polyester contains 1 to 15 mol % of diol units (I) based on the total number of moles of the diol units (α) and the triol units (β) and contains 0.005 to 1 mol % of triol units (II) based on the total number of moles of the diol units (α) and the triol units (β), and has a biomass plastic degree of 5% or more and 40% or less; [ka] [In the formula, A represents a group represented by -CH2CH2- or -CH(CH3)CH2-, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and j and k each independently represent an integer of 1 to 8.] [ka] [In the formula, A represents a group represented by -CH2CH2- or -CH(CH3)CH2-, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and p, q and r each independently represent an integer of 1 to 8] [2] The copolymer polyester according to [1], wherein the ethylene glycol units include ethylene glycol units derived from biomass-derived ethylene glycol, and the content of the ethylene glycol units derived from biomass-derived ethylene glycol in the total ethylene glycol units is 20% by mass or more and 100% by mass or less; [3] The copolymer polyester according to [1] or [2], characterized in that the ethylene glycol unit derived from the biomass-derived ethylene glycol is an ethylene glycol unit derived from ethylene glycol made from sugarcane molasses. [4] The copolymer polyester according to any one of [1] to [3], wherein the terephthalic acid units contain terephthalic acid units derived from biomass-derived terephthalic acid, and the content of the terephthalic acid units derived from biomass-derived terephthalic acid in all the terephthalic acid units is 15 mass% or less; [5] The copolymer polyester according to any one of [1] to [4], wherein the terephthalic acid units are composed solely of terephthalic acid units derived from terephthalic acid derived from a fossil fuel; [6] any one of the copolymer polyesters [1] to [5], characterized in that the intrinsic viscosity is 0.6 to 1.5 dl / g; [7] Molded articles made of any one of the copolymer polyesters [1] to [6]; [8] The molded article according to [7], which is an extrusion blow molded article; [9] A method for producing a molded article, comprising a step of extrusion blow molding any one of the copolymer polyesters described in [1] to [6];
[10] A method for producing a copolymerized polyester according to any one of [1] to [6], comprising esterifying or transesterifying a reaction raw material containing a dicarboxylic acid mainly composed of terephthalic acid or an ester-forming derivative thereof, ethylene glycol, a diol (III) represented by the following formula (III), and a triol (IV) represented by the following formula (IV), melt-polycondensing the reaction raw material to form a polyester prepolymer, and solid-phase polymerizing the polyester prepolymer, wherein the content of the diol (III) is 1.9 parts by mass to 15 parts by mass relative to 100 parts by mass of dicarboxylic acid, the content of the triol (IV) is 0.005 to 2 parts by mass relative to 100 parts by mass of dicarboxylic acid, the content of biomass-derived terephthalic acid or an ester-forming derivative thereof in the terephthalic acid or an ester-forming derivative thereof is 15% by mass or less, and the content of biomass-derived ethylene glycol in the ethylene glycol is 20% by mass or more and 100% by mass or less; [ka] [In the formula, A represents a group represented by the formula: -CH2CH2- or the formula: -CH(CH3)CH2-, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and j and k each independently represent an integer of 1 to 8.] [ka] [In the formula, A represents a group represented by the formula: -CH2CH2- or the formula: -CH(CH3)CH2-; B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-); and p, q and r each independently represent an integer of 1 to 8.]
[11] The method for producing a copolymerized polyester according to
[10] , wherein the biomass-derived ethylene glycol is ethylene glycol derived from sugar cane molasses; This is solved by providing Effect of the Invention
[0010] The copolymerized polyester of the present invention has a biomass plastic content of 5% to 40%, and has the effect of reducing the environmental load by reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases, while providing molded products that are excellent in parison drawdown during extrusion blow molding, and have good hardness, impact resistance during long-term storage, and color tone. According to the production method of the present invention, such polyester resin pellets can be easily produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Copolymer polyester> The copolymer polyester of the present invention is a copolymer polyester mainly composed of dicarboxylic acid units mainly composed of terephthalic acid units, diol units (α) mainly composed of ethylene glycol units and diol units (I) represented by the following formula (I), and triol units (β) including triol units (II) represented by the following formula (II), characterized in that the copolymer polyester contains 1 to 15 mol % of diol units (I) based on the total number of moles of the diol units (α) and the triol units (β), contains 0.005 to 1 mol % of triol units (II) based on the total number of moles of the diol units (α) and the triol units (β), and has a biomass plastic degree of 5% or more and 40% or less.
[0012] The dicarboxylic acid units of the copolymer polyester of the present invention are mainly composed of terephthalic acid units. The content of terephthalic acid units relative to the total of dicarboxylic acid units is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 95 mol% or more, and it is most preferable that the dicarboxylic acid units in the copolymer polyester are substantially only terephthalic acid units. If the content of terephthalic acid units is less than 80 mol%, the melting point may decrease and the impact resistance during long-term storage may decrease.
[0013] For the terephthalic acid units constituting the copolymerized polyester of the present invention, terephthalic acid units derived from biomass-derived terephthalic acid can be used from the viewpoint of reducing the use of petroleum resources and reducing the environmental load by suppressing the emission of greenhouse gases. The content of biomass-derived terephthalic acid in the total terephthalic acid or its ester-forming derivatives used as the raw material is preferably 15% by mass or less, more preferably 8% by mass or less, and most preferably, only fossil fuel-derived terephthalic acid is used without using biomass-derived terephthalic acid. If the content of biomass-derived terephthalic acid exceeds 15% by mass, the impact resistance during long-term storage may decrease.
[0014] The diol unit (α) of the copolymerized polyester of the present invention is mainly composed of ethylene glycol units and diol units (I) represented by the following formula (I). The content ratio of ethylene glycol units is preferably 75 to 98 mol% based on the total number of moles of the diol units (α) and the triol units (β). When the content ratio of the ethylene glycol units is less than 75 mol%, it becomes difficult to increase the solid-phase polymerization temperature, the productivity decreases, and the color tone of the obtained molded article deteriorates. The content ratio of the ethylene glycol units is more preferably 90 mol% or more. On the other hand, when the content ratio of the ethylene glycol units exceeds 98 mol%, the impact resistance, impact resistance during long-term storage, and hardness of the obtained molded article decrease. The content ratio of the ethylene glycol units is more preferably 97 mol% or less.
[0015] As the ethylene glycol unit constituting the copolymerized polyester of the present invention, from the viewpoint of the effect of reducing the environmental load by reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases, ethylene glycol units derived from biomass-derived ethylene glycol are preferred. The content ratio of the ethylene glycol unit derived from biomass-derived ethylene glycol is proportional to the content ratio of the ethylene glycol derived from biomass in the raw ethylene glycol. The content ratio of the ethylene glycol unit derived from biomass-derived ethylene glycol is preferably 20% by mass or more and 100% by mass or less. If the lower limit of the content ratio of the ethylene glycol unit derived from biomass-derived ethylene glycol is less than 20% by mass, the effect of reducing the environmental load by reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases decreases. The ethylene glycol unit derived from biomass-derived ethylene glycol is more preferably 40% by mass or more, and particularly preferably 75% by mass or more, because it has the effect of reducing the environmental load by reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases, and the impact resistance of the obtained molded product, and the impact resistance and hardness during long-term storage are also good. There is no particular upper limit to the content ratio of ethylene glycol units derived from biomass-derived ethylene glycol, but it is most preferable that the ethylene glycol units are solely derived from biomass-derived ethylene glycol, because this has the effect of reducing the environmental load by reducing the amount of petroleum resources used and suppressing greenhouse gas emissions, and because the obtained molded article has good impact resistance, and good impact resistance and hardness during long-term storage.
[0016] The ethylene glycol unit constituting the copolymerized polyester is preferably an ethylene glycol unit derived from ethylene glycol made from sugarcane molasses, which will be described later. By using ethylene glycol made from sugarcane molasses, the impact resistance and hardness of the resulting molded product during long-term storage are improved.
[0017] The diol unit (α) constituting the copolymer polyester of the present invention contains a diol unit (I) represented by the following formula (I). [ka] [In the formula, A represents a group represented by -CH2CH2- or -CH(CH3)CH2-, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and j and k each independently represent an integer of 1 to 8.] The triol unit (β) constituting the copolymer polyester of the present invention contains a triol unit (II) represented by the following formula (II). [ka] [In the formula, A represents a group represented by -CH2CH2- or -CH(CH3)CH2-, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and p, q and r each independently represent an integer of 1 to 8]
[0018] In the diol unit (I) and the triol unit (II), the group A is a group represented by the formula: -CH2CH2- (ethylene group) or a group represented by the formula: -CH(CH3)CH2- (1,2-propylene group). In the copolymerized polyester of the present invention, all of the groups A may be ethylene groups, all of the groups A may be 1,2-propylene groups, or a part of the groups A may be ethylene groups and the remaining groups A may be 1,2-propylene groups. Among these, it is preferable that the group A is an ethylene group, since the molded article obtained from the copolymerized polyester is excellent in impact resistance, impact resistance during long-term storage, transparency, and hardness.
[0019] In addition, the group B in the diol unit (I) and the triol unit (II) is a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom, or a direct bond (-). When the group B is a divalent hydrocarbon group, it is preferably an alkylene group, an alkylidene group, or a divalent aromatic group having 1 to 8 carbon atoms, and specific examples thereof include a methylene group, an ethylene group, an ethylidene group, a propylene group, a propylidene group, a trimethylene group, an isopropylidene group, a butylidene group, an ethylethylene group, a tetramethylene group, a 1-methylpropylidene group, a 1,2-dimethylethylene group, a pentylidene group, a 1-methylbutylidene group, a pentamethylene group, a 1-ethyl-2-methylethylene group, a 1,3-dimethyltrimethylene group, a 1-ethyl Examples of such groups include a phenylpropylidene group, a trimethylethylene group, an isopropylmethylene group, a 1-methylbutylidene group, a 2,2-dimethylpropylidene group, a hexamethylene group, a 1-ethylbutylidene group, a 1,2-diethylethylene group, a 1,3-dimethylbutylidene group, an ethyltrimethylethylene group, a heptamethylene group, an octamethylene group, a 1,1-cyclopentylidene group, a 1,1-cyclohexylidene group, a 1,1-cycloheptylidene group, a 1,1-cyclooctylidene group, a benzylidene group, and a 1,1-phenylethylidene group.
[0020] In the copolymer polyester of the present invention, the groups B in the diol units (I) and triol units (II) present in the copolymer polyester may all be the same or different. Among them, in the copolymer polyester of the present invention, it is preferred that the group B in the diol units (I) and triol units (II) is an isopropylidene group, a sulfonyl group and / or a 1,1-cyclohexylidene group, from the viewpoint of excellent impact resistance, impact resistance during long-term storage, transparency and hardness of a molded article obtained from the copolymer polyester.
[0021] Furthermore, j and k in the diol unit (I) are each independently an integer of 1 to 8, and j and k may be the same or different numbers. Of these, it is preferred that j and k are each independently 1 or 2, in that a molded article obtained from the copolymer polyester will be excellent in impact resistance, impact resistance during long-term storage, transparency, and hardness.
[0022] In the copolymer polyester of the present invention, from the viewpoints of impact resistance, impact resistance transparency and hardness during long-term storage of a molded article obtained from the copolymer polyester, it is particularly preferable that the diol unit (I) is a group represented by the following formula (V). [ka]
[0023] In the copolymer polyester of the present invention, p, q and r in the triol unit (II) are each independently an integer of 1 to 8, and therefore p, q and r may be the same or different numbers. Among these, it is preferred that p, q and r are each independently 1 or 2, in view of excellent impact resistance, impact resistance during long-term storage, transparency and hardness of a molded article obtained from the copolymer polyester.
[0024] In the copolymer polyester of the present invention, the triol unit (II) is particularly preferably a group represented by the following formula (VI), from the viewpoint of excellent impact resistance, impact resistance during long-term storage, transparency, and hardness of a molded article obtained from the copolymer polyester. [ka]
[0025] The copolymer polyester of the present invention contains 1 to 15 mol % of diol units (I) based on the total number of moles of diol units (α) and triol units (β) constituting the copolymer polyester. If the content of diol units (I) is less than 1 mol %, the solid-phase polymerization rate during the production of the copolymer polyester slows down, and the melting point of the resulting copolymer polyester increases, so that the cycle time during extrusion blow molding or other melt molding is extended, and the productivity during the production of molded products decreases and the impact resistance decreases. On the other hand, if the content of diol units (I) exceeds 15 mol %, the melting point of the polyester prepolymer, which is an intermediate product during the production of the copolymer polyester, decreases, and there is a risk that the chips of the polyester prepolymer will stick together during preliminary crystallization or solid-phase polymerization in the polymerization process, making solid-phase polymerization impossible. Furthermore, there is a risk that the color tone of the resulting copolymer polyester will be poor. Based on the total number of moles of all diols and triols, the lower limit of the content of diol units (I) is preferably 2 mol % or more, more preferably 2.5 mol % or more. The upper limit of the content of the diol unit (I) is preferably 10 mol % or less, more preferably 7 mol % or less.
[0026] The copolymer polyester of the present invention contains 0.005 to 1 mol % of triol unit (II) based on the total mole number of diol unit (α) and triol unit (β) constituting the copolymer polyester. If the content of triol unit (II) is less than 0.005 mol %, the crosslinked structure portion in the copolymer polyester is small, the hardness of the molded product is insufficient, and the surface of the molded product is easily scratched. In addition, the polymerization rate of solid-phase polymerization during the production of the copolymer polyester is reduced, resulting in poor productivity.
[0027] On the other hand, if the content of the triol unit (II) exceeds 1 mol %, the crosslinked structure portion in the copolymer polyester becomes too large, so that the impact resistance of the molded article and the impact resistance during long-term storage are both reduced.
[0028] The lower limit of the content of the triol unit (II) is more preferably 0.01 mol% or more based on the total number of moles of the diol unit (α) and the triol unit (β). The upper limit of the content of the triol unit (II) is preferably 0.5 mol% or less, particularly preferably 0.1 mol% or less. When the content of the triol unit is within the above range, the melt viscosity is sufficiently high, and the melt moldability such as extrusion blow molding is improved, and a molded product with excellent mechanical strength can be obtained, and the productivity of the copolymerized polyester itself is also high.
[0029] In the copolymer polyester of the present invention, the molar ratio of the contents of the diol unit (I) and the triol unit (β) constituting the copolymer polyester (diol unit (I) / triol unit (β)) is preferably 35 to 400, from the viewpoint of excellent impact resistance and hardness of the molded article obtained from the copolymer polyester. If the lower limit of the molar ratio of the contents of the diol unit (I) and the triol unit (β) is less than 35, the hardness is high, but the impact resistance is low, resulting in a hard and brittle property, and there is a possibility that the desired molded article cannot be obtained. The molar ratio of the contents of the diol unit (I) and the triol unit (β) is more preferably 50 or more, and even more preferably 65 or more. If the upper limit of the molar ratio of the contents of the diol unit (I) and the triol unit (β) exceeds 400, the impact resistance is high, but the hardness is low, and the surface of the obtained molded article may be easily scratched. The molar ratio of the contents of the diol units (I) and the triol units (β) is more preferably 350 or less, further preferably 300 or less, and particularly preferably 280 or less.
[0030] In terms of impact resistance and hardness of a molded article obtained from the copolymerized polyester, the copolymerized polyester preferably has a molar ratio (ethylene glycol unit / triol unit (β)) of the content of the ethylene glycol unit and the triol unit (β) constituting the copolymerized polyester of 500 to 15,000. If the lower limit of the molar ratio of the content of the ethylene glycol unit and the triol unit (β) is less than 500, the hardness is high, but the impact resistance is low, resulting in a hard and brittle property, and there is a risk that the desired molded article cannot be obtained. The molar ratio of the content of the ethylene glycol unit and the triol unit (β) is more preferably 700 or more, further preferably 800 or more, and particularly preferably 2,000 or more. If the upper limit of the molar ratio of the content of the ethylene glycol unit and the triol unit (β) exceeds 15,000, the impact resistance is high, but the hardness is low, and the surface of the obtained molded article may be easily scratched. The molar ratio of the content of ethylene glycol units to the triol units (β) is more preferably 13,000 or less, and further preferably 10,000 or less.
[0031] The copolymer polyester of the present invention may contain, as necessary, structural units derived from other bifunctional compounds, in addition to the above-mentioned terephthalic acid units, ethylene glycol units, diol units (I), and triol units (II), as long as the structural units are 10 mol % or less based on the total structural units. Examples of structural units derived from other bifunctional compounds include aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, naphthalene dicarboxylic acid, biphenyl dicarboxylic acid, diphenyl ether dicarboxylic acid, diphenyl sulfone dicarboxylic acid, diphenyl ketone dicarboxylic acid, and sodium sulfoisophthalate; aliphatic dicarboxylic acids such as malonic acid, succinic acid, adipic acid, azelaic acid, and sebacic acid; alicyclic dicarboxylic acids such as decalin dicarboxylic acid and cyclohexane dicarboxylic acid; glycolic acid, hydroxyacrylic acid, hydroxypropionic acid, asiatic acid, quinocalic acid, hydroxybenzoic acid, mandelic acid, and methyl methacrylate. Examples of the structural units include structural units derived from bifunctional components such as hydroxycarboxylic acids such as lactic acid, aliphatic lactones such as ε-caprolactone, aliphatic diols such as trimethylene glycol, tetramethyl glycol, hexamethylene glycol, neopentyl glycol, diethylene glycol, and polyethylene glycol, aromatic diols such as hydroquinone, catechol, naphthalene diol, resorcin, bisphenol A, an ethylene oxide adduct of bisphenol A, bisphenol S, and an ethylene oxide adduct of bisphenol S, and alicyclic diols such as cyclohexane dimethanol. In addition, the copolymerized polyester of the present invention may contain structural units derived from polyfunctional compounds such as polycarboxylic acids such as trimellitic acid, trimesic acid, pyromellitic acid, and tricarballylic acid, and polyhydric alcohols such as trimethylolpropane and pentaerythritol, as long as the amount of the structural units is 0.1 mol % or less based on the total structural units in the copolymerized polyester.
[0032] The biomass plastic degree of the copolymer polyester of the present invention is 5% or more and 40% or less. Here, the biomass plastic degree means the ratio of units composed of raw materials derived from biomass in the copolymer polyester. The biomass plastic degree can be calculated by the method described in the examples described later. From the viewpoint of the effect of reducing the environmental load by reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases, a higher biomass plastic degree is preferable, but if it exceeds 40%, the impact resistance during long-term storage may decrease. The upper limit of the biomass plastic degree is preferably 35% or less, more preferably 30% or less, from the viewpoint of the impact resistance and hardness during long-term storage of the copolymer polyester. The lower limit of the biomass plastic degree is more preferably 10% or more, more preferably 15% or more, from the viewpoint of the effect of reducing the environmental load by reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases.
[0033] In addition, the copolyester of the present invention can be measured for its bio-based carbon content in the total carbon of the components constituting the copolyester by measuring the bio-based carbon content by the 14C method specified in ISO16620-2:2019. From the viewpoint of reducing the amount of petroleum resources used and reducing the environmental load by suppressing greenhouse gas emissions, the bio-based carbon content is more preferably 5% or more, and even more preferably 15% or more. The upper limit of the bio-based carbon content of the copolyester of the present embodiment is preferably 30% or less, and more preferably 20% or less, from the viewpoint of the impact resistance and hardness during long-term storage of the copolyester.
[0034] The intrinsic viscosity of the copolymerized polyester of the present invention may vary depending on the type of melt molding method of the copolymerized polyester, but when used in melt molding involving melt extrusion, particularly extrusion blow molding, it is preferably 0.6 to 1.5 dl / g, and more preferably 0.9 to 1.4 dl / g in terms of the mechanical properties and appearance of the resulting extrusion blow molding, and the productivity during the production of the molded product. In particular, when extrusion blow molding is performed, if the intrinsic viscosity of the copolymerized polyester is less than 0.6 dl / g, the drawdown of the parison during extrusion blow molding becomes large, which tends to cause molding defects, and the mechanical properties such as tensile strength and impact resistance of the resulting molded product tend to decrease. On the other hand, if the intrinsic viscosity of the copolymerized polyester is greater than 1.5 dl / g, the melt viscosity becomes too high, which tends to cause molding problems such as poor appearance of the resulting molded product, and uneven extrusion amount due to high torque during extrusion. In addition, the time required to extrude a given amount of copolymerized polyester becomes long, which tends to cause a decrease in productivity of the molded product.
[0035] When the copolymerized polyester of the present invention is used to produce molded products such as sheets and films by extrusion molding such as the T-die method or the inflation method, there is no occurrence of drawdown, neck-in, film vibration, or unmelted particles, and high-quality sheets or films can be produced with good productivity. When the thus obtained sheet or film is used for secondary processing such as thermoforming, when a deep-draw molded product or a large molded product is molded, the drawdown is small, the degree of crystallization is good, and thickness unevenness and whitening are unlikely to occur in the process of applying an external force such as vacuum suction or compressed air, and the desired molded product can be obtained with good formability.
[0036] Among the extrusion moldings, the copolymer polyester of the present invention is particularly suitable for use in extrusion blow molding. The method of extrusion blow molding is not particularly limited, and can be carried out in the same manner as the conventionally known extrusion blow molding. For example, the copolymer polyester pellets of the present invention are melt-extruded to form a cylindrical parison, and while the parison is in a softened state, the parison is sandwiched between blow molds and gas such as air is blown in to expand the parison into a predetermined hollow shape that conforms to the shape of the mold cavity. When the copolymer polyester pellets of the present invention are used, the drawdown property of the extruded parison is good, and hollow molded products can be produced with good productivity.
[0037] The molded article thus obtained has excellent transparency, good appearance and color tone, and high mechanical strength, especially impact resistance. Furthermore, it has excellent properties such as gas barrier property, flavor barrier property, moisture resistance, and chemical resistance, so it can be used for various purposes. It can also be made into a molded article having a laminated structure with other thermoplastic resins.
[0038] In addition, the copolymer polyester of the present invention preferably has a glass transition temperature (Tg) of 60° C. or higher, and more preferably has a glass transition temperature of 70° C. or higher in order to prevent shrinkage of molded articles obtained by extrusion blow molding or other melt molding. If the copolymer polyester has a glass transition temperature of less than 60° C., the molded article, particularly an extrusion blow molded article, may shrink due to relaxation of residual stress after being removed from the mold, which may impair the appearance of the molded article. From the viewpoint of the impact resistance of molded articles obtained by extrusion blow molding or other melt molding, the glass transition temperature is preferably 85° C. or lower. If the glass transition temperature exceeds 85° C., the impact resistance of molded articles obtained by extrusion blow molding or other melt molding may decrease.
[0039] The copolymerized polyester of the present invention can be produced with good productivity in a short time by subjecting reactive raw materials including a dicarboxylic acid mainly composed of terephthalic acid or an ester-forming derivative thereof, ethylene glycol, a diol (III) represented by the following formula (III), and a triol (IV) represented by the following formula (IV) to an esterification reaction or an ester exchange reaction, followed by melt polycondensation to form a polyester prepolymer, and then solid-phase polymerization of the polyester prepolymer. [ka] [In the formula, A represents a group represented by the formula: -CH2CH2- or the formula: -CH(CH3)CH2-, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and j and k each independently represent an integer of 1 to 8.] [ka] [In the formula, A represents a group represented by the formula: -CH2CH2- or the formula: -CH(CH3)CH2-; B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-); and p, q and r each independently represent an integer of 1 to 8.]
[0040] Terephthalic acid or its ester-forming derivative used as the reaction raw material of the present invention can be biomass-derived terephthalic acid or its ester-forming derivative. Biomass-derived terephthalic acid or its ester-forming derivative is terephthalic acid or its ester-forming derivative produced using biomass resources as raw materials. Biomass resources include renewable carbon-neutral organic resources produced from water and carbon dioxide using solar energy through the photosynthetic action of plants, specifically products made by processing the stored materials converted into starch, cellulose, etc., and are resources other than fossil resources. Biomass resources are classified into three types based on the form of generation: waste, unused, and resource crops. Specific examples of biomass resources include cellulosic crops (pulp, kenaf, wheat straw, rice straw, waste paper, papermaking residues, etc.), wood, charcoal, compost, natural rubber, cotton, sugarcane, soybean pulp, oils and fats (rapeseed oil, cottonseed oil, soybean oil, coconut oil, castor oil, etc.), carbohydrate crops (corn, potatoes, wheat, rice, rice husks, rice bran, old rice, cassava, sago palm, etc.), bagasse, buckwheat, soybeans, essential oils (pine oil, orange oil, eucalyptus oil, etc.), black pulp liquor, and vegetable oil residue.
[0041] In the present invention, as long as terephthalic acid or its ester-forming derivatives can be produced from biomass resources, the production method is not particularly limited, and examples thereof include known methods such as biological treatment methods using the action of microorganisms such as fungi and bacteria, chemical treatment methods using acids, alkalis, catalysts, thermal energy, light energy, etc., and physical treatment methods such as pulverization, compression, microwave treatment, and electromagnetic wave treatment. For example, a method for producing terephthalic acid or its ester-forming derivatives from bioethanol obtained from sugars, etc., includes a method in which bioethanol is catalytically converted into an aromatic mixture on a zeolite (H-ZSM-5 type, etc.) catalyst, the aromatic mixture is purified by distillation, etc. to obtain paraxylene, and the obtained paraxylene is oxidized using a catalyst to obtain terephthalic acid, but is not limited thereto.
[0042] Specific examples of raw materials for terephthalic acid or its ester-forming derivatives obtained from biomass resources include alkanes such as methane, alkenes such as ethylene, alkynes such as acetylene, sugars such as xylose, glucose, cellulose, and hemicellulose, alcohols such as methanol, ethanol, propanol, butanol, and glycerol, lignin, isoprene, turpentine oil, α-pinene, limonene, paracymene, 1,8-cineole, linalool, bisabolane, and caryophyllene, terpene compounds such as unsaturated fatty acids such as oleic acid, and linear saturated dibasic acids such as sebacic acid. Specific examples of terephthalic acid or its ester-forming derivatives produced from biomass resources include terephthalic acid, dimethyl terephthalate, diethyl terephthalate, diisopropyl terephthalate, and di-n-propyl terephthalate.
[0043] The method for producing terephthalic acid or its ester-forming derivatives of the present invention is described below. As raw materials for forming the aromatic moiety, olefins, aliphatic alcohols, cyclic terpenes, unsaturated fatty acids, linear saturated dibasic acids, etc., synthesized from biomass resources can be used. Specific examples of olefins include ethylene, propylene, butene, 1,2-butadiene, 1,3-butadiene, 1,3-pentadiene, 1,4-pentadiene, and isooctene. Specific examples of aliphatic alcohols include alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, pentanol, hexanol, octanol, decanol, allyl alcohol, benzyl alcohol, ethylene glycol, propylene glycol, butylene glycol (tetramethylene glycol, butanediol), glycerol, diglycerol, pentaerythritol, dipentaerythritol, and terpene alcohol compounds such as linalool and geraniol. Specific examples of cyclic terpenes include α-pinene, β-pinene, limonene, paracymene, 1,8-cineole, and 1,4-cineole. Specific examples of unsaturated fatty acids include oleic acid. Specific examples of linear saturated dibasic acids include sebacic acid. When producing aromatic compounds having two or more rings or aromatic compounds having multiple condensed rings, ortho-xylene and meta-xylene can also be used. Among these, cyclic terpenes are preferred, and para-cymene is more preferred.
[0044] Para-cymene has an aromatic ring in its structure, and terephthalic acid can be obtained by oxidizing the alkyl group directly bonded to the aromatic ring by a commonly used oxidation reaction. Furthermore, the obtained terephthalic acid can be esterified with a lower alcohol such as methanol, ethanol, propanol, or butanol in the presence of an acid catalyst or the like by a commonly used method to obtain an ester-forming derivative of terephthalic acid. When terephthalic acid and a lower alcohol are esterified, it may be necessary to select conditions under which the reaction is performed under high temperature and high pressure conditions. In such a case, a method may be adopted in which the esterification reaction is first performed with a dihydroxy compound such as ethylene glycol, and then the reaction is performed with the above-mentioned lower alcohol in the presence of an ester exchange reaction catalyst. This method of producing via para-cymene can produce terephthalic acid relatively easily, and therefore can be preferably adopted for producing an ester-forming derivative of terephthalic acid.
[0045] The content of biomass-derived terephthalic acid or its ester-forming derivative in the terephthalic acid or its ester-forming derivative used as the raw material in the present invention is preferably 15% by mass or less. The use of biomass-derived terephthalic acid or its ester-forming derivative has the effect of reducing the environmental load by reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases, but if the content exceeds 15% by mass, there is a risk of the impact resistance decreasing during long-term storage. It is more preferable that the biomass-derived terephthalic acid or its ester-forming derivative is 8% by mass or less, and it is most preferable to use only fossil fuel-derived terephthalic acid without using biomass-derived terephthalic acid.
[0046] The ethylene glycol used as the reaction raw material in the present invention can be ethylene glycol derived from biomass. The ethylene glycol derived from biomass is ethylene glycol produced using a biomass resource as a raw material, and the biomass resource can be the same as that used for the above-mentioned terephthalic acid or its ester-forming derivative.
[0047] In the present invention, the method of production is not particularly limited as long as ethylene glycol can be produced from biomass resources, but examples of the method include known methods such as biological treatment methods using the action of microorganisms such as fungi and bacteria, chemical treatment methods using acids, alkalis, catalysts, thermal energy, light energy, and physical treatment methods such as pulverization, compression, microwave treatment, and electromagnetic wave treatment, as in the case of the above-mentioned terephthalic acid or its ester-forming derivatives. For example, biomass-derived ethylene glycol can be obtained by a method in which ethylene glycol is produced from biomass ethanol obtained from sugars, etc. via ethylene oxide by a conventionally known method. Examples of raw materials for biomass ethanol include corn, sugar cane, beet, and manioc.
[0048] Alternatively, commercially available biomass ethylene glycol may be used, and for example, biomass ethylene glycol commercially available from India Glycoal Limited can be suitably used. The biomass ethylene glycol from India Glycoal Limited is made from sugarcane molasses as a raw material. Biomass-derived ethylene glycol may contain more impurities derived from the raw materials and manufacturing process than fossil fuel-derived ethylene glycol. Also, the impact resistance, impact resistance and hardness during long-term storage of the obtained copolymer polyester molded product are affected by the type of biomass resource. Regarding the physical properties of the molded product, even if it is a biomass-derived copolymer polyester, the same physical properties as those of a fossil fuel-derived copolymer polyester can be obtained, so that ethylene glycol derived from sugar cane blackstrap molasses can be used as the biomass-derived ethylene glycol.
[0049] The content of biomass-derived ethylene glycol in the ethylene glycol used as the raw material in the present invention is preferably 20% by mass or more and 100% by mass or less. If the lower limit of the content of biomass-derived ethylene glycol is less than 20% by mass, the effect of reducing the environmental load of reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases decreases. The use of biomass-derived ethylene glycol is more preferably 40% by mass or more, and particularly preferably 75% by mass or more, because it has the effect of reducing the environmental load of reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases, as well as the impact resistance of the obtained molded product, and the impact resistance and hardness during long-term storage. The upper limit of the content of biomass-derived ethylene glycol in the ethylene glycol used as the raw material is not particularly limited, but it is preferably 100% by mass or less, and it is most preferable to use only biomass-derived ethylene glycol, because it has the effect of reducing the environmental load of reducing the amount of petroleum resources used and suppressing the emission of greenhouse gases, as well as the impact resistance of the obtained molded product, and the impact resistance and hardness during long-term storage.
[0050] The copolymer polyester of the present invention uses the above-mentioned raw materials and undergoes a series of reactions, so that the diol unit (I) is formed from the diol (III) represented by the above formula (III) in the copolymer polyester. The triol unit (II) is formed from the triol (IV) represented by the above formula (IV). Therefore, in the above formula (III) relating to the diol and the above formula (IV) relating to the triol, the types and contents of the group A and the group B, the types of preferred groups, and the detailed contents and preferred values of j, k, p, q, and r are as described for the diol unit (I), diol unit (III), triol unit (II), and triol unit (IV) in the copolymer polyester of the present invention. In particular, preferred specific examples of the diol (III) and the triol (IV) are as follows.
[0051] Preferred examples of the diol (III) used in the production of the copolymerized polyester of the present invention include 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane, 2-{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-2-[4'-(2-hydroxyethoxy)phenyl]propane, 2,2-bis{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}propane, bis[4-(2-hydroxyethoxy)phenyl]sulfone, {4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-[4'-(2-hydroxyethoxy(phenyl)sulfone, bis{4-[2'-(2-hydroxy Examples of the diol (III) include 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1-{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-1-[4'-(2-hydroxyethoxy)phenyl]cyclohexane, and 1,1-bis{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}cyclohexane. Among these, 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane is preferred as the diol (III) in terms of excellent impact resistance, impact resistance during long-term storage, transparency, and hardness of the copolymer polyester.
[0052] Preferred examples of the triol (IV) used in the production of the copolymerized polyester of the present invention include 2-[3-(2-hydroxyethyl)-4-(2-hydroxyethoxy)phenyl]-2-[4-(2-hydroxyethoxy)phenyl]propane, 2-{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-2-[3'-(2-hydroxyethyl)-4'-(2-hydroxyethoxy)phenyl]propane, 2-[4-(2-hydroxyethoxy)phenyl]-2-{3'-(2-hydroxyethyl)-4'-[2-(2-hydroxy ethoxy)ethoxy]phenyl}propane, 2-[4-(2-hydroxyethoxy)phenyl]-2-{3'-[2-(2-hydroxyethoxy)ethyl]-4'-(2-hydroxyethoxy)phenyl}propane, 2-{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-2-{3'-(hydroxyethyl)-4'-[2-(2-hydroxyethoxy)ethoxy]phenyl}propane, 2-{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-2-{3'-[2-(2-hydroxyethoxy)ethyl]-4' -[2-(2-hydroxyethoxy)ethoxy]phenyl}propane, [4-(2-hydroxyethoxy)phenyl]-[3'-(2-hydroxyethyl)-4'-(2-hydroxyethoxy)phenyl]sulfone, {4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-[3'-(2-hydroxyethyl)-4'-(2-hydroxyethoxy)phenyl]sulfone, [4-(2-hydroxyethoxy)phenyl]-{3'-(2-hydroxyethyl)-4-[2'-(2-hydroxyethoxy)ethoxy]phenyl}sulfon. , [4-(2-hydroxyethoxy)phenyl]-3'-[2-(2-hydroxyethoxy)ethyl]-4'-(2-hydroxyethoxy)phenyl}sulfone, {4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-{3'-(hydroxyethyl)-4'-[2-(2-hydroxyethoxy)ethoxy]phenyl}sulfone, {4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-{3'-[2-(2-hydroxyethoxy)ethyl]-4'-[2-(2-hydroxyethoxy)ethoxy]phenyl}sulfone,1-[4-(2-hydroxyethoxy)phenyl]-1-[3'-(2-hydroxyethyl)-4'-(2-hydroxyethoxy)phenyl]cyclohexane, 1-{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-1-[3'-(2-hydroxyethyl)-4'-(2-hydroxyethoxy)phenyl]cyclohexane, 1-[4-(2-hydroxyethoxy)phenyl]-1-{3'-(2-hydroxyethyl)-4'-[2-(2-hydroxyethoxy)ethoxy]phenyl}cyclohexane, 1-[4-(2-hydroxyethoxy)phenyl 1-{3'-[2-(2-hydroxyethoxy)ethyl]-4'-(2-hydroxyethoxy)phenyl}cyclohexane, 1-{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-1-{3'-(hydroxyethyl)-4'-[2-(2-hydroxyethoxy)ethoxy]phenyl}cyclohexane, 1-{4-[2-(2-hydroxyethoxy)ethoxy]phenyl}-1-{3'-[2-(2-hydroxyethoxy)ethyl]-4'-[2-(2-hydroxyethoxy)ethoxy]phenyl}cyclohexane, etc. Among them, 2-[3-(2-hydroxyethyl)-4-(2-hydroxyethoxy)phenyl]-2-[4-(2-hydroxyethoxy)phenyl]propane is preferably used as triol (IV) in terms of excellent impact resistance, impact resistance during long-term storage, transparency and hardness of the copolymerized polyester. ,
[0053] In producing the copolymerized polyester of the present invention, in addition to the above-mentioned terephthalic acid, ethylene glycol, diol (III), and triol (IV), the same structural units derived from other bifunctional compounds that may be contained in the copolymerized polyester of the present invention as described above may be used, so long as the amount of such structural units is 10 mol % or less based on the total reaction components.
[0054] In producing the copolymerized polyester, as described above, a dicarboxylic acid mainly composed of terephthalic acid or an ester-forming derivative thereof is subjected to an esterification reaction or an ester exchange reaction with a diol mainly composed of ethylene glycol containing a diol (III) and a reaction raw material containing a triol (IV) to generate a low polymer. In this case, the reaction components are mixed so that the content of the diol (III) is 1.9 parts by mass to 15 parts by mass relative to 100 parts by mass of the dicarboxylic acid and the content of the triol (IV) is 0.005 parts by mass to 2 parts by mass relative to 100 parts by mass of the dicarboxylic acid, and the esterification reaction or the ester exchange reaction is carried out.
[0055] The above esterification reaction or transesterification reaction is usually carried out at normal pressure or under an absolute pressure of 0.3 MPa or less at a temperature of 230 to 280°C while distilling off the water produced. Then, additives such as a polycondensation catalyst and a coloring inhibitor are added as necessary, and then melt polycondensation is usually carried out at a temperature of 200 to 280°C under a reduced pressure of 5 mmHg or less to form a polyester prepolymer having a desired viscosity. From the viewpoint of the handleability of the polyester prepolymer, the intrinsic viscosity of the polyester prepolymer is preferably 0.40 to 0.80 dl / g.
[0056] When a polycondensation catalyst is used in the melt polycondensation reaction, it is possible to use one that is commonly used in the production of polyesters, and examples of such catalysts include antimony compounds such as antimony oxide; germanium compounds such as germanium dioxide; titanium compounds such as tetramethoxytitanium, tetraethoxytitanium, tetra-n-propoxytitanium, tetraisopropoxytitanium, and tetrabutoxytitanium; and tin compounds such as di-n-butyltin dilaurate, di-n-butyltin oxide, and dibutyltin diacetate. These catalyst compounds may be used alone or in combination of two or more. When a polycondensation catalyst is used, it is preferable that the amount of the catalyst is within the range of 0.002 to 0.8% by mass based on the weight of the dicarboxylic acid component.
[0057] In addition, in the melt polycondensation reaction, a coloring inhibitor may be used, for example, phosphorous acid, phosphoric acid, trimethyl phosphite, triphenyl phosphite, tridecyl phosphite, trimethyl phosphate, tridecyl phosphate, triphenyl phosphate, and other phosphorus compounds may be used alone or in combination of two or more. When using a coloring inhibitor made of the above phosphorus compound, it is preferable that the content is within the range of 0.001 to 0.5 mass% based on the weight of the dicarboxylic acid component. In addition, in order to suppress coloring due to thermal decomposition of the copolymerized polyester, it is preferable to add 0.001 to 0.5 mass% of a manganese compound, such as manganese acetate, based on the weight of the dicarboxylic acid component.
[0058] The above esterification reaction or transesterification reaction, and melt polycondensation reaction are preferably carried out in the presence of a by-product inhibitor for diethylene glycol, such as tetraalkylammonium hydroxides, e.g., tetraethylammonium hydroxide, and organic amines, e.g., triethanolamine and triethylamine.
[0059] Next, the polyester prepolymer obtained by the melt polycondensation reaction is made into chips or pellets of any shape such as a die shape or a cylinder shape, and is pre-dried at a temperature of usually 190°C or less. The solid-phase polymerization is carried out until the intrinsic viscosity, MFR, etc. reach the desired values to form the desired copolymerized polyester. The solid-phase polymerization is preferably carried out under vacuum, reduced pressure, or in an inert gas such as nitrogen gas. In addition, it is preferable to carry out the solid-phase polymerization while fluidizing the chips or pellets by a suitable method such as a rolling method or a gas fluidized bed method so that the chips or pellets of the polyester prepolymer do not stick to each other. The solid-phase polymerization is preferably carried out at a temperature in the range of usually 180 to 240°C, more preferably at a temperature in the range of 200 to 240°C. Furthermore, from the viewpoint of preventing sticking between the chips or pellets, the temperature of the solid-phase polymerization is preferably within the above-mentioned range and is 15°C or more lower than the melting point of the copolymerized polyester to be produced (the copolymerized polyester finally obtained), preferably 20°C or more lower. Moreover, the polymerization time for the solid-phase polymerization is usually preferably in the range of 4 to 40 hours from the viewpoint of productivity, etc. By carrying out the above-mentioned series of steps, the copolymerized polyester of the present invention can be produced with good productivity in a short time.
[0060] The copolymer polyester of the present invention is excellent in melt moldability, transparency, heat resistance, mechanical properties, etc., and can be molded into various molded products by extrusion blow molding, injection-extrusion blow molding, extrusion molding, injection molding, and other melt molding methods. Among them, the copolymer polyester of the present invention is suitable for use in molding involving a melt extrusion process, and is particularly suitable for use in extrusion blow molding. When the copolymer polyester of the present invention is used for melt molding, particularly extrusion blow molding involving melt extrusion, injection-extrusion blow molding, extrusion molding, etc., it can be produced with good productivity without causing deformation after extrusion, and the molded product obtained is excellent in various properties such as transparency, impact resistance, other mechanical properties, heat resistance, and moisture resistance. In particular, when the copolymer polyester of the present invention is used for extrusion blow molding, the drawdown property of the extruded parison is good, the drawdown time of the parison is kept within an appropriate range, the diameter of the parison is uniform, the blow moldability is good, and a hollow molded product having a good shape and dimensional accuracy without distortion or deformation can be smoothly and productively produced without causing any trouble during molding. Furthermore, the resulting extrusion blow molded articles are excellent in transparency, mechanical properties such as impact resistance, tensile strength and hardness, and heat resistance.
[0061] When extrusion blow molding is performed using the copolymer polyester of the present invention, the copolymer polyester is melt-extruded to form a cylindrical parison, and the parison is inserted into a blow mold while in a softened state, and gas such as air is blown into the parison to expand it into a predetermined hollow shape that conforms to the shape of the mold cavity. When extrusion blow molding is performed by the above-mentioned method, it is preferable to set the melt extrusion temperature within the range of (melting point of copolymer polyester + 10°C) to (melting point of copolymer polyester + 70°C) in terms of moldability, etc. In addition, the shape and structure of the molded product of the present invention are not particularly limited, and can be any shape or structure such as a hollow molded product, a tubular body, a plate, a sheet, a film, a rod-shaped body, a molded product, etc., depending on each application, and the dimensions are not limited at all. Among them, the manufacturing method of the molded product of the present invention is particularly suitable for hollow molding by extrusion blow molding.
[0062] Furthermore, the molded article obtained from the copolymerized polyester of the present invention may be formed solely from the copolymerized polyester of the present invention, may be in the form of a laminate with other materials such as other plastics, metals, fibers, and fabrics, or may be a molded article in a form other than the laminate structure of the copolymerized polyester of the present invention and the other materials described above, and is not limited in any way. In particular, when the molded article of the present invention is an extrusion blow molded article, it may be, for example, a single-layer hollow molded article (hollow container, etc.) made only of the copolymerized polyester of the present invention, or a multi-layer hollow molded article made of the copolymerized polyester of the present invention and other plastics such as polyethylene, polypropylene, ethylene-vinyl alcohol copolymer, or polyethylene terephthalate (PET). More specifically, for example, a three-layer bottle made of a PET layer / copolymerized polyester layer / PET layer, a five-layer bottle made of a PET layer / copolymerized polyester layer / PET layer / copolymerized polyester layer / PET layer, etc. may be mentioned.
[0063] The copolymer polyester of the present invention may be blended with various additives used for other thermoplastic resins or polyester resins, such as colorants such as dyes and pigments, stabilizers such as ultraviolet absorbers, antistatic agents, flame retardants, flame retardant assistants, lubricants, plasticizers, inorganic fillers, etc. When various additives are blended, the blending amount is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, based on 100 parts by mass of the copolymer polyester, in order to provide a molded article having excellent impact resistance, impact resistance during long-term storage, and hardness. EXAMPLES
[0064] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0065] (1) Biomass plastic content In the copolymerized polyesters obtained in the Examples and Comparative Examples, the mass % of units composed of raw materials derived from biomass was calculated as the biomass plastic degree. Specifically, the ratio of units derived from biomass-derived ethylene glycol or biomass-derived terephthalic acid used as raw materials in each Example and Comparative Example was calculated, and the mass % was calculated from the molecular weight of each unit based on the ratio, and was defined as the biomass plastic degree. Note that the calculation was made taking into consideration that in the polymerization of polyester, two hydrogen atoms in the diol, two oxygen atoms in the dicarboxylic acid, and two hydrogen atoms generate two moles of water molecules when an ester bond is formed.
[0066] (2) Bio-based carbon content The bio-based carbon content in the total carbon of the components constituting the copolymerized polyester obtained in each of the Examples and Comparative Examples was measured in accordance with ISO16620-2:2019.
[0067] (3) Intrinsic viscosity (IV) The copolymerized polyester obtained in each of the Examples and Comparative Examples was put into a weight mixed solvent of phenol and 1,1,2,2-tetrachloroethane, and the intrinsic viscosity was measured at 30°C using an Udderohde viscometer (automatic viscosity measuring device "VMC-422 type" manufactured by Rigo Co., Ltd.).
[0068] (4) Melting point (Tm), glass transition temperature (Tg) The melting point (Tm) and glass transition temperature (Tg) of the crystal pellets after melt polymerization or solid-state polymerization were measured using a differential scanning calorimeter (TA Instruments, TA Q2000). The melting point was measured as the melting peak when the temperature was increased from 30°C to 280°C at a heating rate of 10°C / min, and the glass transition temperature (Tg) was calculated from the data obtained when the temperature was increased from 30°C to 280°C at a heating rate of 10°C / min, then quenched to 30°C at -50°C / min, and then increased again at a heating rate of 10°C / min.
[0069] (5) Resin color (b* value, L value) The copolymer polyester pellets were measured using a spectrophotometer (Hunter's "LabScan XE"). The pellets to be measured were packed into a glass cell, and the position of the glass cell was changed to perform five measurements, and the average value was calculated. If the b value exceeds 7, the color tone of the bottle becomes strongly yellowish, and the appearance becomes poor. A b value of 4 or less is preferable in terms of color tone. If the L value is 75 or less, the bottle becomes dull, and the appearance becomes poor. An L value of 80 or more is preferable in terms of color tone.
[0070] (6) Impact resistance (bottle drop strength, accelerated bottle drop strength) Using an extrusion blow molding machine (Tahara Co., Ltd., "MSE-40E / 32M-A (T1) type"), a transparent bottle with a volume of 220 mL (27.5 g ± 0.5 g) was molded at a cylinder maximum temperature of 280 to 290 ° C, a die temperature of 240 to 250 ° C, a screw rotation speed of 24 rpm, an extrusion resin pressure of 19 to 30 MPa, and a mold temperature of 30 ° C. The temperature of the molded bottle was controlled at 23 ° C for 24 hours. The bottle was filled with water controlled to 23 ° C so that no air bubbles remained in the bottle, sealed with a cap, and then passed through a vertically installed 10 cm diameter cylinder and dropped alternately from a height of 125 cm onto a horizontal concrete surface and a concrete surface inclined at 45 degrees. The number of cycles until the bottle cracked or cracked and the water filled inside leaked was measured (the bottle was dropped twice per cycle, once on a horizontal surface and once on a 45 degree incline). A maximum of 20 cycles were repeated. For each composition, five bottles were subjected to a drop test, and the average value was taken as the bottle drop strength. The molded bottles were stored in a thermostatic chamber at 50°C and 6% RH for 67 hours, and then the bottle drop test was performed in the same manner as above, and the average value of the number of cycles was taken as the accelerated bottle drop strength. The bottle drop strength was used as an index of impact resistance, and it was evaluated that the more the number of cycles, the better the impact resistance.
[0071] (7) Rockwell hardness The transparent bottles molded in (6) were kept at 23°C for 24 hours, and the smooth parts were cut out (length 3 cm, width 2 cm) to be used as samples. The Rockwell hardness was measured on the R scale using a hardness tester Rockwell type 3R (manufactured by Imai Seiki). Each sample was measured five times at room temperature, and the average value was taken as the Rockwell hardness.
[0072] (8) Drawdown properties of parison during extrusion blow molding In (6), the drawdown time of the parison was measured when a transparent bottle with a volume of 220 mL was manufactured using an extrusion blow molding device. When the parison was drawn down to 25 cm, it was clamped in a mold and blown. The time (seconds) required to draw down 25 cm was taken as the drawdown time, and the drawdown property was evaluated according to the following criteria. A: Drawdown time is between 16 and 18 seconds B: Drawdown time is between 18 and 25 seconds C: Drawdown time is less than 16 seconds or more than 25 seconds
[0073] [Synthesis Example 1] 300 parts by mass of Para-Cymene manufactured by Yasuhara Chemical Co., Ltd., which is a Para-Cymene synthesized using biomass (orange peel and pulp black liquor) as a raw material, 501 parts by mass of acetic acid, 1.059 parts by mass of cobalt acetate as a catalyst, 1.101 parts by mass of manganese acetate, and 1.317 parts by mass of lithium bromide were charged into a titanium autoclave, and the reaction temperature was 180 ° C., the pressure in the reaction system was adjusted to 1.5 MPa with compressed air, and the reaction was carried out by stirring for 5 hours while supplying compressed air to the reactor. After the reaction, the reaction liquid was suction filtered to separate the solid and liquid, and the obtained solid was washed and filtered twice with pure water and dried at 90 ° C. for a day and night to obtain 240 parts by mass of terephthalic acid derived from biomass. The obtained terephthalic acid derived from biomass was used as a raw material for copolymerized polyester.
[0074] [Example 1] 100 parts by mass of terephthalic acid (TA) derived from fossil fuels, 42.59 parts by mass of ethylene glycol (EG; manufactured by India Glycol) derived from biomass The following chemical formula (V):
[0075] [ka] 9.49 parts by mass of 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane (hereinafter referred to as "EOBPA") represented by the following chemical formula (VI) [ka] A slurry consisting of 0.039 parts by mass of 2-[3-(2-hydroxyethyl)-4-(2-hydroxyethoxy)phenyl]-2-[4-(2-hydroxyethoxy)phenyl]propane (hereinafter referred to as "HEPP") represented by the formula was prepared, to which 0.012 parts by mass of germanium dioxide and 0.012 parts by mass of phosphorous acid were added. The slurry was heated to 250°C under pressure (absolute pressure 0.25MPa) and esterification reaction was carried out until the esterification rate reached 95%, to produce a low polymer. Next, the low polymer was melt-polycondensed at a temperature of 270°C under a reduced pressure of 1mmHg to produce a prepolymer of a copolymerized polyester having an intrinsic viscosity of 0.76dl / g, which was extruded from a nozzle in the form of a strand and cut to obtain cylindrical pellets (diameter 2.5mm, length 3.5mm). Next, the obtained copolymer polyester prepolymer pellets were pre-dried at a temperature of 150°C for 5 hours, and then solid-phase polymerization was carried out for 29 hours at a temperature (205°C) 25°C lower than the melting point under a reduced pressure of 0.1 mmHg to obtain copolymer polyester pellets with a high molecular weight. In order to prevent the pellets from sticking together, the solid-phase polymerization was carried out while fluidizing the pellets in a rotary solid-phase polymerization apparatus. The ratio of the monomer components constituting the copolymer polyester obtained was 1 The results were confirmed by H-NMR spectroscopy (instrument: JNM-GX-500 manufactured by JEOL, solvent: deuterated trifluoroacetic acid). The ratio of each monomer component is shown in Table 1. The results of the above-mentioned various measurements are shown in Table 2.
[0076] [Examples 2 to 8, Comparative Examples 1 to 3] Copolymerized polyester pellets were obtained by carrying out the esterification reaction, melt polymerization reaction, and solid-state polymerization in the same manner as in Example 1, except that the types and amounts of the dicarboxylic acid component, diol component, and triol component, and the temperature and time of the solid-state polymerization were changed as shown in Table 1. The contents of the structural units in the obtained copolymerized polyester, and the physical properties of the copolymerized polyester were evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.
[0077] [Table 1]
[0078] [Table 2]
[0079] <Consideration> As shown in Table 2, Example 1 has a higher biomass plastic degree of 27.8% and a higher bio-based carbon content of 17.5% compared to Comparative Example 1, and thus has an environmental load reduction effect. In addition, the color tone, bottle drop strength immediately after molding and after accelerated testing, and Rockwell hardness are similar to those of Comparative Example 1, and it has become clear that even though it is a biomass-derived copolymer polyester, it exhibits physical properties comparable to those of fossil fuel-derived copolymer polyester. Furthermore, Example 2 has a high environmental load reduction effect with a biomass plastic degree of 29.2% and a bio-based carbon content of 18.5%, and since the diol unit (I) / triol unit (β) is 72 and the ethylene glycol unit / triol unit (β) is 2295, a molded product can be obtained that has good bottle drop strength immediately after molding and after accelerated testing, Rockwell hardness, and parison drawdown properties.
[0080] Comparing Example 2 with Comparative Example 3, the biomass plastic content in Comparative Example 3 was 40.7%, which was a higher environmental load reduction effect than the 29.2% in Example 2. However, the b* value was 7.2, and the copolymer polyester pellets in Comparative Example 3 were colored yellow, and the bottle drop strength immediately after molding was 2.0, indicating low impact resistance.
[0081] In Example 5, the amount of HEPP blended was large, the diol unit (I) / triol unit (β) was 40, and the ethylene glycol unit / triol unit (β) was 759. Therefore, although the Rockwell hardness was high, the bottle drop strength was low and the molded body tended to be hard and brittle.
[0082] In Examples 6 to 8, biomass-derived terephthalic acid was used, and the b* value was 4.4 to 6.1, the copolymer polyester pellets were slightly colored yellow, and the bottle drop strength after the accelerated test tended to be low. [Industrial Applicability]
[0083] The copolymer polyester of the present invention is useful as various molded articles, particularly as extrusion blow molded articles.
Claims
1. A copolymer polyester mainly composed of dicarboxylic acid units mainly composed of terephthalic acid units, diol units (α) mainly composed of ethylene glycol units and diol units (I) represented by the following formula (I), and triol units (β) including triol units (II) represented by the following formula (II): Contains 1 to 15 mol % of diol units (I) based on the total number of moles of diol units (α) and triol units (β); Contains 0.005 to 1 mol % of triol units (II) based on the total number of moles of diol units (α) and triol units (β), the molar ratio of the contents of ethylene glycol units and triol units (β) (ethylene glycol units / triol units (β)) is 2,000 or more and 13,000 or less; A copolymer polyester having a biomass plastic content of 5% or more and 40% or less. 【Chemistry 1】 [Wherein A is -CH 2 CH 2 - or -CH(CH 3 ) CH 2 -, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and j and k each independently represent an integer of 1 to 8. 【Chemistry 2】 [Wherein A is -CH 2 CH 2 - or -CH(CH 3 ) CH 2 -, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and p, q and r each independently represent an integer of 1 to 8.
2. the ethylene glycol units include ethylene glycol units derived from biomass-derived ethylene glycol; 2. The copolymer polyester according to claim 1, wherein a content of ethylene glycol units derived from biomass-derived ethylene glycol in all ethylene glycol units is 20% by mass or more and 100% by mass or less.
3. 3. The copolymer polyester according to claim 2, wherein the ethylene glycol units derived from the biomass-derived ethylene glycol are ethylene glycol units derived from ethylene glycol made from sugar cane molasses.
4. the terephthalic acid units comprise terephthalic acid units derived from biomass-derived terephthalic acid; The copolymer polyester according to any one of claims 1 to 3, characterized in that the content of terephthalic acid units derived from biomass-derived terephthalic acid in all terephthalic acid units is 15 mass% or less.
5. 5. The copolymer polyester according to claim 1, wherein the terephthalic acid units are composed solely of terephthalic acid units derived from fossil fuel-derived terephthalic acid.
6. The copolymer polyester according to any one of claims 1 to 5, characterized in that the intrinsic viscosity is 0.6 to 1.5 dl / g.
7. A molded article made of a copolymer polyester mainly composed of dicarboxylic acid units mainly composed of terephthalic acid units, diol units (α) mainly composed of ethylene glycol units and diol units (I) represented by the following formula (I), and triol units (β) including triol units (II) represented by the following formula (II): Contains 1 to 15 mol % of diol units (I) based on the total number of moles of diol units (α) and triol units (β); Contains 0.005 to 1 mol % of triol units (II) based on the total number of moles of diol units (α) and triol units (β), A molded article made of a copolymer polyester, characterized in that the biomass plastic content is 5% or more and 40% or less. 【Chemistry 3】 [In the formula, A represents a group represented by --CH 2 CH 2 -- or --CH(CH 3 )CH 2 --; B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-); and j and k each independently represent an integer of 1 to 8.] 【Chemistry 4】 [In the formula, A represents a group represented by --CH 2 CH 2 -- or --CH(CH 3 )CH 2 --; B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-); and p, q and r each independently represent an integer of 1 to 8.]
8. 8. The article of claim 7 which is an extrusion blow molded article.
9. A method for producing a molded article, comprising a step of extrusion blow molding the copolymer polyester according to any one of claims 1 to 6.
10. A method for producing a copolymerized polyester according to any one of claims 1 to 6, comprising esterifying or transesterifying reactants including a dicarboxylic acid mainly composed of terephthalic acid or an ester-forming derivative thereof, ethylene glycol, a diol (III) represented by the following formula (III), and a triol (IV) represented by the following formula (IV), melt-polycondensing the reactants to form a polyester prepolymer, and then solid-phase polymerizing the polyester prepolymer, The content of the diol (III) is 1.9 parts by mass to 15 parts by mass based on 100 parts by mass of the dicarboxylic acid, The content of the triol (IV) is 0.005 to 2 parts by mass based on 100 parts by mass of the dicarboxylic acid, The content of biomass-derived terephthalic acid or its ester-forming derivative in the terephthalic acid or its ester-forming derivative is 15% by mass or less, A method for producing a copolymer polyester, characterized in that a content of ethylene glycol derived from biomass in the ethylene glycol is 20% by mass or more and 100% by mass or less. 【Chemistry 5】 [wherein A is a group of the formula: -CH 2 CH 2 - or the formula: -CH(CH 3 ) CH 2 -, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and j and k each independently represent an integer of 1 to 8. 【Chemistry 6】 [wherein A is a group of the formula: -CH 2 CH 2 - or the formula: -CH(CH 3 ) CH 2 -, B represents a divalent hydrocarbon group, a carbonyl group, a sulfonyl group, an oxygen atom or a direct bond (-), and p, q and r each independently represent an integer of 1 to 8.
11. 11. The method for producing a copolymerized polyester according to claim 10, wherein the biomass-derived ethylene glycol is ethylene glycol made from sugar cane molasses as a raw material.
Citation Information
Patent Citations
Copolyester and moldings therefrom
JP1996208818A
Copolymerized polyester pellet and molding product of the same
JP1998251387A
Polyester resin composition
JP2012097163A
Polyester resin composition
JP2012097164A
Bio-based polyethylene terephthalate packaging and method for manufacturing the same
JP2012519748A