Process for polymerizing olefins using alkane-soluble nonmetallocene precatalysts
The two-part bimodal catalyst system for olefin polymerization addresses gel formation and transition complexity by separately feeding components into a mixer, achieving controlled polyethylene compositions with reduced gel content and enhanced properties.
Patent Information
- Application Number
- JP2021521020
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-27
- Filing Date
- 2019-10-11
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2039-10-11
AI Technical Summary
Existing bimodal catalyst systems for olefin polymerization face issues such as undesirable gel formation, complexity in catalyst transitions, and instability of non-metallocene precatalysts, leading to inconsistent polyethylene compositions with high gel content, which are unsuitable for applications requiring clarity and strength.
A bimodal catalyst system is formulated in two parts, with the first part containing a slurry of a support, activator, and non-metallocene precatalyst, and the second part containing a metallocene precatalyst, which are separately fed into an in-line mixer to create a bimodal catalyst system in a single reactor, allowing for controlled polymerization rates and improved mixing of high and low molecular weight polyethylene components.
This method reduces gel content, enables flexible production of various bimodal polyethylene compositions, and simplifies catalyst transitions, resulting in improved clarity and strength of polyethylene products.
Smart Images

Figure 0007590961000008 
Figure 0007590961000009 
Figure 0007590961000010
Abstract
Description
[Technical field]
[0001] Catalytic olefin polymerization.
[0002] Publications and patents in or about this field include US2005 / 0182210A1, US2018 / 0002464A1, US2018 / 0079836A1, US5318935, US5506184, US5889128, US6255419B1, US6274684B1, US6534604B2, US6841631B2, US685868 US6967184B2, US6894128B2, US6949612B2, US6967184B2, US6995217B2, US7163991B2, US7196032B2, US7276566B2, US7479529B2, US7566677B2, US7718566B2, US7754840B2, US7973112B2, and US9902790B2. US6967184B2 refers to the synthesis of HN5Zr(NMe2)2. US2018 / 0002464A1 refers to biphenylphenol precatalysts ("procatalysts", e.g., compounds 1-7 in paragraph
[0104] ). US7973112B2 refers to a spray-dried catalyst containing bis(phenylmethyl)[N'-(2,3,4,5,6-pentamethylphenyl)-N-[2-(2,3,4,5,6-pentamethylphenyl)amino-κN]ethyl]-1,2-ethane-diaminato(2-)κN,κN']zirconium, or "HN5Zr" herein abbreviated as "HN5Zr dibenzyl", and (n-propylcyclopentadienyl)(tetramethylcyclopentadienyl)zirconium dichloride. US6858684B2, US6949612B2, US6995217B2, and US2018 / 0079836A1 refer to catalyst migration.
[0003] Introduction Solutions are described to one or more problems associated with the polymerization of olefin monomers using a bimodal catalyst system, including a catalyst made from an alkane-insoluble nonmetallocene precatalyst (e.g., HN5Zr dibenzyl) to make high molecular weight (HMW) polyethylene, and an activator, and a metallocene (MCN) catalyst to make low molecular weight (LMW) polyethylene. The bimodal catalyst system makes a bimodal polyethylene composition, including an HMW polyethylene component and an LMW polyethylene component, in a single reactor. Some of the problems are related to undesirable gels in the melt-blended bimodal polyethylene composition after the reactor. Other problems are related to the transition complexities and stability of the bimodal catalyst system.
[0004] The bimodal catalyst system includes or is made from a metallocene (MCN) pre-catalyst, a non-metallocene pre-catalyst that is insoluble in alkanes ("insoluble non-MCN" pre-catalyst), at least one activator, and a support material (solid). The insoluble non-MCN pre-catalyst (e.g., HN5Zr dibenzyl) makes the HMW polyethylene component of the bimodal polyethylene composition. The MCN pre-catalyst is soluble in alkanes, and the MCN catalyst makes the LMW polyethylene component of the bimodal polyethylene composition. If the insoluble non-MCN pre-catalyst and its activator are fed to the polymerization reactor separately from the MCN pre-catalyst and its activator feed, gel problems can occur. The resulting HMW and LMW polyethylene components, when first made separately in the reactor, may not be homogeneously mixed thereafter. This can make the comparative bimodal polyethylene composition undesirable with increased gel content (the gel constitutes part of the HMW polyethylene component). Comparative bimodal polyethylene compositions may have too high a gel content for applications requiring clarity, such as films, and / or high strength, such as pipes.
[0005] To reduce or avoid the gel problem, the bimodal catalyst system is formulated in two parts. The first part contains a slurry of the support, alkane solvent, at least one activator, all of the insoluble non-MCN pre-catalyst, and a portion of the MCN pre-catalyst. The second part contains a solution of the remaining MCN pre-catalyst in the alkane(s) solvent, but does not contain any of the insoluble non-MCN pre-catalyst, activator, or support. In the "combining-the-parts" feeding method, the first and second parts are fed separately to an in-line mixer where they are mixed to create the bimodal catalyst system. This new bimodal catalyst system is fed to a single polymerization reactor.
[0006] The partial combination feed method has a degree of flexibility that allows for achieving different polymerization rates and making different bimodal polyethylene compositions with different polymer attributes in a single polymerization reactor. For example, the flow rate of the feed of the second portion can be adjusted to compensate for the effect of a portion of the MCN pre-catalyst in the first portion (e.g., making more LMW polyethylene components) or to "trim" or adjust the effect of the insoluble non-MCN pre-catalyst in the first portion (e.g., increasing the LMW / HMW ratio), allowing for the making of different bimodal polyethylene compositions. Therefore, the second portion is called a "trim catalyst". The partial combination feed method allows for the making of bimodal polyethylene compositions with control within the limits of the polymerization reaction and the transition between different bimodal polyethylene compositions by varying the LMW / HMW ratio within the limits in a single polymerization reactor.
[0007] The first part contains all of the insoluble non-MCN pre-catalyst, the activator, and a portion of the MCN pre-catalyst, and is advantageously premixed with the desired amount of the second part (the trim catalyst) to create a bimodal catalyst system before being placed in the polymerization reactor. This is done to create a so-called reactor blend of the HMW and LMW polyethylene components in the polymerization reactor, whereby the HMW and LMW polyethylene components are created in situ in intimate contact with each other. This reactor blend results in a bimodal polyethylene composition in which the HMW and LMW polyethylene components are better mixed, and therefore the gel content is reduced.
[0008] Unfortunately, the HMW / LMW ratio of the partial combined feed method cannot be zero or near zero because the first portion of the bimodal catalyst system contains both the MCN pre-catalyst and the insoluble non-MCN pre-catalyst, and therefore the bimodal polyethylene composition will always contain some amount of both LMW and HMW polyethylene components.
[0009] Furthermore, transitions between bimodal catalyst systems ("catalyst transitions"), such as between different pre-catalysts or different amounts of the same pre-catalyst in a single polymerization reactor, are complicated. For example, transitioning from a first bimodal catalyst system that includes a first MCN catalyst (abbreviated LMW-CAT-1) and a first insoluble non-MCN pre-catalyst to a second bimodal catalyst system that includes a second MCN catalyst (abbreviated LMW-CAT-2) and the same first insoluble non-MCN pre-catalyst (where LMW-CAT-1 and LMW-CAT-2 are different from each other and from the insoluble non-MCN pre-catalyst) is complicated. To transition to the second bimodal catalyst system, both the first and second parts of the first bimodal catalyst system must be replaced, even if the insoluble non-MCN pre-catalyst of the first part of both the first and second bimodal catalyst systems is the same. This is because both the first and second parts contain the LMW-CAT-1 component that is no longer needed.
[0010] Also, certain insoluble non-MCN pre-catalysts become unstable after mixing with the activator. These first parts of the bimodal catalyst system (containing the unstable / insoluble non-MCN pre-catalyst) need to be cooled to about -10 degrees Celsius (°C) for their shipping or storage. The second part may then need to be reformulated to withstand the cooling "shock" when it comes into contact with the cooled first part in the in-line mixer. Alternatively, the first part may need to be warmed before being fed to the in-line mixer.
[0011] Also, the insoluble non-MCN pre-catalyst is not suitable for use in the second portion (trim catalyst) of the partial combined feed process because it is insoluble in alkanes. Summary of the Invention
[0012] 1. A method for polymerizing olefin monomers to make a polyolefin composition, comprising: contacting a solution of an alkane-soluble nonmetallocene pre-catalyst dissolved in an alkane solvent with an activator to make a trim catalyst comprising an alkane-soluble nonmetallocene catalyst; feeding the trim catalyst supported on a support material as a solution in the alkane solvent or as a dry powder or a slurry thereof in the alkane solvent to a polymerization reactor; and polymerizing olefin monomers in the polymerization reactor with the trim catalyst, thereby making a polyolefin composition. [Brief description of the drawings]
[0013] [Figure 1] 1 is a gel permeation chromatogram (GPC) of a bimodal polyethylene composition made according to the method of Inventive Example 9A.
[0014] [Diagram 2] 1 includes structural formulas of several embodiments of alkane soluble nonmetallocene precatalysts.
[0015] [Diagram 3]Included are structural formulas of several embodiments of intermediates useful for synthesizing embodiments of the alkane-soluble nonmetallocene precatalysts of FIG.
[0016] [Figure 4] An example of an alkane soluble nonmetallocene precatalyst includes the structural formula of one embodiment of a biphenylphenol precatalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The Summary, Claims, and Abstract are incorporated herein by reference.Certain aspects and embodiments are described below and are numbered for ease of cross-referencing.
[0018] Aspect 1. A method of polymerizing olefin monomers to make a first polyolefin composition comprising a first polyolefin polymer, comprising: (A) contacting a solution of a first alkane soluble nonmetallocene pre-catalyst (abbreviated first ASNM pre-catalyst) dissolved in an alkane solvent with an activator, for example, in a mixer device (such as in an in-line mixer device or catalyst mix tank) or in piping, such as by feeding the solution of the first ASNM pre-catalyst through a first pipe (e.g., as a slurry in an alkane solvent) and feeding the activator through a second pipe to a junction (e.g., a "Y" or "T" junction where the first and second pipes merge into one pipe), to produce a first polyolefin polymer comprising the first alkane soluble nonmetallocene pre-catalyst. 1. A method for producing a polyolefin composition comprising the steps of: (A) preparing a first trim catalyst comprising a metallocene catalyst (abbreviated as first ASNM catalyst); (B) feeding the first trim catalyst to a polymerization reactor; and (C) polymerizing an olefin monomer with the first trim catalyst in the polymerization reactor, thereby producing a first polyolefin composition comprising a first polyolefin polymer, wherein the first ASNM pre-catalyst is characterized by a solubility of at least 0.10 weight percent (wt%) in hexane containing at least 60 weight percent n-hexane (CH3(CH2)4CH3), based on the total weight of the ASNM pre-catalyst and hexane, as measured using a Solubility Test Method (Enhanced Solubility). In contrast, the insoluble pre-catalyst has a solubility of 0.00 to 0.099 weight percent in hexane containing at least 60 weight percent n-hexane (CH3(CH2)4CH3), based on the total weight of the insoluble pre-catalyst and hexane, as measured using the Solubility Test Method. Step (B) may occur after and / or during step (A). Step (C) may occur after and / or during step (B). The first trim catalyst is the reaction product of the first alkane-soluble nonmetallocene pre-catalyst and the activator. The olefin may be fed to the polymerization reactor once, intermittently (e.g., periodically), or continuously. The first polyolefin polymer may be removed from the polymerization reactor once, intermittently (e.g., periodically), or continuously.The first polyolefin composition can be unimodal (consisting essentially of the first polyolefin polymer) or multimodal (consisting essentially of the first polyolefin polymer and at least one second polyolefin polymer different from the first polyolefin polymer). The first polyolefin polymer can be a high molecular weight (HMW) polyolefin. In some embodiments, the process and reactor do not include a metallocene (pre)catalyst. In some embodiments, the process and reactor further include the use of a first metallocene (pre)catalyst. (Pre)catalyst means a precatalyst, a catalyst, or both. The activator can be an alkylaluminoxane or a trialkylaluminum compound.
[0019] Aspect 2. The method of aspect 1, wherein the first trim catalyst comprises a solution of the first ASNM catalyst dissolved in an alkane solvent, and step (B) comprises feeding the solution to the reactor, the solution being free of support material (finely divided solids). The alkane solvent of the feeding step can be the same or different from the alkane solvent used in the contacting step. When the solvent is different, the method can further comprise a solvent exchange or replacement step.
[0020] Aspect 3. The method of aspect 1 or 2, further comprising steps (a) and (b) of: (a) separately from step (A), contacting a first metallocene pre-catalyst with an activator and optionally a support material to produce a first metallocene catalyst, optionally disposed on and / or in the support material; and (b) separately from step (B), feeding the first metallocene catalyst to a polymerization reactor, wherein step (C) further comprises polymerizing an olefin monomer with the first metallocene catalyst in the polymerization reactor, thereby producing a first bimodal polyolefin composition comprising a first polyolefin polymer and a second polyolefin polymer. The second polyolefin polymer is produced by the first metallocene catalyst and is different from the first polyolefin polymer produced by the trim catalyst. The activator in step (a) may be the same or different from the activator in step (A). The first metallocene catalyst is a reaction product of the first metallocene pre-catalyst and the activator of step (a). In some embodiments, the support material is absent or present in the first trim catalyst. In some embodiments, the support material is absent or present in the first metallocene catalyst. The support material can independently be untreated silica, or calcined untreated silica, or silica treated with a hydrophobing agent, or silica calcined and treated with a hydrophobing agent. The hydrophobing agent can be dichlorodimethylsilane.
[0021] Aspect 4. The method of aspect 3, wherein step (B) comprises feeding the first trim catalyst to the polymerization reactor as a solution of the first ASNM catalyst dissolved in a first alkane solvent, and step (b) comprises separately feeding the polymerization reactor with a solution of the first metallocene catalyst dissolved in a second alkane solvent, the first and second alkane solvents being the same or different, and the solutions being free of support material. By separately feeding, it is meant that the solutions enter the polymerization reactor through different injection devices at the same time or through the same injection device at different times.
[0022] Aspect 5. After step (C), (D) the method further comprises steps (a) and (b), respectively: (a1) contacting a second metallocene pre-catalyst different from the first metallocene pre-catalyst with an activator, and optionally a support material, to produce a second metallocene catalyst different from the first metallocene catalyst in the structure of at least one cyclopentadienyl ligand, wherein the second metallocene catalyst does not include a support material or is disposed on and / or in the support material; and (b1) decreasing the feeding of the first metallocene catalyst from a steady state value until the first metallocene catalyst is no longer fed to the polymerization reactor, and and independently starting and increasing the feed of the second metallocene catalyst to the polymerization reactor until the second metallocene catalyst is fed to the polymerization reactor at a steady state value, and step (C) further comprises polymerizing the olefin monomer with the second metallocene catalyst in the polymerization reactor, thereby making a second multimodal (e.g., bimodal) polyolefin composition comprising a first polyolefin polymer made by the first trim catalyst and a third polyolefin polymer made by the second metallocene catalyst, the third polyolefin polymer being different from each of the first and second polyolefin polymers. The first bimodal polyolefin composition may be removed from the polymerization reactor during step (D) such that ultimately the polymerization reactor no longer contains the first multimodal polyolefin composition, but only the second multimodal polyolefin composition. Thus, the transition includes a catalyst transition feature and a polymer transition feature. The activator in step (a1) may be the same as or different from the activator in step (a). The second metallocene catalyst is structurally different from the first metallocene catalyst in the structure of the cyclopentadienyl ligand. For example, the first metallocene catalyst may have at least one unsubstituted cyclopentadienyl ligand, and the second metallocene catalyst may have two of the same or different substituted cyclopentadienyl ligands, but no unsubstituted cyclopentadienyl ligands.Alternatively, the first metallocene catalyst may have methylcyclopentadienyl and butylcyclopentadienyl ligands and the second metallocene catalyst may have methylcyclopentadienyl and propylcyclopentadienyl ligands.
[0023] Example 6. The method of example 1, wherein the first trim catalyst further comprises a support material upon which the first ASNM catalyst is disposed.
[0024] Aspect 7. A method of polymerizing olefin monomers to make a first bimodal polyolefin composition comprising a first high molecular weight (HMW) polyolefin component and a first low molecular weight (LMW) polyolefin component, comprising the steps of: (1) contacting (e.g., in a mixer device or piping) a solution of a first alkane soluble nonmetallocene pre-catalyst (first ASNM pre-catalyst) dissolved in an alkane solvent with an activator to make a first trim catalyst comprising the first alkane soluble nonmetallocene catalyst (first ASNM catalyst); (2) contacting (e.g., in a mixer device or piping) the first metallocene pre-catalyst and an additional amount (first additional amount) of the first alkane soluble nonmetallocene pre-catalyst (a mixture thereof) with an activator and optionally a support material to produce a first bimodal polyolefin composition comprising the first metallocene catalyst and the additional amount of the first ASNM catalyst, optionally not including a support material or disposed on and / or in a support material. (3) contacting (e.g., in a first mixer device (e.g., a first in-line mixer device) or a first piping) the first bimodal catalyst system with a first trim catalyst to produce a first mixed catalyst system comprising a mixture of the first bimodal catalyst system and the first trim catalyst; (4) feeding the first mixed catalyst system to a polymerization reactor; and (5) polymerizing olefin monomers with the first mixed catalyst system in the polymerization reactor, thereby producing a first HMW polyolefin component and a first LMW polyolefin component of the first bimodal polyolefin composition, wherein the first ASNM pre-catalyst is characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane (CH3(CH2)4CH3), based on the total weight of the first ASNM pre-catalyst and the hexane, as measured using a Solubility Test Method.
[0025] Embodiment 8. After step (5), (6) modifying the method from steps (2) through (5), respectively, further comprising: (2a) contacting the second metallocene pre-catalyst and a second additional amount of the first alkane-soluble nonmetallocene pre-catalyst with an activator and optionally a support material (e.g., in a mixer device such as a third catalyst tank or in piping) to produce a second bimodal catalyst system comprising the second metallocene catalyst and a second additional amount of the first ASNM catalyst, optionally free of support material or disposed on and / or in the support material; (3a) contacting the second bimodal catalyst system with the first trim catalyst (e.g., in a second mixer device (e.g., a second in-line mixer device, which may be the same or different from the first in-line mixer device) or in a second piping, which may be the same or different from the first piping); 8. The method of embodiment 7, further comprising: (4a) decreasing the feed of the first mixed catalyst system from a steady state value until the first mixed catalyst system is no longer fed to the polymerization reactor and independently starting and increasing the feed of the second mixed catalyst system to the polymerization reactor until the second mixed catalyst is fed to the polymerization reactor at the steady state value; and (5a) polymerizing olefin monomers in the polymerization reactor with the second mixed catalyst system, thereby producing a second bimodal polyolefin composition comprising the first HMW polyolefin component and a second LMW polyolefin component, wherein the second LMW polyolefin component is distinct from each of the first HMW polyolefin component and the first LMW polyolefin component. The first bimodal polyolefin composition may be removed from the polymerization reactor during step (6) such that ultimately the polymerization reactor no longer contains the first bimodal polyolefin composition, but only the second bimodal polyolefin composition. Thus, the transition includes catalyst transition characteristics and polymer transition characteristics.
[0026] Aspect 9. The olefin monomer is (i) ethylene, (ii) propylene, (iii) (C4-C 20(v) a combination of (i) and (ii); (vi) a combination of (i) and (iii); and (vii) a combination of (i), (ii), and (iv); wherein the first polyolefin polymer or the HMW polyolefin component (as the case may be) is, respectively, any one of (i) to (vii): (a) a polyethylene homopolymer; (b) a polypropylene homopolymer; (c) a poly(C4-C8) alpha-olefin; or (d) a poly(C4-C8) alpha-olefin; or 1-butene; or 1-hexene; or 1-octene; (iv) 1,3-butadiene; (v) a combination of (i) and (ii); (vi) a combination of (i) and (iii); and (vii) a combination of (i), (ii), and (iv); 20 ) alpha-olefin polymers, (d) polybutadiene polymers, (e) ethylene-propylene copolymers, (f) poly(ethylene-co-(C4-C 20 The method of any one of embodiments 1-8, comprising any one of (a)-(g): (i) an alpha-olefin) copolymer, and (g) an ethylene-propylene-butadiene copolymer. The method may comprise (i) and (a), or (vi) and (f).
[0027] Embodiment 10. The method of any one of embodiments 1 to 9, wherein the first polyolefin polymer or the HMW polyolefin component (as the case may be) has a weight average molecular weight of at least 110,000 grams per mole (g / mol), alternatively from 130,000 to 1,900,000 g / mol, alternatively from 150,000 to 990,000 g / mol.
[0028] Embodiment 11. The method of any one of embodiments 1-10, wherein the polymerization is a gas phase polymerization process and the polymerization reactor is a single gas phase polymerization reactor (e.g., a fluidized bed gas phase polymerization reactor). In other embodiments, the method employs two polymerization reactors, where a first HMW polyolefin component is made by a first ASNM catalyst in a first polymerization reactor and a first LMW polyolefin component is made by a first metallocene catalyst in a second polymerization reactor, or vice versa.
[0029] Aspect 12. (D1) The method further comprises transitioning from step (B) to (B1) feeding a second trim catalyst to a polymerization reactor to produce a second alkane soluble nonmetallocene catalyst (second ASNM catalyst), the second trim catalyst being made by contacting a solution of a second alkane soluble nonmetallocene pre-catalyst (second ASNM pre-catalyst) dissolved in an alkane solvent with an activator, the second ASNM pre-catalyst differing from the first ASNM pre-catalyst in the structure of at least one nonmetallocene ligand, the second ASNM catalyst being different from the first ASNM catalyst in the structure of at least one nonmetallocene ligand. The method of any one of the embodiments 1-11, wherein the second ASNM pre-catalyst is characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane based on the total weight of the second ASNM pre-catalyst and hexane, as measured using a solubility test method, and the transition comprises decreasing the feed of the first trim catalyst from a steady state value until the first trim catalyst is no longer fed to the polymerization reactor, and independently starting and increasing the feed of the second trim catalyst to the polymerization reactor until the second trim catalyst is fed to the polymerization reactor at a steady state value. The trim catalyst transition is useful for transitioning from a steady state polymerization process making a first grade of polyolefin polymer to another steady state polymerization process making a different grade of polyolefin polymer. The second ASNM pre-catalyst differs from the first ASNM pre-catalyst in the structure of at least one nonmetallocene ligand. For example, a first ASNM pre-catalyst can have a ligand of formula (1) described below and a second ASNM pre-catalyst can have a biphenylphenol ligand described below. Alternatively, the first and second ASNM pre-catalysts can have different ligands of formula (1) described below.
[0030] Embodiment 13. Each of the ASNM pre-catalysts independently has a solubility of 0.10 to 25 wt.%, alternatively 0.50 wt.% to 24 wt.%, alternatively 1.0 wt.% to 25 wt.%, alternatively 2.0 wt.% to 25 wt.%, alternatively 3.0 wt.% to 25 wt.%, alternatively 5.0 wt.% to 25 wt.%, alternatively 10.0 wt.% to 25 wt.%, in hexane containing at least 60 weight percent n-hexane (CH3(CH2)4CH3), as measured using the Solubility Test Method. 13. The method of any one of the preceding aspects, characterized by a solubility of from 15% to 25% by weight, alternatively from 20.0% to 25% by weight, alternatively from 0.10 to 20.0% by weight, alternatively from 0.5% to 20.0% by weight, alternatively from 1% to 15% by weight, alternatively from 2% to 15% by weight, alternatively from 3% to 15% by weight, alternatively from 5% to 15% by weight, alternatively from 1.0% to 15% by weight, alternatively from 1.0% to 10.0% by weight. Advantageously, the solubility of the ASNM pre-catalyst(s) in hexane containing at least 60 weight percent n-hexane is improved as compared to the solubility of HN5Zr dibenzyl, which has a solubility of only 0.03% by weight in hexane containing 60 weight percent n-hexane, as measured by the Solubility Test Method.
[0031] A catalyst transition involves ramping down a first catalyst feed from a steady state value to an off (stopped) state, and starting and ramping up a second catalyst (different) feed from an off (not started) state to a steady state value. The ramps up and down may be independent, continuous or intermittent (e.g., periodically, e.g., in stepwise increments), may start at the same time or at different times, may be completed at the same time or at different times, and may take the same or different times. Typically, the period taken by the ramp step overlaps with the period taken by the ramp step by at least 50%, alternatively 79%-100%, alternatively 91%-100%. The time at which the transition period begins is the first part of either the start of the ramp step or the start of the ramp step. The time at which the transition period ends is the end of the ramp step (0 feed rate) or the end of the ramp step (steady state feed rate), whichever is later. A typical transition period may be 1-48 hours, alternatively 2-24 hours, alternatively 3-12 hours.
[0032] The catalyst transition may optionally further include changing one or more other process conditions, such as the reactor temperature, the (co)monomer flow rate(s), the superficial gas velocity within the reactor, and / or, in a continuous reactor (not a batch reactor), the rate at which the polymer product is removed from the reactor.
[0033] Catalyst transfer can be performed in a "closed" polymerization reactor, meaning that the reactor is not shut down or shut down during the transfer. Shutting down a polymerization reactor usually means opening the reactor, purging the open reactor of hydrocarbons with a purge gas (e.g., nitrogen gas), emptying the purged reactor of polymer and catalyst particles, and cleaning the emptied reactor. Alternatively, or in addition, catalyst transfer can be performed without introducing a catalyst "kill" reagent or polymerization neutralizing reagent into the reactor.
[0034] Catalyst transition is useful for transitioning between different grades of the same polyolefin composition (first and second grades) or between different polyolefin polymers (first and second polymers). During the transition, an intermediate grade polymer may be made that is different from the steady-state grade that was started and transitioned. The intermediate grade polymer may have its own use or small amounts of it may be melt blended with other polymers to make useful post-reactor polymer blends.
[0035] The method is useful for liquid phase, slurry phase, or gas phase polymerization reactions. The polymerization reactor can be a reactor configured for liquid phase, slurry phase, or gas phase polymerization of at least one olefin monomer. Reactors and effective polymerization conditions for liquid phase, slurry phase, or gas phase polymerization are well known.
[0036] In some embodiments, the method includes a gas phase polymerization and a gas phase polymerization reactor (e.g., a fluidized bed gas phase polymerization reactor), and the olefin monomer includes ethylene, and optionally, 1-butene, 1-hexene, or 1-octene. In some embodiments, the method does not include Cr, Ti, Mg, or unsubstituted or substituted cyclopentadienyl groups, or Cr, Ti, and Mg, or unsubstituted or substituted cyclopentadienyl groups.
[0037] Alkane-soluble nonmetallocene precatalysts (ASNM precatalysts) The alkane-soluble nonmetallocene pre-catalyst (ASNM pre-catalyst) can be any compound lacking an unsubstituted or substituted cyclopentadienyl group, characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane (CH3(CH2)4CH3), based on the total weight of the ASNM pre-catalyst and hexane, as measured using the Solubility Test Method (Enhanced Solubility), and converted by an activator into an effective catalyst for the polymerization of olefin monomers. The ASNM pre-catalyst can include aprotic solvates and solvent-free embodiments thereof. In any one of the foregoing aspects, the ASNM pre-catalyst can be any one of those described in the following numbered embodiments and examples.
[0038] Embodiment 1. The ASNM pre-catalyst can be any one of the biphenylphenol pre-catalysts described in paragraphs
[0036] to
[0080] and
[0104] of US2018 / 0002464A1, or paragraph
[0080] of US2018 / 0002464A1, or paragraph
[0104] of US2018 / 0002464A1, or biphenylphenol pre-catalyst (5) of Figure 4. In some aspects, the biphenylphenol pre-catalyst is a compound characterized by a solubility of 0.10 to 25 wt%, alternatively 1 wt% to 20.0 wt%, alternatively 0.5 wt% to 15 wt%, in hexane containing at least 60 weight percent n-hexane, as measured using the Solubility Test Method.
[0039] Embodiment 2. The ASNM precatalyst can be a compound of formula (1) in Figure 2, where M is a group 4 metal and each R is independently selected from silicon-containing organic solubilizing groups and silicon-free organic solubilizing groups. By "solubilizing" it is meant that the R groups together provide improved solubility to compound (1), which can be described as HN5MR2. In some aspects, at least one R is a silicon-containing organic solubilizing group and the other R is a silicon-containing organic solubilizing group or a silicon-free organic solubilizing group. In some aspects, each R is independently a silicon-containing organic solubilizing group. In some aspects, each R is independently an unsubstituted or substituted quaternary silahydrocarbyl group. Each quaternary silahydrocarbyl group contains a quaternary silicon atom and a (C1-C3) alkylene, or a (C7-C8) aryl alkylene, or a (C1-C3) alkylene, or a (C7-C8) aryl alkylene, or a (C1-C2) hydrocarbylene. The (C1-C3) alkylene or the (C7-C8) aryl alkylene is disposed between the quaternary silicon atom and the metal M. Thus, the quaternary silicon atom is indirectly bonded to the metal M via the (C1-C3) alkylene or the (C7-C8) aryl alkylene (e.g., benzylene), which in turn is directly bonded to the metal M (e.g., M-CH2-phenylene-). The quaternary silicon atom is an element having atomic number 14 in the periodic table of elements, and is bonded to four carbon atoms, one of which is (C1-C 3) A carbon atom of an alkylene or (C7-C8)arylalkylene. In some embodiments, each R is independently a silicon-free organic solubilizing group. In some embodiments, each R group is unsubstituted.
[0040] Embodiment 3. The ASNM pre-catalyst can be compound (1) as described in embodiment 2, wherein at least one, or each R is independently represented by the formula -(C(R A )2) m QZR 1 R 2 R 3 where the subscript m is 1, 2, or 3; and each R Ais independently H or (C-C)alkyl, or each R A But R A′ -R A′ Combined together as R A′ -R A′ is (C1-C3)alkylene; each Q is independently absent, (C1-C3)alkylene, or unsubstituted or substituted phenylene; each Z is independently C or Si; and each R 1 , R 2 , and R 3 are independently unsubstituted or substituted with one or more substituents (C1-C 15 )alkyl, each substituent independently selected from unsubstituted (C1-C5)alkyl, halogen, -Oalkyl, -N(alkyl)2, and -Si(alkyl)3, provided that in some embodiments, when subscript m is 2, the resulting (C(R A )2) m is C(R A )2CH(R A ) or C(R A )2CH2, but when the subscript m is 3, (C(R A )2) m But, C(R A )2CH(R A )C(R A )2 or C(R A )2CH2C(R A )2. The optional provisos are intended to exclude compounds that may be susceptible to beta-hydrogen elimination. In some embodiments, the subscript m is 2 or 1. In some embodiments, each R Ais independently H or unsubstituted (C1-C4) alkyl, or H or methyl, or H. In some embodiments, each Q is absent. In some embodiments, at least one, or each Q, is present. When present, each Q can independently be (C1-C3) alkylene, or CH2, or CH2CH2, or CH2CH2CH2, or CH2CH(CH3). Alternatively, each Q can independently be unsubstituted 1,4-phenylene, unsubstituted 1,3-phenylene, or unsubstituted 1,2-phenylene, or can be selected from any two of unsubstituted 1,4-, 1.3-, and 1,2-phenylene, or unsubstituted 1,2-phenylene, or unsubstituted 1,3-phenylene, or unsubstituted 1,4-phenylene. 1,2-phenylene is benzene-1,2-diyl, 1,3-phenylene is benzene-1,3-diyl, and 1,4-phenylene is benzene-1,4-diyl. By "unsubstituted phenylene" is meant that the phenylene is of the formula CH.
[0041] Embodiment 4. The ASNM pre-catalyst can be compound (1) described in Example 2 or 3, wherein at least one, or each R is independently -CH2SiR 1 R 2 R 3 And each R 1 , R 2 , and R 3 are independently unsubstituted (C1-C 15 )alkyl, or (C1-C3)alkyl, or methyl. In some embodiments, one R is -CH2SiR 1 R 2 R 3 and the other R is unsubstituted (C1-C 15 ) alkyl.
[0042] Embodiment 5. The ASNM pre-catalyst can be compound (1) as described in Examples 2, 3, or 4, wherein at least one or each R is -CH2-(unsubstituted phenylene)-ZR 1 R 2 R 3each Z is Si or C, each unsubstituted phenylene is unsubstituted 1,4-phenylene, unsubstituted 1,3-phenylene, or unsubstituted 1,2-phenylene, and each R 1 , R 2 , and R 3 are independently unsubstituted (C1-C 15 )alkyl, or (C1-C3)alkyl, or methyl. In some embodiments, one R is -CH2SiR 1 R 2 R 3 and the other R is tert-butyl-phenylmethyl. At least one or each Z can be Si or C.
[0043] Embodiment 6. The ASNM pre-catalyst can be compound (1) described in embodiment 2, where each R is independently CH2Si(CH3)3 or CH2-(phenylene)-SiR 1 R 2 R 3 (i) R 1 and R 2 is methyl, and R 3 But unsubstituted (C2-C 15 ) alkyl, or unsubstituted (C3-C5) alkyl, or unsubstituted (C6-C 15 ) alkyl; or (ii) each R 1 , R 2 , and R 3 is methyl.
[0044] Embodiment 7. The ASNM pre-catalyst can be compound (1) described in embodiment 2, where one R is CH2Si(CH3)3 or CH2-(phenylene)-SiR 1 R 2 R 3 (i) R 1 and R 2 is methyl, and R 3 But unsubstituted (C2-C 15 ) alkyl, or unsubstituted (C-C) alkyl; or (ii) R 1 , R 2 , and R 3Each of R is methyl and the other R is a quaternary alkyl-substituted (C7-C8) arylalkyl group or an unsubstituted (C1-C 15 ) alkyl group. In some embodiments, the quaternary alkyl-substituted (C7-C8) arylalkyl group is tert-butyl-phenylmethyl (i.e., 1,1-dimethylethylphenylmethyl), or CH2-(1,4-phenylene)-C(CH3)3. In other embodiments, the other R is methyl, 2,2-dimethylpropyl, 2,2-dimethylhexyl, or hexyl, 2-ethylhexyl.
[0045] Embodiment 8. The ASNM pre-catalyst can be compound (1) as described in embodiment 6 or 7, where phenylene is (i) unsubstituted 1,4-phenylene, (ii) unsubstituted 1,3-phenylene, or (iii) unsubstituted 1,2-phenylene. The phenylene can be unsubstituted 1,4-phenylene.
[0046] Embodiment 9. The ASNM pre-catalyst can be compound (1) as described in any one of embodiments 2-8, wherein each R can be independently the same or different and can be selected from trimethylsilylmethyl, dimethylethylsilylmethyl, dimethyl(n-propyl)silylmethyl, dimethyl(n-butyl)silylmethyl, dimethyl(n-pentyl)silylmethyl, dimethyl(n-hexyl)silylmethyl, dimethyl(n-heptyl)silylmethyl, dimethyl(n-octyl)silylmethyl, dimethyl(n-decyl)silylmethyl, dimethyl(n-dodecyl)silylmethyl, triethylsilylmethyl, methyldiethylsilylmethyl, dimethyl(2-ethylhexyl)silylmethyl, dimethyl(trimethylsilylmethyl)silylmethyl, dimethyl(3,3-dimethylbutyl)silylmethyl, dimethyl(1,1-dimethylethyl)silylmethyl, and dimethyl(2-methylpropyl)silylmethyl.
[0047] Embodiment 10. The ASNM pre-catalyst is compound (1A) of FIG.
[0048] Embodiment 11. An embodiment in which each R is independently a silicon-free organic solubilizing group. The ASNM pre-catalyst can be compound (1) described in embodiment 2, wherein each R is independently methyl, an unsubstituted (C2-C4) alkyl group, an unsubstituted (C5-C6) alkyl group, an unsubstituted (C7-C8) alkyl group, an unsubstituted (C9-C10) alkyl group, an unsubstituted (C11-C12) alkyl group, an unsubstituted (C12-C13) alkyl group, an unsubstituted (C13-C14) alkyl group, an unsubstituted (C14-C15) alkyl group, an unsubstituted (C15-C16) alkyl group, an unsubstituted (C16-C17) alkyl group, an unsubstituted (C17-C18) alkyl group, an unsubstituted (C18-C19) alkyl group, an unsubstituted (C19-C20) alkyl group, an unsubstituted (C2-C40) alkyl group, an 12 ) alkyl groups (e.g., unsubstituted (C5-C9) alkyl groups, or unsubstituted (C 10 -C 12 ) alkyl group), unsubstituted or substituted quaternary arylalkyl group, or both R groups are bonded together to give R'-R', where R'-R' is unsubstituted or substituted (aryl) alkylene. Each R group and R'-R' group according to embodiment 11 does not include a cyclopentadienyl group, a silicon atom, a carbon-carbon double bond, and a carbon-carbon triple bond. Each substituent can be independently selected from unsubstituted (C1-C5) alkyl, halogen, -O alkyl, and -N(alkyl)2. Each quaternary arylalkyl group sequentially includes a quaternary alkyl, a phenylene, and a (C1-C3) alkylene linker. The quaternary alkyl is bonded to the phenylene which is bonded to the (C1-C3) alkylene linker which is bonded to the metal M. The (C1-C3) alkylene linker and the R'-R' group are divalent. The quaternary alkyl contains a quaternary carbon atom which can be bonded directly or indirectly to the phenylene. A quaternary carbon atom is an element having atomic number 6 in the periodic table of the elements and is bonded to four other carbon atoms.
[0049] Embodiment 12. The ASNM pre-catalyst can be compound (1) as described in embodiment 11, wherein each R is independently methyl, an unsubstituted (C2-C4) alkyl group, or an unsubstituted (C5-C 12 ) alkyl group (e.g., an unsubstituted (C5-C9) alkyl group). In some embodiments, each R is methyl, or each R is an unsubstituted (C2-C4) alkyl group, or each R is an unsubstituted (C5-C9) alkyl group, or one R is methyl and the other R is an unsubstituted (C5-C9) alkyl group. In some embodiments, the unsubstituted (C5-C9) alkyl group is 2,2-dimethylpropyl (neopentyl).
[0050] Embodiment 13. The ASNM pre-catalyst can be compound (1) as described in embodiment 11, where both R groups are bonded together to give R'-R', where R'-R' is an unsubstituted or substituted alkylene, or a substituted (C4-C5) alkylene. In some aspects, R'-R' is -(CH2)3C(H)(R 4 )CH2- or -CH2(C(R 4 )))2CH2-, where each R 4 is independently unsubstituted (C1-C5) alkyl. R'-R' may be 2,2,3,3-tetramethylbutane-1,4-diyl or 2-(2',2'-dimethylpropyl)-pentane-1,5-diyl.
[0051] Embodiment 14. The ASNM pre-catalyst can be compound (1) as described in embodiment 11, where both R groups are bonded together to give R'-R', and R'-R' is a substituted aryl alkylene, or alternatively, 4-(unsubstituted (C1-C5) alkyl)-1,2-bezene dimethylene. The 4-(unsubstituted (C1-C5) alkyl)-1,2-bezene dimethylene is -CH2-[4-(unsubstituted (C1-C5) alkyl-(1,2-phenylene)]-CH2-. In some aspects, the 4-(unsubstituted (C1-C5) alkyl)-1,2-bezene dimethylene is 4-(2,2-dimethylpropyl)-1,2-benzene dimethylene (i.e., -CH2-[4-(CH3C(CH3)2CH2)-(1,2-phenylene)]-CH2-).
[0052] Embodiment 15. The ASNM pre-catalyst can be compound (1) according to any one of embodiments 11-14, wherein each R is the same or different and is independently selected from methyl, 2,2-dimethylpropyl, 2,2-dimethylhexyl, 2,2-dimethyloctyl, 2-ethylhexyl, 2-ethyloctyl, 2-tert-butylphenylmethyl, 3-tert-butylphenylmethyl, 4-tert-butylphenylmethyl, 2-ethylphenylmethyl, 3-n-butylphenylmethyl, 4-n-butylphenylmethyl, 2-n-butylphenylmethyl, 3-ethylphenylmethyl, 4-ethylphenylmethyl, 2-n-octylphenylmethyl, 3-n-octylphenylmethyl, and 4-n-octylphenylmethyl. In some aspects, each R is the same.
[0053] Embodiment 16. The ASNM pre-catalyst is compound (1B), (1C), (1D), or (1E) of Figure 2. In some aspects, compound (1) is any one of compounds (1A)-(1E), or compound (1) is selected from any four of compounds (1A)-(1E), or compound (1) is compound (1B) or (1C), or compound (1) is compound (1D) or (1E), or compound (1) is compound (1A), or compound (1) is compound (1B), or compound (1) is compound (1C), or compound (1) is compound (1D), or compound (1) is compound (1E).
[0054] Embodiment 17. The ASNM pre-catalyst can be compound (1) according to any one of embodiments 2 to 16, wherein M is Zr. In other aspects, M is Hf.
[0055] Embodiment 18. The ASNM pre-catalyst of any one of embodiments 1 to 17, characterized by a solubility of 0.50 to 24 wt % in hexane containing at least 60 weight percent n-hexane (CH3(CH2)4CH3).
[0056] Synthesis of compound (1) The compound of formula (1) can be prepared by reacting a compound of formula (2) in FIG. 3 (wherein M is as defined for compound (1) and each X is independently Cl, Br, or I) with a compound of formula X 1 MgR or M 1 R n (R is as defined for compound (1) according to any one of the preceding embodiments; X 1 is Cl, Br, or I, and M 1 is selected from Li, Zn, Sn, and Cu, the subscript n is an integer from 1 to 4, and M 1 (equivalent to the formal oxidation state of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 6
[0057] The synthesis of compound (1) can be carried out by reacting a compound represented by formula (3) in FIG. 10 But independently, (C1-C 15 )alkyl, or (C1-C6)alkyl), with a reagent of formula X-Si(CH3)3, where X is as defined for the synthesis of compound (2), in an aprotic solvent under reaction conditions effective to synthesize compound (2).
[0058] The synthesis of compound (1) can be carried out by reacting a compound of formula (4) of FIG. 3 with a compound of formula M(N(R 10 2) 4 (wherein M is as defined for compound (1), and each R 10 However, independently (C1-C 15 ) alkyl) in an aprotic solvent under effective reaction conditions to synthesize compound (3). 10 are independently 6) M(N(R 10 The molar ratio of 2) to 4 can be from 1:10 to 10:1.
[0059] The aprotic solvent may independently be a hydrocarbon solvent such as an alkylarenes (e.g., toluene, xylene), an alkane, a chlorinated aromatic hydrocarbon (e.g., chlorobenzene), a chlorinated alkane (e.g., dichloromethane), a dialkyl ether (e.g., diethyl ether), or a mixture of any two or more thereof.
[0060] The synthesis may be carried out under effective reaction conditions. Effective reaction conditions may include techniques for manipulating reactants such as air-sensitive and / or moisture-sensitive reagents, as well as Schlenk line techniques and inert gas atmospheres (e.g., nitrogen, helium, or argon). Effective reaction conditions may also include sufficient reaction time, sufficient reaction temperature, and sufficient reaction pressure. Each reaction temperature may independently be from -78°C to 120°C, alternatively from -30°C to 30°C. Each reaction pressure may independently be from 95 to 105 kPa, alternatively from 99 to 103 kPa. The progress of any particular reaction step may be monitored by analytical methods such as nuclear magnetic resonance (NMR) spectroscopy or mass spectrometry. Reaction times may independently be from 30 minutes to 48 hours.
[0061] Compound (1) solves the instability problem of conventional alkane-insoluble non-MCN precatalysts because compound (1) can be stored as a solution in an alkane without activator.
[0062] The embodiment of the trim catalyst made from compound (1) and an activator ignites faster than the comparative catalyst system made from HN5Zr dibenzyl and the same activator. Furthermore, compound (1) can produce polyethylene with the same MWD as the polyethylene made by the comparative catalyst system. The faster light-off of the trim catalyst system made from compound (1) and an activator can advantageously result in reduced fouling of the distributor plate of a gas phase polymerization reactor containing a recycle loop (some polymer particles containing active catalyst are returned to the reactor, where they can grow and cause fouling of the distributor plate). The faster light-off of the trim catalyst can be characterized by a shorter time to maximum temperature as measured in vitro using 1-octene as the monomer according to the light-off test method described below.
[0063] The trim catalyst (e.g., made from compound (1) and an activator) allows for the production of polyethylene resins with a smaller percentage of particles characterized as "fines" as defined below. There are many well-known reasons why fines can cause problems in the operation of gas-phase polymerization reactors with recycle tubes and / or extended top sections, such as UNIPOL™ reactors from Univation Technologies, LLC or other reactors. Fines are known to result in an increased tendency to settle and sheet in such reactors. Fines can increase particle carryover from the reactor to the recycle tube and cause fouling inside the recycle loop, such as heat exchangers, compressors, and / or distributor plates. Fines can also accumulate in the extended sections of the reactor, as they are believed to be more susceptible and / or sensitive to electrostatic forces. Fines can also cause problems in polyethylene polymers made by gas-phase polymerization in such reactors. The fines may continue to polymerize in the lower temperature zones of the reactor, either in the recycle loop or in the expansion section, producing polyethylene with a higher molecular weight than is targeted in the bulk fluidized bed. The fines may eventually return from the recycle loop back to the fluidized bed and then back to the polyethylene product, resulting in higher gel levels in the polyethylene product. Polyethylene resins made with a trim catalyst made from compound (1) and an activator have a reduced weight percent fines.
[0064] The trim catalyst (e.g., made from compound (1) and an activator) allows for the production of polyethylene resins having a particle size larger than that of polyethylene resins made by a comparative catalyst system made from HN5Zr dibenzyl and the same activator. The larger particle size of the polyethylene resins made by the catalyst system of the present invention can be useful for reducing the settled bulk density of the resin. Resins with a higher percentage of fines can have a higher settled bulk density because the smaller particles of fines can move down and fill the spaces between the larger particles. If the settled bulk density is too high, the resin can be difficult to fluidize, causing localized overheating and forming resin chunks in certain areas of the reactor process, such as near the edges of the distributor plate or in the product discharge system.
[0065] The polyethylene resin can be made using a bimodal catalyst system where an alkane solution of the (first or second) ASNM catalyst is used as the trim catalyst (second portion) and a combination of all of the MCN pre-catalyst, activator, and the remaining (first or second) ASNM catalyst is used as the first portion, and the all portion combination feed method can have reduced gel content compared to a polyethylene resin made using the same bimodal catalyst system except that supported HN5Zr dibenzyl is used as the trim catalyst and the remaining HN5Zr dibenzyl and the same MCN pre-catalyst are used as the first portion. Since the (first or second) ASNM catalyst has a solubility in hexane containing at least 60 weight percent n-hexane that is significantly higher than the solubility of HN5Zr dibenzyl, the (first or second) ASNM catalyst can be fed as an alkane solution (e.g., typically in mineral oil) as the trim catalyst in the "partial combination" feeding method described above, thereby providing a trim bimodal catalyst system that can be mixed with the bimodal catalyst system in an in-line mixer to make a bimodal polyethylene composition without the increased gel content seen with HN5Zr dibenzyl for the reasons described above, thus solving the previous gel problem.
[0066] A hydrocarbon solvent is a liquid material at 25°C, consisting of carbon and hydrogen atoms, and optionally one or more halogen atoms, and does not contain carbon-carbon double bonds and carbon-carbon triple bonds. The hydrocarbon solvent can be an alkane, an arene (toluene), or an alkyl arene (i.e., arylalkane, xylene). Examples of hydrocarbon solvents are alkanes such as mineral oil, Isopar-C, Isopar-E, and mineral oils such as white mineral oil, pentane, hexane (e.g., hexane containing at least 60 weight percent n-hexane), heptane, octane, nonane, decane, undecane, dodecane, hexane, 1-methylpentane (isohexane), heptane, 1-methylhexane (isoheptane), octane, nonane, decane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, methylcyclopentane, methylcyclohexane, dimethylcyclopentane, or a mixture of any two or more thereof. Alternatively, the method may be free of mineral oil.
[0067] Hexane containing at least 60 weight percent n-hexane is essentially a mixture of the formula CH and not 60% to 70% n-hexane, 40% to 10% n-hexane. 14 and 0% to 30% by weight methylcyclopentane. In some embodiments, the alkane mixture is 60% to 70% by weight n-hexane, 40% to 30% by weight of one or more compounds of the formula CH that are not n-hexane. 14 In another embodiment, the alkane mixture consists essentially of one or more compounds of the formula CH that are not n-hexane, and does not include methylcyclopentane. 14 and greater than 0% to 30% by weight of methylcyclopentane (e.g., 20% to 30% by weight of methylcyclopentane). 14Examples of compounds of the formula are 2-methylpentane, 3-methylpentane, and mixtures thereof. The phrase "consisting essentially of" means free of solvents other than the aforementioned alkanes. Hexane, containing at least 60 weight percent n-hexane, may be anhydrous and / or free of dissolved molecular oxygen.
[0068] The metallocene pre-catalyst can be any one of the metallocene catalyst components described in US 7,873,112 B2, column 11, line 17 to column 22, line 21. In some embodiments, the metallocene pre-catalyst is selected from the metallocene pre-catalyst species named in US 7,873,112 B2, column 18, line 51 to column 22, line 5. In some embodiments, the metallocene pre-catalyst is a bis(η 5 -Tetramethylcyclopentadienyl)zirconium dichloride, bis(η 5 -Tetramethylcyclopentadienyl)zirconium dimethyl, bis(η 5 -Pentamethylcyclopentadienyl)zirconium dichloride, bis(η 5 In some embodiments, the metallocene pre-catalyst is selected from the group consisting of bis(n-propylcyclopentadienyl)hafnium dichloride, bis(n-propylcyclopentadienyl)hafnium dimethyl, bis(n-butylcyclopentadienyl)zirconium dichloride, and bis(n-butylcyclopentadienyl)zirconium dimethyl. In some embodiments, the metallocene pre-catalyst is an activated reaction product of an activator and any one of the foregoing metallocene pre-catalysts.
[0069] The ASNM and MCN catalysts can be made under effective activation conditions. Effective activation conditions can include techniques for operating the catalyst, such as an in-line mixer, a catalyst preparation reactor, and a polymerization reactor. Activation can be carried out under an inert gas atmosphere (e.g., nitrogen, helium, or argon). Effective activation conditions can also include a sufficient activation time and a sufficient activation temperature. Each activation temperature can be independently 20°C to 800°C, or alternatively 300°C to 650°C. Activation times can be 10 seconds to 2 hours.
[0070] An activator, also known as a cocatalyst, is a compound or composition, including a combination of reagents, that increases the rate at which a transition metal compound (e.g., compound (1) or a metallocene precatalyst) oligomerizes or polymerizes an unsaturated monomer, such as an olefin, such as ethylene or 1-octene. The activator may also affect the molecular weight, degree of branching, comonomer content, or other properties of the oligomer or polymer (e.g., polyolefin). The transition metal compound (e.g., compound (1) or a metallocene precatalyst) may be activated for oligomerization and / or polymerization catalysis in any manner sufficient to permit coordination or cationic oligomerization and / or polymerization. Typically, the activator contains aluminum and / or boron, or aluminum. Examples of suitable activators are alkylaluminoxanes and trialkylaluminum compounds.
[0071] Aluminoxane activators (also known as alumoxanes) can be utilized as activators for one or more precatalyst compositions including compound (1) or metallocene precatalysts. Aluminoxane(s) are generally oligomeric compounds containing --Al(R)--O-- subunits, where R is an alkyl group, and are referred to as alkylaluminoxanes (alkylaluminoxanes). Alkylaluminoxanes can be unmodified or modified. Examples of alkylaluminoxanes include methylaluminoxane (MAO), modified methylaluminoxane (MMAO), ethylaluminoxane, and isobutylaluminoxane. Unmodified and modified alkylaluminoxanes are suitable as activators for precatalysts such as compound (1). Mixtures of different aluminoxanes and / or different modified aluminoxanes may also be used. For further description, see U.S. Patent Nos. 4,665,208, 4,952,540, 5,041,584, 5,091,352, 5,206,199, 5,204,419, 4,874,734, 4,924,018, 4,908,463, 4,968,827, 5,329,032, 5,248,801, 5,235,081, 5,157,137, 5,103,031, and EP 0 561 476, EP 0 279 586, EP 0 516 476, EP 0 594 218, and PCT Publication No. WO94 / 10180.
[0072] When the activator is an aluminoxane (modified or unmodified), the maximum amount of activator can be selected to be a 5,000-fold molar excess of the precursor, based on the molar ratio of the moles of Al metal atom in the aluminoxane to the moles of metal atom M (e.g., Zr or Hf) in the pre-catalyst (e.g., compound (1)). Alternatively, or in addition, the minimum amount of activator to pre-catalyst precursor can be a 1:1 molar ratio (Al / M).
[0073] Trialkylaluminum compounds can be utilized as activators for precatalysts (e.g., Compound (1) or metallocene precatalysts) or as scavengers to remove residual water from a polymerization reactor prior to its start-up. Examples of suitable alkylaluminum compounds are trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, and tri-n-octylaluminum.
[0074] The support material is a particulate solid that can be non-porous, semi-porous, or porous. The carrier material is a porous support material. Examples of support materials are talc, inorganic oxides, inorganic chlorides, zeolites, clays, resins, and mixtures of any two or more thereof. Examples of suitable resins are functionalized or crosslinked organic supports such as polystyrene, polystyrene divinylbenzene polyolefins, etc.
[0075] Inorganic oxide support materials include oxides of metals of groups 2, 3, 4, 5, 13, or 14. Preferred supports include silica, which may or may not be dehydrated, fumed silica, alumina (see, for example, PCT Publication No. WO 99 / 60033), silica-alumina, and mixtures thereof. Other useful supports include magnesia, titania, zirconia, magnesium chloride (U.S. Pat. No. 5,965,477), montmorillonite (EP 0 511665), phyllosilicates, zeolites, talc, clays (U.S. Pat. No. 6,034,187), and the like. Combinations of these support materials may also be used, such as silica-chromium, silica-alumina, silica-titania, and the like. Additional support materials may include those porous acrylic polymers described in EP 0 767 184, which is incorporated herein by reference. Other support materials include nanocomposites as disclosed in PCT Publication No. WO 99 / 47598, aerogels as disclosed in PCT Publication No. WO 99 / 48605, spherulites as disclosed in U.S. Patent No. 5,972,510, and polymer beads as disclosed in PCT Publication No. WO 99 / 50311.
[0076] The supporting material is approximately 10 m 2 / g~about 700m 2 / g range, approximately 0.1 cm 3 / g ~ approx. 4.0cm 3 The support material may have a pore volume in the range of 100 / g and an average particle size in the range of about 5 microns to about 500 microns. The support material may be silica (e.g., fumed silica), alumina, clay, or talc. The fumed silica may be hydrophilic (untreated) or hydrophobic (treated). In some aspects, the support is a hydrophobic fumed silica, which may be prepared by treating untreated fumed silica with a hydrophobic agent, such as dimethyldichlorosilane, polydimethylsiloxane fluid, or hexamethyldisilazane. In some aspects, the treating agent is dimethyldichlorosilane. In one embodiment, the support is Cabosil™ TS-610.
[0077] The one or more pre-catalysts and / or the one or more activators may be deposited, contacted, vaporized, bound or incorporated, adsorbed or absorbed onto one or more supports or carrier materials.
[0078] The metallocene precatalyst may be spray dried according to the general methods described in US 5648310. The supports used with compound (1) and any other precatalysts may be functionalized as generally described in EP 0 802 203 or may have at least one substituent or leaving group selected as described in US 5688880.
[0079] Polymerization reactor and method Liquid phase and / or slurry phase polymerization of olefin monomer(s) is well known, see for example US8291115B2.
[0080] Gas phase polymerization (GPP) is well known. For polymerization, GPP reactors such as stirred bed gas phase polymerization reactors (SB-GPP reactors) or fluidized bed gas phase polymerization reactors (FB-GPP reactors) are used. Such reactors and methods are generally well known. For example, the FB-GPP reactor / method may be one described in any one of US 3,709,853, US 4,003,712, US 4,011,382, US 4,302,566, US 4,543,399, US 4,882,400, US 5,352,749, US 5,541,270, US 2018 / 0079836 A1, EP-A-0 802 202, and Belgian Patent No. 839,380. These SB-GPP and FB-GPP polymerization reactors and processes are either mechanically agitated or fluidized by continuous flow of the polymerization medium of gaseous monomer and diluent inside the reactor, respectively. Other useful reactors / processes contemplated include continuous or multi-stage polymerization processes such as those described in US 5,627,242, US 5,665,818, US 5,677,375, EP-A-0 794 200, EP-B1-0 649 992, EP-A-0 802 202, and EP-B-634421.
[0081] Gas phase polymerization operating conditions are any variable or combination of variables that can affect the polymerization reaction in the GPP reactor or the composition or properties of the polyolefin copolymer composition product produced thereby. Variables can include reactor design and size, precatalyst composition and amount, reactant composition and amount, molar ratio of two different reactants, presence or absence of feed gas such as H2, molar ratio of feed gas to reactant, absence or concentration of interfering substances (e.g., H2O and / or O2), presence or absence of induced condensing agent (ICA), polymer mean residence time in the reactor, component partial pressure, monomer feed rate, reactor bed temperature (e.g., fluidized bed temperature), nature or sequence of process steps, transition period between steps. Variables other than those described or changed by the method or use may be kept constant.
[0082] The GPP methodology uses ethylene ("C2"), hydrogen ("H2"), and 1-hexene ("C6" or "C where x is 6"). x ") to provide a fixed molar ratio of comonomer to ethylene monomer gas (C) equal to the stated value (e.g., 0.00560 or 0.00703). x Maintain a constant molar ratio of hydrogen to ethylene gas ("H2 / C2") equal to a stated value (e.g., 0.00229 or 0.00280), and a constant partial pressure of ethylene ("C2") equal to a stated value (e.g., 1000 kPa). Measure the concentration of gases by an in-line gas chromatograph to understand and maintain the composition of the recycle gas stream. Maintain the reaction bed of growing polymer particles in a fluidized state by continuously flowing make-up feed and recycle gas through the reaction zone. Use a superficial gas velocity of 0.49 to 0.67 meters per second (m / s) (1.6 to 2.2 feet per second (ft / s)). Operate the FB-GPP reactor at a total pressure of about 2344 to about 2413 kilopascals (kPa) (about 340 to about 350 pounds per square inch gauge (psig)), and a first reactor bed temperature, RBT, as stated. The fluidized bed is maintained at a constant height by withdrawing a portion of the bed at a rate equal to the production rate of the particulate form of the polyolefin polymer composition, which can be 10 to 20 kilograms per hour (kg / hr). The product polyolefin polymer composition is semi-continuously withdrawn through a series of valves into a fixed volume chamber, and the withdrawn bimodal ethylene-co-1-hexene copolymer composition is purged to remove entrained hydrocarbons and treated with a humidified nitrogen (N2) gas stream to deactivate traces of residual catalyst.
[0083] The catalyst system may be fed to the polymerization reactor(s) in "dry mode" or "wet mode", or in dry mode, or in wet mode. Dry mode is as a dry powder or granules. Wet mode is as a suspension in an inert liquid such as mineral oil.
[0084] Induced Coagulant (ICA). An inert liquid useful for cooling the material in the GPP reactor(s). Its use is optional. ICA is a type of (C5-C20 ) an alkane, such as 2-methylbutane (i.e., isopentane). See US 4,453,399, US 4,588,790, US 4,994,534, US 5,352,749, US 5,462,999, and US 6,489,408. The ICA concentration in the reactor can be 1-10 mol%.
[0085] The GPP conditions may further include one or more additives such as chain transfer agents or accelerators. Chain transfer agents are well known and may be alkyl metals such as diethyl zinc. Accelerators are known such as in US 4,988,783 and may include chloroform, CFCl3, trichloroethane, and difluorotetrachloroethane. A scavenger may be used to react with moisture prior to reactor start-up and with excess activator during reactor transition. The scavenger may be trialkylaluminum. The GPP may be operated without a scavenger (not intentionally added). The GPP reactor / process may further include a quantity (e.g., 0.5-200 ppm based on all feeds to the reactor) of a static control agent and / or a continuity additive such as aluminum stearate or polyethyleneimine. A static control agent may be added to the FB-GPP to inhibit the formation or accumulation of static charge in the FB-GPP.
[0086] The GPP reactor can be a commercial-scale FB-GPP reactor, such as a UNIPOL™ reactor or a UNIPOL™ II reactor, available from Univation Technologies, LLC, a subsidiary of The Dow Chemical Company (Midland, Michigan, USA).
[0087] Any compound, composition, formulation, material, mixture, or reaction product herein may be any of the following: H, Li, Be, B, C, N, O, F, Na, Mg, Al, Si, P, S, Cl, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Br, Rb, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, I, Cs, Ba, Hf, Ta, W, Re, Os, Ir, Pt , Au, Hg, Tl, Pb, Bi, lanthanides, and actinides, except for chemical elements required by the compound, composition, formulation, material, mixture, or reaction product (e.g., Zr required by zirconium compounds, or C and H required by polyethylene, or C, H, and O required by alcohol).
[0088] definition Alkane (solvent). Formula C n H 2n+2 and / or one or more acyclic compounds of formula C m H 2m wherein the subscripts n and m are independently an integer from 5 to 50 (e.g., 6).
[0089] Bimodal. Has two (only) maxima in the frequency distribution. Used as bimodal polymer composition or bimodal catalyst system. Bimodal catalyst system contains two different catalysts to make a bimodal polymer composition, consisting essentially of a high molecular weight (HMW) component and a low molecular weight (LMW) component. Bimodal polymer compositions include post-reactor blends (LMW and HMW components are synthesized separately at different times in different reactors or in the same reactor, and then blended together by melt extrusion or the like) and reactor blends (LMW and HMW components are synthesized in the same reactor). Bimodal copolymer compositions can be characterized by two peaks separated by a discernible local minimum in a plot of dW / dLog(MW) on the y-axis against Log(MW) on the x-axis to obtain a gel permeation chromatograph (GPC) chromatogram, where Log(MW) and dW / dLog(MW) are as defined herein and measured by the GPC test method described herein.
[0090] Dry. Generally, moisture content of 0 to less than 5 parts per million, based on total weight. The materials fed to the reactor(s) during the polymerization reaction are dry.
[0091] High molecular weight (HMW) components. A subgroup of macromolecules that have a peak in a GPC plot of dW / dLog(MW) on the y-axis versus Log(MW) on the x-axis, and are of high molecular weight.
[0092] Hydrocarbyl. A monovalent radical derived from a hydrocarbon compound consisting of C and H atoms by removing an H atom.
[0093] Hydrocarbylene, a divalent radical of the type derived from a hydrocarbon compound consisting of a C atom and an H atom by removing two H atoms, the two H atoms being removed from different carbon atoms of the hydrocarbon compound.
[0094] Inert. Generally, not (appreciably) reactive in or not (appreciably) interfering with the polymerization reaction of the present invention. The term "inert" as applied to the purge gas or ethylene feed means a molecular oxygen (O2) content of 0 to less than 5 parts per million, based on the total weight of the purge gas or ethylene feed.
[0095] Low molecular weight (LMW) components. A subgroup of macromolecules that have a peak in a GPC plot of dW / dLog(MW) on the y-axis versus Log(MW) on the x-axis, and are of low molecular weight.
[0096] Metallocene catalysts. Homogeneous or heterogeneous materials containing (substituted or unsubstituted)-cyclopentadienyl ligand-metal complexes to enhance the rate of olefin polymerization reactions. Single-site or dual-site in nature. Each metal is a transition metal, Ti, Zr, or Hf.
[0097] Multimodal. Has two or more maxima in the frequency distribution.
[0098] Ziegler-Natta catalyst. A heterogeneous material that enhances the polymerization reaction rate of olefins and is prepared by contacting an inorganic titanium compound, such as a titanium halide supported on a magnesium chloride support, with an activator.
[0099] or precedes different embodiments. ASTM is ASTM International, West Conshohocken, Pennsylvania, USA, a standardization organization. Any comparative examples are used for illustrative purposes only and are not prior art. Not containing or lacking means completely absent or undetectable. Terms used herein have their IUPAC meaning unless otherwise defined. See, e.g., Compendium of Chemical Terminology. (Gold Book, ed. 2.3.3, Feb. 24, 2014) IUPAC is IUPAC Secretariat, Research Triangle Park, North Carolina, USA). Periodic Table of Elements, May 1, 2018 edition of IUPAC. May is not required, granting latitude of choice. Operative means functionally capable or effective. Optional(ly) means absent (or excluded) or present (or included). Properties can be measured using standard tests and conditions. Ranges include endpoints, subranges, and integer and / or fractional values subsumed therein, but integer ranges do not include fractional values. Room temperature: 23°C ± 1°C. "HN5" is not pentazole. EXAMPLES
[0100] Isoparaffinic fluid: ISOPAR-C from ExxonMobil.
[0101] Mineral Oil: HYDROBRITE 380 PO white mineral oil from Sonneborn.
[0102] Preparation 1A: Preparation of an activator formulation comprising spray dried methylaluminoxane / treated fumed silica in hexane / mineral oil (sdMAO). 1.6 kg of treated fumed silica (CABOSIL TS-610) is slurried in 16.8 kg toluene, then 10 wt% MAO solution in toluene (11.6 kg) is added to obtain a mixture. A spray dryer set at 160°C with an outlet temperature of 70°-80°C is used, and the mixture is introduced into the atomizing device of the spray dryer to generate droplets of the mixture, which are then contacted with a hot nitrogen gas stream to evaporate the liquid from the mixture to obtain a powder. The powder is separated from the gas mixture in a cyclone separator, and the separated powder is discharged into a container to obtain sdMAO as a fine powder.
[0103] Preparation 1B: Preparation of a slurry of the activator formulation of Preparation 1A. The sdMAO powder of Preparation 1A is slurried in a mixture of 10 wt% n-hexane and 78 wt% mineral oil to obtain an activator formulation having 12 wt% sdMAO / treated fumed silica solids in hexane / mineral oil.
[0104] Preparation 2: Preparation of spray-dried metallocene with activator blend. Replicate preparations 1A and 1B, except prepare the activator blend by slurrying 1.5 kg of treated fumed silica (CABOSIL TS-610) in 16.8 kg of toluene, followed by the addition of a 10 wt% solution of MAO in toluene (11.1 kg) and (MeCp)(1,3-dimethyl-4,5,6,7-tetrahydroindenyl)ZrMe2 (where Me is methyl, Cp is cyclopentadienyl, and MeCp is methylcyclopentadienyl) in an amount sufficient to provide a loading of 40 micromoles of Zr per gram of solids. Slurry the resulting powder to obtain an activator blend of 22 wt% solids in 10 wt% isoparaffin fluid and 68 wt% mineral oil. Advantageously, the activator blend can be used to produce polymer compositions that do not contain HMW pre-catalysts and have very low ratios of HMW / LMW components. Moreover, the transition to other catalyst systems is simplified compared to the partial combination feed method of the introductory part of this specification.
[0105] Preparation 3: Synthesis of compound (4) {(HN(CH2CH2NHC6(CH3)5)2)} Duplicate step 2 in US6967184B2, column 33, line 53 to column 34, line 9 to obtain compound (4) depicted above.
[0106] Preparation 4: Synthesis of 4-tert-butylbenzyl magnesium chloride. Under nitrogen atmosphere in a glove box with a freezer component, load 1.33 g (54.7 mmol) of magnesium turnings into a first oven-dried 120 mL glass bottle equipped with three small PTFE-coated magnetic stirrers. Seal the bottle with a PTFE-lined cap and vigorously stir the contents for 40 h. PTFE is poly(tetrafluoroethylene). Then add 40 mL of anhydrous degassed diethyl ether. Place the bottle in the glove box freezer for 15 min to cool the contents of the bottle to -30 °C. In a second oven-dried 120 mL glass bottle, prepare a solution of 4-(1,1,-dimethylethyl)benzyl chloride (2.0 g, 10.9 mmol) in 60 mL of anhydrous degassed diethyl ether. Seal the bottle with a PTFE-lined cap and place the second glass bottle in a glove box freezer for 15 minutes to cool the contents to -30 °C. Add the solution from the second bottle to the addition funnel and add the contents of the addition funnel dropwise to the contents of the first glass bottle over 45 minutes. Use 10 mL of diethyl ether to rinse the remaining contents of the addition funnel into the reaction mixture in the first glass bottle. Stir the resulting mixture and allow it to return to room temperature for 2.5 hours. Filter the mixture through a PTFE frit into a clean vial to obtain a solution of 4-tert-butylbenzyl magnesium chloride in diethyl ether. Titrate a portion of the filtrate with iodine / LiCl to determine the concentration of 4-tert-butylbenzyl magnesium chloride in the solution.
[0107] Preparation 5: Synthesis of 3-n-butylbenzyl alcohol. Under nitrogen atmosphere in a glovebox, charge an oven-dried round-bottom flask equipped with a PTFE-coated magnetic stirrer and a reflux condenser with 3-n-butylbenzoic acid (2.0 g, 11.2 mmol) and 10 mL of dry degassed THF. Add a solution of borane in tetrahydrofuran (22.4 mL, 22.4 mmol), attach a reflux condenser to the flask, and heat the mixture to reflux for 4 h. Remove the flask from the glovebox, place under nitrogen atmosphere on a Schlenk line, then cool to 0 °C in an ice bath. Slowly add 5 mL of ethanol, then pour the resulting mixture into 30 mL of water and extract three times with 30 mL of diethyl ether. Combine the diethyl ether extracts, dry over anhydrous magnesium sulfate, filter through diatomaceous earth, and concentrate under reduced pressure to give a pale orange oil. The oil is dissolved in a minimum amount of hexane and the solution is passed through a plug of silica eluting with a 1:1 volume / volume (v / v) mixture of ethyl acetate and hexane. The filtrate is concentrated under reduced pressure to give 3-n-butylbenzyl alcohol as a pale orange oil. 1 H NMR (400MHz, chloroform-d) δ7.28-7.23(m,1H),7.19-7.14(m,3H),7.10(dd,J=7.5,1.5Hz,1H),4.65(s,2H) ,2.63-2.55(m,2H),1.64(d,J=11.9Hz,2H),1.64-1.54(m,2H),1.41-1.28(m,2H),0.91(t,J=7.3Hz,4H). 13 C NMR (101 MHz, chloroform-d) δ 143.31, 140.76, 128.44, 127.77, 127.08, 124.26, 65.49, 35.60, 33.63, 22.38, 13.94.
[0108] Preparation 6: Synthesis of 3-n-butylbenzyl chloride. In a Schlenk line under nitrogen atmosphere, charge a 100 mL round-bottom flask with n-butylbenzyl alcohol (1.57 g, 9.6 mmol) prepared in preparation 5 and add 12 mL of dry degassed dichloromethane. Cool the flask to 0 °C in an ice bath, add 0.1 mL of triethylamine (0.8 mmol), and slowly add thionyl chloride (1.39 mL, 19.1 mmol) via syringe. Stir the mixture under nitrogen atmosphere and allow it to warm to room temperature over 22 h. Carefully pour the mixture into 50 mL of ice water and extract three times with 30 mL of dichloromethane. Wash the combined dichloromethane layers twice with 50 mL of saturated aqueous bicarbonate solution and twice with 50 mL of saturated aqueous sodium chloride solution, then dry over magnesium sulfate and concentrate under reduced pressure. Obtain 3-n-butylbenzyl chloride as a pale yellow liquid. 1 H NMR(400MHz,chloroform-d)δ7.25(dd,J=8.3,7.4Hz,1H),7.21-7.16(m,2H),7.12(dt,J=7.4,1.6Hz,1H),4 .56(s,2H),2.64-2.56(m,2H),1.65-1.50(m,3H),1.34(dq,J=14.6,7.3Hz,2H),0.92(t,J=7.3Hz,3H). 13 C NMR (101 MHz, chloroform-d) δ 143.51, 137.32, 128.63, 128.59, 128.51, 125.83, 46.43, 35.50, 33.53, 22.37, 13.93.
[0109] Preparation 7: Synthesis of 3-n-butylbenzyl magnesium chloride. Under nitrogen atmosphere in a glove box with a freezer component, load 330 mg (13.7 mmol) of magnesium turnings into a first oven-dried 40 mL glass vial equipped with three small PTFE-coated magnetic stirrers. Seal the vial with a PTFE-lined septum cap and vigorously stir the contents for 40 h. Then add 10 mL of anhydrous degassed diethyl ether. Place the vial in the glove box freezer for 15 min to cool the contents of the vial to -30 °C. In a second oven-dried 40 mL glass vial, prepare a solution of 3-(n-butyl)benzyl chloride (0.5 g, 10.9 mmol) of Preparation 6 in 15 mL of anhydrous degassed diethyl ether. Seal the bottle with a PTFE-lined septum cap and place the second glass vial in a glove box freezer for 15 minutes to cool the contents to -30 °C. Add the solution from the second bottle to the addition funnel and add the contents of the addition funnel dropwise to the contents of the first glass vial over 10 minutes. Use 2 mL of diethyl ether to rinse the remaining contents of the addition funnel into the reaction mixture in the first glass vial. Stir the resulting mixture and allow it to return to room temperature for 1.5 hours. Filter the mixture through a PTFE frit into a clean vial to obtain a solution of 3-n-butylbenzyl magnesium chloride in diethyl ether. Titrate a portion of the filtrate with iodine / LiCl to determine the concentration of 3-n-butylbenzyl magnesium chloride in the solution.
[0110] Preparation 8: Synthesis of tetra(3-methylbenzyl)zirconium. Under nitrogen atmosphere in a glove box with a freezer component, charge an oven-dried 40 mL vial equipped with a PTFE-coated magnetic stirrer with zirconium(IV) chloride (0.25 g, 0.6 mmol) and 10 mL of toluene. Seal the vial with a PTFE-lined septum cap and place the vial in the glove box freezer for 15 minutes to cool the contents of the vial to -30 °C. Slowly add the solution of 3-methylbenzylmagnesium chloride from preparation 7 (7.35 mL, 2.6 mmol), then cover the vial with aluminum foil and stir the mixture in the dark for 16 hours until it reaches room temperature. Add 15 mL of diethyl ether and filter the mixture through diatomaceous earth, then concentrate the mixture to a volume of approximately 2 mL. Add 10 mL of pentane and place the vial in the glove box freezer overnight. The resulting yellow precipitate is collected by filtration, then the resulting solid is triturated with 5 mL of hexane and dried under vacuum three times to remove residual THF. 5 mL of toluene is added to the resulting solid and filtered through a 0.45 μM PTFE syringe filter. The filtrate is concentrated under reduced pressure, then triturated with 5 mL of hexane and dried under vacuum three times. 5 mL of pentane is added and the vial is placed in a glove box freezer for 72 h. The mixture is filtered through diatomaceous earth and the filter cake is washed with 10 mL of hexane. The filtrate is concentrated under reduced pressure to give tetra(3-methylbenzyl)zirconium as a tan oil. 1 H NMR (400MHz, benzene-d6) δ7.03(t,J=7.6Hz,1H),6.82(ddt,J=7.5,1.8,0.9Hz,1H ),6.34(dt,J=8.0,1.4Hz,1H),6.11(d,J=1.9Hz,1H),2.06(s,3H),1.52(s,2H). 13 C NMR (101 MHz, benzene-d6) δ 140.90, 140.02, 130.97, 128.68, 125.92, 124.99, 71.42, 21.68.
[0111] Bimodality test method: Plot dWf / dLogM (mass detector response) on the y-axis and LogM on the x-axis to obtain a GPC chromatogram curve containing the maximum log(MW) values of the peaks of LMW and HMW polyethylene components, and observe the presence or absence of minimum values between the peaks of LMW and HMW polyethylene components to determine the presence or absence of decomposed bimodality. dWf is the change in weight fraction, dLogM is also called dLog(MW) and is the change in logarithm of molecular weight. LogM is also called Log(MW) and is the logarithm of molecular weight.
[0112] Deconvolution test method: The chromatogram obtained using the bimodality test method is divided into nine Schulz-Flory molecular weight distributions. Such a deconvolution method is described in US Pat. No. 6,534,604. The smallest 4 MW distributions are assigned to the LMW polyethylene component and the largest 5 MW distributions are assigned to the HMW polyethylene component. The sum of the weight fractions (Wf) of the LMW and HMW polyethylene components, as well as their respective number average molecular weights (M n ), and weight average molecular weight (M w ) is used to determine the respective weight percent (wt %) of each of the LMW and HMW polyethylene components in the bimodal ethylene-co-1-hexene copolymer composition by known mathematical treatment of the tabulated Schultz-Flory MW distribution.
[0113] Density is measured according to ASTM D792-13, Standard Test Method for Density and Specific Gravity (Relative Density) of Plastics by Displacement, Method B (for testing solid plastics in liquids other than water, e.g., in liquid 2-propanol). Results are reported in grams per cubic centimeter (g / cm 3 ) units.
[0114] Gel Permeation Chromatography (GPC) Test Method: Weight-average molecular weight test method: Using a chromatogram obtained with a high-temperature gel permeation chromatography device (HTGPC, Polymer Laboratories), M w, number average molecular weight (M n ), and M w / M n The HTGPC is equipped with a transfer line, a differential refractive index detector (DRI), and three Polymer Laboratories PLgel 10 μm Mixed-B columns, all housed in an oven maintained at 160 °C. The method uses a solvent consisting of BHT-treated TCB at a nominal flow rate of 1.0 milliliters per minute (mL / min.) and a nominal injection volume of 300 microliters (μL). The solvent is prepared by dissolving 6 grams of butylated hydroxytoluene (BHT, an antioxidant) in 4 liters (L) of reagent-grade 1,2,4-trichlorobenzene (TCB) and filtering the resulting solution through a 0.1 micrometer (μm) PTFE filter to obtain the solvent. PTFE is poly(tetrafluoroethylene). The solvent is degassed with an in-line degasser before it enters the HTGPC instrument. The column is calibrated with a series of monodisperse polystyrene (PS) standards. Separately, prepare a known concentration of the test polymer dissolved in the solvent by heating a known amount of the test polymer in a known volume of solvent at 160 °C for 2 h with continuous shaking to obtain a solution. (All amounts are measured gravimetrically.) The target solution concentration c of the test polymer is 0.5 to 2.0 milligrams polymer per milliliter solution (mg / mL), with lower concentrations of c being used for higher molecular weight polymers. Before running each sample, purge the DRI detector. Then, increase the flow rate in the instrument to 1.0 mL / min and allow the DRI detector to stabilize for 8 h before injecting the first sample. Using the general calibration relationship for column calibration, determine the M w and M. n Calculate the following formula:
number
[0334] to
[0341] . GPC chromatograms are obtained by plotting dW / dLog(MW) on the y-axis and Log(MW) on the x-axis (Log(MW) and dW / dLog(MW) are as defined above).
[0115] High Load Melt Index (HLMI) I 21 Test Method: Standard Test Method for Melt Flow Rates of Thermoplastics (ASTM D1238-13) using 190°C / 21.6 kilograms (kg). Results are in grams dissolved per 10 minutes (g / 10 min).
[0116] Ignition Test Method: Under nitrogen atmosphere in a glove box, a 40 mL glass vial equipped with a PTFE-coated magnetic stirrer is charged with 0.16 g of spray-dried methylaluminoxane powder of Preparation 1A. 11 mL of 1-octene is added to the charged vial, then the vial is inserted into an insulated sleeve attached to a magnetic stir plate and rotated at approximately 300 revolutions per minute (rpm). 8 micromoles (μmol) of pre-catalyst (e.g., Compound (1) or HN5Zr dibenzyl) are added to the insulated vial. The vial is capped with a rubber septum. A thermocouple probe is inserted into the vial through the rubber septum so that the tip of the thermocouple probe is below the liquid level. The temperature of the contents of the vial is recorded at 5 second intervals until the maximum temperature is reached. The temperature and time data are downloaded into a spreadsheet and the thermokinetic profile is plotted for analysis.
[0117] Melt Index I5 ("I5") Test Method: Using ASTM D1238-13, using the following conditions: 190°C / 5.0 kg. Results are reported in grams dissolved per 10 minutes (g / 10 min).
[0118] Melt Flow Ratio (MFR5): ("I 21 / I5) Test method: HLMI I 21 Calculated by dividing the value from the test method by the value from the Melt Index I5 test method.
[0119] Solubility Test Method: To a 20 mL vial, at room temperature and atmospheric pressure, is added a known mass of test pre-catalyst (e.g., compound (1)) and a known volume of hexane containing at least 60 weight percent n-hexane. A PTFE-coated magnetic stir bar is added and the mixture is stirred for 1 hour, after which the vial is removed from the stir plate and the mixture is allowed to stand overnight. The next day, the suspension is filtered through a 0.4 μm PTFE syringe filter into a tared vial to obtain a known mass of supernatant, and the hexane is removed under reduced pressure leaving a measurable mass of compound of formula (1) from which the soluble weight % is calculated.
[0120] Invention Example 1 (IE1): Compound (3a) of FIG. 3 (each R 10 Synthesis of compound (3) where is methyl. In a glove box under nitrogen atmosphere, an oven-dried 400 mL glass bottle equipped with a PTFE-coated magnetic stirrer is charged with compound (4) (10 g, 25.3 mmol) and 200 mL of dry degassed n-pentane. Tetrakis(dimethylamino)zirconium(IV) (6.76 g, 25.3 mmol) is then added in small portions as a solid, and the resulting reaction mixture is then stirred at 25 °C for 16 h. The mixture is cooled in a freezer in a glove box for 1 h to precipitate compound (3a). The precipitated (3a) is removed by filtration, and the filter cake is washed with cold n-pentane. The washed compound (3a) is dried under reduced pressure to obtain 12.62 g (87.1% yield) of compound (3a) as a white powder. 1 H NMR (400MHz, benzene-d6) δ3.37(dt,2H),3.10(d,6H),3.02(dd,3H),2.68(dq,4H),2.51(d,12H),2.20(q,18H),2.14(s,7H),1.84(s,1H); 13 C NMR (101 MHz, benzene-d6) δ 149.77, 132.34, 132.14, 130.04, 129.98, 129.32, 56.29, 48.86, 44.35, 40.91, 17.31, 17.27, 16.72, 16.65, 16.09.
[0121] Inventive Example 2 (IE2): Synthesis of compound (2a) of FIG. 3 (compound (2) where M is Zr and each X is Cl) from compound (3a) of FIG. 3. In a nitrogen atmosphere in a glove box, an oven-dried 400 mL glass bottle equipped with a PTFE-coated magnetic stirrer was charged with compound (3a) (12.62 g, 22.0 mmol) and 250 mL of dry, degassed diethyl ether. Chlorotrimethylsilane (6.2 mL, 48.5 mmol) was added and the mixture was stirred at 25° C. for 24 hours. The mixture was cooled in a glove box freezer for 1 hour to precipitate compound (2a). The precipitated (2a) was collected by filtration and the filter cake was washed with cold n-pentane. The washed (2a) is dried under reduced pressure to give 10.77 g (88.0% yield) of compound (2a), i.e., bis(2-(pentamethylphenylamido)ethyl)-aminezirconium(IV) dichloride, as a white powder. 1 H NMR (400MHz, benzene-d6) δ3.40(dt,1H),2.95(dt,1H),2.59(dp,2H),2.49(s, 3H),2.46(s,3H),2.43-2.34(m,1H),2.13(s,3H),2.06(s,3H),2.04(s,3H). 13 C NMR (101 MHz, benzene-d6) δ 145.64, 133.37, 133.20, 132.61, 129.84, 129.57, 57.69, 48.97, 17.03, 17.01, 16.70, 16.47.
[0122] Inventive Example 3 (IE3): Synthesis of compound (1A) of FIG. 2 (compound (1) where M is Zr and each R is CH2Si(CH3)3) from compound (2a) of FIG. 3. Under nitrogen atmosphere in a glove box, an oven-dried 400 mL glass bottle equipped with a PTFE-coated magnetic stirrer is charged with compound (2a) (5.0 g, 9.0 mmol) and 250 mL of dry degassed toluene. A 1.0 M solution of trimethylsilylmethyl magnesium chloride in hexane is added and the reaction mixture is stirred at 25 °C for 23 h. The reaction mixture is quenched with 2 mL of 1,4-dioxane, and then the quenched mixture is filtered through diatomaceous earth. The filtrate is concentrated under reduced pressure. The residual concentrate is triturated with 20 mL of hexane and the remaining triturated material is dried under reduced pressure. The trituration / drying is repeated twice. The resulting pale orange solid is slurried in 200 mL of hexane and the slurry is placed in a glove box freezer for several hours. The resulting fine precipitate is removed by filtration through diatomaceous earth, and the filtrate is then concentrated under reduced pressure and dried under vacuum to give compound (1A) as a pale orange powder. Compound (1A) is bis(2-(pentamethylphenylamido)ethyl)-aminezirconium(IV) bis-trimethylsilylmethyl. The procedure in IE3 is repeated twice to give a combined total of 14.2 g (average yield of 79.8% for three runs) of compound (1A). 1 H NMR (400MHz, benzene-d6) δ3.38(dt,J=12.6,5.4Hz,2H),3.14(ddd,J=12.3,6.7,5.3Hz,2H),2.69-2.62(m,3H),2.60(s,8H),2.44 (s,6H),2.22(s,6H),2.17(s,6H),2.10(s,7H),1.25-1.19(m,1H),0.42-0.38(m,2H),0.24(s,9H),-0.12(s,2H),-0.28(s,9H). 13C NMR (101 MHz, benzene-d6) δ 147.18, 133.07, 132.73, 130.97, 129.74, 129.67, 57.49, 55.96, 54.74, 48.29, 16.80, 16.70, 16.67, 16.37, 16.23, 3.40, 2.02. Ignition performance is measured according to the ignition test method and solubility test method. Solubility, and time to maximum temperature results are reported later in Table 1.
[0123] Invention Example 4 (IE4): Synthesis of compound (1B) of FIG. 2 (compound (1) where M is Zr and each R is CH2-(1,4-phenylene)-C(CH3)3) from compound (2a) of FIG. 3. A clean, oven-dried bottle equipped with a PTFE-coated magnetic stirrer is charged with compound (2a) (1.5 g, 2.69 mmol) and 100 mL of dry, degassed toluene to make a solution of compound (2a) in toluene. The bottle, along with a separate bottle containing the solution of 4-tert-butylbenzyl magnesium chloride from preparation 4, is placed in a glove box freezer and cooled to −30° C. for 15 minutes. The solution of 4-tert-butylbenzyl magnesium chloride is then added to the addition funnel and the contents of the addition funnel are added dropwise to the solution of compound (2a). The mixture is stirred and allowed to warm to room temperature (rt) over 1 hour. Then, 0.5 mL of 1,4-dioxane is added and the resulting mixture is filtered through diatomaceous earth. The filtrate is concentrated under reduced pressure and the resulting residue is taken up in 30 mL of toluene. It is filtered again and concentrated under reduced pressure to obtain a twice filtered / concentrated residue. The residue is triturated three times with 10 mL of hexane and the triturated residue is dried under reduced pressure to ensure complete removal of toluene. 20 mL of pentane is added to the residue and the resulting mixture is placed in a glove box freezer for 72 hours to obtain a yellow precipitate which is collected by filtration through a chilled PTFE frit and dried under reduced pressure to obtain 0.95 g of compound (1B) (45% yield). 1H NMR (400MHz, benzene-d6) δ7.31-7.23(m,2H),7.18-7.07(m,4H),5.73-5.66(m ,2H),3.45(dt,J=11.8,5.5Hz,2H),3.25(dd,J=9.8,4.5Hz,1H),3.15(dt,J= 12.0,5.7Hz,2H),2.76-2.65(m,2H),2.49(d,J=4.4Hz,13H),2.28(s,6H),2 .14(d,J=18.8Hz,11H),1.77(s,2H),1.33(s,8H),1.21(s,8H),0.87(s,2H). 13 C NMR (101 MHz, benzene-d6) δ 152.70, 148.52, 147.67, 142.21, 136.97, 133.69, 132.32, 131.19, 130.57, 130.41, 129.41, 126.93, 125.50, 124.38, 63.41, 58.04, 53.38, 49.37, 34.13, 34.08, 31.90, 31.88, 17.18, 17.14, 17.06, 16.68, 16.61. Ignition performance is measured according to the ignition test method and solubility test method. Solubility, and time to maximum temperature results are reported later in Table 1.
[0124] Inventive Example 5 (IE5): Synthesis of compound (1C) of FIG. 2 (compound (1) where M is Zr and each R is CH3) from compound (2a) of FIG. 3. Under nitrogen atmosphere in a glove box, an oven-dried 100 mL glass bottle equipped with a PTFE-coated magnetic stirrer was charged with compound (2a) (0.5 g, 0.9 mmol) and 25 mL of dry, degassed dichloromethane. The mixture was placed in the glove box freezer for 1 h to cool to -30°C. A solution of 3.0 M methylmagnesium bromide in diethyl ether (0.6 mL, 1.8 mmol) was slowly added with stirring, and the mixture was then allowed to warm to room temperature with stirring for 30 min. The mixture was quenched with 0.2 mL of 1,4-dioxane, then it was filtered through PTFE, and the filtrate was concentrated under reduced pressure. The residue was triturated with 20 mL of n-pentane, and the resulting solid was filtered. The solid was dried under reduced pressure to give 0.32 g (69% yield) of compound (1B) as a pale orange powder.1 H NMR (400 MHz, benzene-d6) δ 3.40 (ddd, J = 12.3, 8.9, 5.5 Hz, 3H), 3.11 (ddd, J = 12.3, 5.2, 3.3 Hz, 2H), 2.51 (s, 7H), 2.49 (s, 7H), 2.47-2.42 (m, 5H), 2.21 (s, 6H), 2.18 (s, 7H), 2.11 (s, 7H), 0.17 (s, 3H), 0.07 (s, 3H). Ignition performance is measured according to the ignition test method and solubility test method. Solubility, and time to maximum temperature results are reported later in Table 1.
[0125] Invention Example 5A (IE5A): Synthesis of Compound (1D) (Compound (1) Wherein M is Zr and Each R is CH2-(1,3-phenylene)-CH2CH2CH2CH3) from Compound (2a) [ka] . (2a) (1D). A clean oven-dried bottle equipped with a PTFE-coated magnetic stirrer is charged with compound (2a) (0.4 g, 0.7 mmol) and 20 mL of dry, degassed toluene to make a solution of compound (2a) in toluene. The bottle, along with a separate bottle containing the solution of 3-n-butylbenzyl magnesium chloride from preparation 7, is placed in a glove box freezer and cooled to −30° C. for 15 minutes. The solution of 3-n-butylbenzyl magnesium chloride is then added to the addition funnel and the contents of the addition funnel are added dropwise to the solution of compound (2a). The mixture is stirred and allowed to warm to room temperature (rt) over 16 hours. 20 mL of diethyl ether is then added and the resulting mixture is filtered through diatomaceous earth. The filtrate is concentrated under reduced pressure and the resulting residue is taken up in 30 mL of toluene. It is again filtered through diatomaceous earth and concentrated under reduced pressure to give a residue that has been filtered / concentrated twice. Triturate the residue with 10 mL of hexane three times and dry the triturated residue under reduced pressure to ensure complete removal of toluene. Add 20 mL of pentane to the residue and place the resulting mixture in a glove box freezer for 72 h to obtain a yellow precipitate, which is collected by filtration through a chilled PTFE frit and dried under reduced pressure to obtain 0.12 g of compound (1D) (22% yield). 1 H NMR (400MHz, benzene-d6) δ7.21(t,J=7.4Hz,1H),7.08-7.01(m,2H),6.88(t,J=7.5Hz,1H),6.81(dt,J=7.6,1.4Hz,1H), 6.76-6.71(m,1H),5.58-5.51(m,2H),3.48(dt,J=11.8,5.6Hz,2H),3.34(s,1H),3.19(dt,J=12.1,5.8Hz,2H),2.73( dq,J=12.2,6.0Hz,3H),2.61(td,J=7.5,6.9,4.0Hz,5H),2.48(d,J=5.8Hz,10H),2.27(s,6H),2.15(s,7H),2.11(s,7 H),1.83(s,2H),1.72-1.61(m,3H),1.44-1.35(m,3H),1.31(dd,J=14.8,7.4Hz,3H),0.93(s,2H),0.93-0.86(m,3H). 13C NMR (101 MHz, benzene-d6) δ 147.35, 146.46, 142.43, 133.37, 132.09, 131.93, 130.96, 130.25, 130.11, 124.83, 123.77, 121.68, 119.94, 63.63, 57.68, 53.33, 49.12, 36.11, 36.07, 32.67, 22.32, 16.82, 16.78, 16.70, 16.35, 16.29, 13.79. Ignition performance is measured according to the ignition test method and solubility test method. Solubility, and time to maximum temperature results are reported later in Table 1.
[0126] Invention Example 5B (IE5B): Synthesis of Compound (1E) (Compound (1) Wherein M is Zr and Each R is CH2-(1,3-phenylene)-CH3) from Compound (4) [ka] .. (4) (1E). A clean, oven-dried 40 mL vial equipped with a PTFE-coated magnetic stirrer is charged with preparation 8 tetra(3-methylbenzyl)zirconium (0.12 g, 0.2 mmol) and 5 mL of dry, degassed toluene. Compound 4 is added to the vial as a solid and the mixture is stirred at room temperature for 2 h. 30 mL of pentane is added to the mixture and the beige solid is collected by filtration, then the solid is washed with 10 mL of cold pentane to give 88 mg of compound (1E) (53.4% yield). 1H NMR (400MHz, benzene-d6) δ7.25-7.10(m,1H),7.05-6.98(m,2H),6.86-6.70(m,3H),5.50(d,J=7. 8Hz,1H),5.44(s,1H),3.53-3.40(m,2H),3.29-3.20(m,1H),3.15(dt,J=12.0,5.8Hz,2H),2.69 (q,J=6.1,5.5Hz,3H),2.57(td,J=10.9,5.3Hz,2H),2.47(s,6H),2.42(s,6H),2.29(s,3H),2. 24(s,7H),2.15(s,7H),2.10(s,7H),1.98(s,3H),1.78(s,2H),0.91-0.83(m,0H),0.87(s,2H). 13 C NMR (101 MHz, benzene-d6) δ 147.27, 141.46, 137.28, 133.33, 132.11, 131.90, 130.95, 130.22, 130.14, 125.71, 124.35, 121.30, 120.39, 63.48, 57.66, 53.13, 49.13, 21.59, 16.77, 16.71, 16.34, 16.27. Ignition performance is measured according to the ignition test method and solubility test method. Solubility, and time to maximum temperature results are reported later in Table 1.
[0127] Invention Example 6A (IE6A): Preparation of a unimodal catalyst system from compound (1A) and an activator. An in-line mixer is separately fed with the slurry activator blend of Preparation 1B through a catalyst injection tube, and fed with the freshly prepared pre-catalyst system of IE3 through a different catalyst injection tube, where they are contacted with each other to obtain a unimodal catalyst system, which is then flowed into the reactor through the injection tube.
[0128] Inventive Examples 6B and 6C (Prophetic, IE6B and IE6C): The procedure of IE6A is replicated, except that compound (1A) is replaced by compound (1B) of IE4 or (1C) of IE5 to obtain unimodal catalytic systems made from compound (1B) or (1C), respectively.
[0129] Inventive Example 6D (IE6D): The procedure of IE6A was replicated, except that a freshly prepared solution of compound (1A) (compound (1) where M is Zr and each R is CH2Si(CH3)3) in hexane and a freshly prepared solution of methylaluminoxane (MAO) in hexane were used. Different solutions of compound (1A) were prepared by dissolving measured amounts of compound (1A) in separate aliquots of hexane to obtain 700 mL of compound (1A) at 0.91 wt% in hexane, 700 mL of compound (1A) at 1.18 wt% in hexane, and 550 mL of compound (1A) at 0.91 wt% in hexane, respectively. The solutions do not need to be cooled, but can be shipped or stored at 25°C. An in-line mixer was fed with an activator solution separately through a catalyst injection tube and a freshly prepared solution of compound (1A) through a different catalyst injection tube, where they were contacted with each other to obtain a solution of the unimodal catalyst system, which was then run through the injection tube into the reactor.
[0130] Inventive Examples 6E and 6F (Prophetic, IE6E and IE6F): The procedure of IE6D is replicated, except that compound (1A) is replaced by compound (1B) in IE4 or (1C) in IE5 to obtain unimodal catalyst systems made from compound (1B) or (1C), respectively.
[0131] Inventive Example 6G (IE6G): The procedure of IE6A was replicated except that a freshly prepared solution of compound (1A) (compound (1) where M is Zr and each R is CH2Si(CH3)3) in hexane / isopentane and a freshly prepared solution of methylaluminoxane (MAO) in hexane were used. A different solution of compound (1A) was prepared by adding a measured amount of compound (1A) of IE3 to a cylinder of 106 liter (L) volume containing hexane. 11.3 kilograms (kg) of high purity isopentane was added to the cylinder to obtain a pre-catalyst formulation of a 0.10 wt% solution of compound (1A) in the hexane / isopentane mixture. The solution does not need to be cooled, but can be shipped or stored at 25°C. The in-line mixer was fed separately with an activator solution through a catalyst injection tube and a freshly prepared solution of compound (1A) through a different catalyst injection tube where they contacted each other to obtain a solution of the unimodal catalyst system, which then flowed into the reactor through the injection tube.
[0132] Inventive Examples 6H and 6I (Prophetic, IE6H and IE6I): The procedure of IE6G is replicated, except that compound (1A) is replaced by compound (1B) in IE4 or (1C) in IE5 to obtain unimodal catalytic systems made from compound (1B) or (1C), respectively.
[0133] Invention Example 7A (IE7A): Preparation of a bimodal catalyst system comprising an alkane-soluble nonmetallocene catalyst made from compound (1A) and a metallocene catalyst made from (MeCp)(1,3-dimethyl-4,5,6,7)-tetrahydroindenyl)ZrMe2 (Me is methyl, Cp is cyclopentadienyl, and MeCp is methylcyclopentadienyl). An in-line mixer is separately fed with spray-dried metallocene with activator blend of preparation 2 through a catalyst injection tube and fed with pre-catalyst blend of compound (1A) of IE5 through a different catalyst injection tube, where the feeds contact each other to form a catalyst system, which then flows into the reactor through the injection tube.
[0134] Inventive Examples 7B-7I (Prophetic, IE7B-IE7I): To obtain a bimodal catalyst system comprising an alkane soluble nonmetallocene catalyst, an activator, and a metallocene catalyst made from (MeCp)(1,3-dimethyl-4,5,6,7-tetrahydroindenyl)ZrMe2, the procedure of IE7A is replicated except that the spray dried metallocene with activator formulation of Preparation 2 is replaced with any one of the catalyst formulations IE6B-IE6I.
[0135] Inventive Example 8A (IE8A): Copolymerization of ethylene and 1-hexene using a unimodal catalyst system of IE6A prepared from compound (1A) to make unimodal poly(ethylene-co-1-hexene) copolymer. Each experiment uses a gas-phase fluidized bed reactor with an internal diameter of 0.35 m, a bed height of 2.3 m, and a fluidized bed composed mainly of polymer granules. A fluidizing gas is passed through the bed at a velocity of 0.51 meters per second (m / s) to 0.58 m / s. The fluidizing gas is discharged from the top of the reactor, and the discharged gas is passed through a recycle gas line having a recycle gas compressor and a heat exchanger, and then re-enters the reactor under a distribution grid. A constant fluidized bed temperature of 105°C is maintained by continuously adjusting the temperature and / or flow rate of the cooling water used for temperature control. Gaseous feed streams of ethylene, nitrogen, and hydrogen are introduced into the recycle gas line together with the 1-hexene comonomer. Operate the reactor at a total pressure of 2410 kilopascal gauge (kPa gauge). Vent the reactor to a flare to control the total pressure. Adjust the individual flow rates of ethylene, nitrogen, hydrogen, and 1-hexene to maintain the target gas composition. Set the ethylene partial pressure at 1.52 megapascals (MPa). Set the 1-hexene / ethylene (C6 / C2) molar ratio to 0.0050 and the hydrogen / ethylene (H2 / C2) molar ratio to 0.0020. Maintain the ICA (isopentane) concentration at 8.5-9.5 mol%. Measure the concentrations of all gases using an online gas chromatograph. Feed the freshly prepared unimodal catalyst system of IE6A to the polymerization reactor at a rate sufficient to maintain a production rate of poly(ethylene-co-1-hexene) copolymer of approximately 13-16 kg / hr, while also controlling the feed rate to achieve a loading of 50 micromoles of zirconium per gram of spray-dried solids. The poly(ethylene-co-1-hexene) copolymer ("Resin") has a unimodal molecular weight distribution, a high load melt index (HLMI or I) of 0.21 g / 10 min. 21 ), 0.9311g / cm 3 density of 79,727, number average molecular weight (M n ), weight average molecular weight (M w ), z-average molecular weight (Mz ), and a molecular weight distribution (M w / M n IE8A uses a unimodal catalyst system that includes an activator formulation without pre-catalyst and a pre-catalyst formulation with activator-free pre-catalyst (1) to produce a unimodal high molecular weight copolymer. Resin particle size and particle size distribution data are shown in Table 2 below.
[0136] Inventive Examples 8B-8I (Prophetic, IE8B-IE8I): The procedure of IE8A is replicated except that the unimodal catalyst system of IE6A is replaced with a different one of the unimodal catalyst systems of IE6B-IE6I, respectively, to obtain unimodal poly(ethylene-co-1-hexene) copolymers.
[0137] Inventive Example 9A (IE9A): Copolymerization of ethylene and 1-hexene using a bimodal catalyst system prepared from compound (1A) and a metallocene to prepare a bimodal poly(ethylene-co-1-hexene) copolymer. The polymerization procedure of IE8A is replicated, except that instead of feeding the unimodal catalyst system of IE6A, the bimodal catalyst system of IE7A is fed to the reactor. The feed ratio of compound (1A) to the spray-dried metallocene slurry is adjusted to obtain a bimodal poly(ethylene-co-1-hexene) copolymer in the reactor at high load melt index (I 21 Adjust the IQ to approximately 6 g / 10 min. Increase the C6 / C2 molar ratio to 0.0060 to reduce the density of the bimodal poly(ethylene-co-1-hexene) copolymer. Adjust the feed rates of the spray-dried metallocene slurry and compound (1A) solution at a rate sufficient to maintain a production rate of bimodal poly(ethylene-co-1-hexene) copolymer of approximately 13-16 kg / hr. The bimodal poly(ethylene-co-1-hexene) copolymer produced is bimodal with an IQ of 6.1 g / 10 min. 21 , Melt Flow Index (I 21 / I5), 0.9476g / cm 3 Density of 19,194 m n, 353,348 M w , 2,920,833 M z , and M of 18.41 w / M n The bimodality of the IE9A bimodal poly(ethylene-co-1-hexene) copolymer is illustrated by the GPC plot shown in Figure 1. The particle size and particle size distribution data for the resin are shown in Table 2 below.
[0138] Inventive Examples 9B-9I (Prophetic, IE9B-IE9I): The procedure of IE9A is replicated except that one of the bimodal catalyst systems IE7B-IE7I, respectively, is used to obtain the respective bimodal poly(ethylene-co-1-hexene) copolymers.
[0139] Comparative Example 1 (CE1): The synthesis of [N'-(2,3,4,5,6-pentamethylphenyl)-N-[2-(2,3,4,5,6-pentamethylphenyl)amino-κN]ethyl]-1,2-ethane-diaminato(2-)κN,κN']zirconium dichloride (abbreviated as "HN5Zr dichloride" herein) is described in US6967184B2. The ignition performance is measured according to the ignition test method. The results of the time to maximum temperature are reported later in Table 1.
[0140] Comparative Example 2 (CE2): The synthesis of bis(phenylmethyl)[N'-(2,3,4,5,6-pentamethylphenyl)-N-[2-(2,3,4,5,6-pentamethylphenyl)amino-κN]ethyl]-1,2-ethane-diaminato(2-)κN,κN']zirconium (abbreviated herein as "NHZr dibenzyl") can be achieved by reacting the NHZr dichloride of CE1 with 2 molar equivalents of benzyl magnesium chloride in anhydrous tetrahydrofuran. Ignition performance is measured according to the Ignition Test Method and Solubility Test Method. Solubility and time to maximum temperature results are reported later in Table 1.
[0141] Comparative Example 3 (CE3): Copolymerization of ethylene and 1-hexene using the comparative unimodal catalyst system made with HN5Zr dibenzyl of CE2 in a spray dried formulation with hydrophobic fumed silica and MAO to make a comparative unimodal poly(ethylene-co-1-hexene) copolymer. The procedure of IE8A is replicated except that the comparative unimodal catalyst system is used instead of the unimodal catalyst system of IE6A. The comparative poly(ethylene-co-1-hexene) copolymer has a high loading molecular weight distribution (HLMI or I) of 0.20 g / 10 min as the unimodal molecular weight distribution. 21 ), and 0.9312 g / cm 3 The particle size and particle size distribution of the resin are shown in Table 2 below.
[0142] [Table 1]
[0143] Compound (1A) has a solubility of at least 23.3 weight percent in hexane containing at least 60 weight percent n-hexane as measured according to the Solubility Test Method. Unexpectedly, the solubility of Compound (1A) in hexane is 700-800 times higher than the solubility of HN5Zr dibenzyl (CE2) in hexane.
[0144] In the ignition test method, compound (1A) has a time to maximum temperature of 1.3 minutes. Unexpectedly, the time to maximum temperature of compound (1A) is 4 times better than that of HN5Zr dichloride (CE1) and 60-61 times better than that of HN5Zr dibenzyl (CE2).
[0145] As shown by the data in Table 1, compound (1) has significantly increased solubility in alkanes, thereby allowing for reduced transitional complexity between catalyst systems, has significantly higher light-off performance than that of the comparative precatalyst HN5Zr dibenzyl, and can reduce fouling of the distributor plate of a gas-phase polymerization reactor. Compound (1) therefore solves the aforementioned problems of conventional non-MCN precatalysts.
[0146] [Table 2]
[0147] In Table 2, APS(mm) is the average particle size in millimeters. As shown by the data in Table 2, the average particle size of the particles of the unimodal poly(ethylene-co-1-hexene) copolymer of IE8A is 32 times larger than the average particle size of the particles of the comparative unimodal poly(ethylene-co-1-hexene) copolymer of CE3. The average particle size of the particles of the bimodal poly(ethylene-co-1-hexene) copolymer of the present invention of IE9A is 15 times larger than the APS of the particles of the comparative unimodal poly(ethylene-co-1-hexene) copolymer of CE3.
[0148] In Table 2, the bottom catch pan collects particles that pass through the 0.074 mm (200 mesh) screen. The percentage of fines is equal to the weight percent of particles captured on the 0.074 mm (200 mesh) screen plus the weight percent of particles that pass through the 0.074 mm (200 mesh) screen and are collected in the bottom catch pan. The percentage of fines for the comparative unimodal poly(ethylene-co-1-hexene) copolymer of CE3 is four times higher than the percentage of fines for the inventive unimodal poly(ethylene-co-1-hexene) copolymer of IE8A. The present invention may include the following aspects. [1] A method for polymerizing olefin monomers to produce a first polyolefin composition comprising a first polyolefin polymer, the method comprising the steps of: (A) contacting a solution of a first alkane-soluble nonmetallocene pre-catalyst dissolved in an alkane solvent with an activator to produce a first trim catalyst comprising a first alkane-soluble nonmetallocene catalyst; (B) feeding the first trim catalyst to a polymerization reactor; and (C) polymerizing the olefin monomers in the polymerization reactor with the first trim catalyst, thereby producing the first polyolefin composition comprising the first polyolefin polymer, wherein the first alkane-soluble nonmetallocene pre-catalyst is characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane, based on the total weight of the first alkane-soluble nonmetallocene pre-catalyst and hexane, as measured using a Solubility Test Method. [2] The method of [1] above, wherein the first trim catalyst comprises a solution of the first alkane-soluble nonmetallocene catalyst dissolved in an alkane solvent, and step (B) comprises feeding the solution to the reactor, the solution being free of support material. [3] The method of [1] or [2] above, further comprising the steps of (a) contacting a first metallocene pre-catalyst with an activator, and optionally a support material, separately from step (A), to produce a first metallocene catalyst, optionally free of the support material or disposed on and / or in the support material, and (b) feeding the first metallocene catalyst to the polymerization reactor, separately from step (B), wherein step (C) further comprises polymerizing the olefin monomer with the first metallocene catalyst in the polymerization reactor, thereby producing a first bimodal polyolefin composition comprising the first polyolefin polymer and a second polyolefin polymer. [4] The method of [3] above, wherein step (B) comprises supplying the first trim catalyst to the polymerization reactor as a solution of the first alkane-soluble nonmetallocene catalyst dissolved in a first alkane solvent, and step (b) comprises separately supplying a solution of the first metallocene catalyst dissolved in a second alkane solvent to the polymerization reactor, the first and second alkane solvents being the same or different, and the solution being free of support material. [5] After step (C), (D) dividing the process from steps (a) and (b), respectively, further comprises: (a1) contacting a second metallocene pre-catalyst, which differs from the first metallocene pre-catalyst in the structure of at least one cyclopentadienyl ligand, with an activator, and optionally a support material, to produce a second metallocene catalyst different from the first metallocene catalyst, wherein the second metallocene catalyst does not include a support material or is disposed on and / or in the support material; and (b1) decreasing the feeding of the first metallocene catalyst from a steady state value until the first metallocene catalyst is no longer fed to the polymerization reactor, and activating the second metallocene catalyst. and transitioning to steps (a1) and (b1), independently starting and increasing the feed of the second metallocene catalyst to the polymerization reactor until a steady state value of the second metallocene catalyst is fed to the polymerization reactor, and step (C) further comprises polymerizing the olefin monomer with the second metallocene catalyst in the polymerization reactor, thereby making a second multimodal polyolefin composition comprising the first polyolefin polymer made by the first trim catalyst and a third polyolefin polymer made by the second metallocene catalyst, wherein the third polyolefin polymer is different from each of the first and second polyolefin polymers. [6] The method of [1] above, wherein the first trim catalyst further comprises a support material on which the first alkane-soluble nonmetallocene catalyst is disposed. [7] A method for polymerizing olefin monomers to make a first bimodal polyolefin composition comprising a first high molecular weight (HMW) polyolefin component and a first low molecular weight (LMW) polyolefin component, the method comprising the steps of: (1) contacting a solution of a first alkane-soluble nonmetallocene pre-catalyst dissolved in an alkane solvent with an activator to make a first trim catalyst comprising a first alkane-soluble nonmetallocene catalyst; (2) contacting the first metallocene pre-catalyst and an additional amount of said first alkane-soluble nonmetallocene pre-catalyst with an activator and optionally a support material to make a first bimodal catalyst system comprising a first metallocene catalyst and an additional amount of said first alkane-soluble nonmetallocene catalyst, optionally free of said support material or disposed on and / or in said support material; (3) contacting the first bimodal catalyst system with the first trim catalyst to produce a first mixed catalyst system comprising a mixture of the first bimodal catalyst system and the first trim catalyst; (4) feeding the first mixed catalyst system to a polymerization reactor; and (5) polymerizing the olefin monomers with the first mixed catalyst system in the polymerization reactor, thereby producing the first HMW polyolefin component and the first LMW polyolefin component of the first bimodal polyolefin composition, wherein the first ASNM pre-catalyst is characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane, based on the total weight of the first ASNM pre-catalyst and hexane, as measured using a Solubility Test Method. [8] After step (5), (6) modifying the method from steps (2) through (5), respectively, further comprising the steps of: (2a) contacting a second metallocene pre-catalyst and a second additional amount of the first alkane-soluble nonmetallocene pre-catalyst with an activator and optionally a support material to produce a second bimodal catalyst system comprising the second metallocene catalyst and the second additional amount of the first alkane-soluble nonmetallocene catalyst, optionally free of the support material or disposed on and / or in the support material; (3a) contacting the second bimodal catalyst system with the same trim catalyst as in step (1) to produce a second mixed catalyst system comprising a mixture of the second bimodal catalyst system and the first trim catalyst; (4a) contacting the first mixed catalyst system with a trim catalyst to produce a second mixed catalyst system comprising a mixture of the second bimodal catalyst system and the first trim catalyst; 5. The method of claim 4, further comprising: decreasing the supply of the first mixed catalyst system from a steady state value until it is no longer being supplied to the polymerization reactor; and independently starting and increasing the supply of the second mixed catalyst system to the polymerization reactor until the second mixed catalyst is supplied to the polymerization reactor at a steady state value; and (5a) polymerizing the olefin monomers in the polymerization reactor with the second mixed catalyst system, thereby producing a second bimodal polyolefin composition comprising the first HMW polyolefin component and a second LMW polyolefin component distinct from each of the first HMW polyolefin component and the first LMW polyolefin component. [9] The olefin monomer is (i) ethylene, (ii) propylene, (iii) (C 4 -C 20 (v) a combination of (i) and (ii); (vi) a combination of (i) and (iii); and (vii) a combination of (i), (ii), and (iv), wherein the first polyolefin polymer or the HMW polyolefin component is, respectively, (a) a polyethylene homopolymer, (b) a polypropylene homopolymer, (c) a poly(C 4 -C 20 ) alpha-olefin polymers, (d) polybutadiene polymers, (e) ethylene-propylene copolymers, (f) poly(ethylene-co-(C 4 -C20 The method according to any one of the above [1] to [8], comprising any one of (a) to (g): (a) an alpha-olefin copolymer; and (b) an ethylene-propylene-butadiene copolymer.
[10] The method according to any one of [1] to [9] above, wherein the first polyolefin polymer or the HMW polyolefin component has a weight average molecular weight of at least 110,000 grams / mole (g / mol).
[11] The method according to any one of the above [1] to
[10] , wherein the polymerization is a gas phase polymerization process and the polymerization reactor is a single gas phase polymerization reactor.
[12] The method further comprises transitioning from step (B) to a step of (B1) supplying a second trim catalyst to the polymerization reactor to produce a second alkane-soluble nonmetallocene catalyst, the second trim catalyst being prepared by contacting a solution of a second alkane-soluble nonmetallocene pre-catalyst dissolved in an alkane solvent with an activator, the second alkane-soluble nonmetallocene pre-catalyst differing from the first alkane-soluble nonmetallocene pre-catalyst in the structure of at least one nonmetallocene ligand, the second alkane-soluble nonmetallocene catalyst differing from the first alkane-soluble nonmetallocene catalyst in the structure of the at least one nonmetallocene ligand, and the second alkane-soluble nonmetallocene pre-catalyst differing from the first alkane-soluble nonmetallocene catalyst in the structure of the at least one nonmetallocene ligand. The method of any of [1] to
[11] above, wherein the alkane-soluble nonmetallocene precatalyst is characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane, based on the total weight of the second alkane-soluble nonmetallocene precatalyst and hexane, as measured using a solubility test method, and the transitioning comprises decreasing the feeding of the first trim catalyst from a steady state value until the first trim catalyst is no longer fed to the polymerization reactor, and independently starting and increasing the feeding of the second trim catalyst to the polymerization reactor until the second trim catalyst is fed to the polymerization reactor at a steady state value.
[13] The first alkane-soluble nonmetallocene pre-catalyst, and any second alkane-soluble nonmetallocene pre-catalyst, independently, have at least 60 weight percent n-hexane (CH), based on their combined weights. 3 (CH 2 ) 4 CH 3 The method according to any one of the above [1] to
[12] , characterized in that the compound has a solubility of 0.50 to 24% by weight in hexane containing 2,4-dichlorophenyl ether.
Claims
1. 1. A method for polymerizing olefin monomers to make a first polyolefin composition comprising a first polyolefin polymer, comprising: (A) contacting a solution of a first alkane-soluble nonmetallocene pre-catalyst dissolved in an alkane solvent with an activator to produce a first trim catalyst comprising a first alkane-soluble nonmetallocene catalyst; (B) feeding the first trim catalyst to a polymerization reactor; and (C) polymerizing said olefin monomers in said polymerization reactor with said first TRIM catalyst, thereby producing said first polyolefin composition comprising said first polyolefin polymer; The method includes the steps (A) to (C) of: the first alkane-soluble nonmetallocene pre-catalyst is characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane, based on the total weight of the first alkane-soluble nonmetallocene pre-catalyst and hexane, as measured using a Solubility Test Method; The first alkane soluble nonmetallocene pre-catalyst has the following formula (1): 【Chemistry 1】 (In the above formula, M is a Group 4 metal and each R is independently a group represented by the formula -(C(R A ) 2 ) m QZR 1 R 2 R 3 and In this case, in the above formula, R A are independently H or (C 1 -C 3 ) alkyl, or Each R A But, R A '-R A ' and R A '-R A ', (C 1 -C 3 ) alkylene; m is 1, 2, or 3; Q is not present or (C 1 -C 3 ) alkylene, or unsubstituted or substituted phenylene; Z is C or Si; R 1 , R 2 , and R 3 is independently unsubstituted or substituted with one or more substituents (C 1 -C 15 ) alkyl; The substituents are independently unsubstituted (C 1 -C 5 ) alkyl, halogen, -Oalkyl, -N(alkyl) 2 and -Si(alkyl) 3 is selected from However, when m is 2, (C(R A ) 2 ) m is C(R A ) 2 CH(R A ) or C(R A ) 2 CH 2 Instead, When m is 3, (C(R A ) 2 ) m is C(R A ) 2 CH(R A ) C(R A ) 2 or C(R A ) 2 CH 2 C(R A ) 2 isn't it) The method of claim 1,
2. 2. The method of claim 1, wherein the first trim catalyst comprises a solution of the first alkane-soluble nonmetallocene catalyst dissolved in an alkane solvent, and step (B) comprises feeding the solution to the reactor, the solution being free of support material.
3. (a) separately from step (A), contacting a first metallocene pre-catalyst with an activator, and optionally a support material, to produce a first metallocene catalyst, optionally free of said support material or disposed on and / or in said support material; (b) separately from step (B), feeding said first metallocene catalyst to said polymerization reactor; 3. The method of claim 1 or 2, wherein step (C) further comprises polymerizing the olefin monomer with the first metallocene catalyst in the polymerization reactor, thereby making a first bimodal polyolefin composition comprising the first polyolefin polymer and a second polyolefin polymer.
4. step (B) comprises feeding the first trim catalyst to the polymerization reactor as a solution of the first alkane-soluble nonmetallocene catalyst dissolved in a first alkane solvent; wherein step (b) comprises separately feeding a solution of the first metallocene catalyst in a second alkane solvent to the polymerization reactor; 4. The method of claim 3, wherein the first and second alkane solvents are the same or different, and the solution is free of support material.
5. After said step (C), (D) dividing said method by steps (a) and (b), respectively, (a1) contacting a second metallocene pre-catalyst, which differs from the first metallocene pre-catalyst in the structure of at least one cyclopentadienyl ligand, with an activator, and optionally a support material, to produce a second metallocene catalyst different from the first metallocene catalyst, wherein the second metallocene catalyst does not include a support material or is disposed on and / or in the support material; and (b1) decreasing the feed of the first metallocene catalyst from a steady state value until the first metallocene catalyst is no longer fed to the polymerization reactor, and independently starting and increasing the feed of the second metallocene catalyst to the polymerization reactor until the second metallocene catalyst is fed to the polymerization reactor at a steady state value; and further proceeding to steps (a1) and (b1) of step (C) further comprises polymerizing said olefin monomer with said second metallocene catalyst in said polymerization reactor, thereby making a second multimodal polyolefin composition comprising said first polyolefin polymer made by said first TRIM catalyst and a third polyolefin polymer made by said second metallocene catalyst; 5. The method of claim 3 or 4, wherein the third polyolefin polymer is different from each of the first and second polyolefin polymers.
6. 10. The method of claim 1, wherein the first trim catalyst further comprises a support material upon which the first alkane-soluble nonmetallocene catalyst is disposed.
7. 1. A method for polymerizing olefin monomers to make a first bimodal polyolefin composition comprising a first high molecular weight (HMW) polyolefin component and a first low molecular weight (LMW) polyolefin component, the method comprising the steps of: (1) contacting a solution of a first alkane-soluble nonmetallocene pre-catalyst dissolved in an alkane solvent with an activator to produce a first trim catalyst comprising a first alkane-soluble nonmetallocene catalyst; (2) contacting a first metallocene pre-catalyst and an additional amount of said first alkane-soluble nonmetallocene pre-catalyst with an activator and optionally a support material to produce a first bimodal catalyst system comprising a first metallocene catalyst and an additional amount of said first alkane-soluble nonmetallocene catalyst, optionally free of said support material or disposed on and / or in said support material; (3) contacting the first bimodal catalyst system with the first trim catalyst to form a first mixed catalyst system comprising a mixture of the first bimodal catalyst system and the first trim catalyst; (4) feeding the first mixed catalyst system into a polymerization reactor; and (5) polymerizing said olefin monomers with said first mixed catalyst system in said polymerization reactor, thereby producing said first HMW polyolefin component and said first LMW polyolefin component of said first bimodal polyolefin composition; The method includes steps (1) to (5). the first alkane-soluble nonmetallocene pre-catalyst is characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane, based on the total weight of the first alkane-soluble nonmetallocene pre-catalyst and hexane, as measured using a Solubility Test Method; The first alkane soluble nonmetallocene pre-catalyst has the following formula (1): 【Chemistry 2】 (In the above formula, M is a Group 4 metal and each R is independently a group represented by the formula -(C(R A ) 2 ) m QZR 1 R 2 R 3 and In this case, in the above formula, R A are independently H or (C 1 -C 3 ) alkyl, or Each R A But, R A '-R A ' and R A '-R A ', (C 1 -C 3 ) alkylene; m is 1, 2, or 3; Q is not present or (C 1 -C 3 ) alkylene, or unsubstituted or substituted phenylene; Z is C or Si; R 1 , R 2 , and R 3 is independently unsubstituted or substituted with one or more substituents (C 1 -C 15 ) alkyl; The substituents are independently unsubstituted (C 1 -C 5 ) alkyl, halogen, -Oalkyl, -N(alkyl) 2 and -Si(alkyl) 3 is selected from However, when m is 2, (C(R A ) 2 ) m is C(R A ) 2 CH(R A ) or C(R A ) 2 CH 2 Instead, When m is 3, (C(R A ) 2 ) m is C(R A ) 2 CH(R A ) C(R A ) 2 or C(R A ) 2 CH 2 C(R A ) 2 isn't it) The method of claim 1,
8. After step (5), (6) dividing the method into steps (2) to (5), respectively, (2a) contacting a second metallocene pre-catalyst and a second additional amount of said first alkane-soluble nonmetallocene pre-catalyst with an activator and optionally a support material to produce a second bimodal catalyst system comprising a second metallocene catalyst and said second additional amount of said first alkane-soluble nonmetallocene catalyst, optionally free of said support material or disposed on and / or in said support material; (3a) contacting the second bimodal catalyst system with the same trim catalyst as in step (1) to form a second mixed catalyst system comprising a mixture of the second bimodal catalyst system and the first trim catalyst; (4a) decreasing the feeding of the first mixed catalyst system from a steady state value until the first mixed catalyst system is no longer fed to the polymerization reactor, and independently starting and increasing the feeding of the second mixed catalyst system to the polymerization reactor until the second mixed catalyst system is fed to the polymerization reactor at a steady state value; and (5a) polymerizing said olefin monomers in said polymerization reactor with said second mixed catalyst system, thereby producing a second bimodal polyolefin composition comprising said first HMW polyolefin component and a second LMW polyolefin component, said second LMW polyolefin component being different from each of said first HMW polyolefin component and said first LMW polyolefin component; The method of claim 7, further comprising proceeding to steps (2a)-(5a).
9. The olefin monomer is (i) ethylene, (ii) propylene, (iii) (C 4 -C 20 (iv) 1,3-butadiene; (v) a combination of (i) and (ii); (vi) a combination of (i) and (iii); and (vii) a combination of (i), (ii), and (iv); The first polyolefin polymer is: (a) a polyethylene homopolymer; (b) a polypropylene homopolymer; (c) a poly(C 4 -C 20 ) alpha-olefin polymers, (d) polybutadiene polymers, (e) ethylene-propylene copolymers, (f) poly(ethylene-co-(C 4 -C 20 7. The method of claim 1, comprising any one of (a) through (g): (a) an alpha-olefin) copolymer; and (g) an ethylene-propylene-butadiene copolymer.
10. The method of any one of claims 1 to 6 and 9, wherein the first polyolefin polymer has a weight average molecular weight of at least 110,000 grams per mole (g / mol).
11. The process for producing a polymerizable composition comprising the steps of: (i) ethylene, (ii) propylene, (iii) a (C4-C20) alpha-olefin, (iv) 1,3-butadiene, (v) a combination of (i) and (ii), (vi) a combination of (i) and (iii), and (vii) a combination of (i), (ii), and (iv); 9. The method of claim 7 or 8, wherein the HMW polyolefin component comprises any one of (a)-(g) of: (a) polyethylene homopolymer, (b) polypropylene homopolymer, (c) poly(C4-C20) alpha-olefin polymer, (d) polybutadiene polymer, (e) ethylene-propylene copolymer, (f) poly(ethylene-co-(C4-C20) alpha-olefin) copolymer, and (g) ethylene-propylene-butadiene copolymer.
12. The method of any one of claims 7, 8 and 11, wherein the HMW polyolefin component has a weight average molecular weight of at least 110,000 grams / mole (g / mol).
13. The process according to any one of claims 1 to 12, wherein the polymerization is a gas phase polymerization process and the polymerization reactor is a single gas phase polymerization reactor.
14. From step (B), (B1) feeding a second trim catalyst to the polymerization reactor, the second trim catalyst being prepared by contacting a solution of a second alkane-soluble nonmetallocene pre-catalyst dissolved in an alkane solvent with an activator to prepare a second alkane-soluble nonmetallocene catalyst; [0023] the second alkane-soluble nonmetallocene pre-catalyst differs from the first alkane-soluble nonmetallocene pre-catalyst in the structure of at least one nonmetallocene ligand; the second alkane-soluble nonmetallocene catalyst differs from the first alkane-soluble nonmetallocene catalyst in the structure of the at least one nonmetallocene ligand; the second alkane-soluble nonmetallocene pre-catalyst is characterized by a solubility of at least 0.10 weight percent in hexane containing at least 60 weight percent n-hexane, based on the total weight of the second alkane-soluble nonmetallocene pre-catalyst and hexane, as measured using a Solubility Test Method; 7. The method of any one of claims 1 to 6, wherein the transitioning comprises decreasing the feeding of the first trim catalyst from a steady state value until the first trim catalyst is no longer fed to the polymerization reactor, and independently initiating and increasing the feeding of the second trim catalyst to the polymerization reactor until the second trim catalyst is fed to the polymerization reactor at a steady state value.
15. The first alkane soluble nonmetallocene pre-catalyst, and any second alkane soluble nonmetallocene pre-catalyst, independently, have at least 60 weight percent n-hexane (CH 3 (CH 2 ) 4 CH 3 15. The process according to claim 1, characterized in that the solubility of the ester in hexane containing 0.50 to 24% by weight is 0.50 to 24% by weight.
Citation Information
Patent Citations
Fluoroalcohol leaving group for non-metallocene olefin polymerization catalysts
US20050182212A1
Ligands for catalysts
US20160032025A1
Methods for operating a polymerization reactor
US20180118862A1
Polyethylene compositions
WO2010008964A1
Methods of preparing a catalyst system
WO2013070601A2