Polycarbonate composite using solid or molten dispersion of anhydrous sugar alcohol, its manufacturing method, and molded article containing same
A polycarbonate composite with uniformly dispersed nanomaterials in anhydrous sugar alcohol dispersions enhances tensile strength and modulus, addressing the aggregation issues of conventional composites.
Patent Information
- Application Number
- JP2022527085
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-11
- Filing Date
- 2020-11-11
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-11-11
AI Technical Summary
Conventional biopolycarbonate resin composites face limitations due to the hydrophilic nature of nanomaterials like nanocellulose, leading to aggregation and non-uniform dispersion, which deteriorates the mechanical properties such as tensile strength and modulus.
A polycarbonate composite is developed using a matrix resin with nanomaterials dispersed in anhydrous sugar alcohol through solid or molten dispersions, ensuring uniform distribution by introducing nanomaterials into anhydrous sugar alcohol in an aqueous dispersion form.
The composite exhibits significantly improved tensile strength and modulus with uniform physical properties, outperforming conventional composites by maintaining consistent mechanical performance across specimens.
Smart Images

Figure 0007591051000001 
Figure 0007591051000002 
Figure 0007591051000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polycarbonate composite, a manufacturing method thereof, and a molded article containing the same. More specifically, the present invention relates to a polycarbonate composite containing a matrix resin, which is a polycarbonate resin copolymerized with an anhydrous sugar alcohol, and a nanomaterial dispersed in the matrix resin, and the polycarbonate composite shows significantly improved tensile modulus and tensile strength compared to conventional bio-polycarbonate resin composites by using a solid dispersion or molten dispersion obtained by introducing a nanomaterial (dispersoid) in the form of an aqueous dispersion into an anhydrous sugar alcohol (dispersion medium) as a diol component during the manufacturing process, and the polycarbonate composite has uniform physical properties because the nanomaterial is uniformly dispersed in the composite, a manufacturing method thereof, and a molded article containing the polycarbonate composite. [Background technology]
[0002] Nanomaterials such as nanocellulose can be produced from biomass in a variety of ways, and much research has been conducted recently, such as adding nanoparticles to polyurethane to improve its mechanical properties. However, due to the hydrophilic nature of nanocellulose, most products are produced using about 1 wt% of the nanomaterial dispersed in water as a dispersion medium, limiting its application for producing composites with polymer resins.
[0003] In addition, if solid crystal or powdered nanocellulose is used directly without dispersing it in water, etc., the nanocellulose will become entangled (aggregated), which has the disadvantage that the physical properties of the polymer resin composite material produced from it will deteriorate and it will not be uniform.
[0004] Therefore, there is a demand for the development of a resin composite comprising a matrix resin and a nanomaterial dispersed therein, which contains a higher content of nanomaterial than conventional resin composites while still being uniformly dispersed within the matrix resin, thereby resulting in a resin composite with significantly improved physical properties (especially tensile strength and tensile modulus) compared to conventional resin composites. Summary of the Invention [Problem to be solved by the invention]
[0005] The object of the present invention is to provide a polycarbonate composite having uniform physical properties, which exhibits significantly improved tensile strength and tensile modulus compared to conventional bio-polycarbonate resin composites, and has nanomaterials uniformly dispersed within the composite, as well as a method for producing the same, and a molded article containing the same. [Means for solving the problem]
[0006] In order to solve the above-mentioned technical problems, the present invention provides a polycarbonate composite comprising a matrix resin and a nanomaterial dispersed in the matrix resin, wherein the matrix resin is a polycarbonate resin which is a polymerization reaction product of a diol component and a carbonate diester component, and which contains a solid dispersion or molten dispersion of an anhydrosugar alcohol having the nanomaterial dispersed therein, and the solid dispersion or molten dispersion of anhydrosugar alcohol is obtained by introducing the nanomaterial into the anhydrosugar alcohol in the form of an aqueous dispersion.
[0007] Another aspect of the present invention provides a method for producing a polycarbonate composite, which includes a step of polymerizing a diol component containing a solid dispersion or molten dispersion of an anhydrosugar alcohol having a nanomaterial dispersed therein, with a carbonate diester component, wherein the solid dispersion or molten dispersion of an anhydrosugar alcohol is obtained by introducing a nanomaterial in the form of an aqueous dispersion into the anhydrosugar alcohol.
[0008] Yet another aspect of the present invention provides a molded article comprising the polycarbonate composite of the present invention. Effect of the Invention
[0009] The polycarbonate composite according to the present invention exhibits significantly improved tensile strength and tensile modulus compared to conventional bio-polycarbonate resin composites, particularly resin composites in which nanomaterials (e.g., nanocellulose) are used directly in solid crystal or powder form without being dispersed in water, and has uniform physical properties because the nanomaterials are uniformly dispersed within the composite. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. The polycarbonate composite of the present invention comprises a matrix resin and a nanomaterial dispersed in the matrix resin.
[0011] In the present invention, the "nanomaterial" refers to an organic or inorganic material having a submicron size (length or particle size), ie, less than 1 micrometer (eg, 10 to 900 nm, or 10 to 500 nm).
[0012] Regarding such nanomaterials, materials that satisfy the above-mentioned meaning of nanomaterials can be used, for example, nanocellulose, carbon nanofibers, carbon nanotubes, iron, aluminum, chromium, nickel, cobalt, zinc, tungsten, indium, tin, palladium, zirconium, titanium, copper, silver, gold, platinum, kaolin, clay, talc, mica, silica, bentonite, dolomite, calcium silicate, magnesium silicate, asbestos, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, barium sulfate, aluminum sulfate, aluminum hydroxide, iron hydroxide, aluminum silicate, zirconium oxide, magnesium oxide, aluminum oxide, titanium oxide, iron oxide, zinc oxide, antimony trioxide, indium oxide, indium oxide The material may be selected from the group consisting of tin, silicon carbide, silicon nitride, boron nitride, barium titanate, diatomaceous earth, carbon black, rock wool, graphene, graphite, graphene oxide, azo compounds, diazo compounds, condensed azo compounds, thioindigo compounds, indanthrone compounds, quinacridone compounds, anthraquinone compounds, benzimidazolone compounds, perylene compounds, phthalocyanine compounds, anthrapyridine compounds, dioxazine compounds, polyethylene resins, polypropylene resins, polyester resins, nylon resins, polyamide resins, aramid resins, urethane resins, polystyrene resins, polylactic acid, cellulose acetate fibers, hemicellulose, lignin, chitin, chitosan, starch, or mixtures thereof.
[0013] In one embodiment, the nanomaterial may be selected from, but is not limited to, nanocellulose, carbon nanofibers, carbon nanotubes, or a mixture thereof.
[0014] In one embodiment, the nanocellulose may be selected from the group consisting of nanocellulose fibers, nanocellulose crystals, or a mixture thereof.
[0015] In one embodiment, the carbon nanotubes may be selected from the group consisting of single-walled carbon nanotubes, multi-walled carbon nanotubes, or a mixture thereof.
[0016] In one embodiment, the content of the nanomaterial in the polycarbonate composite of the present invention may be 0.2 wt% or more, 0.3 wt% or more, 0.4 wt% or more, 0.5 wt% or more, or 0.55 wt% or more, or 10 wt% or less, 9 wt% or less, 8 wt% or less, 7 wt% or less, or 6.5 wt% or less, for example, 0.2 wt% to 10 wt%, more specifically, 0.5 wt% to 10 wt%, and even more specifically, 0.5 wt% to 7 wt%. If the content of the nanomaterial in the composite is less than the above level, there may be almost no effect of improving the mechanical properties of the composite, such as the tensile strength and tensile modulus, and if the content exceeds the above level, it may be difficult to disperse the nanomaterial in the matrix resin, and the nanomaterial may not be uniformly dispersed, making it difficult to obtain a polymer composite with uniform physical properties.
[0017] The matrix resin contained in the polycarbonate composite of the present invention is a polycarbonate resin which is a polymerization reaction product of a diol component and a carbonate diester component, comprising a solid dispersion or molten dispersion of an anhydrosugar alcohol having the nanomaterial dispersed therein, and the solid dispersion or molten dispersion of anhydrosugar alcohol is obtained by introducing the nanomaterial in the form of an aqueous dispersion into the anhydrosugar alcohol.
[0018] Anhydrous sugar alcohols can be produced by dehydration of hydrogenated sugars derived from natural products. Hydrogenated sugars (also called "sugar alcohols") are compounds obtained by adding hydrogen to the reducing end group of sugars, and generally have the chemical formula HOCH2(CHOH). n It is CH2OH (where n is an integer of 2 to 5) and is classified into tetritols, pentitols, hexitols and heptitols (having 4, 5, 6 and 7 carbon atoms, respectively) according to the carbon atoms. Among them, hexitols having 6 carbon atoms include sorbitol, mannitol, iditol, galactitol, etc., and in particular, sorbitol and mannitol are very useful materials.
[0019] In the present invention, the anhydrosugar alcohol may be a monoanhydrosugar alcohol, a dianhydrosugar alcohol, or a mixture thereof, and can be obtained in the process of producing an anhydrosugar alcohol by dehydration of a hydrogenated sugar (e.g., a hexitol such as sorbitol, mannitol, or iditol).
[0020] The monoanhydrosugar alcohol is an anhydrosugar alcohol formed by removing one molecule of water from the inside of a hydrogenated sugar, and has a tetraol form having four hydroxyl groups in the molecule. The type of monoanhydrosugar alcohol that can be used in the present invention is not particularly limited, and may be preferably a monoanhydrosugar hexitol, more specifically, 1,4-anhydrohexitol, 3,6-anhydrohexitol, 2,5-anhydrohexitol, 1,5-anhydrohexitol, 2,6-anhydrohexitol, or a mixture of two or more thereof.
[0021] The dianhydrosugar alcohol is an anhydrosugar alcohol formed by removing two molecules of water from the inside of a hydrogenated sugar, and is in the form of a diol having two hydroxyl groups in the molecule, and can be produced using hexitol derived from starch. Since dianhydrosugar alcohols are environmentally friendly substances derived from renewable natural resources, they have long been of interest, and research into their production has been ongoing. Among such dianhydrosugar alcohols, isosorbide produced from sorbitol currently has the widest industrial applicability. In the present invention, the type of dianhydrosugar alcohol that can be used is not particularly limited, and may be preferably dianhydrosugar hexitol, more specifically 1,4:3,6-dianhydrohexitol. The 1,4:3,6-dianhydrohexitol may be isosorbide, isomannide, isoidide, or a mixture of two or more thereof, and more preferably isosorbide.
[0022] In one embodiment, the solid dispersion of the anhydrosugar alcohol is a room temperature solid dispersion obtained by adding the nanomaterial in the form of an aqueous dispersion (e.g., a state in which the nanomaterial is dispersed in water at 0.1 to 5% by weight), mixing uniformly, melting the nanomaterial at a temperature equal to or higher than the melting point of the anhydrosugar alcohol (e.g., a temperature equal to or higher than 80°C) while removing moisture under vacuum, and then cooling the molten mixture to room temperature.
[0023] In one embodiment, the molten dispersion of the anhydrosugar alcohol is a liquid dispersion obtained by adding the nanomaterial in the form of an aqueous dispersion (e.g., 0.1 to 5% by weight of the nanomaterial dispersed in water), mixing them uniformly, and melting them under vacuum at a temperature above the melting point of the anhydrosugar alcohol (e.g., 80°C or higher) while removing moisture.In the present invention, such a molten dispersion can be used directly when producing a polycarbonate resin, without being cooled to a solid.
[0024] In one embodiment, the content of the nanomaterial introduced into the solid dispersion or molten dispersion of the anhydrosugar alcohol may be 0.2 wt% or more, 0.3 wt% or more, 0.4 wt% or more, 0.5 wt% or more, 0.6 wt% or more, 0.7 wt% or more, 0.8 wt% or more, 0.9 wt% or more, or 1 wt% or more, and may be 15 wt% or less, 14 wt% or less, 13 wt% or less, 12 wt% or less, 11 wt% or less, or 10 wt% or less, for example, 0.2 wt% to 15 wt%, more specifically 0.5 wt% to 12 wt%, and even more specifically 1 wt% to 10 wt%, based on the total weight of the solid dispersion or molten dispersion.
[0025] The matrix resin contained in the polycarbonate composite of the present invention is a polycarbonate resin which is a polymerization reaction product of a diol component containing a solid dispersion or molten dispersion of such anhydrous sugar alcohol and a carbonate diester component.
[0026] In one embodiment, the carbonate diester component is represented by the following formula (1): [ka] (wherein R1 may be independently selected from an unsubstituted or halogen-substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 25 carbon atoms).
[0027] In one embodiment, the carbonate diester component represented by the formula (1) may be selected from the group consisting of diphenyl carbonate, bischlorophenyl carbonate, dimethyl carbonate, diethyl carbonate, di-t-butyl carbonate, or a mixture thereof, and more preferably diphenyl carbonate or dimethyl carbonate can be used.
[0028] In one embodiment, the diol component may further comprise an additional diol component in addition to the solid or melt dispersion of the anhydrosugar alcohol.
[0029] In one embodiment, the additional diol component is represented by formula (2): [ka] (In the formula, X represents a mononuclear or polynuclear arylene group having 6 to 30 carbon atoms; a linear alkylene group having 1 to 15 carbon atoms; a branched alkylene group having 3 to 15 carbon atoms; or a cyclic alkylene group having 3 to 15 carbon atoms; The arylene group, linear alkylene group, branched alkylene group and cyclic alkylene group may each be unsubstituted or substituted with a halogen atom, an alkyl group, a cycloalkyl group, an alkenyl group, an alkoxy group, an aryl group, a nitro group or a carboxyl group.
[0030] In one embodiment, in the formula (2), the halogen atom may be F, Cl, or Br, the alkyl group may be an alkyl group having 1 to 20 carbon atoms (more specifically, an alkyl group having 1 to 13 carbon atoms, such as methyl, ethyl, propyl, or butyl), the cycloalkyl group may be a cycloalkyl group having 3 to 10 carbon atoms (more specifically, a cycloalkyl group having 3 to 6 carbon atoms), the alkenyl group may be an alkenyl group having 2 to 20 carbon atoms (more specifically, an alkenyl group having 2 to 13 carbon atoms), the alkoxy group may be an alkoxy group having 1 to 20 carbon atoms (more specifically, an alkoxy group having 1 to 13 carbon atoms, such as methoxy, ethoxy, propoxy, or butoxy), and the aryl group may be an aryl group having 6 to 30 carbon atoms (more specifically, an aryl group having 6 to 20 carbon atoms, such as a phenyl group, a tolyl group, a xylenyl group, or a naphthyl group).
[0031] In one embodiment, in the formula (2), X may be an arylene group that can be derived from a substituted or unsubstituted bisphenol (e.g., bisphenol A, bisphenol F, or bisphenol TMC, etc.), a substituted or unsubstituted resorcinol, a substituted or unsubstituted hydroquinone (e.g., hydroquinone, 2-nitrohydroquinone, 2-sulfonylhydroquinone, etc.), a substituted or unsubstituted biphenol, a substituted or unsubstituted naphthalenediol, or a substituted or unsubstituted diphenylphenol, and can be represented, for example, by the following formulas (2a) to (2h).
[0032] [ka]
[0033] In one embodiment, in the formula (2), X may be an alkylene group that can be derived from substituted or unsubstituted ethylene glycol, substituted or unsubstituted propylene glycol, or substituted or unsubstituted butanediol, for example, an ethylene group, a propylene group, or a butylene group.
[0034] In one embodiment, in the formula (2), X may be a cycloalkylene group that can be derived from substituted or unsubstituted cyclohexanediol, substituted or unsubstituted cyclohexanedimethanol, or substituted or unsubstituted tetramethylcyclobutanediol, and can be represented by, for example, the following formulas (2i) to (2k).
[0035] [ka]
[0036] In one embodiment, the diol component represented by the formula (2) may be an aromatic diol, an aliphatic diol, an alicyclic diol other than anhydrosugar alcohol, or a mixture thereof.
[0037] As the aromatic diol, for example, bisphenol (e.g., bisphenol A, bisphenol F, bisphenol TMC, etc.), resorcinol, hydroquinone, biphenol, naphthalenediol, or a mixture thereof, which are substituted or unsubstituted with a halogen atom, an alkyl group, a cycloalkyl group, an alkenyl group, an alkoxy group, an aryl group, a nitro group, or a carboxyl group, can be used. Preferably, bisphenol A, which is substituted or unsubstituted with a halogen atom, an alkyl group, a cycloalkyl group, an alkenyl group, an alkoxy group, an aryl group, a nitro group, or a carboxyl group, can be used.
[0038] The aliphatic diol may be, for example, an aliphatic diol having 2 to 10 carbon atoms, which is substituted or unsubstituted with a halogen atom, an alkyl group, a cycloalkyl group, an alkenyl group, an alkoxy group, an aryl group, a nitro group, or a carboxyl group. For example, ethylene glycol, diethylene glycol, triethylene glycol, propanediol (1,2-propanediol, 1,3-propanediol, etc.), butanediol (1,2-butanediol, 1,3-butanediol, 1,4-butanediol, etc.), pentanediol (1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, etc.), hexanediol (1,2-hexanediol, 1,3-hexanediol, 1,4-hexanediol, 1,5-hexanediol, 1,6-hexanediol, etc.), neopentyl glycol, or a mixture thereof, and preferably butanediol.
[0039] The alicyclic diol other than the anhydrosugar alcohol may be, for example, cyclohexanediol (1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, etc.), cyclohexanedimethanol (1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, etc.), tetramethylcyclobutanediol, or a mixture thereof, which is unsubstituted or substituted with a halogen atom, an alkyl group, a cycloalkyl group, an alkenyl group, an alkoxy group, an aryl group, a nitro group, or a carboxyl group, and is preferably cyclohexanediol.
[0040] In one embodiment, the number average molecular weight (Mn) of the polycarbonate resin may be 10,000 to 70,000, more specifically, 15,000 to 50,000, and even more specifically, 20,000 to 40,000. If the number average molecular weight is less than 10,000, there is a problem in obtaining sufficient mechanical properties, and if it exceeds 70,000, there is a problem in that the molecular weight becomes too high, the melting properties become poor, and processing becomes difficult.
[0041] In one embodiment, the amount of the carbonate diester component used in producing the polycarbonate resin may be 0.8 moles to 1.2 moles (more specifically, 0.9 moles to 1.1 moles) per mole of the total diol component including the anhydrosugar alcohol and the additional diol, and this component can be polymerized, for example, melt polymerized, in the presence of a polymerization catalyst.
[0042] As the polymerization catalyst, an alkali metal salt compound (e.g., sodium hydroxide, sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium carbonate, etc.); an alkaline earth metal salt compound (e.g., calcium hydroxide, barium oxide, magnesium oxide, etc.); a nitrogen-containing basic compound (e.g., tetramethylammonium hydroxide, tetraethylammonium hydroxide, triethylamine, etc.); or a mixture thereof can be used, which can be used alone or in combination of two or more of them. Among them, it is more preferable to use a nitrogen-containing basic compound in combination with an alkali metal salt compound.
[0043] The amount of the polymerization catalyst used is preferably 1×10 -9 ~1×10 -3 Molar equivalent, more preferably 1×10 -8 ~5×10 -4 It may be a molar equivalent.
[0044] The melt polymerization can be carried out at high temperatures, for example, from 140° C. to 240° C. (more specifically, from 160° C. to 220° C.), under atmospheric pressure or reduced pressure (for example, from 0.1 Torr to 120 Torr).
[0045] In one embodiment, the melt polymerization can be carried out by a process including a step of mixing the solid dispersion or molten dispersion of the anhydrosugar alcohol described above, a carbonic acid diester, and an optional additional diol component under atmospheric pressure, reacting them in the presence of a polymerization catalyst at a temperature of 140°C to 240°C (e.g., 160°C), and then reacting them under reduced pressure (e.g., 120 Torr or less, specifically 0.1 Torr to 120 Torr) at a temperature of 160°C to 240°C while removing the by-product alcohol (e.g., phenol or methanol).
[0046] The polycarbonate composite according to the present invention exhibits significantly improved tensile strength and tensile modulus compared to conventional bio-polycarbonate resin composites, particularly compared to resin composites in which nanomaterials (e.g., nanocellulose, etc.) are used directly in solid crystal or powder form without being dispersed in water, etc., and the nanomaterials are uniformly dispersed within the composite, resulting in uniform physical properties.
[0047] In one embodiment, the polycarbonate composites of the present invention can exhibit a tensile strength of greater than 80 MPa.
[0048] In one embodiment, the polycarbonate composites of the present invention can exhibit a tensile modulus of greater than 2,500 MPa.
[0049] The tensile strength and tensile modulus may be values measured, for example, using a universal testing machine (UTM) according to ASTM D638.
[0050] In addition, since the polycarbonate composite according to the present invention has nanomaterials uniformly dispersed within the matrix resin, it is possible to maintain the physical properties (especially the tensile strength and tensile modulus) more uniformly than conventional resin composites.
[0051] In one embodiment, the polycarbonate composites of the present invention can exhibit a tensile strength standard deviation of less than or equal to 3 MPa.
[0052] More specifically, the standard deviation of the tensile strength may be 2.5 MPa or less, 2.0 MPa or less, 1.5 MPa or less, 1.3 MPa or less, 1.2 MPa or less, 1.15 MPa or less, or 1.12 MPa or less.
[0053] In one embodiment, the polycarbonate composites of the present invention can exhibit a tensile modulus standard deviation of less than or equal to 200 MPa.
[0054] More specifically, the standard deviation of the tensile modulus may be 100 MPa or less, 50 MPa or less, 30 MPa or less, 10 MPa or less, 9 MPa or less, 8.5 MPa or less, 8.35 MPa or less, or 8.3 MPa or less.
[0055] The tensile strength standard deviation and the tensile modulus standard deviation may be, for example, the standard deviation of values measured for four test specimens using a universal testing machine (UTM) based on ASTM D638.
[0056] According to another aspect of the present invention, there is provided a method for producing a polycarbonate composite, which comprises a step of polymerizing a diol component containing a solid dispersion or molten dispersion of an anhydrosugar alcohol having a nanomaterial dispersed therein with a carbonate diester component, wherein the solid dispersion or molten dispersion of an anhydrosugar alcohol is obtained by introducing the nanomaterial in the form of an aqueous dispersion into the anhydrosugar alcohol.
[0057] In one embodiment, the solid dispersion of the anhydrosugar alcohol may be a room temperature solid dispersion obtained by adding the nanomaterial in the form of an aqueous dispersion (e.g., a state in which 0.1 to 5% by weight of the nanomaterial is dispersed in water) to the anhydrosugar alcohol, mixing uniformly, melting it under vacuum at a temperature equal to or higher than the melting point of the anhydrosugar alcohol (e.g., 80°C or higher) while removing moisture, and then cooling the molten mixture to room temperature.
[0058] In one embodiment, the molten dispersion of the anhydrosugar alcohol may be a liquid dispersion obtained by adding the nanomaterial in the form of an aqueous dispersion (e.g., a state in which the nanomaterial is dispersed in water at a concentration of 0.1 to 5% by weight) to the anhydrosugar alcohol, mixing uniformly, and melting the mixture under vacuum at a temperature equal to or higher than the melting point of the anhydrosugar alcohol (e.g., 80°C or higher) while removing moisture.
[0059] The nanomaterial, anhydrosugar alcohol, diester carbonate component, and additional diol component used in the preparation method are the same as those described above, and the solid or molten dispersion of the anhydrosugar alcohol, the preparation method thereof, and the polymerization reaction of the diol component and the diester carbonate component are the same as those described above.
[0060] In yet another aspect of the present invention, there is provided a molded article comprising the polycarbonate composite of the present invention.
[0061] The polycarbonate composite of the present invention has uniform physical properties (particularly tensile strength and tensile modulus) because the nanomaterial is uniformly dispersed within the composite. Therefore, the physical properties of the molded product constituting the composite are excellent and uniform, resulting in a very low defect rate when used in products.
[0062] The method for producing a molded article by processing the polycarbonate composite of the present invention is not particularly limited, and the molded article can be produced using a method commonly used in the plastic processing field. For example, the molded article of the present invention can be produced by extrusion molding or injection molding of the polycarbonate composite of the present invention.
[0063] Hereinafter, the present invention will be described in more detail through examples and comparative examples. However, the scope of the present invention is not limited thereby in any manner. EXAMPLES
[0064] [Part I] [Production of solid dispersion containing nanocellulose] <Dispersion containing nanocellulose fiber (NCF) and anhydrous sugar alcohol> Preparation Example I-A1: Preparation of a dispersion containing 1 wt.% nanocellulose fibers 99 g of isosorbide (NOVASORB®, manufactured by SAMYANG CORPORATION) and 100 g of an aqueous solution (KB101, manufactured by Asia Nanocellulose) in which 1 wt% nanocellulose fiber was dispersed were added to a rotary evaporator and mixed uniformly. The mixture was then melted while removing moisture under vacuum at a temperature of 80°C, which is higher than the melting point of isosorbide. The molten mixture was then cooled to room temperature to produce isosorbide (solid dispersion) containing nanocellulose fiber dispersed therein. The solid dispersion contained 1 wt% nanocellulose fiber based on the total weight of the solid dispersion.
[0065] Preparation Example I-A2: Preparation of a dispersion containing 3 wt.% nanocellulose fibers The same method as in Preparation Example I-A1 was carried out to prepare isosorbide (solid dispersion) having nanocellulose fibers dispersed therein, except that the content of isosorbide was changed from 99 g to 97 g and the content of the aqueous solution having 1 wt% nanocellulose fibers dispersed therein was changed from 100 g to 300 g. The solid dispersion contained 3 wt% nanocellulose fibers based on the total weight of the solid dispersion.
[0066] Preparation Example I-A3: Preparation of a dispersion containing 5% by weight of nanocellulose fibers The same procedure as in Preparation Example I-A1 was carried out except that the content of isosorbide was changed from 99 g to 95 g, and the content of the aqueous solution in which 1 wt% nanocellulose fiber was dispersed was changed from 100 g to 500 g, to produce isosorbide (solid dispersion) in which nanocellulose fiber was dispersed. The solid dispersion contained 5 wt% nanocellulose fiber based on the total weight of the solid dispersion.
[0067] Preparation Example I-A4: Preparation of a dispersion containing 10% by weight of nanocellulose fibers The same procedure as in Preparation Example I-A1 was carried out except that the content of isosorbide was changed from 99 g to 90 g, and the content of the aqueous solution in which 1 wt% nanocellulose fiber was dispersed was changed from 100 g to 1,000 g, to produce isosorbide (solid dispersion) in which nanocellulose fiber was dispersed. The solid dispersion contained 10 wt% nanocellulose fiber based on the total weight of the solid dispersion.
[0068] <Dispersion containing nanocellulose crystals (NCC) and anhydrous sugar alcohol> Preparation Example I-B1: Preparation of a dispersion containing 1% by weight of nanocellulose crystals The same procedure as in Preparation Example I-A1 was carried out, except that 100 g of an aqueous solution (CelluForce) in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution (KB101, Asia Nanocellulose) in which 1 wt% nanocellulose fibers were dispersed, to prepare isosorbide (solid dispersion) in which nanocellulose crystals were dispersed. The solid dispersion contained 1 wt% nanocellulose crystals based on the total weight of the solid dispersion.
[0069] Preparation Example I-B2: Preparation of a dispersion containing 3% by weight of nanocellulose crystals The isosorbide content was changed from 99 g to 97 g, and 300 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed, but the same procedure as in Preparation Example I-A1 was used to prepare isosorbide (solid dispersion) in which nanocellulose crystals were dispersed. The solid dispersion contained 3 wt% nanocellulose crystals based on the total weight of the solid dispersion.
[0070] Preparation Example I-B3: Preparation of a dispersion containing 5% by weight of nanocellulose crystals The isosorbide content was changed from 99 g to 95 g, and 500 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed, but the same procedure as in Preparation Example I-A1 was used to prepare isosorbide (solid dispersion) in which nanocellulose crystals were dispersed. The solid dispersion contained 5 wt% nanocellulose crystals based on the total weight of the solid dispersion.
[0071] Preparation Example I-B4: Preparation of a dispersion containing 10% by weight of nanocellulose crystals The isosorbide content was changed from 99 g to 90 g, and 1,000 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed, but the same procedure as in Preparation Example I-A1 was used to prepare isosorbide (solid dispersion) in which nanocellulose crystals were dispersed. The solid dispersion contained 10 wt% nanocellulose crystals based on the total weight of the solid dispersion.
[0072] <A mixture of nanocellulose fibers and nanocellulose crystals, and a dispersion containing anhydrous sugar alcohol> Preparation Example I-C1: Preparation of a dispersion containing 1% by weight of a mixture of nanocellulose fibers and nanocellulose crystals Isosorbide (solid dispersion) in which nanocellulose fibers and nanocellulose crystals are dispersed was prepared in the same manner as in Preparation Example I-A1, except that a mixture of 50 g of an aqueous solution in which 1 wt% nanocellulose fibers are dispersed and 50 g of an aqueous solution in which 1 wt% nanocellulose crystals are dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers are dispersed. The solid dispersion contained 1 wt% of a mixture of nanocellulose fibers and nanocellulose crystals based on the total weight of the solid dispersion.
[0073] Preparation Example I-C2: Preparation of a dispersion containing 3% by weight of a mixture of nanocellulose fibers and nanocellulose crystals The content of isosorbide was changed from 99 g to 97 g, and a mixture of 150 g of an aqueous solution in which 1 wt% nanocellulose fiber was dispersed and 150 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fiber was dispersed. The same method as in Preparation Example I-A1 was used to prepare isosorbide (solid dispersion) in which nanocellulose fiber and nanocellulose crystals were dispersed. The solid dispersion contained 3 wt% of a mixture of nanocellulose fiber and nanocellulose crystals based on the total weight of the solid dispersion.
[0074] Preparation Example I-C3: Preparation of a dispersion containing 5% by weight of a mixture of nanocellulose fibers and nanocellulose crystals The content of isosorbide was changed from 99 g to 95 g, and a mixture of 250 g of an aqueous solution in which 1 wt% nanocellulose fiber was dispersed and 250 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fiber was dispersed. The same method as in Preparation Example I-A1 was used to prepare isosorbide (solid dispersion) in which nanocellulose fiber and nanocellulose crystals were dispersed. The solid dispersion contained 5 wt% of a mixture of nanocellulose fiber and nanocellulose crystals based on the total weight of the solid dispersion.
[0075] Preparation Example I-C4: Preparation of a dispersion containing 10% by weight of a mixture of nanocellulose fibers and nanocellulose crystals The content of isosorbide was changed from 99g to 90g, and a mixture of 500g of an aqueous solution in which 1wt% nanocellulose fiber was dispersed and 500g of an aqueous solution in which 1wt% nanocellulose crystals were dispersed was used instead of 100g of an aqueous solution in which 1wt% nanocellulose fiber was dispersed. The same method as in Preparation Example I-A1 was used to prepare isosorbide (solid dispersion) in which nanocellulose fiber and nanocellulose crystals were dispersed. The solid dispersion contained 10wt% of a mixture of nanocellulose fiber and nanocellulose crystals based on the total weight of the solid dispersion.
[0076] [Polycarbonate resin composite using solid dispersion containing nanocellulose] <Production and property evaluation of polycarbonate resin composite using solid dispersion containing nanocellulose fiber and anhydrous sugar alcohol> Example I-A1: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-A1 A vacuum pump for reducing pressure equipped with a nitrogen gas pipe and a trap for removing by-products was connected to a five-neck flask equipped with a stirrer, a thermometer and a heater, and 100 g of the solid dispersion produced in Preparation Example I-A1, 29.6 g of cyclohexane dimethanol and 190.6 g of diphenyl carbonate were supplied and heated to 100°C under a nitrogen atmosphere. After the reaction mixture was confirmed to be melted, 100 mg of magnesium acetate tetrahydrate was added and stirred. After the reaction temperature reached 160°C, the reaction was carried out while maintaining the temperature for 1 hour, and then the pressure was slowly reduced to 100-120 Torr using a vacuum pump, and the reaction was further carried out for 1-2 hours while removing phenol generated as a by-product. Then, the temperature was slowly increased to 220°C, the pressure was reduced to 5-10 Torr, and the reaction was further carried out for 1 hour. As a result, about 130 g of polycarbonate resin composite was obtained. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,500 g / mol, and a PDI of 1.7. To measure the content of nanocellulose fibers in the obtained polycarbonate resin composite, 50 g of the polycarbonate resin composite was dissolved in 1 L of chloroform, the remaining crystalline components were filtered, and the mixture was dried in a vacuum oven for 24 hours and weighed to be 0.31 g. Thus, the content of nanocellulose fibers in the obtained polycarbonate resin composite was calculated to be 0.62 wt%. The polycarbonate resin composite thus obtained was used to prepare four identical tensile test specimens according to ASTM D638. The tensile strength and tensile modulus of the four tensile test specimens were measured using a universal testing machine (UTM). As a result, the average tensile strength was 97 MPa and the average tensile modulus was 2,900 MPa.
[0077] Example I-A2: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-A2 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-A2 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 128 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,210 g / mol, and a PDI of 1.7. The content of nanocellulose fibers in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 1.9% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 98.5 MPa and the average tensile modulus was 2,923 MPa.
[0078] Example I-A3: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-A3 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-A3 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 126 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, and had a number average molecular weight of about 30,620 g / mol and a PDI of 1.8. The content of nanocellulose fibers in the obtained polycarbonate resin composite was measured by the same method as in Example I-A1, and was found to be 3.1% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured by the same method as in Example I-A1, and the average tensile strength was 101.5 MPa and the average tensile modulus was 2,950 MPa.
[0079] Example I-A4: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-A4 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-A4 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 130 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, and had a number average molecular weight of about 30,840 g / mol and a PDI of 1.7. The content of nanocellulose fibers in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 6.4% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 105.75 MPa and the average tensile modulus was 2,990 MPa.
[0080] <Production and property evaluation of polycarbonate resin composite using solid dispersion containing nanocellulose crystals and anhydrous sugar alcohol> Example I-B1: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-B1 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-B1 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 125 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,200 g / mol, and a PDI of 1.8. The content of nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was 0.59% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 93.5 MPa and the average tensile modulus was 2,700 MPa.
[0081] Example I-B2: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-B2 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-B2 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 128 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,150 g / mol, and a PDI of 1.6. The content of nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 1.8% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 94.5 MPa and the average tensile modulus was 2,783 MPa.
[0082] Example I-B3: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-B3 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-B3 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 131 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,500 g / mol, and a PDI of 1.6. The content of nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 3.5% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 96.0 MPa and the average tensile modulus was 2,818 MPa.
[0083] Example I-B4: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-B4 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-B4 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 125 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,670 g / mol, and a PDI of 1.9. The content of nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 6.2% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 100.0 MPa and the average tensile modulus was 2,930 MPa.
[0084] <Production and property evaluation of polycarbonate resin composite using a solid dispersion containing a mixture of nanocellulose fibers and nanocellulose crystals and anhydrous sugar alcohol> Example I-C1: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-C1 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-C1 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 128 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,650 g / mol, and a PDI of 1.8. The total content of nanocellulose fibers and nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 0.62% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 94.5 MPa and the average tensile modulus was 2,850 MPa.
[0085] Example I-C2: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-C2 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-C2 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 130 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,630 g / mol, and a PDI of 1.9. The total content of nanocellulose fibers and nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 1.87% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 96.25 MPa and the average tensile modulus was 2,900 MPa.
[0086] Example I-C3: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-C3 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-C3 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 130 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,800 g / mol, and a PDI of 1.8. The total content of nanocellulose fibers and nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 3.18% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 100.5 MPa and the average tensile modulus was 2,958 MPa.
[0087] Example I-C4: Preparation of polycarbonate resin composite using solid dispersion of Preparation Example I-C4 The same procedure as in Example I-A1 was carried out, except that 100 g of the solid dispersion prepared in Preparation Example I-C4 was used instead of 100 g of the solid dispersion prepared in Preparation Example I-A1, to obtain about 130 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,450 g / mol, and a PDI of 1.8. The total content of nanocellulose fibers and nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example I-A1, and was found to be 6.49% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example I-A1, and the average tensile strength was 101.25 MPa and the average tensile modulus was 2,993 MPa.
[0088] <Evaluation of the uniform dispersion of nanocellulose particles in polycarbonate resin composite> For each of the polycarbonate resin composites obtained in Examples I-A1 to I-A4, I-B1 to I-B4, and I-C1 to I-C4, the tensile strength and tensile modulus, as well as their average values and standard deviations, were measured on four tensile test specimens, and the results are shown in Table 1 below.
[0089] [Table 1]
[0090] As shown in Table 1, the average and standard deviation of the tensile strength of four tensile test specimens of each of the polycarbonate resin composites of Examples I-A1 to I-A4, I-B1 to I-B4, and I-C1 to I-C4 according to the present invention were measured. As a result, the tensile strengths of the four tensile test specimens were equal, and the tensile strength deviation of the four tensile test specimens was very small, at 1.12 MPa or less, which indicates that nanocellulose particles are uniformly dispersed within the polycarbonate resin composite. In addition, when the average and standard deviation of the tensile modulus of four tensile test specimens for each of the polycarbonate resin composites of Examples I-A1 to I-A4, I-B1 to I-B4, and I-C1 to I-C4 according to the present invention were measured, it was found that the tensile modulus of the four tensile test specimens was equivalent, and the tensile modulus deviation of the four tensile test specimens was very small, at 8.30 MPa or less, which indicates that the nanocellulose particles are uniformly dispersed within the polycarbonate resin composite. Furthermore, the polycarbonate resin composites of Examples I-A1 to I-A4, I-B1 to I-B4, and I-C1 to I-C4 according to the present invention have excellent mechanical properties, since the average tensile strength of the four tensile test specimens is 93.5 MPa or more and the average tensile modulus of the four tensile test specimens is 2,700 MPa or more.
[0091] [Part II] [Polycarbonate resin composite using melt dispersion containing nanocellulose] <Production and property evaluation of polycarbonate resin composite using molten dispersion containing nanocellulose fiber (NCF) and anhydrous sugar alcohol> Example II-A1: Preparation of polycarbonate resin composite with 0.63 wt% nanocellulose fibers dispersed therein 99 g of isosorbide (NOVASORB®, manufactured by SAMYANG CORPORATION) and 100 g of an aqueous solution (KB101, manufactured by Asia Nanocellulose) in which 1 wt% nanocellulose fiber was dispersed were added to a rotary evaporator and mixed uniformly. The mixture was then melted while removing moisture under vacuum at a temperature of 80°C, which is higher than the melting point of isosorbide, to produce a liquid molten dispersion. The molten dispersion contained 1 wt% nanocellulose fiber based on the total weight of the molten dispersion. Next, a vacuum pump for reducing pressure equipped with a nitrogen gas pipe and a trap for removing by-products was connected, and 100 g of the molten dispersion, 29.6 g of cyclohexanedimethanol, and 190.6 g of diphenyl carbonate were supplied to a 5-neck flask equipped with a stirrer, a thermometer, and a heater, and heated to 100°C under a nitrogen atmosphere. After confirming that the reaction mixture had melted, 100 mg of magnesium acetate tetrahydrate was added and stirred. After the reaction temperature reached 160°C, the reaction was carried out while maintaining the temperature for 1 hour, and the pressure was slowly reduced to 100-120 Torr using a vacuum pump, and the reaction was further carried out for 1-2 hours while removing phenol generated as a by-product. Thereafter, the temperature was slowly increased to 220°C, the pressure was reduced to 5-10 Torr, and the reaction was further carried out for 1 hour. As a result, 140 g of a polycarbonate resin composite was obtained. The polycarbonate resin composite obtained was a transparent solid, had a number average molecular weight of about 31,000 g / mol, and a PDI of 1.6. In order to measure the content of nanocellulose fibers in the obtained polycarbonate resin composite, 50 g of the polycarbonate resin composite was dissolved in 1 L of chloroform, and the remaining crystalline components were filtered out. The composite was then dried in a vacuum oven for 24 hours and weighed to be 0.316 g. Thus, the content of nanocellulose fibers in the obtained polycarbonate resin composite was calculated to be 0.63 wt%. Four tensile test specimens were prepared from the obtained polycarbonate resin composite in accordance with ASTM D638, and the tensile strength and tensile modulus of the four tensile test specimens were measured using a universal testing machine (UTM). As a result, the average tensile strength was 95.75 MPa, and the average tensile modulus was 2,855 MPa.
[0092] Example II-A2: Preparation of polycarbonate resin composite with 1.89 wt% nanocellulose fibers dispersed therein A melt dispersion was produced in the same manner as in Example II-A1, except that the content of isosorbide was changed from 99 g to 98 g, and the content of the aqueous solution in which 1 wt% nanocellulose fibers were dispersed was changed from 100 g to 200 g. The melt dispersion contained 2 wt% nanocellulose fibers based on the total weight of the melt dispersion. Next, the melt dispersion was used in the same manner as in Example II-A1 to obtain 138 g of polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,890 g / mol, and a PDI of 1.4. The content of nanocellulose fibers in the obtained polycarbonate resin composite was measured by the same method as in Example II-A1, and was found to be 1.89% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured by the same method as in Example II-A1, and the average tensile strength was 98.0 MPa and the average tensile modulus was 2,885 MPa.
[0093] Example II-A3: Preparation of polycarbonate resin composite with 3.21 wt% nanocellulose fibers dispersed therein A melt dispersion was produced in the same manner as in Example II-A1, except that the content of isosorbide was changed from 99 g to 95 g, and the content of the aqueous solution in which 1 wt% nanocellulose fibers were dispersed was changed from 100 g to 500 g. The melt dispersion contained 5 wt% nanocellulose fibers based on the total weight of the melt dispersion. Next, the melt dispersion was used in the same manner as in Example II-A1 to obtain 132 g of polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,900 g / mol, and a PDI of 1.5. The content of nanocellulose fibers in the obtained polycarbonate resin composite was measured by the same method as in Example II-A1, and was found to be 3.21% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured by the same method as in Example II-A1, and the average tensile strength was 100.5 MPa and the average tensile modulus was 2,935 MPa.
[0094] Example II-A4: Preparation of polycarbonate resin composite with 6.34 wt% nanocellulose fibers dispersed therein A melt dispersion was produced in the same manner as in Example II-A1, except that the content of isosorbide was changed from 99 g to 90 g, and the content of the aqueous solution in which 1 wt% nanocellulose fibers were dispersed was changed from 100 g to 1,000 g. The melt dispersion contained 10 wt% nanocellulose fibers based on the total weight of the melt dispersion. Next, the melt dispersion was used in the same manner as in Example II-A1 to obtain 135 g of polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 31,050 g / mol, and a PDI of 1.8. The content of nanocellulose fibers in the obtained polycarbonate resin composite was measured using the same method as in Example II-A1, and was found to be 6.34% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example II-A1, and the average tensile strength was 102.25 MPa and the average tensile modulus was 2,993 MPa.
[0095] <Production and property evaluation of polycarbonate resin composite using molten dispersion containing nanocellulose crystals (NCC) and anhydrous sugar alcohol> Example II-B1: Preparation of polycarbonate resin composite with 0.61 wt% nanocellulose crystals dispersed therein A melt dispersion was prepared in the same manner as in Example II-A1, except that 100 g of an aqueous solution (CelluForce) in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution (KB101, Asia Nanocellulose) in which 1 wt% nanocellulose fibers were dispersed. The melt dispersion contained 1 wt% nanocellulose crystals based on the total weight of the melt dispersion. Next, 135 g of a polycarbonate resin composite was obtained using the melt dispersion in the same manner as in Example II-A1. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,920 g / mol, and a PDI of 1.9. The content of nanocellulose crystals in the obtained polycarbonate resin composite was measured by the same method as in Example II-A1, and was 0.61% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured by the same method as in Example II-A1, and the average tensile strength was 92.25 MPa and the average tensile modulus was 2,645 MPa.
[0096] Example II-B2: Preparation of polycarbonate resin composite with 1.87 wt% nanocellulose crystals dispersed therein A melt dispersion was produced in the same manner as in Example II-A1, except that the content of isosorbide was changed from 99 g to 97 g, and 300 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed. The melt dispersion contained 3 wt% nanocellulose crystals based on the total weight of the melt dispersion. Next, the same manner as in Example II-A1 was carried out using the melt dispersion to obtain 130 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,990 g / mol, and a PDI of 1.4. The content of nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example II-A1, and was found to be 1.87% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example II-A1, and the average tensile strength was 95.5 MPa and the average tensile modulus was 2,693 MPa.
[0097] Example II-B3: Preparation of polycarbonate resin composite with 3.2 wt% nanocellulose crystals dispersed therein A melt dispersion was produced in the same manner as in Example II-A1, except that the content of isosorbide was changed from 99 g to 95 g, and 500 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed. The melt dispersion contained 5 wt% nanocellulose crystals based on the total weight of the melt dispersion. Next, the same manner as in Example II-A1 was carried out using the melt dispersion to obtain 135 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 31,110 g / mol, and a PDI of 1.6. The content of nanocellulose crystals in the obtained polycarbonate resin composite was measured by the same method as in Example II-A1, and was 3.2 wt%. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured by the same method as in Example II-A1, and the average tensile strength was 96.25 MPa and the average tensile modulus was 2,728 MPa.
[0098] Example II-B4: Preparation of polycarbonate resin composite with 6.48 wt% nanocellulose crystals dispersed therein A melt dispersion was produced in the same manner as in Example II-A1, except that the content of isosorbide was changed from 99 g to 90 g, and 1,000 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed was used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed. The melt dispersion contained 10 wt% nanocellulose crystals based on the total weight of the melt dispersion. Next, the same manner as in Example II-A1 was carried out using the melt dispersion to obtain 132 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 31,050 g / mol, and a PDI of 1.8. The content of nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example II-A1, and was found to be 6.48% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example II-A1, and the average tensile strength was 100.0 MPa and the average tensile modulus was 2,795 MPa.
[0099] <Production and property evaluation of polycarbonate resin composite using a mixture of nanocellulose fibers and nanocellulose crystals and a molten dispersion containing anhydrous sugar alcohol> Example II-C1: Preparation of polycarbonate resin composites containing a mixture of nanocellulose fibers and nanocellulose crystals dispersed at 0.60 wt% A melt dispersion was prepared in the same manner as in Example II-A1, except that 50 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed and 50 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed were used instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed. The melt dispersion contained 1 wt% of a mixture of nanocellulose fibers and nanocellulose crystals based on the total weight of the melt dispersion. Next, the same method as in Example II-A1 was carried out using the melt dispersion to obtain 133 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,980 g / mol, and a PDI of 1.9. The total content of nanocellulose fibers and nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example II-A1, and was found to be 0.60% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example II-A1, and the average tensile strength was 93.5 MPa and the average tensile modulus was 2,800 MPa.
[0100] Example II-C2: Preparation of polycarbonate resin composite with a mixture of nanocellulose fibers and nanocellulose crystals dispersed at 1.92 wt% The content of isosorbide was changed from 99 g to 97 g, and instead of 100 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed, 150 g of an aqueous solution in which 1 wt% nanocellulose fibers were dispersed and 150 g of an aqueous solution in which 1 wt% nanocellulose crystals were dispersed were used to prepare a melt dispersion in the same manner as in Example II-A1. The melt dispersion contained 3 wt% of a mixture of nanocellulose fibers and nanocellulose crystals based on the total weight of the melt dispersion. Next, the same method as in Example II-A1 was carried out using the melt dispersion to obtain 136 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,850 g / mol, and a PDI of 1.7. The total content of nanocellulose fibers and nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example II-A1, and was found to be 1.92% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example II-A1, and the average tensile strength was 94.75 MPa and the average tensile modulus was 2,853 MPa.
[0101] Example II-C3: Preparation of polycarbonate resin composite with a mixture of nanocellulose fibers and nanocellulose crystals dispersed at 3.19 wt% The content of isosorbide was changed from 99 g to 95 g, and instead of 100 g of the aqueous solution in which 1 wt% nanocellulose fiber was dispersed, 250 g of the aqueous solution in which 1 wt% nanocellulose fiber was dispersed and 250 g of the aqueous solution in which 1 wt% nanocellulose crystals were dispersed were used to prepare a melt dispersion in the same manner as in Example II-A1. The melt dispersion contained 5 wt% of a mixture of nanocellulose fiber and nanocellulose crystals based on the total weight of the melt dispersion. The melt dispersion was then used in the same manner as in Example II-A1 to obtain 135 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,870 g / mol, and a PDI of 1.6. The total content of nanocellulose fibers and nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example II-A1, and was found to be 3.19% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example II-A1, and the average tensile strength was 96.75 MPa and the average tensile modulus was 2,898 MPa.
[0102] Example II-C4: Preparation of polycarbonate resin composite with a mixture of nanocellulose fibers and nanocellulose crystals dispersed at 6.29 wt% The content of isosorbide was changed from 99 g to 90 g, and instead of 100 g of the aqueous solution in which 1 wt% nanocellulose fibers were dispersed, 500 g of the aqueous solution in which 1 wt% nanocellulose fibers were dispersed and 500 g of the aqueous solution in which 1 wt% nanocellulose crystals were dispersed were used to prepare a melt dispersion in the same manner as in Example II-A1. The melt dispersion contained 10 wt% of a mixture of nanocellulose fibers and nanocellulose crystals based on the total weight of the melt dispersion. Next, the same method as in Example II-A1 was carried out using the melt dispersion to obtain 138 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, had a number average molecular weight of about 30,660 g / mol, and a PDI of 1.7. The total content of nanocellulose fibers and nanocellulose crystals in the obtained polycarbonate resin composite was measured using the same method as in Example II-A1, and was found to be 6.29% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in Example II-A1, and the average tensile strength was 100.75 MPa and the average tensile modulus was 2,935 MPa.
[0103] <Evaluation of the uniform dispersion of nanocellulose particles in polycarbonate resin composite> The tensile strength and tensile modulus of each of the four tensile test specimens of the polycarbonate resin composites obtained in Examples II-A1 to II-A4, II-B1 to II-B4, and II-C1 to II-C4 were measured, as well as their average values and standard deviations, and are shown in Table 2 below.
[0104] [Table 2]
[0105] As shown in Table 2, the average and standard deviation of the tensile strength of four tensile test specimens for each of the polycarbonate resin composites of Examples II-A1 to II-A4, II-B1 to II-B4, and II-C1 to II-C4 according to the present invention were measured. As a result, the standard deviation of the tensile strength of the four tensile test specimens was very small, at 1.12 MPa or less, and the tensile strengths of the four tensile test specimens were equivalent, which indicates that nanocellulose particles are uniformly dispersed within the polycarbonate resin composite. In addition, when the average and standard deviation of the tensile modulus of four tensile test specimens of each of the polycarbonate resin composites of Examples II-A1 to II-A4, II-B1 to II-B4, and II-C1 to II-C4 according to the present invention were measured, it was found that the standard deviation of the four tensile modulus was very small, at 8.31 MPa or less, and the tensile modulus of the four tensile test specimens was equivalent, which indicates that the nanocellulose particles are uniformly dispersed within the polycarbonate resin composite. Furthermore, the polycarbonate resin composites of Examples II-A1 to II-A4, II-B1 to II-B4, and II-C1 to II-C4 according to the present invention have excellent mechanical properties, since the average tensile strength of the four tensile test specimens is 92.25 MPa or more and the average tensile modulus of the four tensile test specimens is 2,645 MPa or more.
[0106] [Comparative Example] Comparative Example A1: Preparation and property evaluation of polycarbonate resin using anhydrous sugar alcohol without nanocellulose particles dispersed The same procedure as in the examples was carried out, except that 100 g of pure isosorbide (NOVASORB (registered trademark), manufactured by SAMYANG CORPORATION) was used instead of 100 g of the solid dispersion or molten dispersion prepared in the examples, to obtain about 128 g of polycarbonate resin. The obtained polycarbonate resin was a transparent solid, and had a number average molecular weight of about 30,100 g / mol and a PDI of 1.6. The obtained polycarbonate resin did not contain nanocellulose particles, and the average tensile strength and average tensile modulus of the obtained polycarbonate resin were measured in the same manner as in the examples, and the average tensile strength was 65.0 MPa and the average tensile modulus was 2,000 MPa. It was confirmed that the polycarbonate resin of Comparative Example A1, which does not contain nanocellulose particles, has very low average tensile strength and average tensile modulus, and thus poor mechanical properties, compared to the polycarbonate resin composite of the example according to the present invention.
[0107] Comparative Example B1: Preparation and property evaluation of polycarbonate resin composite using liquid dispersion in which 1 wt% nanocellulose fiber powder was directly added 99 g of isosorbide (NOVASORB®, manufactured by SAMYANG CORPORATION) was heated in an oven at 70° C. to obtain 99 g of molten isosorbide. 1 g of nanocellulose fiber in powder form was directly added to the 99 g of molten isosorbide and stirred to disperse the nanocellulose fiber in the molten isosorbide. Next, an ultrasonic generator was used to disperse the nanocellulose fiber at the same temperature for another hour to produce isosorbide (liquid dispersion) in which the nanocellulose fiber was dispersed. The liquid dispersion contained 1 wt % of nanocellulose fiber based on the total weight of the liquid dispersion. Then, the same procedure as in the examples was carried out except that 100 g of the obtained liquid dispersion was used instead of 100 g of the solid dispersion or molten dispersion produced in the examples, to obtain about 132 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, and had a number average molecular weight of about 30,250 g / mol and a PDI of 1.7. The content of nanocellulose fibers in the obtained polycarbonate resin composite was measured using the same method as in the Examples, and was found to be 0.52% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in the Examples, and the average tensile strength was 73.3 MPa and the average tensile modulus was 2,450 MPa. It was confirmed that the polycarbonate resin composite of Comparative Example B1 had low average tensile strength and average tensile modulus, and was relatively inferior in mechanical properties, compared to the polycarbonate resin composites of the examples of the present invention.
[0108] Comparative Example B2: Preparation and property evaluation of polycarbonate resin composite using liquid dispersion in which 10% by weight of nanocellulose fiber powder was directly added The same method as in Comparative Example B1 was carried out to obtain isosorbide (liquid dispersion) in which nanocellulose fibers were dispersed, except that the content of isosorbide was changed from 99 g to 90 g and the content of powdered nanocellulose fibers was changed from 1 g to 10 g. The liquid dispersion contained 10 wt% nanocellulose fibers based on the total weight of the liquid dispersion. Next, the same procedure as in the examples was carried out except that 100 g of the liquid dispersion obtained above was used instead of 100 g of the solid dispersion or molten dispersion produced in the examples, to obtain about 129 g of a polycarbonate resin composite. The obtained polycarbonate resin composite was a transparent solid, with a number average molecular weight of about 30,150 g / mol and a PDI of 1.8. The content of nanocellulose fibers in the obtained polycarbonate resin composite was measured using the same method as in the Examples, and was found to be 3.0% by weight. The average tensile strength and average tensile modulus of the obtained polycarbonate resin composite were measured using the same method as in the Examples, and the average tensile strength was 80.0 MPa and the average tensile modulus was 2,500 MPa. It was confirmed that the polycarbonate resin composite of Comparative Example B2 had low average tensile strength and average tensile modulus, and was relatively inferior in mechanical properties, compared to the polycarbonate resin composites of the examples of the present invention.
[0109] <Evaluation of the uniform dispersion of nanocellulose particles in polycarbonate resin composite> The tensile strength and tensile modulus of elasticity, as well as the average value and standard deviation thereof, were measured for each of the four tensile test specimens of the polycarbonate resin composites obtained in Comparative Examples B1 and B2. The results are shown in Table 3 below.
[0110] [Table 3]
[0111] As shown in Table 3, in the case of Comparative Examples B1 and B2 not according to the present invention, the nanocellulose particles were not uniformly dispersed in the polycarbonate resin composite, and thus the tensile strength and tensile modulus of the measured tensile test specimens showed large deviations. Specifically, the average and standard deviation of the tensile strength of four tensile test specimens for each of the polycarbonate resin composites of Comparative Examples B1 and B2 were measured. As a result, the standard deviation of the tensile strength of the four tensile test specimens was very large, ranging from 3.27 MPa to 7.78 MPa, which indicated that the nanocellulose particles were dispersed unevenly within the polycarbonate resin composite. Specifically, the average and standard deviation of the tensile modulus of four tensile test specimens for each of the polycarbonate resin composites of Comparative Examples B1 and B2 were measured. As a result, the standard deviation of the tensile modulus of the four tensile test specimens was very large, ranging from 224 MPa to 403 MPa, indicating that the nanocellulose particles were dispersed unevenly within the polycarbonate resin composite.
[0112] As can be seen from the above, in the case of the polycarbonate resin composite of the embodiment according to the present invention, the nanocellulose particles were uniformly dispersed within the composite, so the tensile strength and tensile modulus were high and uniform. However, in the case of the polycarbonate resin composites of Comparative Examples B1 and B2 not according to the present invention, the nanocellulose particles were not uniformly dispersed within the composite, so the tensile strength and tensile modulus were relatively low and non-uniform compared to the polycarbonate resin composites of the embodiment according to the present invention.
Claims
1. 1. A polycarbonate composite comprising: A matrix resin and a nanomaterial dispersed in the matrix resin, wherein the matrix resin is a polycarbonate resin that is a polymerization reaction product of a diol component and a carbonate diester component, the polycarbonate resin including a solid dispersion or a molten dispersion of anhydrous sugar alcohol having the nanomaterial dispersed therein; The solid dispersion or molten dispersion of the anhydrosugar alcohol is obtained by introducing the nanomaterial into the anhydrosugar alcohol in the form of an aqueous dispersion, The nanomaterial is nanocellulose; the anhydrosugar alcohol is a dianhydrosugar alcohol, A polycarbonate composite, wherein the content of the nanomaterial in the polycarbonate composite is 3.1 wt % or more and 6.5 wt % or less, based on the total weight of the polycarbonate composite.
2. 2. The polycarbonate composite of claim 1, wherein the nanocellulose is selected from nanocellulose fibers, nanocellulose crystals, or a mixture thereof.
3. 2. The polycarbonate complex of claim 1, wherein the dianhydrosugar alcohol is isosorbide.
4. The polycarbonate composite according to claim 1, wherein the solid dispersion of the anhydrosugar alcohol is obtained by adding the nanomaterial in the form of an aqueous dispersion to an anhydrosugar alcohol, mixing the nanomaterial, melting the mixture while removing water at a temperature equal to or higher than the melting point of the anhydrosugar alcohol, and then cooling the molten mixture to room temperature.
5. The polycarbonate composite described in claim 1, wherein the molten dispersion of the anhydrous sugar alcohol is obtained by adding the nanomaterial in the form of an aqueous dispersion to the anhydrous sugar alcohol, mixing the nanomaterial, and melting the anhydrous sugar alcohol while removing moisture at a temperature equal to or higher than the melting point of the anhydrous sugar alcohol.
6. The carbonate diester component is represented by the following formula (1): 【Chemistry 1】 (In the formula, R 1 and each of the carbonic acid diester components is independently selected from an unsubstituted or halogen-substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 25 carbon atoms.
7. 2. The polycarbonate composite of claim 1, wherein the diol component further comprises an additional diol component in addition to the solid or melt dispersion of the anhydrosugar alcohol.
8. The additional diol component is represented by the following formula (2): 【Chemistry 2】 (In the formula, X represents a mononuclear or polynuclear arylene group having 6 to 30 carbon atoms; a linear alkylene group having 1 to 15 carbon atoms; a branched alkylene group having 3 to 15 carbon atoms; or a cyclic alkylene group having 3 to 15 carbon atoms; The arylene group, the linear alkylene group, the branched alkylene group and the cyclic alkylene group may each be unsubstituted or substituted with a halogen atom, an alkyl group, a cycloalkyl group, an alkenyl group, an alkoxy group, an aryl group, a nitro group or a carboxyl group.
9. A method for producing a polycarbonate composite, comprising the steps of: The method includes a step of polymerizing a diol component including a solid or molten dispersion of anhydrous sugar alcohol having a nanomaterial dispersed therein and a carbonate diester component, wherein the solid dispersion or molten dispersion of anhydrosugar alcohol is obtained by introducing a nanomaterial into anhydrosugar alcohol in the form of an aqueous dispersion, The nanomaterial is nanocellulose; the anhydrosugar alcohol is a dianhydrosugar alcohol, A method for producing a polycarbonate composite, wherein the content of the nanomaterial in the polycarbonate composite is 3.1 wt % or more and 6.5 wt % or less, based on the total weight of the polycarbonate composite.
10. The method for producing a polycarbonate composite described in claim 9, wherein the solid dispersion of the anhydrosugar alcohol is obtained by adding the nanomaterial in the form of an aqueous dispersion to an anhydrosugar alcohol, mixing the nanomaterial, melting the mixture while removing water at a temperature equal to or higher than the melting point of the anhydrosugar alcohol, and then cooling the molten mixture to room temperature.
11. The method for producing a polycarbonate composite described in claim 9, wherein the molten dispersion of the anhydrous sugar alcohol is obtained by adding the nanomaterial in the form of an aqueous dispersion to the anhydrous sugar alcohol, mixing the nanomaterial, and melting the nanomaterial while removing moisture at a temperature equal to or higher than the melting point of the anhydrous sugar alcohol.
12. A molded article comprising the polycarbonate composite according to any one of claims 1 to 8.
Citation Information
Patent Citations
Cellulose fiber composite material and method for producing it
JP2009167296A
Dispersion containing polysaccharide nanofibers, dispersion medium, and monomer; and resin composition obtained from said dispersion
JP2016153470A
Polycarbonate-nanocellulose composite material and method for preparing the same
KR102116440B1