Process and apparatus assembly useful for producing silicone rubber articles by injection molding from liquid silicone rubber compositions

The method and apparatus assembly for LSR injection molding improve curing speed and temperature control, addressing component imbalance issues and enabling efficient overmolding on heat-sensitive substrates by precise control of inhibitor and catalyst ratios, resulting in rapid and flexible silicone rubber production.

JP7591035B2Active Publication Date: 2024-11-27ELKEM SILICONES USA CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022506294
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-30
Filing Date
2020-07-28
Publication Date
2024-11-27
Estimated Expiration
2040-07-28

AI Technical Summary

Technical Problem

Existing liquid silicone rubber (LSR) injection molding processes face challenges with poor metering and mixing of components, leading to unstable cure rates and varying physical properties, require expensive equipment, and have limitations in curing temperature, especially when overmolding on heat-sensitive substrates.

Method used

A method and apparatus assembly that separates and controls the supply of catalyst-free liquid silicone rubber base, catalyst masterbatch, inhibitor masterbatch, and crosslinker through distinct feed lines, allowing precise control of the molar ratio of hydrosilylation vulcanization inhibitor to platinum catalyst, enabling faster curing at lower temperatures (below 160°C) and flexible production of silicone rubber products.

Benefits of technology

Achieves rapid curing times (Tc90 below 30 seconds at 110°C) with controlled cure rates, allowing overmolding on heat-sensitive materials without compromising quality, and enhances productivity and flexibility in manufacturing conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591035000012
    Figure 0007591035000012
  • Figure 0007591035000013
    Figure 0007591035000013
  • Figure 0007591035000014
    Figure 0007591035000014
Patent Text Reader

Abstract

An apparatus assembly and method useful for producing molded silicone rubber articles from liquid silicone rubber compositions (LSR) by injection molding. The method of the present invention provides a flexible process for producing rapidly cured silicone rubber articles from LSR, allowing for the use of low cure temperatures in the mold cavity without significantly reducing the cure rate of the LSR or the physical properties of the resulting molded silicone rubber material, thereby enabling overmolding of liquid silicone rubber onto or over heat-sensitive substrates. This apparatus allows for a flexible process for faster production of cured silicone rubber articles from liquid silicone rubber (LSR), enabling faster cycles and the use of precise dosing and mixing sections.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel method and apparatus assembly useful for producing silicone rubber articles by injection molding from liquid silicone rubber compositions (hereinafter LSR). [Background technology]

[0002] Liquid silicone rubber injection molding equipment assemblies that use liquid silicone rubber ("LSR") compositions to form silicone rubber articles have been in existence for nearly 50 years. In the silicone rubber field, LSR compositions that react by addition crosslinking are known.

[0003] LSR compositions are a type of thermosetting rubber. They are characterized by their low processing viscosity compared to solid silicones and elastomers. The two-component mixture crosslinks by an addition process, meaning that the reaction takes place without forming decomposition products. This is an important advantage in the area of ​​injection molding, since there are no curing by-products and no risk of deposits forming on the mold.

[0004] Similar to conventional rubber processing equipment, plastic processing machinery is now being employed in the manufacture of LSR products. Injection molding of LSR compositions is often the preferred choice for manufacturers of silicone rubber parts because of ease of processing, the ability to produce large quantities, consistent quality, and increased productivity. Injection molding of LSR is carried out in suitable injection molding presses specifically designed for LSR.

[0005] Typically, LSR molded rubber products are produced using a two-component platinum-catalyzed addition cure reaction, where the first component is a mixture of vinyl siloxane polymer, treated amorphous fumed silica, and platinum catalyst (component A or part A), and the second component is a mixture of vinyl siloxane polymer, treated amorphous fumed silica, hydrogen siloxane cross-polymer, and cure rate inhibitor (component B or part B). Since the LSR composition is shipped from the manufacturer as two-component drums (20 liters or 200 liters), removal of the A and B component materials is performed by inputs designed for LSR. These inputs use a circular device with the same diameter as the drum, called a "follower plate," which presses against the drum and pumps the material under applied pressure into a feed line hose. A piston pump is installed as a conveyor and pump. The two components are sent through a conduit to the mixing section, where they are first combined. Both pumps are set to operate synchronously to achieve a 1:1 mix ratio. For a more homogeneous mixture, a static mixer is installed downstream through which the material components are passed before being sent to the injection molding press. For additives (pigments, colorants, etc.) a dosing system with a separate dosing valve is used.

[0006] In this process, the dosing and mixing sections are critical steps since accurate metering is essential for mixing the A and B components and adding additives. In fact, poor metering and mixing of the two separate components can lead to an imbalance in the ratio of hydrogenated siloxane polymer to siloxane alkenyl polymer present in the crosslinkable LSR composition produced before injection molding. This can result in unstable injection cure rates and fluctuating physical properties of the cured parts.

[0007] The mixture of A and B is further mixed in the transfer screw of the LSR machine before being injected into the mold. Inhibitors for the hydrosilylation vulcanization reaction are important chemicals used in LSR compositions because without the use of inhibitors, the crosslinking reaction can start immediately upon mixing the two components even at room temperature. Therefore, the level of inhibitor is an important parameter required to give the necessary processing time before the crosslinking reaction begins. The mixture of A and B is then heat cured for a specific time and temperature depending on the size of the part. The finished cured product is ejected from the mold using a robotic device or similar and the process is repeated.

[0008] Examples of the prior art include U.S. Pat. No. 3,884,866, which discloses a two-part LSR process using two vinyl siloxane polymers, a platinum catalyst, and a pretreated silica filler as the first component, and the same vinyl siloxane polymer and pretreated silica filler plus a silyl hydride-containing organopolysiloxane and a cure rate inhibitor as the second component. U.S. Pat. No. 4,162,243 discloses a two-part LSR process using an in situ treated amorphous silica filler. U.S. Pat. No. 5,977,220 discloses a two-part LSR process using a nitrogen organic cation salt to improve the compression set of silicone mixtures. U.S. Pat. No. 6,034,199 discloses a two-part LSR process with improved cure rate inhibitors. U.S. Pat. No. 6,464,923 discloses a three-part LSR process. The first component is a diorganopolysiloxane polymer and an inorganic filler, the second component is a mixture of a liquid catalyst and a diorganopolysiloxane polymer, and the third component is a hydrogen siloxane mixed with an organopolysiloxane polymer. This patent also discloses the use of carbon black as an inorganic filler. This separation into three components improves storage stability compared to the two-component LSR process.

[0009] As can be seen, all standard LSR processes have several problems. The first problem is related to poor metering and mixing of the two separate components, which can lead to an imbalance in the amount of silicone hydrogen crosslinker present in the finished part, unstable injection cure rates, and variable physical properties of the cured part. The second problem is the expensive equipment required to deliver the two separate mixtures to the metering and mixing equipment. The third problem is the large and specific (non-variable or set) amount of inhibitor present in component B required to obtain a room temperature work life of several days. This inhibitor level can slow the cure rate of the molded part, thereby increasing the work life.

[0010] In another approach, US Patent No. 8,063,137 and US Patent No. 8,198,357 describe a method for producing molded silicone rubber products using a liquid silicone rubber (LSR) base containing at least one vinyl siloxane polymer, at least one hydride crosslinker, and optionally at least one inhibitor for hydrosilylation vulcanization reactions, but without the presence of a catalyst in the base. This single LSR base is then fed into a mixing device, into which is fed an inhibitor masterbatch containing at least one liquid inhibitor for hydrosilylation vulcanization reactions and at least one vinyl siloxane polymer, and a catalyst masterbatch containing at least one catalyst and at least one vinyl siloxane polymer. Molding is then performed, allowing some improvement in cycle time. However, there remains a need to improve the productivity of the injection molding cycle without compromising the cure rate, especially when low temperature cure is required, for example at temperatures between 80 and 120°C.

[0011] In fact, it is well known that the vulcanization rate of liquid silicone rubber depends on three main factors: the temperature of the mold, the geometric thickness of the part (the gap between the heated surfaces of the mold and the relationship between surface area and volume), and the general vulcanization behavior and the curing chemistry. The cycle time can be reduced (i.e. productivity increases) by increasing the mold temperature, the cold runner is set at 40-80 °C using a temperature regulator and fast curing materials. However, using fast curing materials means changing the composition of the liquid silicone rubber feedstock, which may result in variable behavior for the wide range of injection molding equipment already available for injection molding machines.

[0012] Additionally, there is a strong need for an equipment assembly that can increase the productivity of the injection molding cycle while providing greater flexibility in the manufacture of silicone rubber products.

[0013] Furthermore, LSR compositions can also be used to overmold thermoplastic objects or substrates. However, non-silicone-based substrates such as thermoplastic materials are often prone to deformation at high temperatures (e.g., above 160°C) due to their composition. In fact, thermoplastic materials do not exhibit a precise melting point that indicates the transition from solid to liquid, but they slowly soften with increasing temperature. Therefore, two types of techniques have been introduced to describe the softening of the surface (Vicat softening temperature) or the softening of the body (heat deformation (or distortion) temperature, HDT).

[0014] The Vicat softening temperature is the temperature at which a flat-tipped needle penetrates a sample to a depth of 1 mm under a specific load (10N or 50N, see ASTM D1525-09 and ISO 306). The Vicat softening temperature reflects the expected softening point of a material when used in high temperature applications.

[0015] Deflection temperature under load methods, such as ASTM D648-07, measure the deflection temperature at which a given deformation occurs when a test specimen is subjected to a given set of test conditions that reflect the ability of the polymer to withstand a given load at elevated temperature.

[0016] Examples of heat-sensitive materials that have a Vicat softening temperature (under 1 kg load) below 160°C and may be damaged by the surface crosslinking of the LSR composition include polyvinyl chloride (PVC, 92°C), polyethylene (PE, 127.3°C), polypropylene (PP, 152.2°C), acrylonitrile butadiene styrene (ABS, 102.3°C), and polycarbonate (PC, 156.2°C).

[0017] Therefore, overmolding liquid silicone rubber onto heat-sensitive substrates such as thermoplastics is difficult to do without compromising quality. Furthermore, silicone rubber crosslinked materials can act as protective covers against dust, water, impact, heat, and electric shock, so they may be widely utilized in implantable devices where heat-sensitive plastic materials are widely used. Other applications that may benefit from solving the challenge of overmolding LSR compositions onto heat-sensitive plastic substrates include medical encapsulation of electronic devices, overmolded gaskets, surgical handles, radio-opaque markers for positioning medical devices, wearables, keypads, guards, electrical and thermal insulation, etc.

[0018] However, in standard LSR injection molding, lowering the molding temperature would drastically slow down the cure rate of the liquid silicone rubber, which would impact economic viability and is therefore unacceptable. [Prior art documents] [Patent documents]

[0019] [Patent Document 1] U.S. Pat. No. 3,884,866 [Patent Document 2] U.S. Pat. No. 4,162,243 [Patent Document 3] U.S. Patent No. 5,977,220 [Patent Document 4] U.S. Patent No. 6,034,199 [Patent Document 5] U.S. Patent No. 6,464,923 [Patent Document 6] U.S. Pat. No. 8,063,137 [Patent Document 7] U.S. Pat. No. 8,198,357 Summary of the Invention [Problem to be solved by the invention]

[0020] Therefore, there remains a need to provide a new, flexible method for producing silicone rubber articles using LSR compositions that allows well-defined, reproducible production conditions using fully automated production sequences, where appropriate, to significantly reduce the cure temperature in the mold cavity (below 160°C, below 140°C, below 120°C, below 110°C, or below 100°C) without compromising the cure speed of the LSR and the physical properties of the produced silicone rubber moldings. [Means for solving the problem]

[0021] SUMMARY OF THE PRESENT APPLICATION One object of the present invention is to provide a flexible process for producing fast cure silicone rubber products from liquid silicone rubber (LSR).

[0022] Another object of the present invention is to provide a novel and flexible process that allows the use of low cure temperatures (less than 160°C, less than 140°C, less than 120°C, less than 110°C or less than 100°C) in the mold cavity, thereby allowing the overmolding of liquid silicone rubber onto or over heat-sensitive substrates, without significantly decreasing the cure rate of the LSR and the physical properties of the produced silicone rubber molding material.

[0023] Another object of the present invention is to provide an equipment assembly useful for producing molded silicone rubber articles by injection molding that allows for faster cycles and the use of precise dosing and mixing sections, thereby creating a flexible process for producing faster cured silicone rubber articles from liquid silicone rubber (LSR).

[0024] For a further understanding of the nature, objects, and advantages of the present invention, reference should be made to the ensuing detailed description taken in conjunction with the following drawings, in which like reference numerals represent like elements and in which: [Brief description of the drawings]

[0025] [Figure 1] 1 is a schematic diagram of an apparatus assembly useful for producing molded silicone rubber articles by the method and injection molding according to the present invention, in which the inhibitor masterbatch E1 (31), catalyst masterbatch C1 (30) and crosslinker XL (32) are separated from the catalyst-free liquid silicone rubber base A1 (3) and fed to a mixing tank (18), preferably a static mixer, prior to introduction into the barrel (25) of an injection molding press. In this diagram, the optional presence of separate feed lines and containers of additives is not shown. [Diagram 2] Figure 2 is an embodiment of the present invention, a schematic diagram of an apparatus assembly useful for producing molded silicone rubber products by injection molding according to the method of the present invention. The inhibitor masterbatch E1 (31), the catalyst masterbatch C1 (30) and the crosslinker XL (32) are separated from the two liquid silicone rubber bases A1 and A2 without catalyst and fed to a mixing tank (18), preferably a static mixer (18), before being introduced into the barrel (25) of the injection molding press. The silicone rubber bases A1 (3) and A2 (4) can have similar compositions to allow a continuous process, or different compositions to give greater flexibility in terms of a wide range of Shore A durometers of the final molded silicone products. In this figure, the optional presence of separate feed lines and containers of additives is not shown. [Diagram 3] FIG. 3 shows a hardening curve or torque curve of torque versus time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Detailed Description of the Invention Before further describing the present invention, it should be understood that the present invention is not limited to the specific embodiments of the present invention described below, but that the specific embodiments may be modified and still be encompassed by the scope of the claims. It should also be understood that the terminology used is for the purpose of describing the specific embodiments and is not intended to be limiting. Instead, the scope of the present invention will be defined by the claims.

[0027] In this specification and claims, the singular forms "a," "an," and "the" include the plural forms unless the context clearly dictates otherwise. All technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, unless otherwise defined.

[0028] Such an object is achieved, inter alia, by the present invention, which relates to a method useful for producing a silicone rubber article M1 by injection molding, comprising the following steps: (a) does not contain a catalyst; and at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms, optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, preferably at least 3 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and optionally, at least one additive F into the base supply line a liquid silicone rubber base composition A1 comprising (b) feeding a catalyst masterbatch C1 containing at least one platinum-based catalyst D into another catalyst feed line; (c) feeding an inhibitor masterbatch E1, which comprises at least one inhibitor E for the hydrosilylation vulcanization reaction, into another feed line; (d) feeding into another feed line, or into any feed line containing the catalyst masterbatch C1 or the inhibitor masterbatch E1, at least one crosslinker XL, said crosslinker being an organopolysiloxane having at least three silicon-bonded hydrogen atoms per molecule if linear or cyclic, or at least two silicon-bonded hydrogen atoms per molecule if branched, preferably at least three silicon-bonded hydrogen atoms per molecule if branched; (e) optionally, feeding at least one additive F into a separate additive feed line; (f) conducting said liquid silicone rubber base composition A1, said catalyst masterbatch C1, said crosslinker XL, said inhibitor masterbatch E1 and optionally said additives F into a mixing tank (18) before conducting the resulting mixture into the barrel of an injector or directly into said barrel to produce the following: (1) at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms; (2) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms, preferably at least three silicon-bonded hydrogen atoms, per molecule B; (3) optionally, at least one filler C, (4) at least one platinum-based catalyst D; (5) at least one inhibitor E for the hydrosilylation vulcanization reaction, (6) at least one crosslinker XL, said crosslinker XL being an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear or cyclic polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer; and (7) optionally, at least one additive F wherein the amounts of said platinum-based catalyst D and said hydrosilylation vulcanization reaction inhibitor E added in said crosslinkable liquid silicone rubber composition A3 are controlled and adjusted so that the molar ratio of the hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of said platinum-based catalyst D is within the range of 0.1 to 900 (0.1:1 to 900:1), most preferably 10 to 900 (10:1 to 900:1), and even more preferably 20 to 250 (20:1 to 250:1); (g) introducing said cross-linkable liquid silicone rubber composition A3 into a mold placed in a molding press and curing said cross-linkable liquid silicone rubber composition A3 by heating it at a temperature preferably from 80°C to 220°C to obtain a molded silicone rubber product M1.

[0029] The Applicant has carried out extensive research in order to achieve this object and has unexpectedly discovered that it is possible to feed the inhibitor masterbatch E1, the liquid silicone rubber base A1 and the catalyst masterbatch C1 via different feed lines and to feed the crosslinker XL into another feed line or into any feed line containing the catalyst masterbatch C1 or the inhibitor masterbatch E1, (1) Controlling the amount of crosslinker XL added, and (2) In the liquid silicone rubber composition A3, immediately before the injection molding step, the molar ratio of the hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of the platinum-based catalyst D is maintained within the range of 0.1 to 900 (0.1:1 to 900:1), most preferably 10 to 900 (10:1 to 900:1), and even more preferably 20 to 250 (20:1 to 250:1). It has been demonstrated that by molding in an injection molding machine the crosslinkable liquid silicone rubber composition A3 according to the present invention, which is produced by feeding in the above-mentioned manner, it is possible to dramatically improve the optimum cure time (Tc90), at which 90% cure occurs as measured by a moving die rheometer (MDR) at 110°C, without serious loss of cure rate, as compared to the methods described in the prior art U.S. Pat. Nos. 8,063,137 and 8,198,357.

[0030] Indeed, optimum cure times of less than 30 seconds for 90% cure at 110°C (Tc90) and less than 20 seconds for 10% cure at 110°C (Tc10) are achieved, eliminating the need for post-curing steps, which can include several hours of residence time in an oven, typically required after the object is removed from the mold.

[0031] The advantages of lowering the cure (molding) temperature without significantly compromising cure rate are numerous, including energy savings from operating the molded part at a lower temperature.

[0032] Another advantage of the present invention is the flexibility in choosing a low cure temperature (80°C-120°C) without compromising the optimal cure rate of the LSR material, thereby allowing overmolding onto heat-sensitive materials, which are materials that experience distortion or deformation problems upon thermal contact.

[0033] The method of the present invention allows efficient use of molding temperature ranges of 80°C to 220°C, 80°C to 160°C, 80°C to 140°C, 80°C to less than 120°C, 80°C to less than 110°C, or 80°C to less than 100°C without compromising the optimal cure rate of the LSR material.

[0034] Also, faster cure times at standard elevated temperatures allow for shorter cycle times for standard parts.

[0035] In a preferred embodiment, the present invention relates to a method useful for producing a silicone rubber article M1 by injection molding, comprising the steps of: (a) does not contain a catalyst; and at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms, optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, preferably at least 3 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and optionally, at least one additive F into the base supply line (8) a liquid silicone rubber base composition A1 comprising (b) feeding a catalyst masterbatch C1 comprising at least one platinum-based catalyst D into another catalyst feed line (12); (c) feeding an inhibitor masterbatch E1, which comprises at least one inhibitor E for the hydrosilylation vulcanization reaction, into another feed line (14); (d) feeding into another feed line (16) at least one crosslinker XL, said crosslinker XL being an organopolysiloxane having at least three silicon-bonded hydrogen atoms per molecule if linear or cyclic, or at least two silicon-bonded hydrogen atoms per molecule if branched, preferably at least three silicon-bonded hydrogen atoms per molecule if branched; (e) optionally, feeding at least one additive F into a separate additive feed line (38); (f) conducting said liquid silicone rubber base composition A1, said catalyst masterbatch C1, said crosslinker XL, said inhibitor masterbatch E1 and optionally said additives F into a mixing tank (18) before conducting the resulting mixture into the barrel of an injector or directly into said barrel to produce the following: (1) at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms; (2) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms, preferably at least three silicon-bonded hydrogen atoms, per molecule B; (3) optionally, at least one filler C, (4) at least one platinum-based catalyst D; (5) at least one inhibitor E for the hydrosilylation vulcanization reaction, (6) at least one crosslinker XL, said crosslinker XL being an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear or cyclic polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer; and (7) optionally, at least one additive F wherein the amounts of said platinum-based catalyst D and said hydrosilylation vulcanization reaction inhibitor E added in said crosslinkable liquid silicone rubber composition A3 are controlled and adjusted so that the molar ratio of the hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of said platinum-based catalyst D is within the range of 0.1 to 900 (0.1:1 to 900:1), most preferably 10 to 900 (10:1 to 900:1), and even more preferably 20 to 250 (20:1 to 250:1); (g) introducing said cross-linkable liquid silicone rubber composition A3 into a mold placed in a molding press and curing said cross-linkable liquid silicone rubber composition A3 by heating it at a temperature preferably from 80°C to 220°C to obtain a molded silicone rubber product M1.

[0036] Suitable crosslinking agents XL, provided in a separate supply line, are linear organopolysiloxanes containing at least three silicon-bonded hydrogen atoms per molecule, cyclic organopolysiloxane polymers containing at least three silicon-bonded hydrogen atoms per molecule, or branched organopolysiloxane polymers containing at least three silicon-bonded hydrogen atoms per molecule.

[0037] In another preferred embodiment, the crosslinker is a mixture of at least one linear organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule and at least one branched organopolysiloxane polymer containing at least three silicon-bonded hydrogen atoms per molecule.

[0038] A "branched organopolysiloxane polymer" is a polymer having the formula SiO 4 / 2 Q siloxy units of the formula RSiO 3 / 2(wherein R has a hydrogen atom or a monovalent hydrocarbon group of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon group of 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl, and most preferably selected from the group consisting of methyl and phenyl.

[0039] In a preferred embodiment, the crosslinker XL is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule and containing at least two silicon-bonded hydrogen atoms and having within its structure the formula SiO 4 / 2 Q siloxy units of the formula RSiO 3 / 2 In the above formula, R is a hydrogen atom or a monovalent hydrocarbon group having 1 to 40 carbon atoms, preferably a monovalent hydrocarbon group having 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl, and most preferably selected from the group consisting of methyl and phenyl. 1 / 2 M is a siloxy unit of the formula RSiO 2 / 2 Other standard siloxy units may also be present, such as D siloxy units of the formula: where the symbols R are the same or different and are selected from a hydrogen atom or a monovalent hydrocarbon radical having 1 to 40 carbon atoms, preferably selected from monovalent hydrocarbon radicals having 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, t-butyl, pentyl, hexyl, heptyl, phenyl, benzyl and mesityl, and most preferably selected from the group consisting of methyl and phenyl.

[0040] Such a component acts as a crosslinker for organopolysiloxane A by addition reaction between silicon-bonded hydrogen atoms of crosslinker XL and alkenyl groups of organopolysiloxane A component in the presence of a catalyst described below, forming a network structure, thereby curing the composition.

[0041] Examples of suitable crosslinkers XL which, when linear, contain at least three silicon-bonded hydrogen atoms per molecule include, but are not limited to, trimethylsiloxy endblocked methylhydrogenpolysiloxane; trimethylsiloxy endblocked dimethylsiloxane-methylhydrogensiloxane copolymer; trimethylsiloxy endblocked methylhydrogensiloxane-methylphenylsiloxane copolymer; trimethylsiloxy endblocked dimethylsiloxane-methylhydrogensiloxane-methylphenylsiloxane copolymer; dimethylhydrogensiloxy endblocked dimethylpolysiloxane; dimethylhydrogensiloxy endblocked methylhydrogensiloxane; dimethylhydrogensiloxy endblocked dimethylsiloxane-methylhydrogensiloxane copolymer; dimethylhydrogensiloxy endblocked dimethylsiloxane-methylhydrogensiloxane copolymer; and dimethylhydrogensiloxy endblocked methylphenylpolysiloxane.

[0042] The viscosity is typically 0.001 to 100 Pa·s at 25° C., and preferably 0.001 to 1 Pa·s at 25° C., in order to obtain good miscibility with other components.

[0043] In a preferred embodiment, when the crosslinker XL containing at least 3 silicon-bonded hydrogen atoms per molecule is linear, the crosslinker XL is selected from those containing less than 15 mmol / g SiH per molecule.

[0044] Examples of suitable crosslinkers XL which, when branched, contain at least two silicon-bonded hydrogen atoms per molecule include branched polymers of formula (I): (R2HSiO 1 / 2 ) x (R3SiO 1 / 2 )y (RHSiO2 / 2) z (R2SiO 2 / 2 ) p (RSiO 3 / 2 ) q (HSiO 3 / 2 ) v (SiO 4 / 2 ) r (I) During the ceremony, H is hydrogen and R is a monovalent hydrocarbon radical of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon radical of 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl; most preferably selected from the group consisting of methyl and phenyl, x≧2, y≧0, z≧0, p≧0, v≧0, and at least one of q or r is ≧1; or x≧2, y≧0, z≧0, p≧0, q≧0; v≧0, r≧1; or x≧2, y≧0, r≧1 (with the proviso that r=1, x+y=4) and z, p, q, v=0. Or x>2, y>0, r>1 and z, p, q, v=0.

[0045] Specific crosslinkers XL that, when branched, contain at least two silicon-bonded hydrogen atoms per molecule include, but are not limited to, (H)(CH)SiO 1 / 2 Siloxy unit (M H ) and SiO 4 / 2 Silicone resin M containing siloxy units (Q units) H Q, (CH3)3SiO 1 / 2 Siloxy unit (M), (CH3)2HSiO 1 / 2 Siloxy unit (M H ) and SiO 4 / 2 Silicone resin MM containing (Q) H Q, (CH3)2HSiO 1 / 2 Siloxy unit (M H ), (CH3)HSiO 2 / 2 (D H ) and SiO 4 / 2 Silicone resin M containing siloxy units (Q)H D H Q, and (CH3)3SiO 1 / 2 Units (M units), (CH3)2HSiO 1 / 2 (M H ), (CH3)HSiO 2 / 2 (D H ) and SiO 4 / 2 Silicone resin containing unit (Q) MM H D H Q.

[0046] In a preferred embodiment, the crosslinker XL has the formula R2HSiO 1 / 2 At least two, preferably at least three, M H Siloxy units and the formula SiO 4 / 2 M containing Q siloxy units H Q silicone resin, in which H is a hydrogen atom and R is a monovalent hydrocarbon group of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon group of 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl, and most preferably selected from the group consisting of methyl and phenyl.

[0047] In a preferred embodiment, the crosslinker XL has the formula H Q Silicone resin: M H w Q z where Q is a group of formula SiO 4 / 2 M H is the formula R2HSiO 1 / 2wherein H is a hydrogen atom, R is a monovalent hydrocarbon radical of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon radical of 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentaerythritol, hexyl, heptyl, phenyl, benzyl, and mesityl, and most preferably selected from the group consisting of methyl and phenyl, and the subscripts w and z have a ratio of 0.5 to 4.0, preferably 0.6 to 3.5, more preferably 0.75 to 3.0, and most preferably 1.0 to 3.0, respectively.

[0048] In another preferred embodiment, the crosslinker XL has the formula H Q Silicone resin: (M H w Q z ) j where Q is a group of formula SiO 4 / 2 M H is the formula R2HSiO 1 / 2 where H is a hydrogen atom, R is a monovalent hydrocarbon group of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon group of 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentaerythritol, hexyl, heptyl, phenyl, benzyl, and mesityl, and most preferably selected from the group consisting of methyl and phenyl, the subscripts w and z have a ratio of 0.5 to 4.0, preferably 0.6 to 3.5, more preferably 0.75 to 3.0, and most preferably 1.0 to 3.0, and the subscript j is in the range of about 2.0 to about 100, preferably about 2.0 to about 30, more preferably about 2.0 to about 10, and most preferably about 3.0 to about 5.0.

[0049] In another preferred embodiment, the crosslinker XL has 0.10 wt. % to 2.00 wt. % H as SiH and has the formula R2HSiO 1 / 2 M H Siloxy units with the formula SiO 4 / 2In the above formula, H is a hydrogen atom and R is a monovalent hydrocarbon group having 1 to 40 carbon atoms, preferably a monovalent hydrocarbon group having 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl, and most preferably selected from the group consisting of methyl and phenyl.

[0050] Suitable commercially available M H Examples of Q silicone resins are Silmer® HQ20 (ratio M / Q is 2:1, weight % H as SiH is 0.65%) and HQ203 (ratio M / Q is 1.2:1, weight % H as SiH is 0.12%) sold by Siltech, and silicone resins HQM®-105 and HQM-107 sold by Gelest.

[0051] Most preferred M H Q Silicone resins have the formula R2HSiO 1 / 2 and SiO 4 / 2 (wherein H is a hydrogen atom, and R is a methyl having 1.10 to 1.30% by weight of H as SiH) H Q Silicone resin.

[0052] In another preferred embodiment, the crosslinking agent according to the present invention is selected from the following group and corresponding mixtures thereof: XL1 = polyphenyl(dimethylhydrosiloxy)siloxane hydride terminated, manufactured by Gelest, reference number HDP-111, viscosity 50-80 mPa s, total SiH (mmol / g) = 5.2; formula (M H ) 2+n (T Ph ) n Silicone resin (where M = RHSiO 1 / 2 Siloxy unit and T Ph =PhSiO 3 / 2 where H is a hydrogen atom, R is methyl and Ph is phenyl; [ka] XL1 · XL2: Copolymer of dimethylsiloxane and methylhydrogensiloxane, partially capped at both molecular ends with dimethylhydrogensiloxy groups (viscosity 18-26 mPa·s; total SiH (mmol / g) = 7.2 (linear crosslinker); XL3:R2HSiO 1 / 2 and the formula SiO 4 / 2 Q Siloxy unit M H Q silicone resin (where H is hydrogen, R is methyl, and total SiH (mmol / g)=7.3); Milliken, reference number SiVance MQH-8MQ hydride resin; ·XL4:Formula M H Q branched silicone resin (where MH = RHSiO 1 / 2 and Q is of the formula SiO 4 / 2 where H is a hydrogen atom, R is a methyl, and total SiH (mmol / g)=8.8; ·XL5:Formula M H Q branched silicone resin (where M H =R2HSiO 1 / 2 and Q is of the formula SiO 4 / 2 where H is hydrogen, R is methyl, and total SiH (mmol / g)=9.7) (Milliken Corporation reference SiVance MQH-9 hydride resin); ·XL6: Formula (M H )3(T Ph ) branched silicone resin (where M = RHSiO 1 / 2 Siloxy units, T Ph =PhSiO 3 / 2 where H is a hydrogen atom, R is methyl, and Ph is phenyl), from Gelest, reference number SIP6826, phenyltris(dimethylhydrosiloxy)silane, total SiH (mmol / g)=5.2; [ka] XL6 ·XL7:Formula M HQ branched silicone resin (where M H =R2HSiO 1 / 2 and Q is of the formula SiO 4 / 2 where H is a hydrogen atom and R is a methyl), manufactured by Gelest, reference number SIT7278.0, total SiH (mmol / g)=6.7: [ka] XL7

[0053] In another preferred embodiment, the crosslinker XL according to the invention is a mixture comprising: (a) Formula R2HSiO 1 / 2 At least two, preferably at least three, M H Siloxy units and the formula (Ph)SiO 3 / 2 T Ph at least one branched silicone resin containing siloxy units (wherein Ph is a phenyl group, H is a hydrogen atom, and R is a monovalent hydrocarbon group having 1 to 40 carbon atoms, preferably a monovalent hydrocarbon group having 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl, and most preferably selected from the group consisting of methyl and phenyl); and (b) at least one linear organopolysiloxane B containing at least three silicon-bonded hydrogen atoms per molecule, and / or a polysiloxane of the formula R2HSiO 1 / 2 At least two, preferably at least three, M H Siloxy units with the formula SiO 4 / 2 Q siloxy units and branched M HQ Silicone Resin, wherein H is a hydrogen atom and R is a monovalent hydrocarbon group of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon group of 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl, and most preferably selected from the group consisting of methyl and phenyl.

[0054] In another preferred embodiment, in step (d), the amount of crosslinker XL added is controlled and maintained in the range of 0.1 to 5.0 wt.%, preferably 0.1 to 3.5 wt.%, based on the weight of the crosslinkable liquid silicone rubber composition A3. Crosslinker XL is used in said amount sufficient to cure the composition, preferably an amount providing from about 1.0 to about 10 silicon-bonded hydrogen atoms per alkenyl group in the alkenyl-containing organopolysiloxane A.

[0055] In another preferred embodiment, in step (g), the curing temperature is 80 to 140°C, preferably 90 to 130°C.

[0056] In another preferred embodiment, in step (g), the curing temperature is 80-140°C, preferably 90-130°C, and the crosslinkable liquid silicone rubber composition A3 is cured around or over the substrate P to form a composite part comprising the molded silicone rubber product M1.

[0057] The substrate P may be rigid or flexible. In a preferred embodiment, the substrate P is selected from plastic substrates, thermoplastic substrates, metal substrates and textile substrates.

[0058] Examples of plastic and thermoplastic substrates (including organic resins) include acrylonitrile-butadiene-styrene, polyphenylene / styrene blends, polystyrene, polycarbonate, polyurethane, styrene resin, polyethylene, polypropylene, acrylic, polyacrylamide, polyester, polyethylene terephthalate, polybutylene terephthalate, polyphenylene oxide, polyphenylene sulfide, polysulfone, nylon, polyamide, polyimide, fluororesin, liquid crystal resin, and non-resin-containing polyetherimide.

[0059] In preferred embodiments, the substrate P is polyvinyl chloride (PVC), polyethylene (PE), polypropylene (PP), acrylonitrile butadiene styrene (ABS) and polycarbonate (PC).

[0060] Examples of metal substrates include those selected from copper, alclad aluminum, anodized aluminum, titanium, galvanized steel, cold rolled steel, cast aluminum, and cast magnesium.

[0061] Such composite parts include structures that use either a plastic substrate or a thermoplastic substrate and a silicone elastomer as an integral part. Examples of such composite parts can be found in a variety of industries, including, but not limited to, automotive, medical, consumer, industrial, and electronic applications.

[0062] Organopolysiloxane A containing at least two alkenyl groups bonded to silicon atoms per molecule Organopolysiloxane A is a liquid polydiorganosiloxane containing at least two alkenyl groups bonded to silicon atoms per molecule. Suitable alkenyl groups contain 2 to 10 carbon atoms, and preferred examples are vinyl, isopropenyl, allyl, and 5-hexenyl. Organopolysiloxane A contains silicon-bonded organic groups other than alkenyl groups. Such silicon-bonded organic groups are typically selected from monovalent saturated hydrocarbon groups containing 1 to 10 carbon atoms, and monovalent aromatic hydrocarbon groups containing typically 6 to 12 carbon atoms, either unsubstituted or substituted with groups that do not interfere with curing, such as halogen atoms. Preferred silicon-bonded organic groups are, for example, alkyl groups such as methyl, ethyl, propyl, etc.; halogenated alkyl groups such as 3,3,3-trifluoropropyl; and aryl groups such as phenyl.

[0063] Examples of suitable organopolysiloxanes A according to the present invention include polymers of the following formula (1): [ka] (1) During the ceremony, R and R″ are selected independently of each other and are monovalent saturated hydrocarbon groups typically containing 1 to 10 carbon atoms, or monovalent aromatic hydrocarbon groups typically containing 6 to 12 carbon atoms, which are unsubstituted or substituted with groups that do not interfere with the curing reaction, such as halogen atoms. Preferred types of silicon-bonded organic groups include, for example, alkyl groups such as methyl, ethyl, and propyl; halogenated alkyl groups such as 3,3,3-trifluoropropyl; and aryl groups such as phenyl. R' are alkenyl groups each containing 2 to 14 carbon atoms, preferably the alkenyl groups are selected from the group consisting of vinyl, allyl, hexenyl, decenyl and tetradecenyl, most preferably the alkenyl groups are vinyl groups, most preferably R' is a vinyl group, and n represents the degree of polymerization, which should be sufficient to achieve a viscosity of at least 100 mPa·s at 25° C. The upper limit of the degree of polymerization is not particularly limited and is typically limited only by the processability of the LSR composition of the present invention.

[0064] All viscosities considered herein correspond to the magnitude of the kinematic viscosity measured in a manner known per se using a rotational rheometer Anton-Paar M302 at 25° C. For fluid products, the viscosities considered herein are the kinematic viscosities at 25° C. known as “Newtonian” viscosities, i.e. measured in a manner known per se at shear rate gradients sufficiently low so that the measured viscosity is independent of the rate gradient.

[0065] Other examples of organopolysiloxane A that can be used include: Other examples of suitable organopolysiloxane A include trimethylsiloxy endblocked dimethylsiloxane-methylvinylsiloxane copolymers; trimethylsiloxy endblocked methylvinylsiloxane-methylphenylsiloxane copolymers; trimethylsiloxy endblocked dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers; dimethylvinylsiloxy endblocked dimethylpolysiloxanes; dimethylsiloxy endblocked methylvinylpolysiloxanes; dimethylvinylsiloxy endblocked methylvinylphenylsiloxanes; dimethylvinylsiloxy endblocked dimethylvinylsiloxane-methylphenylsiloxane copolymers; dimethylvinylsiloxy endblocked dimethylsiloxane-methylphenylsiloxane copolymers; dimethylvinylsiloxy endblocked dimethylsiloxane-methylphenylsiloxane copolymers; and mixtures containing at least one of the above organopolysiloxanes.

[0066] In a preferred embodiment, organopolysiloxane A is selected from: dimethylvinylsiloxy-terminated polydimethylsiloxane, dimethylvinylsiloxy-terminated polymethyl-3,3,3-trifluoropropylsiloxane, dimethylvinylsiloxane-3,3,3-trifluoropropylmethylsiloxane copolymers, and dimethylvinylsiloxane / methylphenylsiloxane copolymers.

[0067] Organopolysiloxane B containing at least two silicon-bonded hydrogen atoms per molecule Organopolysiloxane B is an optional component that may be present and contains at least two silicon-bonded hydrogen atoms, preferably at least three silicon-bonded hydrogen atoms. If such a component contains three silicon-bonded hydrogen atoms, it can act as a crosslinker for organopolysiloxane A. The molecular structure of organopolysiloxane B is not particularly limited and can be linear, branched, or cyclic. The molecular weight of this component is not particularly limited, but the viscosity is typically 0.001 to 100 Pa·s at 25°C, preferably 0.001 to 1 Pa·s at 25°C, in order to obtain good miscibility with the other components.

[0068] Examples of suitable organopolysiloxanes B include trimethylsiloxy endblocked methylhydrogenpolysiloxanes; trimethylsiloxy endblocked dimethylsiloxane-methylhydrogensiloxane copolymers; trimethylsiloxy endblocked methylhydrogensiloxane-methylphenylsiloxane copolymers; trimethylsiloxy endblocked dimethylsiloxane-methylhydrogensiloxane-methylphenylsiloxane copolymers; dimethylhydrogensiloxy endblocked dimethylpolysiloxanes; dimethylhydrogensiloxy endblocked methylhydrogenpolysiloxanes; dimethylhydrogensiloxy endblocked dimethylsiloxane-methylhydrogensiloxane copolymers; dimethylhydrogensiloxy endblocked methylsiloxane-methylphenylsiloxane copolymers; dimethylhydrogensiloxy endblocked methylphenylpolysiloxanes, (H)(CH3)2SiO 1 / 2 Unit (M H (units) and SiO 4 / 2 Silicone resin M containing units (Q units) H Q, and (CH3)3SiO 1 / 2 Units (M units), (CH3)2HSiO 1 / 2 Unit (M H (units) and SiO 4 / 2 Silicone resin MM containing units H Examples include, but are not limited to, Q.

[0069] In a preferred embodiment, the amounts of the components of the crosslinkable liquid silicone rubber composition A3 are selected so that the ratio RHalk=nH / tAlk is 1.1 to 3.5, where nH=the number of moles of hydrogen atoms directly bonded to silicon atoms of said liquid silicone rubber composition A3 and tAlk=the number of moles of alkenyl groups directly bonded to silicon atoms of said liquid silicone rubber composition A3.

[0070] Filler C In order to achieve high levels of physical properties, reinforcing fillers such as finely divided silica and other reinforcing fillers are often treated with one or more known filler treating agents to prevent a phenomenon known as "creping" or "crepe hardening" during processing of the hardenable composition.

[0071] Typically the fillers are surface treated, for example with fatty acids or fatty acid esters such as stearic acid, or with organosilanes, polydiorganosiloxanes or organosilazanes such as hexaalkyldisilazanes or short chain siloxanediols to render the fillers hydrophobic, thus facilitating handling and allowing for homogeneous mixing with the other ingredients.

[0072] Colloidal silica typically has a density of at least 50 ml per gram. 2 Colloidal silica is particularly preferred because it has a relatively high surface area of ​​1000 nm. Colloidal silica can be provided as fumed silica or as precipitated silica which may be surface treated. One method of surface treatment involves exposing the fumed or precipitated silica to a cyclic organopolysiloxane under heat and pressure. An additional method of treating the filler involves exposing the silica to siloxanes or silanes in the presence of an amine compound.

[0073] Another surface treatment method for silica fillers is to use a methylsilane or silazane surface treatment. Methylsilane or silazane surface-treated fumed or precipitated silica fillers exhibit properties that produce pumpable silicone compounds, but do not excessively increase the low viscosity of the uncured liquid precursor silicone composition. After curing, the silazane-treated silica imparts improved tear strength to the cured elastomer. U.S. Pat. Nos. 3,365,743 and 3,847,848 describe such methods.

[0074] More preferred silica fillers have a surface area of ​​about 50 m per gram as measured by the Brunauer-Emmett-Teller (BET) method. 2 ~ approx. 600m 2 , and most preferably about 100 m per gram 2 ~ approx. 400m 2 In situ treated fumed silica occurs when the silanols on the surface of the fumed silica are capped with silicon atoms containing alkyl, aryl, or alkenyl pendant groups during compounding with the polymer in the mixer. This process can utilize suitable silanol capping agents known in the art, such as hexamethyldisilazane, tetramethyldivinyldisilazane, or trimethylsilanol and dimethylvinylsilanol, to treat the filler.

[0075] The amount of finely divided silica or other reinforcing filler used in the curable LSR compositions of the present invention is determined, at least in part, by the physical properties desired in the cured elastomer. The curable LSR compositions of the present invention typically contain from 5 to 100 parts, typically from 10 to 60 parts, of reinforcing filler per 100 parts of organopolysiloxane A.

[0076] Another example of a suitable filler is hydrophobic silica aerogel, which is a nanostructure with high specific surface area, high porosity, low density, low dielectric constant and excellent thermal insulation. Silica aerogel is synthesized by supercritical drying or atmospheric drying to obtain a porous structure. It is now widely available commercially.

[0077] Hydrophobic silica aerogel is 500-1500m 2 / g, or 500-1200m 2 The hydrophobic silica aerogel is characterized by a surface area in the range of 1000 μm / g, in each case determined by the BET method. The hydrophobic silica aerogel may further be characterized by a porosity of 80% or more, alternatively 90% or more. The hydrophobic silica aerogel may have an average particle size in the range of 5 to 1000 μm, alternatively 5 to 100 μm, alternatively 5 to 25 μm, as measured by laser light scattering. An example of a hydrophobic silica aerogel is trimethylsilylated aerogel. The hydrophobic silica aerogel may be present in the curable liquid silicone rubber composition in an amount of 1 to 30% by weight, based on the total weight of the curable liquid silicone rubber.

[0078] Platinum catalyst D Examples of suitable catalysts include hydrosilylation catalysts such as the Karstedt catalyst shown in U.S. Pat. No. 3,715,334 or other platinum catalysts known in the art, and also microencapsulated hydrosilylation catalysts such as those known in the art, for example those described in U.S. Pat. No. 5,009,957. The catalyst may be optionally combined with an inert or active carrier. Examples of preferred catalysts that can be used include platinum-type catalysts such as chloroplatinic acid, alcohol solutions of chloroplatinic acid, complexes of platinum with olefins, complexes of platinum with 1,3-divinyl-1,1,3,3-tetramethyldisiloxane (known as Karstedt catalyst), and platinum-supported powders. Platinum catalysts are well described in the literature. In particular, complexes of platinum with organic substances include those complexes of platinum with organic products described in U.S. Pat. Nos. 3,159,601, 3,159,602, and 3,220,972, and European Patent Nos. 057459, 188,978, and 190,530, as well as complexes of platinum with vinylated organopolysiloxanes described in U.S. Pat. Nos. 3,419,593, 3,715,334, 3,377,432, 3,814,730, and 3,775,452.

[0079] Hydrosilylation vulcanization reaction inhibitor E Inhibitors for hydrosilylation reactions are designed to slow down the curing reaction and are also known as cure rate control agents. Curing rate control agents are well known in the art and examples of such materials are described in U.S. Patents. U.S. Patent No. 3,923,705 mentions the use of vinyl-containing cyclic siloxanes. U.S. Patent No. 3,445,420 describes the use of acetylenic alcohols. U.S. Patent No. 3,188,299 shows the effectiveness of heterocyclic amines. U.S. Patent No. 4,256,870 describes alkyl maleates used to control curing. Olefinic siloxanes can also be used as described in U.S. Patent No. 3,989,667. Polydiorganosiloxanes containing vinyl groups have also been used, and this technology is described in U.S. Patents Nos. 3,498,945, 4,256,870, and 4,347,346. Preferred inhibitors for this composition are 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane; 3-methyl-1-butyn-3-ol, 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-butyn-2-ol, propargyl alcohol, 2-phenyl-2-propyn-1-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 1-phenyl-2-propynol, 3-methyl-1-penten-4-yn-3-ol, 1-ethynyl-1-cyclohexanol (ECH) and mixtures thereof, most preferably 1-ethynyl-1-cyclohexanol (ECH).

[0080] Further suitable inhibitor classes include hydrazines, triazoles, phosphines, mercaptans, organic nitrogen compounds, acetylenic alcohols, silylated acetylenic alcohols, maleates, fumarates, ethylenically or aromatic unsaturated amides, ethylenically unsaturated isocyanates, olefinic siloxanes, unsaturated hydrocarbon mono- and diesters, conjugated ene-ynes, hydroperoxides, nitriles and diaziridines.

[0081] In a preferred embodiment of the present invention, the inhibitor E for the hydrosilylation vulcanization reaction is selected from the group consisting of 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-butyn-2-ol, propargyl alcohol, 2-phenyl-2-propyn-1-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 1-phenyl-2-propynol, 3-methyl-1-penten-4-yn-3-ol and mixtures thereof.

[0082] For example, to extend the working time or "pot life" of the crosslinkable liquid silicone rubber composition A3 in the mixing tank 18, the amount of inhibitor E for the hydrosilylation vulcanization reaction is precisely regulated via the feed line hose (12) to reach the desired "pot life." The concentration of added catalyst inhibitor, if present in the silicone rubber base compositions A1 and A2, is kept very low and will vary widely depending on the particular inhibitor used and the nature of the organohydrogenpolysiloxane.

[0083] Additive F Representative additives useful in the present invention include additive color masterbatches, UV stabilizers, wetting agents, compression set additives, plasticizers, self-fusing agents, antimicrobial agents, heat stabilizers, flame retardants, adhesion promoters, conductive fillers, thermally conductive fillers, non-conductive fillers, lubricants, antistatic agents, low compression set additives, durometer modifiers, low coefficient of friction additives (such as tung oil), oil resistance additives, anti-crepe hardening additives, mold release agents, plasticizers, thickening or viscosity increasing additives, chain extenders, blowing agents and combinations thereof.

[0084] If the additive is not liquid, it may be combined with a silicone diluent, such as polydimethylsiloxane and / or organopolysiloxane A, and added directly to the silicone rubber base compositions A1 and A2, for example in the mixing tank 18, via the feed line hose (38), or added to the crosslinkable liquid silicone rubber composition A3.

[0085] Any pigments and dyes that are applicable to silicone elastomers but do not inhibit the hydrosilylation catalyzed addition reaction may be used in the present invention. In a preferred embodiment of the present invention, the pigments and dyes are used in the form of a pigment masterbatch in which the pigment is dispersed in polydiorganosiloxane. Examples of additives include pigments such as carbon black, iron oxide, titanium dioxide, chromium oxide, bismuth vanadium oxide, and mixtures or derivatives thereof. By "pigment" we mean colored, black, white, or fluorescent particulate organic or inorganic solids that are usually insoluble in the vehicle or substrate into which they are introduced and essentially physically and chemically unaffected. Pigments change appearance by selective absorption and / or scattering of light. Pigments generally retain their crystalline or particle structure throughout the coloring process. Also included are colorants such as vat dyes, reactive dyes, acid dyes, chrome dyes, disperse dyes, cationic dyes, and mixtures thereof. By "dye" we mean only colored or fluorescent organic substances that impart color to a substrate by selective absorption of light. Pigments and dyes are well known in the art and need not be described in detail here.

[0086] Examples of conductive fillers include, but are not limited to, carbon, such as graphite, carbon black, vapor-grown carbon fiber, and carbon nanotubes; and conductive metals. Examples of particulate and fine conductive materials that cause electrical conductivity in cured silicone include powders and fine powders of gold, silver, nickel, copper, and the like, as well as alloys containing at least one of the above-mentioned metals. Also included are powders and fine powders made by vacuum deposition or plating of metals such as gold, silver, nickel, and copper or alloys thereof on the surface of fine powders of ceramic, glass, quartz, organic resin, and the like. Examples of fillers that fit the above description include silver, silver-coated aluminum, silver-coated copper, silver-coated solid and hollow glass, silver-coated ceramic, silver-coated nickel, nickel, nickel-coated graphite, carbon, and the like.

[0087] Examples of heat stabilizers include iron oxide and carbon black, iron carboxylates, cerium hydrate, titanium dioxide, barium zirconate, cerium and zirconium octoate, and porphyrins.

[0088] Flame retardants include, for example, carbon black, hydrated aluminum hydroxide, magnesium hydroxide, huntite / hydromagnesite blends, silicates such as zinc borate and wollastonite, platinum and platinum compounds, and mixtures or derivatives thereof. Aluminum trihydrate (ATH) is a common flame retardant. It decomposes when heated above 180-200°C, at which point it absorbs heat and releases water, extinguishing the flame. Magnesium hydroxide (MDH) is more thermally stable than ATH. Endothermic decomposition begins at 300°C, where water is released and can act as a flame retardant. Huntite / hydromagnesite blends (Mg3Ca(CO3)4 / Mg5(CO3)4(OH)2·4H2O). Huntite and hydromagnesite almost always occur as mixtures in nature. Hydromagnesite begins to decompose at temperatures between 220°C (atmospheric) and 250°C (under pressure in an extruder), high enough for it to be used as a flame retardant. Hydromagnesite, like ATH and MDH, releases water and absorbs heat, whereas huntite decomposes above 400°C, absorbing heat but releasing carbon dioxide.

[0089] Examples of non-conductive fillers include quartz powder, diatomaceous earth, talc, clay, alumina, mica, calcium carbonate, magnesium carbonate, hollow glass, especially hollow glass beads such as hollow borosilicate glass microspheres, also known as glass bubbles or glass microbubbles, glass fibers, hollow resins, plating powders, and mixtures or derivatives thereof.

[0090] Examples of chain extenders include disiloxanes or low molecular weight polyorganosiloxanes containing two silicon-bonded hydrogen atoms in the terminal positions, such as tetramethyldihydrogendisiloxane or dimethylhydrogen-terminated polydimethylsiloxane.

[0091] Examples of adhesion promoters include zirconium chelates, as well as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 4-glycidoxybutyltrimethoxysilane, 5,6-epoxyhexyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, methacryloxymethyltrimethoxysilane, 3-methacryloxypropyltrimethysilane, and the like. Examples of silanes include silanes such as 3-acryloxypropylmethyldimethoxysilane, 3-methacryloxypropyldimethylmethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxyisobutyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropylmethyldimethoxysilane, 3-acryloxypropyldimethylmethoxysilane, 3-acryloxypropyltriethoxysilane and mixtures thereof.

[0092] Examples of suitable blowing agents include any liquid or solid that generates a gas by chemical decomposition or evaporation as is well known to those skilled in the art. Preferably, the blowing agent is a chemical blowing agent, and most preferably, the blowing agent is selected from the group consisting of ammonium bicarbonate, ammonium hydrogen carbonate, alkali metal hydrogen carbonates, and mixtures thereof.

[0093] The present invention also relates to an apparatus assembly useful for producing molded silicone rubber products by injection molding according to any one of claims 1 to 12, the apparatus assembly comprising: 1) a dosing system (2) for transporting liquids and comprising a platform (1) or a pallet (1'); 2) a first supply container (3) and optionally a second supply container (4) are placed on said standing platform (1) or on said pallet (1') and contain liquid silicone rubber based compositions A1 and A2, respectively, free of catalyst and comprising: at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms, optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, preferably at least 3 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and optionally at least one additive F, 3) a follower plate (5) placed on the surface of said liquid silicone rubber base compositions A1 and A2, the size and shape of which are selected to seal said supply containers (3) and (4) and held by a vertically adjustable holder (6); 4) a pump (7) connected to the follower plate (5) and driven by a drive unit (19) operated by a control unit (20) and optionally an adjustment unit (21) to transport the liquid silicone rubber base composition A1 and optionally the silicone rubber base composition A2; 5) a first base supply line hose (8) for transporting the liquid silicone rubber base composition A1, the first base supply line hose (8) including a flow control element (9) operated by the control unit (20); 6) optionally a second base supply line hose (10) for transporting the liquid silicone rubber base composition A2, comprising a flow control element (11) operated by the control unit (20); 7) a supply vessel (30) containing a catalyst masterbatch C1 comprising at least one platinum-based catalyst D, connected to a supply line (12) containing a flow control element (13) and optionally a sensor (22), both of which are operated by said control unit (20); 8) a supply vessel (31) containing an inhibitor masterbatch E1 comprising at least one inhibitor E for the hydrosilylation vulcanization reaction, connected to a supply line (14) containing a flow control element (15) and, optionally, a sensor (23), both of which are operated by said control unit (20); 9) one of supply vessels (30) and (31) further comprises at least one crosslinking agent XL which is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if linear or at least two silicon-bonded hydrogen atoms per molecule if branched, and is connected to a supply line hose (16) which contains a flow control element (17) and optionally a sensor (24), both of which are operated by said control unit (20); 10) a supply vessel (37) containing at least one additive F, optionally connected to a supply line hose (38) containing a flow control element (39) and optionally a sensor (40), both of which are operated by said control unit (20); 11) Optionally, a mixing tank (18), preferably a static mixer (18'), in which said liquid silicone rubber base A1, said catalyst masterbatch C1, said inhibitor masterbatch E1, said crosslinker XL, optionally said liquid silicone rubber base A2 and said additives F are transferred and mixed to obtain a crosslinkable liquid silicone rubber composition A3 comprising: (a) at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms; (b) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms, preferably at least three silicon-bonded hydrogen atoms, per molecule B; (c) optionally at least one filler C, (d) at least one platinum-based catalyst D; (e) at least one inhibitor E for the hydrosilylation vulcanization reaction, (f) at least one crosslinker XL, which is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer; and (g) optionally at least one additive F, 12) a control unit (20), optionally connected to a display unit (29), for controlling the sensors (21), (22), (23), (24), and (40) and the flow rate control elements (9), (13), (15), (17), and (39) to adjust the amounts of the platinum-based catalyst D and the hydrosilylation vulcanization reaction inhibitor E added to the crosslinkable liquid silicone rubber composition A3, preferably adjusting the amounts so that the molar ratio of the hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of the platinum-based catalyst D is in the range of 0.1 to 900 (0.1:1 to 900:1), most preferably 10 to 900 (10:1 to 900:1), and even more preferably 20 to 250 (20:1 to 250:1); 13) Part of an injection molding press (26); the crosslinkable liquid silicone rubber composition A3 from the mixing tank (18), or said liquid silicone rubber base A1, said catalyst masterbatch C1, said inhibitor masterbatch E1, said crosslinker XL, optionally said liquid silicone rubber base A2 and said additive F, so as to obtain said crosslinkable liquid silicone rubber composition A3; A barrel (25) into which 14) A mold (27) that is placed in the injection molding press (26), into which the crosslinkable liquid silicone rubber composition A3 is transferred and cured by heating, preferably at a temperature of 80°C to 220°C, to obtain a molded silicone rubber product. Equipped with.

[0094] In a preferred embodiment, the present invention also relates to an apparatus assembly useful for producing molded silicone rubber articles by injection molding as described above, the apparatus assembly comprising: 1) a dosing system (2) for transporting liquids and comprising a platform (1) or a pallet (1'); 2) a first supply container (3) and optionally a second supply container (4) are placed on said standing platform (1) or on said pallet (1') and contain liquid silicone rubber based compositions A1 and A2, respectively, free of catalyst and comprising: at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms, optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, preferably at least one organopolysiloxane B containing at least 3 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and optionally at least one additive F, 3) a follower plate (5) placed on the surface of said liquid silicone rubber base compositions A1 and A2, the size and shape of which are selected to seal said supply containers (3) and (4) and held by a vertically adjustable holder (6); 4) a pump (7) connected to the follower plate (5) and driven by a drive unit (19) operated by a control unit (20) and optionally an adjustment unit (21) to transport the liquid silicone rubber base composition A1 and optionally the silicone rubber base composition A2; 5) a first base supply line hose (8) for transporting the liquid silicone rubber base composition A1, the first base supply line hose (8) including a flow control element (9) operated by the control unit (20); 6) optionally a second base supply line hose (10) for transporting the liquid silicone rubber base composition A2, comprising a flow control element (11) operated by the control unit (20); 7) a supply vessel (30) containing a catalyst masterbatch C1 comprising at least one platinum-based catalyst D, connected to a supply line (12) containing a flow control element (13) and optionally a sensor (22), both of which are operated by said control unit (20); 8) a supply vessel (31) containing an inhibitor masterbatch E1 comprising at least one inhibitor E for the hydrosilylation vulcanization reaction, connected to a supply line (14) containing a flow control element (15) and, optionally, a sensor (23), both of which are operated by said control unit (20); 9) a supply vessel (32) further comprising at least one crosslinking agent XL which is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is linear or at least two silicon-bonded hydrogen atoms per molecule if it is branched, and connected to a supply line hose (16) containing a flow control element (17) and optionally a sensor (24), both of which are operated by said control unit (20); 10) a supply vessel (37) containing at least one additive F, optionally connected to a supply line hose (38) containing a flow control element (39) and optionally a sensor (40), both of which are operated by said control unit (20); 11) Optionally, a mixing tank (18), preferably a static mixer (18'), in which said liquid silicone rubber base A1, said catalyst masterbatch C1, said inhibitor masterbatch E1, said crosslinker XL, optionally said liquid silicone rubber base A2 and said additives F are transferred and mixed to obtain a crosslinkable liquid silicone rubber composition A3 comprising: (a) at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms; (b) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms, preferably at least three silicon-bonded hydrogen atoms, per molecule; (c) optionally at least one filler C, (d) at least one platinum-based catalyst D; (e) at least one inhibitor E for the hydrosilylation vulcanization reaction, (f) at least one crosslinker XL, said crosslinker XL being an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear polymer or at least two silicon-bonded hydrogen atoms if it is a branched polymer; and (g) optionally at least one additive F, 12) a control unit (20), optionally connected to a display unit (29), for controlling the sensors (21), (22), (23), (24), and (40) and the flow rate control elements (9), (13), (15), (17), and (39) to adjust the amounts of the platinum-based catalyst D and the hydrosilylation vulcanization reaction inhibitor E added to the crosslinkable liquid silicone rubber composition A3, preferably adjusting the amounts so that the molar ratio of the hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of the platinum-based catalyst D is in the range of 0.1 to 900 (0.1:1 to 900:1), most preferably 10 to 900 (10:1 to 900:1), and even more preferably 20 to 250 (20:1 to 250:1); 13) Part of an injection molding press (26); the crosslinkable liquid silicone rubber composition A3 from the mixing tank (18), or said liquid silicone rubber base A1, said catalyst masterbatch C1, said inhibitor masterbatch E1, said crosslinker XL, optionally said liquid silicone rubber base A2 and said additive F, so as to obtain said crosslinkable liquid silicone rubber composition A3; A barrel (25) into which 14) A mold (27) that is placed in the injection molding press (26), into which the crosslinkable liquid silicone rubber composition A3 is transferred and cured by heating, preferably at a temperature of 80°C to 220°C, to obtain a molded silicone rubber product. Equipped with.

[0095] All chemical components of the device assembly according to the present invention are as described above.

[0096] The device assembly according to the invention makes it possible to carry out the method according to the invention efficiently.

[0097] Indeed, according to the present invention, the equipment assembly uses a single container containing the catalyst-free LSR-based composition, and the required amounts of catalyst, crosslinker and inhibitor are added only on-site prior to molding via separate supply lines containing flow control elements and optional sensors operated by the control unit (20), thereby avoiding problems associated with pre-curing during long-term storage of the container.

[0098] Another advantage associated with the use of the equipment assembly of the present invention is that it allows the Inhibitor Masterbatch E1, Crosslinker XL, Catalyst-free Liquid Silicone Rubber Base, Catalyst Masterbatch C1 and Additive F to be fed to the mixer just prior to mold injection through separate feed line hoses, all operated by a single control device (20) providing complete control over the entire process.

[0099] Furthermore, the amounts of the crosslinking agent XL, the platinum catalyst D, and the liquid injection molding inhibitor E added to the silicone rubber base composition can be easily adjusted from the control unit (20), which is optionally connected to a display unit (29), thereby controlling the curing speed of the crosslinkable liquid silicone rubber composition. By controlling the molar ratio of the injection molding inhibitor E to the platinum atoms of the platinum catalyst D within the working range of injection molding, the device assembly according to the present invention is further provided with flexibility. The preferred working ranges of such ratios are 0.1-900 (0.1:1-900:1), 10-900 (10:1-900:1), and 20-250 (20:1-250:1).

[0100] In a preferred embodiment, the control unit (20) is connected to a display unit (29) so that all necessary information is visible to an operator who can modify the conditions of the molding process, in particular the control of the sensors (21), (22), (23), (24) and (40) and the flow control elements (9), (13), (15), (17) and (39). Additionally or alternatively, the control unit may be configured to monitor and identify deviations outside of predefined operating ranges for the addition of the crosslinking agent XL and the molar ratio of the injection molding inhibitor E to the platinum atoms of the platinum-based catalyst D. The control unit may also monitor the flow rates of the materials conveyed through the different supply lines and maintain predefined minimum flow rates to ensure optimal operating accuracy.

[0101] In another preferred embodiment, a second supply container (4) containing the liquid silicone rubber base A2 is added to the equipment assembly, allowing the use of standard LSR mixing equipment configured for a standard two-component LSR process, thus avoiding the need to set up a complex dosing system. The use of the supply container (4) allows for a continuous automated production sequence, and provides the flexibility to remove an empty container and replace it with a new filled container without stopping the molding sequence.

[0102] Moreover, in another preferred embodiment, the use of pallets (1') eliminates the need for laborious transfer of containers to the equipment assembly, as they can be easily moved using a stacker dolly or similar device. For example, the pallets (1') on which the containers are delivered can be pushed directly into the equipment assembly. Multiple containers can be loaded into the equipment assembly in one loading operation. In another preferred embodiment, the pallets (1') are cleanroom compatible, preferably made of plastic, steel, galvanized steel or stainless steel. These materials are cleanroom compatible as they are easy to clean.

[0103] In another preferred embodiment, said follower plate (5) comprises at least one air purge valve (28) connected to a pressure sensor operable by said control unit (20), because after placing the follower plate on the liquid surface, the vessel may contain air, which must be removed before starting to discharge the material from the vessel, since air contained in the liquid must not enter the production process, resulting in inaccurate measurements.

[0104] In another preferred embodiment, the vertically adjustable holding device (6) is a piston that drives a follower plate (5) downwards to displace the liquid silicone rubber base composition A1 and optionally the liquid silicone rubber base composition A2.

[0105] In another preferred embodiment, a sensor may be arranged in said vertically adjustable holding device (6), which measures the level in the container and is connected to a regulator which is in turn connected to a pump used for emptying the container. By arranging the sensor to measure the level in the container and controlling the emptying via the regulator, it is possible to avoid residual liquid that may remain in the container and thereby ensure a complete emptying of the container.

[0106] In another preferred embodiment, said pump (7) is a dipper piston pump, a gear pump, an eccentric screw pump, an extrusion pump, a screw shaft pump or a scoop piston pump, preferably said pump (7) is a screw shaft pump. An important advantage of a screw shaft pump is its constant delivery pressure and constant delivery volume giving a precise mixture ratio maintained at any point in time.

[0107] In another preferred embodiment, the pump (7) is a screw shaft pump and is connected to a follower plate (5) that is vertically adjustable and rests on the respective liquid level to seal the respective vessel. The advantage of the screw shaft pump is its constant delivery pressure and constant delivery volume.

[0108] In another aspect of this embodiment, the pump (7) is an extrusion pump that is pneumatically, hydraulically or electrically driven and operated by an electronic control (20).

[0109] In another preferred embodiment, the flow control elements (9), (11), (13), (15), (17) and (39) are flow control valves.

[0110] In another preferred embodiment, said supply vessels (3) and (4) are drums having a volume of up to 500 liters, preferably up to 250 liters.

[0111] In another preferred embodiment, the supply vessels (30), (31) and (32), as well as the optional vessel (37), are connected to an air line (36) which delivers their contents into the mixing tank (18), or into the barrel (25) if the mixing tank (18) is not present.

[0112] In another embodiment, the sensors (21), (22), (23), (24) and (40) are flow sensors that may be volumetric meters, flow meters or differential pressure flow sensors. Various flow sensors are known in the art. Flow sensors are classified as volumetric meters (i.e., volumetric flow meters) and flow meters. Volumetric meters (i.e., volumetric flow meters) include direct meters (i.e., displacement meters) such as elliptical wheel meters, vibrating piston meters or rotary piston meters, and indirect meters such as turbine wheel meters, impeller meters, hydrometric vanes, worm wheel meters, vortex meters or spiral flow meters. Flow meters include volumetric flow meters such as differential pressure meters, rotameters, magnetic induction flow meters, ultrasonic flow meters, and mass flow meters such as Coriolis mass flow meters and thermal mass flow meters. Differential pressure flow sensors measure the pressure across a flow control valve and subtract the flow rate from the pressure difference.

[0113] In another embodiment, the mold (27) comprises at least two corresponding parts movable between an open position and a closed position and which define at least one mold cavity when in the closed position.

[0114] In another embodiment, the liquid silicone rubber injection molding equipment assembly further comprises a cold runner system (34) coupled to the mold (27) which keeps the crosslinkable liquid silicone rubber composition A3 cool until it is injected into the hot cavity of the mold (27), thus reducing potential waste.

[0115] In FIG. 1 there is shown a dosing system (2) according to the invention comprising a platform (1) for a drum (3) conveying an LSR material and containing a liquid silicone rubber based composition A1 which is free of catalyst and which comprises: at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms, optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, preferably at least 3 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one liquid injection molding inhibitor E, and optionally at least one additive F.

[0116] A transfer device (33) (not shown) for moving the dosing system (2), the standing platform (1) or the pallet (1') is provided so that it can be displaced without applying large forces. On the surface of the liquid silicone rubber base composition A1, a follower plate (5) is placed, the size and shape of which are selected to seal the supply container (3). This follower plate (5) is held by a vertically adjustable holding device (6) that can move the follower plate (5) up and down. This holding device (6) is preferably a piston that drives the follower plate (5) downwards to displace the liquid silicone rubber base composition A1. The follower plate (5) may have different diameters and is adapted to the supply container (3) to be emptied. When the follower plate (5) is placed on the supply container (3), air must preferably be able to escape, which is ensured by an air purge valve (28) operable by the control unit (20).

[0117] In most cases, the supply vessel (3) is a drum. A static seal can serve the purpose of sealing the vessel. For 20 liter or 200 liter drums, an inflatable seal can be used. This allows drums with minor defects to be processed. The follower plate (5) can be of lightweight construction (for example weighing less than 15 kg so that occupational health and safety regulations allow replacement by the operating staff). The material in the supply vessel (3) is pumped by a supply pump (7), such as a dipper piston pump, a gear pump, an eccentric screw pump, an extrusion pump, a screw shaft pump, a scoop piston pump, etc. Said pump (7) can be driven by a drive (19) (not shown) operated by a control (20) and optionally an adjustment (21). This allows the liquid silicone rubber base composition A1 to be transferred directly via a supply line hose (8) equipped with a flow control element (9) operated by said control unit (20) to a mixing tank (18) which is preferably a static mixer (18') (the option selected for this drawing) or to a barrel (25) which is part of an injection molding press (26) (this option is not shown in the drawing).

[0118] A supply vessel (30) containing a catalyst masterbatch C1 comprising at least one platinum-based catalyst D is connected to a supply line (12) including a flow control element (13) and optionally a sensor (22), both operated by said control unit (20), allowing the transfer of its contents to a mixing tank (18) (option chosen for this drawing) or directly to a barrel (25) (option not shown).

[0119] A supply vessel (31) containing an inhibitor masterbatch E1 comprising at least one liquid injection molding inhibitor E is connected to a supply line hose (14) containing a flow control element (15) and optionally a sensor (23), both operated by the control unit (20). This allows the transfer of its contents to a mixing tank (18) (option selected for this drawing) or directly to a barrel (25) (option not shown). The mixing tank (18) is preferably a static mixing device.

[0120] A supply vessel (32) containing at least one cross-linking agent XL is connected to a supply line (16) containing a flow control element (17) and optionally a sensor (24), both operated by the control unit (20), allowing the transfer of its contents to a mixing tank (18) (option chosen for this drawing) or directly to a barrel (25) (option not shown).

[0121] In the mixing tank (18) (if present) and in the barrel (25) a crosslinkable liquid silicone rubber composition A3 is obtained which comprises: (a) at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms; (b) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms, preferably at least three silicon-bonded hydrogen atoms, per molecule B; (c) optionally at least one filler C, (d) at least one platinum-based catalyst D; (e) at least one inhibitor E for the hydrosilylation vulcanization reaction, (f) at least one crosslinker XL, which is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer; and (g) optionally, at least one additive F.

[0122] A control unit (20), optionally connected to a display unit (29) (optional for this drawing), operates sensors (21), (22), (23), (24) and (40) and flow control elements (9), (13), (15), (17) and (39) to adjust the dosage of the platinum-based catalyst D and the liquid injection molding inhibitor E in the crosslinkable liquid silicone rubber composition A3. The dosage is adjusted so that the molar ratio of the injection molding inhibitor E to the platinum atoms of the platinum-based catalyst D is maintained in the range of 0.1 to 900 (0.1:1 to 900:1), most preferably in the range of 10 to 900 (10:1 to 900:1). In a preferred embodiment, in step (d), the dosage of the crosslinking agent XL is controlled and maintained in the range of 0.1 to 3.5% by weight, based on the weight of the crosslinkable liquid silicone rubber composition A3.

[0123] The barrel (25) is part of an injection molding press (26) into which the following are introduced: the crosslinkable liquid silicone rubber composition A3 from the mixing tank (18), or said liquid silicone rubber base A1, said crosslinking agent XL, said catalyst masterbatch C1, said inhibitor masterbatch E1 comprising an inhibitor E for the hydrosilylation vulcanization reaction, optionally said liquid silicone rubber base A2 and said additive F, so as to obtain said crosslinkable liquid silicone rubber composition A3.

[0124] Pressure regulation may be required before the crosslinkable LSR composition A3 enters the injection section. This device (not shown in the drawings) allows for regulation of the fluid path through which pressure can be increased, thereby allowing for proper shot addition. The pressure regulator is adjustable, but is typically maintained in the range of 0.7-3.5 MPa (100-500 psi) to prevent over-compression of the metered shot.

[0125] During addition and injection, the barrel of the injection section may be water cooled to prevent premature crosslinking or curing, thereby limiting the effects of viscous heating that occurs between the crosslinkable LSR composition A3 and the screw and barrel.

[0126] A positive shutoff valve (not shown) or a screw tip with a check valve may be used, such as a ball check valve, either spring-loaded or with a float, that is in a closed position during injection but opens during shot addition.

[0127] It is preferable to use a water-cooled non-return nozzle to prevent premature crosslinking during injection and addition before the crosslinkable liquid silicone rubber composition A3 is introduced into the mold (27) and to prevent backflow during partial curing. In the nozzle, the material is diverted around a piston that drives a non-return needle and reintroduced into the flow path near the nozzle tip. A cold runner system (34) may also be connected to the mold (27).

[0128] Once filling of the crosslinkable LSR composition A3 into the mold (27) is complete, filling pressure is maintained on the material until curing occurs at a temperature in the range of 80°C to 220°C, which can be reduced, if desired, to temperatures in the range of 80°C to 220°C, 80°C to 160°C, 80°C to 140°C, 80°C to less than 120°C, 80°C to less than 110°C, or 80°C to less than 100°C without compromising the optimum cure rate of the LSR material.

[0129] After injection and filling there is a curing time which depends on the part geometry: longer for thicker parts, shorter for thinner parts.

[0130] Once curing is complete, the mold (27) opens, allowing the part to be demolded and continue to the next shot.

[0131] Referring to Figure 2, another embodiment of a dosing system (2) according to the invention is shown, the only difference from Figure 1 being the addition of a second supply vessel (4) containing a liquid silicone rubber based composition A2 without a catalyst and comprising: at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms, optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, preferably at least 3 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and optionally at least one additive F.

[0132] This second supply container (4) can be used immediately after the first supply container (3) is emptied, thus allowing for optimizing the production cycle time of a continuous process, or can be used together with the first supply container (3) to allow for example the use of two types of LSR base with different durometer properties (different contents of fillers and other ingredients), allowing for further flexibility in the production of different types of silicone rubber materials. EXAMPLES

[0133] Cure was monitored over a 5 minute period at 110°C in a moving die rheometer (MDR) according to ASTM-D5289. Approximately 5g of material was placed between two thin nylon sheets at room temperature and then compressed by an oscillatory force applied between two heated platens. One platen or die rotates and oscillates while the other is attached to a torque transducer. Initially, with an unvulcanized (uncured) rubber sample, little or no torque from the moving die is coupled to the transducer. Heating the compound under pressure causes the viscosity to drop, reducing the torque applied to the rotor. The minimum torque recorded (dN *The moment of inertia (measured in m) is called ML (Minimum Moment). It is a measure of the stiffness of an uncured rubber compound at a certain temperature. As rubber cures or vulcanizes, it becomes more elastic. Rubber becomes more effective when torque is coupled to a transducer. Torque is a parameter that indicates the degree of vulcanization or hardening of rubber. An S-shaped curve can approximate the actual curing curve. As shown below, the black curve (designated 2) is the curing curve or torque curve of torque versus time. The torque starts at a minimum value. The torque increases slowly at first and then increases rapidly. Finally, the curing curve levels out and becomes nearly constant. In Figure 3, the maximum torque is set to a value of 1 unit. The cure progresses from the minimum torque (which may not be exactly 0) to the maximum torque. There are various times in the derived statistics that are reached at points of interest. These are t2 (2% cure), t10 (10% cure), etc., and t90 (90% cure) is usually of great interest as well.

[0134] The curve labeled 1 in Figure 3 is the derivative curve, i.e. the slope of the hardening curve. Using this derivative, we can determine the maximum rate of hardening and the time it takes to reach that maximum. These statistics are Prate and t@Prate, respectively. Some consider t2 and Prate to be the most important statistics.

[0135] Example 1 component Control formulation: Liquid silicone rubber base composition Silbione® LSR-4350 sold by Elkem Silicones USA, Inc., components A and B (standard LSR composition). ·R2HSiO 1 / 2 and the formula SiO 4 / 2 Q Siloxy unit M H Q silicone resin, where H is hydrogen and R is methyl (wt % H as SiH=1.23%). Added M H A control formulation was used according to the process of the present invention with a different amount of Q silicone resin. HA control test was performed without the addition of Q silicone resin. Cure was monitored with a Moving Die Rheometer (MDR) per ASTM-D5289 at 110°C for 5 minutes. The results are shown in Table 1.

[0136] [Table 1] Table 1: Property measurement results when resin is added

[0137] The comparative test shows a t90 (90% cure) value of 139 seconds, which is much slower than all tests according to the invention.

[0138] Example 2 (a) Crosslinkers tested XL1 = polyphenyl(dimethylhydrosiloxy)siloxane hydride terminated, manufactured by Gelest, reference number HDP-111, viscosity 50-80 mPa s, total SiH (mmol / g) = 5.2; formula (M H ) 2+n (T Ph ) n (where M=RSiO 1 / 2 Siloxy unit and T Ph =PhSiO 3 / 2 wherein H is a hydrogen atom, R is methyl, and Ph is phenyl. [ka] XL2: A copolymer of dimethylsiloxane and methylhydrogensiloxane, with both molecular ends partially capped with dimethylhydrogensiloxy groups (viscosity 18-26 mPa·s; total SiH (mmol / g) = 7.2 (linear crosslinker)). XL3:R2HSiO 1 / 2 and the formula SiO 4 / 2 Q siloxy units (where H is hydrogen atom, R is methyl, total SiH (mmol / g) = 7.3 (Milliken, reference number SiVance MQH-8MQ hydride resin)) H Q Silicone resin. XL4:Formula MH Q branched silicone resin (wherein M H =R2HSiO 1 / 2 and Q is of the formula SiO 4 / 2 where H is a hydrogen atom, R is a methyl, and total SiH (mmol / g)=8.8. XL5:Formula M H Q branched silicone resin (wherein M H =R2HSiO 1 / 2 and Q is of the formula SiO 4 / 2 where H is hydrogen and R is methyl, total SiH (mmol / g)=9.7 (Milliken, reference SiVance MQH-9 MQ hydride resin). XL6:Following formula:(M H )3(T Ph ) branched silicone resin (where M = RHSiO 1 / 2 Siloxy units, T Ph =PhSiO 3 / 2 where H is a hydrogen atom, R is methyl and Ph is phenyl (Gelest, reference number SIP6826.0, phenyltris(dimethylhydrosiloxy)silane, total SiH (mmol / g)=5.2)). [ka] XL6 XL7:Formula M H Q branched silicone resin (where M H =R2HSiO 1 / 2 and Q is of the formula SiO 4 / 2 where H is a hydrogen atom and R is a methyl, manufactured by Gelest, reference number SIT7278.0, total SiH (mmol / g)=6.7). [ka] XL7 XL8: α,ω-bis(trimethylsiloxy)polymethylhydrogensiloxane, viscosity 17–27 mPa·s, total SiH (mmol / g) = 15.7.

[0139] Composition of liquid silicone rubber base composition R: Polydimethylsiloxane with dimethylvinylsiloxy groups at the ends (viscosity range 80,000-120,000 mPa s): 35.74% by weight. Polydimethylsiloxane terminated with dimethylvinylsiloxy groups (viscosity range 55,000-65,000 mPa.s): 31.28% by weight. Fumed silica surface treated with divinyltetramethyldisilazane and hexamethyldisilazane (treated in situ) (25.59% by weight). Divinyltetramethyldisilazane and hexamethyldisilazane (total = 6.99% by weight). Plasticizer additive (0.40% by weight).

[0140] To prepare the formulation to be tested, separate feeds are prepared and combined in a mix tank. Supply (1) A liquid silicone rubber base composition R is prepared, to which - Methylvinylsiloxane-dimethylsiloxane copolymer with trimethylsiloxy groups at the ends (viscosity of about 1000 mPa·s) - FLD619; - Methylvinylsiloxane-dimethylsiloxane copolymer with dimethylvinylsiloxy groups at the ends (viscosity range 350-420mPa.s) - FLD-506 Varying amounts of are added. Feed (2) Catalyst masterbatch (LSR SELECT CATA manufactured by Elkem Silicones). Supplies (3) Inhibitor masterbatch (LSR SELECT CONTROL manufactured by Elkem Silicones). ·Supply (4) Tested crosslinker XL.

[0141] After all ingredients were mixed, the overall pot life was determined by a manual "snap time" pot life test, which was started immediately upon completion of the mixture and ended when elastic properties were first observed by monitoring the mixture and manually stirring and scraping the mixture out of its container. Elastic properties were observed when the mixture returned to its "original state" in the container. Cure evaluation was performed using a Paar-MC302 rheometer by starting at 40° C. and increasing the temperature at a rate of 7° C. per minute. The cure data for each formulation was fitted to a logistic equation with parameters To and k. The logistic function used to fit the data from the MDR (moving die rheometer) is shown in Equation 1 below. G'(T) = ML + (MH-ML / 1 + e -k(T-To) ) (1) During the ceremony: G'(T) is the storage modulus as a function of temperature, ML is the minimum observed value of G', MH is the maximum observed value of G', k is a coefficient related to the maximum slope of the curve, T is the temperature independent variable, To is the temperature at the vertical midpoint of the curve. The linear function is: dG' / dT = -k(-MH)e -k(T-To) / 1+2e -k(T-To) +(e (-k(T-To) ) 2 (2) When T=To, the midpoint or inflection point of temperature is To. The exponential expression is e 0 =1, resulting in the following function: dG' / dT=k(MH) / 4;T=To (3) T0 is the parameter of the logistic function, as shown above. This is the point on the horizontal axis that corresponds to the inflection point of the curve. This is also the point where the maximum cure rate is achieved.

[0142] After mixing, the compounds were tested on a Paar MC302 rheometer using an oscillatory torsional strain of 1%. The platens were 25 mm in diameter with a gap of 0.5 mm. The sinusoidal oscillation frequency was 1 Hz. The temperature started at 40°C and was increased at 7°C / min to a maximum temperature of 140°C. Each test lasted for 18 minutes. As the temperature was increased, torque measurements were taken at 18 second intervals. These measurements were decomposed into in-phase and out-of-phase components of torque and finally converted to storage modulus G' and loss modulus G", respectively.

[0143] The compositions (wt % of each component) and measured properties of the formulations with varying RHAlk values ​​are summarized in Tables 2, 3 and 4.

[0144] [Table 2] Table 2: Properties measured at RHAlk=1.5.

[0145] Formula R2HSiO 1 / 2 MH siloxy units with the formula (Ph)SiO 3 / 2 T Ph It is noted that the crosslinkers XL-1 and XL-6, which are branched silicone resins containing siloxy units, can be cured at low temperatures (T0 below 85°C), have a minimum T0 (the point where the maximum rate of cure is achieved), and have improved pot lives (25 and 28 minutes, respectively) compared to other crosslinkers, allowing greater flexibility in using the XL and overmolding over heat-sensitive materials with Vicat softening temperatures, such as polyvinyl chloride (PVC, 92°C), polyethylene (PE, 127.3°C), polypropylene (PP, 152.2°C), acrylonitrile butadiene styrene (ABS, 102.3°C) and polycarbonate (PC, 156.2°C). The same results are summarized in Tables 3 and 4 below.

[0146] [Table 3] Table 3: Properties measured at RHAlk=2.0.

[0147] [Table 4] Table 4: Properties measured at RHAlk=2.5.

Claims

1. A method useful for producing a silicone rubber article M1 by injection molding, comprising the steps of: (a) does not contain a catalyst; and at least one organopolysiloxane A containing at least two alkenyl groups bonded to silicon atoms per molecule; optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and Optionally, at least one additive F into the base supply line a liquid silicone rubber base composition A1 comprising (b) feeding a catalyst masterbatch C1 containing at least one platinum-based catalyst D into another catalyst feed line; (c) feeding an inhibitor masterbatch E1, which comprises at least one inhibitor E for the hydrosilylation vulcanization reaction, into another feed line; (d) feeding into a separate feed line, or into any feed line containing the catalyst masterbatch C1 or the inhibitor masterbatch E1, at least one crosslinker XL, said crosslinker being an organopolysiloxane having at least three silicon-bonded hydrogen atoms per molecule if it is a linear or cyclic polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer; (e) optionally, feeding at least one additive F into a separate additive feed line; (f) conducting said liquid silicone rubber base composition A1, said catalyst masterbatch C1, said crosslinker XL, said inhibitor masterbatch E1 and optionally said additives F into a mixing tank (18) prior to conducting the resulting mixture into the barrel of an injector or directly into said barrel to produce the following: (1) at least one organopolysiloxane A containing at least two alkenyl groups bonded to silicon atoms per molecule; (2) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms per molecule; (3) optionally, at least one filler C; (4) at least one platinum-based catalyst D; (5) at least one inhibitor E for the hydrosilylation vulcanization reaction, (6) at least one crosslinker XL, wherein said crosslinker XL is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear or cyclic polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer, and (7) Optionally, at least one additive F wherein the amounts of said platinum-based catalyst D and said hydrosilylation vulcanization reaction inhibitor E added in said crosslinkable liquid silicone rubber composition A3 are controlled and adjusted so that the molar ratio of said hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of said platinum-based catalyst D is within the range of 0.1 to 900 (0.1:1 to 900:1); (g) introducing said cross-linkable liquid silicone rubber composition A3 into a mold placed in a molding press and heating said cross-linkable liquid silicone rubber composition A3 to harden it, thereby obtaining a molded silicone rubber product M1; wherein the crosslinker XL is represented by the formula R 2 HSiO 1 / 2 M H Siloxy units and the formula SiO 4 / 2 and M H Q silicone resin or a branched silicone resin comprising M H siloxy units of the formula R 2 HSiO 1 / 2 and T Ph siloxy units of the formula (Ph)SiO 3 / 2 , where Ph is a phenyl group, H is a hydrogen atom, and R is a monovalent hydrocarbon group of 1 to 40 carbon atoms.

2. 10. The method of claim 1, comprising the steps of: (a) does not contain a catalyst; and at least one organopolysiloxane A containing at least two alkenyl groups bonded to silicon atoms per molecule; optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and Optionally, at least one additive F into the base supply line (8) a liquid silicone rubber base composition A1 comprising (b) feeding a catalyst masterbatch C1 comprising at least one platinum-based catalyst D into another catalyst feed line (12); (c) feeding an inhibitor masterbatch E1, which comprises at least one inhibitor E for the hydrosilylation vulcanization reaction, into another feed line; (d) feeding at least one crosslinker XL into another feed line, said crosslinker XL being an organopolysiloxane having at least three silicon-bonded hydrogen atoms per molecule if it is a linear or cyclic polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer; (e) optionally, feeding at least one additive F into a separate additive feed line; (f) conducting said liquid silicone rubber base composition A1, said catalyst masterbatch C1, said crosslinker XL, said inhibitor masterbatch E1 and optionally said additives F into a mixing tank (18) prior to conducting the resulting mixture into the barrel of an injector or directly into said barrel to produce the following: (1) at least one organopolysiloxane A containing at least two alkenyl groups bonded to silicon atoms per molecule; (2) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms per molecule; (3) optionally, at least one filler C; (4) at least one platinum-based catalyst D; (5) at least one inhibitor E for the hydrosilylation vulcanization reaction, (6) at least one crosslinker XL, wherein said crosslinker XL is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear or cyclic polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer, and (7) Optionally, at least one additive F wherein the amounts of said platinum-based catalyst D and said hydrosilylation vulcanization reaction inhibitor E added in said crosslinkable liquid silicone rubber composition A3 are controlled and adjusted so that the molar ratio of said hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of said platinum-based catalyst D is within the range of 0.1 to 900 (0.1:1 to 900:1); (g) introducing said cross-linkable liquid silicone rubber composition A3 into a mold placed in a molding press and heating said cross-linkable liquid silicone rubber composition A3 to harden it, thereby obtaining a molded silicone rubber product M1; wherein the crosslinker XL is represented by the formula R 2 HSiO 1 / 2 M H Siloxy units and the formula SiO 4 / 2 and M H Q silicone resin or a branched silicone resin comprising M H siloxy units of the formula R 2 HSiO 1 / 2 and T Ph siloxy units of the formula (Ph)SiO 3 / 2 , where Ph is a phenyl group, H is a hydrogen atom, and R is a monovalent hydrocarbon group of 1 to 40 carbon atoms.

3. The crosslinker XL is represented by the formula R 2 HSiO 1 / 2 M H Siloxy units and the formula SiO 4 / 2 and M H 2. The method of claim 1, which is a Q silicone resin or a branched silicone resin comprising M H siloxy units of the formula R 2 HSiO 1 / 2 and T Ph siloxy units of the formula (Ph)SiO 3 / 2 , where Ph is a phenyl group, H is a hydrogen atom, and R is a monovalent hydrocarbon group having 1 to 20 carbon atoms.

4. The crosslinking agent XL is (a) Formula R 2 HSiO 1 / 2 At least two M H Siloxy units with the formula (Ph)SiO 3 / 2 T Ph at least one branched silicone resin containing siloxy units, where Ph is a phenyl group, H is a hydrogen atom, and R is a monovalent hydrocarbon group of 1 to 40 carbon atoms; and (b) at least one linear organopolysiloxane B containing at least three silicon-bonded hydrogen atoms per molecule, and / or a polysiloxane of formula R 2 HSiO 1 / 2 At least two M H Siloxy units and the formula SiO 4 / 2 and a branch M H Q silicone resin, where H is a hydrogen atom and R is a monovalent hydrocarbon group of 1 to 40 carbon atoms. The method of claim 1 , wherein the mixture comprises

5. The crosslinker XL is represented by the formula R 2 HSiO 1 / 2 M H Siloxy units and the formula SiO 4 / 2 M containing Q siloxy units H 2. The method of claim 1, wherein Q is a silicone resin, and H is a hydrogen atom.

6. The crosslinking agent XL has 0.10 wt % to 2.00 wt % H as SiH and has the formula R 2 HSiO 1 / 2 M H Siloxy units and the formula SiO 4 / 2 and Q siloxy units of the formula:

7. The crosslinker XL has the formula H 2. The method of claim 1, wherein the silicone resin is a silicone resin. M H w Q z where Q is of the formula SiO 4 / 2 M H is the formula R 2 HSiO 1 / 2 where H is a hydrogen atom, R is a monovalent hydrocarbon group of 1 to 40 carbon atoms, and the subscripts w and z each have a ratio of 0.5 to 4.

0.

8. The method of any one of claims 3 to 7, wherein R is selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, pentyl, hexyl, heptyl, phenyl, benzyl and mesityl.

9. 9. The method of claim 8, wherein R is selected from methyl and phenyl.

10. 2. The method according to claim 1, wherein in said step (d), the amount of said crosslinking agent XL added is controlled and maintained in the range of 0.1 to 5.0 weight percent based on the weight of said crosslinkable liquid silicone rubber composition A3.

11. The method according to claim 1, wherein in step (g), the curing temperature is 80 to 140°C.

12. 2. The method of claim 1, wherein in step (g), the curing temperature is 80-140° C. and the crosslinkable liquid silicone rubber composition A3 is cured around or over the substrate P to form a composite part comprising the molded silicone rubber article M1.

13. The method according to claim 12, wherein the substrate P is selected from plastic substrates, thermoplastic substrates, metal substrates and textile substrates.

14. 2. The method of claim 1, wherein the hydrosilylation vulcanization reaction inhibitor E is selected from the group consisting of 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-butyn-2-ol, propargyl alcohol, 2-phenyl-2-propyn-1-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 1-phenyl-2-propynol, 3-methyl-1-penten-4-yn-3-ol, and mixtures thereof.

15. An apparatus assembly useful for producing molded silicone rubber products by injection molding according to any one of claims 1 to 14, said apparatus assembly comprising: 1) A dosing system (2) for transporting liquids and comprising a platform (1) or a pallet (1'); 2) a first supply container (3) and optionally a second supply container (4) placed on said standing platform (1) or on said pallet (1') containing liquid silicone rubber base compositions A1 and A2, respectively, free of catalyst and comprising: at least one organopolysiloxane A containing at least two alkenyl groups bonded to silicon atoms per molecule; optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and optionally at least one additive F, 3) a follower plate (5) placed on the surface of said liquid silicone rubber base compositions A1 and A2, the size and shape of which are selected to seal said supply containers (3) and (4) and held by a vertically adjustable holder (6); 4) a pump (7) connected to the follower plate (5) and driven by a drive unit (19) operated by a control unit (20) and optionally an adjustment unit (21) to transport the liquid silicone rubber base composition A1 and, optionally, the silicone rubber base composition A2; 5) a first base supply line hose (8) for transporting said liquid silicone rubber base composition A1, said first base supply line hose (8) including a flow control element (9) operated by said control unit (20); 6) optionally a second base supply line hose (10) for transporting said liquid silicone rubber base composition A2, comprising a flow control element (11) operated by said control unit (20); 7) a supply vessel (30) containing a catalyst masterbatch C1 comprising at least one platinum-based catalyst D, connected to a supply line (12) containing a flow control element (13) and optionally a sensor (22), both of which are operated by said control unit (20); 8) a supply vessel (31) containing an inhibitor masterbatch E1 comprising at least one inhibitor E for the hydrosilylation vulcanization reaction, connected to a supply line (14) containing a flow control element (15) and optionally a sensor (23), both of which are operated by said control unit (20); 9) one of said supply vessels (30) and (31) further comprises at least one crosslinking agent XL which is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is linear or at least two silicon-bonded hydrogen atoms per molecule if it is branched, and is connected to a supply line hose (16) which contains a flow control element (17) and optionally a sensor (24), both of which are operated by said control unit (20); 10) a supply vessel (37) containing at least one additive F, optionally connected to a supply line hose (38) containing a flow control element (39) and optionally a sensor (40), both of which are operated by said control unit (20); 11) Optionally, a mixing tank (18) in which said liquid silicone rubber base A1, said catalyst masterbatch C1, said inhibitor masterbatch E1, said crosslinker XL, optionally said liquid silicone rubber base A2 and said additives F are transferred and mixed to obtain a crosslinkable liquid silicone rubber composition A3 comprising: (a) at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms; (b) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms per molecule; (c) optionally at least one filler C; (d) at least one platinum-based catalyst D; (e) at least one inhibitor E for the hydrosilylation vulcanization reaction, (f) at least one crosslinker XL, wherein said crosslinker XL is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear polymer, or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer, and (g) optionally, at least one additive F; 12) a control unit (20), optionally connected to a display unit (29), for controlling the sensors (21), (22), (23), (24), and (40) and the flow rate control elements (9), (13), (15), (17), and (39) to adjust the amounts of the platinum-based catalyst D and the hydrosilylation vulcanization reaction inhibitor E added to the crosslinkable liquid silicone rubber composition A3, so as to adjust the molar ratio of the hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of the platinum-based catalyst D to be 0.1 to 900 (0.1:1 to 900:1); 13) Part of the injection molding press (26), the crosslinkable liquid silicone rubber composition A3 from the mixing tank (18), or - mixing said liquid silicone rubber base A1, said catalyst masterbatch C1, said inhibitor masterbatch E1, said crosslinker XL, optionally said liquid silicone rubber base A2 and said additive F so as to obtain said crosslinkable liquid silicone rubber composition A3; A barrel (25) into which 14) A mold (27) that is placed in the injection molding press (26) and into which the crosslinkable liquid silicone rubber composition A3 is transferred and cured to obtain a molded silicone rubber product. Equipped with The crosslinker XL has the formula R 2 HSiO 1 / 2 M H Siloxy units and the formula SiO 4 / 2 and M H A device assembly comprising a Q silicone resin or a branched silicone resin comprising M H siloxy units of the formula R 2 HSiO 1 / 2 and T Ph siloxy units of the formula (Ph)SiO 3 / 2 , where Ph is a phenyl group, H is a hydrogen atom, and R is a monovalent hydrocarbon group of 1 to 40 carbon atoms.

16. An apparatus assembly useful for producing molded silicone rubber products by injection molding according to any one of claims 1 to 14, said apparatus assembly comprising: 1) A dosing system (2) for transporting liquids and comprising a platform (1) or a pallet (1'); 2) a first supply container (3) and optionally a second supply container (4) placed on said standing platform (1) or on said pallet (1') containing liquid silicone rubber base compositions A1 and A2, respectively, free of catalyst and comprising: at least one organopolysiloxane A containing at least two alkenyl groups bonded to silicon atoms per molecule; optionally at least one organopolysiloxane B containing at least 2 silicon-bonded hydrogen atoms per molecule, optionally at least one filler C, optionally at least one inhibitor E for the hydrosilylation vulcanization reaction, and optionally at least one additive F, 3) a follower plate (5) placed on the surface of said liquid silicone rubber base compositions A1 and A2, the size and shape of which are selected to seal said supply containers (3) and (4) and held by a vertically adjustable holder (6); 4) a pump (7) connected to the follower plate (5) and driven by a drive unit (19) operated by a control unit (20) and optionally an adjustment unit (21) to transport the liquid silicone rubber base composition A1 and, optionally, the silicone rubber base composition A2; 5) a first base supply line hose (8) for transporting said liquid silicone rubber base composition A1, said first base supply line hose (8) including a flow control element (9) operated by said control unit (20); 6) optionally a second base supply line hose (10) for transporting said liquid silicone rubber base composition A2, comprising a flow control element (11) operated by said control unit (20); 7) a supply vessel (30) containing a catalyst masterbatch C1 comprising at least one platinum-based catalyst D, connected to a supply line (12) containing a flow control element (13) and optionally a sensor (22), both of which are operated by said control unit (20); 8) a supply vessel (31) containing an inhibitor masterbatch E1 comprising at least one inhibitor E for the hydrosilylation vulcanization reaction, connected to a supply line (14) containing a flow control element (15) and optionally a sensor (23), both of which are operated by said control unit (20); 9) a supply vessel (32) further comprising at least one crosslinking agent XL which is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear polymer or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer, and connected to a supply line hose (16) containing a flow control element (17) and optionally a sensor (24), both of which are operated by said control unit (20); 10) a supply vessel (37) containing at least one additive F, optionally connected to a supply line hose (38) containing a flow control element (39) and optionally a sensor (40), both of which are operated by said control unit (20); 11) Optionally, a mixing tank (18) in which said liquid silicone rubber base A1, said catalyst masterbatch C1, said inhibitor masterbatch E1, said crosslinker XL, optionally said liquid silicone rubber base A2 and said additives F are transferred and mixed to obtain a crosslinkable liquid silicone rubber composition A3 comprising: (a) at least one organopolysiloxane A containing per molecule at least two alkenyl groups bonded to silicon atoms; (b) optionally, at least one organopolysiloxane B containing at least two silicon-bonded hydrogen atoms per molecule; (c) optionally at least one filler C; (d) at least one platinum-based catalyst D; (e) at least one inhibitor E for the hydrosilylation vulcanization reaction, (f) at least one crosslinker XL, wherein said crosslinker XL is an organopolysiloxane containing at least three silicon-bonded hydrogen atoms per molecule if it is a linear polymer or at least two silicon-bonded hydrogen atoms per molecule if it is a branched polymer; and (g) optionally, at least one additive F; 12) a control unit (20), optionally connected to a display unit (29), for controlling the sensors (21), (22), (23), (24), and (40) and the flow rate control elements (9), (13), (15), (17), and (39) to adjust the amounts of the platinum-based catalyst D and the hydrosilylation vulcanization reaction inhibitor E added to the crosslinkable liquid silicone rubber composition A3, so that the molar ratio of the hydrosilylation vulcanization reaction inhibitor E to the platinum atoms of the platinum-based catalyst D is in the range of 0.1 to 900 (0.1:1 to 900:1); 13) Part of the injection molding press (26), the crosslinkable liquid silicone rubber composition A3 from the mixing tank (18), or - mixing said liquid silicone rubber base A1, said catalyst masterbatch C1, said inhibitor masterbatch E1, said crosslinker XL, optionally said liquid silicone rubber base A2 and said additive F so as to obtain said crosslinkable liquid silicone rubber composition A3; A barrel (25) into which 14) A mold (27) that is placed in the injection molding press (26) and into which the crosslinkable liquid silicone rubber composition A3 is transferred and cured to obtain a molded silicone rubber product. Equipped with The crosslinker XL has the formula R 2 HSiO 1 / 2 M H Siloxy units and the formula SiO 4 / 2 and M H A device assembly comprising a Q silicone resin or a branched silicone resin comprising M H siloxy units of the formula R 2 HSiO 1 / 2 and T Ph siloxy units of the formula (Ph)SiO 3 / 2 , where Ph is a phenyl group, H is a hydrogen atom, and R is a monovalent hydrocarbon group of 1 to 40 carbon atoms.

Citation Information

Patent Citations

  • Method for producing silicone rubber molding product

    JP2001234070A

  • Curable organopolysiloxane composition for optical transmission member, flexible optical transmission member comprising organopolysiloxane hardened product, and method for manufacturing flexible optical transmission member

    JP2005227701A

  • Low-temperature curing silicone elastomer

    JP2019504919A

  • High strength organopolysiloxane compositions

    US3884866A

  • High strength, extrudable silicone elastomer compositions

    US4162243A